Liquid metal conductive slurry and preparation method thereof, and electronic device
Through the combination of solid powder coating liquid metal droplets, conductive powder, and basic resin, the problem of liquid metal seepage in the composite conductive slurry is solved, the flexibility and conductivity of the conductive lines are improved, and a higher Resistant to bending and stretching.
Patent Information
- Application Number
- CN201911376461.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-12-27
AI Technical Summary
Existing composite conductive pastes can easily cause liquid metal to leak out after molding, causing contamination and short-circuit risks, while reducing the flexibility and conductivity of conductive lines.
Liquid metal solid-supported powder is used, in which liquid metal droplets are coated with solid-supported powder. Combined with conductive powder, basic resin and solvent, the liquid metal conductive slurry is prepared through specific proportions and processes to ensure that the liquid metal is exposed to conductive lines. It is not easy to seep out when bent, stretched or twisted.
It effectively reduces the risk of liquid metal seepage, ensures the flexibility and conductivity of conductive lines, avoids the risk of pollution and short circuits, and improves the overall performance of conductive lines.
Smart Images

Figure CN113053559B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new materials, and in particular to a liquid metal conductive paste and a preparation method thereof, and an electronic device. Background Art
[0002] In recent years, with the rapid development of electronic information technology, the market has increasingly stringent requirements on the specificity and functionality of conductive materials. Conductive materials have gradually evolved from the original single materials such as metals and carbon to composite conductive pastes. In addition, there are higher requirements for the bending, stretching and twisting resistance of composite conductive pastes after molding. Traditional composite conductive pastes are mostly made of solid conductive media and carrier materials. For example, conductive particles such as silver powder, copper powder, carbon powder, graphene, etc. are compounded with epoxy resin, acrylic resin, polyurethane resin, vinyl chloride-vinyl acetate copolymer resin, silicone resin, etc. However, such composite conductive pastes are generally difficult to have good flexibility, such as bending resistance and stretching resistance.
[0003] In the prior art, liquid metal that is liquid at room temperature is added to the composite conductive slurry to improve its bending and stretching resistance. However, the inventors found that during the use of the above-mentioned composite conductive slurry, the liquid metal is easy to seep out during the winding and stacking of the conductive circuit after solidification, which not only causes pollution but also has a certain short circuit risk. In addition, the seepage of liquid metal will reduce the content of liquid metal in the conductive circuit, thereby reducing the flexibility and conductivity of the conductive circuit. Summary of the invention
[0004] The present invention provides a liquid metal conductive slurry and a preparation method thereof, and an electronic device, which can reduce the risk of liquid metal seepage and ensure that the manufactured conductive circuit has good flexibility and conductivity.
[0005] In a first aspect, the present invention provides a liquid metal conductive slurry, which adopts the following technical solution:
[0006] The liquid metal conductive slurry comprises:
[0007] Liquid metal solid-supported powder, the liquid metal solid-supported powder comprising liquid metal droplets and solid-supported powder coated on the outside of the liquid metal droplets, the melting point of the liquid metal in the liquid metal droplets being lower than room temperature;
[0008] Conductive powder;
[0009] Base resin;
[0010] Solvents;
[0011] Additives.
[0012] Optionally, the liquid metal conductive slurry is composed of 1% to 60% of liquid metal solid powder, 30% to 70% of conductive powder, 0.1% to 2% of additives, 1% to 10% of base resin and 2% to 30% of solvent, in weight percentage.
[0013] Furthermore, the weight ratio of the liquid metal to the solid-supported powder in the liquid metal solid-supported powder is 1:1 to 100:1.
[0014] Optionally, the solid-supported powder includes one or more of fumed silica, silicon aerogel, carbon aerogel, graphene, carbon nanotubes, carbon black, graphite, fullerene, diatomaceous earth, wollastonite, and sepiolite.
[0015] Optionally, the liquid metal is a gallium-indium alloy, a gallium-tin alloy, a single gallium, a gallium-indium-tin alloy or a gallium-indium-tin-zinc alloy.
[0016] Optionally, the diameter of the liquid metal droplet is 0.1 μm to 10 μm.
[0017] Optionally, the base resin is one or more of polyester resin, polyurethane resin, polyacrylic resin, vinyl chloride vinyl acetate resin, epoxy resin, epoxy acrylic resin, epoxy acrylate resin, polyester acrylate resin, phenolic resin, nitrocellulose, ethyl cellulose, alkyd resin, and amino resin.
[0018] Optionally, the conductive powder is one or more of silver powder, copper powder, silver-coated copper powder, iron powder, and iron-nickel powder.
[0019] In a second aspect, the present invention provides a method for preparing a liquid metal conductive slurry, which adopts the following technical solution:
[0020] The preparation method of the liquid metal conductive slurry comprises:
[0021] Step S1, weighing liquid metal and solid support powder in proportion, dispersing the liquid metal into liquid metal droplets after treatment, and coating the solid support powder on the outside of the liquid metal droplets;
[0022] Step S2, weighing the conductive powder and mixing it with the material obtained in step S1;
[0023] Step S3, using a solvent to dissolve the base resin into a uniform resin solution;
[0024] Step S4, weighing the resin solution and the auxiliary agent according to a ratio, and adding the auxiliary agent to the resin solution;
[0025] Step S5, uniformly mixing the material obtained in step S4 and the material obtained in step S2 in proportion to obtain liquid metal conductive slurry.
[0026] Furthermore, in the step S1, the solid-supported powder is coated on the outside of the liquid metal droplet by centrifugal dispersion or ball milling.
[0027] In a third aspect, the present invention provides an electronic device, which adopts the following technical solution:
[0028] The electronic device comprises a conductive circuit, and the conductive circuit is made of any of the liquid metal conductive pastes described above.
[0029] The present invention provides a liquid metal conductive slurry and a preparation method thereof, and an electronic device. Since the liquid metal conductive slurry includes liquid metal solid powder, conductive powder, base resin, solvent and additive, and since liquid metal droplets in the liquid metal solid powder are coated by the solid powder outside thereof, during the processes of winding and stacking of the conductive circuit made of the composite conductive slurry after solidification, the liquid metal is not easy to seep out, will not cause pollution, and there is no risk of short circuit. In addition, the content of liquid metal in the conductive circuit will not be reduced, thereby effectively ensuring the flexibility and conductivity of the conductive circuit. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0031] Figure 1 A flow chart of a method for preparing liquid metal conductive paste provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] It should be noted that the various technical features in the embodiments of the present invention can be combined with each other without conflict.
[0034] An embodiment of the present invention provides a liquid metal conductive paste. Specifically, the liquid metal conductive paste includes: liquid metal solid powder, the liquid metal solid powder includes liquid metal droplets and solid powder coated on the outside of the liquid metal droplets, the melting point of the liquid metal in the liquid metal droplets is lower than room temperature; solid powder, the solid powder coated on the outside of the liquid metal droplets; conductive powder; base resin; solvent; additives.
[0035] Among them, liquid metal, as a conductive material, is mainly used to improve the electrical properties of the conductive circuit made of the above-mentioned liquid metal conductive paste when it is stretched, bent or twisted; the solid support powder is mainly used to coat the liquid metal so that it will not seep out before the conductive circuit is stretched, bent or twisted; the conductive powder, as a conductive material, is mainly used to improve the electrical properties of the liquid metal conductive paste; the base resin, as a film-forming material, is mainly used to enable the liquid metal conductive paste to be formed and adhere to the substrate; the solvent is mainly used to adjust the viscosity and fluidity of the base resin; the additive is mainly used to make the liquid metal conductive paste have better comprehensive performance.
[0036] Since the solid-supported powder is coated on the outside of the liquid metal droplets, the liquid metal is not easy to seep out during the process of winding and stacking the conductive circuit made of the composite conductive slurry after solidification, and there will be no pollution or short circuit risk. In addition, the content of liquid metal in the conductive circuit will not be reduced, thereby effectively ensuring the flexibility and conductivity of the conductive circuit.
[0037] When the conductive circuit made of the above-mentioned liquid metal conductive slurry is bent, stretched, or twisted, the solid powder shell covering the liquid metal droplets will be destroyed, releasing the liquid metal. Since the melting point of the liquid metal is lower than room temperature, it has good fluidity and deformation ability. The released liquid metal can fill the conductive channel well, thereby reducing the resistance change of the conductive circuit when it is bent, stretched, or twisted, and can improve the flexibility of the conductive circuit.
[0038] The liquid metal conductive paste in the embodiment of the present invention can be applied to molding processes such as screen printing, flexographic printing, transfer printing, extrusion dispensing, and steel screen printing. After molding, the conductive circuit can be obtained after heating and curing. No phase separation or metal overflow occurs during the molding process. The liquid metal conductive paste in the embodiment of the present invention can be molded on a variety of non-metallic substrates such as PET, PVC, PI, PMMA, PC, ABS, PE, PP, PU, etc., and can meet the functional requirements of liquid metal conductive paste in different fields of modern industry.
[0039] The following embodiments of the present invention provide detailed descriptions of the specific components in the liquid metal conductive paste.
[0040] Combined with the functions of the components described above, it can be seen that if there is too little liquid metal in the liquid metal conductive slurry, the content of effective conductive material in the conductive material will be reduced, and the conductive performance of the conductive circuit when bent, stretched, or twisted will be reduced. If there is too much liquid metal, the initial resistance of the conductive circuit (the resistance when not bent, stretched, or twisted) will be larger; if there is too little solid powder in the liquid metal conductive slurry, it will be difficult for the powder attached to completely cover the liquid metal, and there is still a risk of seepage. If there is too much solid powder, the outer shell of the solid powder is not easily destroyed when the conductive circuit is bent, stretched, or twisted, which is not conducive to improving its flexibility and will increase the initial resistance of the conductive circuit; if there is too much conductive powder in the liquid metal conductive slurry, the flexibility of the conductive circuit will be poor. If there is too little conductive powder, the initial resistance of the conductive circuit will be higher. If there is too much base resin in the liquid metal conductive slurry, the initial resistance of the conductive circuit will be higher. If there is too little base resin, the molding ability of the conductive circuit will be poor.
[0041] Based on the above, in the embodiment of the present invention, the liquid metal conductive slurry is composed of 1% to 60% of liquid metal solid powder, 30% to 70% of conductive powder, 0.1% to 2% of additives, 1% to 10% of base resin and 2% to 30% of solvent, calculated by weight percentage, so that the conductive circuit made of liquid metal conductive slurry has excellent comprehensive properties (such as molding characteristics, initial electrical properties, flexibility, etc.).
[0042] Exemplarily, the weight percentage of the liquid metal solid powder in the liquid metal conductive paste is 1%, 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%; the weight percentage of the conductive powder in the liquid metal conductive paste is 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65% or 70%; the base resin in the liquid metal conductive paste is 10%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65% or 70%. The weight percentage of the liquid metal conductive paste is 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%; the weight percentage of the solvent in the liquid metal conductive paste is 2%, 5%, 10%, 12%, 15%, 17%, 20%, 24%, 27% or 30%; the weight percentage of the additive in the liquid metal conductive paste is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.7%, 1%, 1.5% or 2%.
[0043] Preferably, the solid-supported powder in the embodiment of the present invention is a powder with light weight and large specific surface area, so that it has a better coating effect on the liquid metal. Optionally, the particle size of the solid-supported powder ranges from 7nm to 4μm, and the specific surface area is 100m 2 / g~3000m 2 / g. Exemplarily, the solid support powder in the embodiment of the present invention includes one or more of fumed silica, silicon aerogel, carbon aerogel, graphene, carbon nanotubes, carbon black, graphite, fullerene, diatomaceous earth, wollastonite, and sepiolite.
[0044] Optionally, the liquid metal in the embodiment of the present invention is a metal element or alloy having a melting point lower than room temperature, such as a gallium-indium alloy, a gallium-tin alloy, a gallium element, a gallium-indium-tin alloy, or a gallium-indium-tin-zinc alloy.
[0045] Optionally, the diameter of the liquid metal droplets in the embodiment of the present invention is 0.1μm to 10μm. Among them, when the diameter of the liquid metal microcapsule is less than 0.1μm, it is difficult to prepare, and the liquid metal microcapsule is difficult to break under the bending destructive force, and then there is a failure to compensate for the resistance increase caused by the reduction of effective contact of the conductive powder; when the diameter of the liquid metal droplet is greater than 10μm, the liquid metal droplet has a large specific gravity, severe phase separation, and is mainly deposited at the bottom of the forming coating, with too little surface distribution. In addition, when the liquid metal droplets with too large a diameter increase further, a certain number of liquid metal droplets will be destroyed in advance during the forming process. The outer shell of the solid powder coated is destroyed, which will not only reduce the overall adhesion of the liquid metal conductive slurry, but also easily cause short circuit risks when making complex patterns with low line spacing, and increase the resistance change of the conductive line during bending, stretching or twisting.
[0046] Optionally, the base resin in the embodiment of the present invention is one or more of polyester resin, polyurethane resin, polyacrylic resin, vinyl chloride vinyl acetate resin, epoxy resin, epoxy acrylic resin, epoxy acrylate resin, polyester acrylate resin, phenolic resin, nitrocellulose, ethyl cellulose, alkyd resin, and amino resin. The reason for selecting the above base resin is that, on the one hand, the above base resin can stably exist with liquid metal for a long time, and the pH is close to neutral, there is no strong alkaline or acidic component, and no significant chemical reaction occurs with liquid metal. On the other hand, the above base resin can ensure that the liquid metal conductive paste has good fusion and no significant phase separation.
[0047] Optionally, the conductive powder in the embodiment of the present invention includes one or more of silver powder, copper powder, silver-coated copper powder, iron powder, and iron-nickel powder. Exemplarily, the conductive powder can be flaky silver powder, spherical silver powder, rod-shaped silver powder, needle-shaped silver powder, dendritic silver powder, etc.
[0048] Optionally, the solvent in the embodiment of the present invention is one or more of ethyl acetate, butyl acetate, isoamyl acetate, n-butyl glycolate, petroleum ether, acetone, butanone, cyclohexanone, methyl isobutyl ketone, diisobutyl ketone, toluene, xylene, butyl carbitol, alcohol ester 12, DBE, ethylene glycol butyl ether, ethylene glycol ethyl ether, dipropylene glycol methyl ether, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, ethylene glycol butyl ether acetate, n-hexane, cyclohexane, n-heptane, n-octane, and isooctane.
[0049] Optionally, the auxiliary agent in the embodiment of the present invention may include one or more of a dispersant, a wetting agent, a defoamer, a leveling agent, etc. The dispersant includes one or more of an anionic surfactant, a nonionic surfactant and a polymer surfactant.
[0050] In addition, an embodiment of the present invention further provides an electronic device, the electronic device includes a conductive circuit, and the conductive circuit is made of any of the liquid metal conductive slurries described above. The above-mentioned electronic device can be any electronic device that requires a conductive circuit, such as a flexible sensor, a wearable device, a flexible electronic tag, an FPC circuit board, etc., and is particularly suitable for electronic devices that require a flexible conductive circuit.
[0051] In addition, the embodiment of the present invention also provides a method for preparing a liquid metal conductive paste, which is used to prepare the liquid metal conductive paste described above. Figure 1 As shown, Figure 1 The present invention provides a flow chart of a method for preparing a liquid metal conductive paste according to an embodiment of the present invention. The method for preparing a liquid metal conductive paste includes:
[0052] Step S1, weighing liquid metal and solid support powder in proportion, dispersing the liquid metal into liquid metal droplets after treatment, and coating the solid support powder on the outside of the liquid metal droplets;
[0053] Optionally, in step S1, the solid-supported powder is coated on the outside of the liquid metal droplet by centrifugal dispersion or ball milling.
[0054] Step S2, weighing the conductive powder and mixing it with the material obtained in step S1;
[0055] Step S3, using a solvent to dissolve the base resin into a uniform resin solution;
[0056] Step S4, weighing the resin solution and the auxiliary agent according to a ratio, and adding the auxiliary agent to the resin solution;
[0057] Step S5, uniformly mixing the material obtained in step S4 and the material obtained in step S2 in a certain proportion to obtain liquid metal conductive slurry.
[0058] Optionally, in step S5, the material obtained in step S4 and the material obtained in step S2 can be first loaded into a sealed container in a certain proportion, then pre-dispersed using a mixer, and then processed using a three-axis roller mill, and finally the bubbles in the mixture are removed using a vacuum degassing machine to obtain liquid metal conductive slurry.
[0059] The liquid metal conductive paste prepared by the above-mentioned preparation method of the liquid metal conductive paste has relatively excellent comprehensive performance, and the main reasons include the following aspects:
[0060] Firstly, in the process of preparing liquid metal conductive paste, when dispersing the liquid metal in step S1, the coating of the solid support powder makes it easier to disperse the liquid metal into smaller droplets, thereby improving the uniformity of the liquid metal distribution in the liquid metal conductive paste.
[0061] On the other hand, since the liquid metal is coated with solid support powder, the liquid metal will not directly contact the conductive powder in step S2, thus avoiding the reaction between the liquid metal and the conductive powder, and increasing the stability of the liquid metal in the process of making the liquid metal conductive slurry. If the liquid metal is in direct contact with the conductive powder, the liquid metal will have a significant wetting and coating effect on the conductive powder in various "high-energy" processing processes (such as stirring, ball milling, sand milling, three-roller grinding, etc.). During the high-speed movement of the conductive powder, the conductive powder will collide with each other and quickly merge with the wetting and coating effect of the liquid metal, and / or the liquid metal changes the original spreading state of the wetting dispersant in the resin system in the solvent and the resin, causing the resin to rapidly change its morphology and flocculate into units with extremely small surface areas, which cannot provide physical barriers and stable double-layer structures for the conductive powder, causing the conductive powder to agglomerate.
[0062] It should be noted that the order of step S3 and step S4, and step S1 and step S2 is not limited, and those skilled in the art can select according to actual needs.
[0063] In order to facilitate understanding and implementation by those skilled in the art, the following embodiments of the present invention provide several specific embodiments.
[0064] Embodiment 1:
[0065] composition type Dosage(g) Liquid Metal Gallium Indium Tin Eutectic Alloy 25 Solid powder Graphene 1 Conductive powder Flake silver powder 75 Base resin Polyurethane resin 6.25 Solvents Ethylene glycol butyl ether acetate 18.75 Defoaming agent Silicone defoamer 0.63
[0066] The viscosity of the obtained liquid metal conductive paste is 59000cp, no diluent is added, and after molding, it is thermally cross-linked at 160°C. The square resistance of the material of Example 1 is 29mΩ (25.4 microns), there is no liquid metal seepage during the molding process, and the pattern has strong resistance to liquid metal seepage after drying, and there is only slight discoloration at the part wiped by the glove.
[0067] Embodiment 2:
[0068] composition type Dosage(g) Liquid Metal Gallium Indium Tin Eutectic Alloy 50 Solid powder Fumed Silica 0.5 Conductive powder Flake silver powder 75 Base resin Polyurethane resin 6.25 Solvents Diethylene glycol butyl ether acetate 18.75 Defoaming agent Silicone defoamer 0.75
[0069] The viscosity of the obtained liquid metal conductive paste is 55000cp, no diluent is added, and after molding, it is thermally cross-linked at 160°C. The square resistance of the material of Example 2 is 27mΩ (25.4 microns), there is no liquid metal seepage during the molding process, and the pattern has strong resistance to liquid metal seepage after drying, and there is only slight discoloration at the part wiped by the glove.
[0070] Embodiment 3:
[0071] composition type Dosage(g) Liquid Metal Gallium Indium Tin Eutectic Alloy 25 Solid powder Graphene 0.25 Conductive powder Flake silver powder 75 Base resin Polyurethane resin 6.25 Solvents Ethylene glycol butyl ether acetate 18.75 Defoaming agent Silicone defoamer 0.63
[0072] The viscosity of the obtained liquid metal conductive paste is 57000cp, no diluent is added, and after molding, it is thermally cross-linked at 160°C. The square resistance of the material of Example 3 is 30mΩ (25.4 microns), there is no liquid metal seepage during the molding process, and the pattern has strong resistance to liquid metal seepage after drying.
[0073] Embodiment 4:
[0074] composition type Dosage(g) Liquid Metal Gallium Indium Tin Eutectic Alloy 25 Solid powder Carbon Nanotubes 0.25 Conductive powder Flake silver powder 75 Base resin Polyurethane resin 6.25 Solvents Ethylene glycol butyl ether acetate 18.75 Defoaming agent Silicone defoamer 0.63
[0075] The viscosity of the obtained liquid metal conductive paste is 54000cp, no diluent is added, and after molding, it is thermally cross-linked at 160°C. The square resistance of the material of Example 4 is 30mΩ (25.4 microns), there is no liquid metal seepage during the molding process, and the pattern has strong resistance to liquid metal seepage after drying.
[0076] Comparative Example 1
[0077] composition type Dosage(g) Liquid Metal Gallium Indium Tin Eutectic Alloy 25 Conductive powder Flake silver powder 75 Base resin Polyurethane resin 6.25 Solvents Ethylene glycol butyl ether acetate 18.75 Defoaming agent Silicone defoamer 0.63
[0078] The preparation method of liquid metal conductive slurry comprises:
[0079] Step S1, dissolving polyurethane resin and ethylene glycol butyl ether acetate in a ratio of 1:3 into a uniform solution;
[0080] Step S2, weigh 25 g of the resin solution obtained in step S1, add 0.63 g of an organosilicon defoamer, and disperse evenly by mechanical stirring;
[0081] Step S3, weighing 75 g of silver powder and adding it to the material obtained in step S2;
[0082] Step S4, dispersing using a stirrer;
[0083] Step S5, weighing 25 g of liquid metal and adding it to the material obtained in step S4;
[0084] Step S6, dispersing using a stirrer;
[0085] Step S7: After the mixing is completed, the above materials are processed by a three-axis rolling mill.
[0086] Step S8: removing bubbles from the mixture by vacuum degassing.
[0087] The viscosity of the obtained liquid metal conductive slurry is 43000cp, and no diluent is added. After molding, it is thermally cross-linked at 160°C. The square resistance of the material of comparative example 1 is 25mΩ (25.4 microns). There is no liquid metal seepage during the molding process, but there is obvious liquid metal seepage when the pattern is wiped after drying, and the glove wiped part is seriously discolored.
[0088] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A liquid metal conductive paste, It is characterized in that The liquid metal conductive paste is composed of 1% to 60% of liquid metal solid-carrying powder, 30% to 70% of conductive powder, 0.1% to 2% of additives, 1% to 10% of base resin and 2% to 30% of solvent by weight percentage; The weight ratio of liquid metal to solid support powder in the liquid metal solid support powder is 1:1 to 100:1; the solid support powder includes one or more of fumed silica, silicon aerogel, carbon aerogel, graphene, carbon nanotubes, carbon black, graphite, fullerene, diatomaceous earth, wollastonite, and sepiolite; the diameter of the liquid metal droplet is 0.1 μm to 10 μm; The base resin is one or more of polyester resin, polyurethane resin, polyacrylic resin, vinyl chloride vinyl acetate resin, epoxy resin, epoxy acrylic resin, epoxy acrylate resin, polyester acrylate resin, phenolic resin, nitrocellulose, ethyl cellulose, alkyd resin, and amino resin.
2. The liquid metal conductive paste according to claim 1, It is characterized in that The conductive powder is one or more of silver powder, copper powder, silver-coated copper powder, iron powder, and iron-nickel powder.
3. The method for preparing the liquid metal conductive paste according to claim 1 or 2, It is characterized in that include: Step S1, weighing liquid metal and solid support powder in proportion, dispersing the liquid metal into liquid metal droplets after treatment, and coating the solid support powder on the outside of the liquid metal droplets; Step S2, weighing the conductive powder and mixing it with the material obtained in step S1; Step S3, using a solvent to dissolve the base resin into a uniform resin solution; Step S4, weighing the resin solution and the auxiliary agent according to a ratio, and adding the auxiliary agent to the resin solution; Step S5, uniformly mixing the material obtained in step S4 and the material obtained in step S2 in proportion to obtain liquid metal conductive slurry.
4. The method for preparing the liquid metal conductive paste according to claim 3, It is characterized in that In the step S1, the solid-supported powder is coated on the outside of the liquid metal droplet by centrifugal dispersion or ball milling.
5. An electronic device, It is characterized in that It comprises a conductive circuit, wherein the conductive circuit is made of the liquid metal conductive paste according to claim 1 or 2.
Citation Information
Patent Citations
High-conductivity silver paste and preparation method thereof
CN105632588A
Conducting ink and preparation method thereof
CN106479272A
Electronic paste based on low-melting-point metal micro-nano powders and manufacture method thereof
CN107274965A
Conductive powder-liquid metal droplet and preparation method and application thereof
CN107452434A
Low cost recyclable conductive paste and preparation method thereof
CN107578838A