Crosslinking type conductive binder, negative pole piece and lithium ion battery

Through the combination of cross-linked conductive adhesive and dispersant, the conductive capacity and volume expansion problems of silicon materials are solved, forming a complete conductive network and high mechanical properties, and improving the cycle stability and capacity retention rate of lithium-ion batteries.

CN118978876APending Publication Date: 2024-11-19JIANGSU RELIANCE ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411049023.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Silicon materials are weak in conductivity as semiconductor materials on the negative electrode of lithium-ion batteries, and volume expansion during charging and discharging leads to increased stress, destroying the interface of solid electrolyte, causing irreversible capacity loss, and existing adhesives are easy to circulate during the cycle. Slide to reduce electrode stability.

Method used

The cross-linked conductive adhesive is used to form a three-dimensional cross-linking network through the amide bond connection of conductive agents such as conductive carbon black, carbon nanotubes, graphene and polyether cross-linking to improve the dispersion ability and adhesion of the conductive agent. Carboxymethyl cellulose is added as a dispersant to the negative electrode sheet to enhance mechanical properties.

Benefits of technology

It improves the integrity and mechanical properties of the conductive network, ensures the long-term cycle stability and electrode integrity of the negative electrode, and enhances the cycle performance and capacity retention rate of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978876A_ABST
    Figure CN118978876A_ABST
Patent Text Reader

Abstract

On the first aspect, the cross-linked conductive adhesive is provided and obtained by modifying a conductive agent, the modified conductive agent is connected with carbon chains through amido bonds, and at least two carbon chains are cross-linked through polyether. In the second aspect and the third aspect, the invention provides a negative pole piece and a preparation method thereof, the negative pole piece comprises a current collector, and at least one surface of the current collector is provided with a negative active material layer; the negative active material layer includes a first cross-linked conductive binder. Based on the defects of a silicon material in a negative pole piece, the cross-linked conductive binder is provided, the dispersing capacity of the conductive agent is improved by grafting the conductive agent to the polymer binder in situ, a three-dimensional cross-linked structure formed through cross-linking enables a conductive network to be more complete and higher in mechanical performance, meanwhile, the flexibility of the pole piece is guaranteed, and the service life of the pole piece is prolonged. And the long-term stability and the electrode integrity of the silicon-containing negative electrode in the circulation process are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a cross-linked conductive adhesive, a negative electrode sheet and a lithium-ion battery. Background Art

[0002] The cylindrical lithium battery includes a cylindrical steel shell, the interior of which is used to accommodate the battery core. The battery core is formed by winding the positive electrode sheet, the negative electrode sheet and the diaphragm. The negative electrode sheet includes a negative electrode coating area, and the negative electrode coating contains a negative electrode active material, mainly graphite. In order to increase the energy density, silicon material can also be introduced into the negative electrode active material to obtain a silicon-based negative electrode, which is an ideal negative electrode for high specific energy lithium-ion batteries with a theoretical capacity of up to 4200mAh / g.

[0003] However, there are two main problems to be solved when using silicon materials as negative electrodes. First, silicon, as a semiconductor material, has weak electrical conductivity. Second, silicon negative electrode materials will experience a huge volume expansion during the charge and discharge process, up to 300%. The huge volume expansion will produce greater stress, causing the active material and the current collector to separate, resulting in capacity loss, and will also destroy the solid electrolyte interface film (SEI), causing the electrolyte to directly contact the silicon, forming an unstable SEI film, which will then consume lithium ions and electrolyte, causing irreversible capacity loss.

[0004] In order to solve the problem of weak conductivity of silicon negative electrode materials, it is necessary to use a conductive agent in the negative electrode coating, usually an inorganic conductive agent, which has poor dispersibility in water and high molecular polymers and is easy to agglomerate in the negative electrode slurry, so that a complete conductive network cannot be formed, and polarization increases. In order to achieve long-term cycle stability and good electrode integrity of silicon-based negative electrodes, a binder is also needed. Poly(acrylic acid) (PAA) has a high density of -COOH polar groups and has strong interfacial adhesion with the hydroxyl groups on the silicon surface. PAA belongs to linear bonding, with a higher degree of anchoring to particles and stronger cohesion of the pole piece. However, the linear chain nature of polymer binders makes them easy to slide during the continuous volume expansion and contraction of Si electrodes, thereby reducing the stability and integrity of the electrode during the cycle. The three-dimensional (3D) cross-linked network can enhance the mechanical properties of these linear binders to achieve long-term cycle stability and good electrode integrity of silicon negative electrodes during the cycle. In addition, PAA material is relatively brittle and the electrode has poor flexibility. Styrene-butadiene rubber (SBR) is usually added in the process for compounding. However, SBR has fewer polar groups than PAA, and compounding will inevitably lead to weakened bonding strength. Summary of the invention

[0005] To solve the above problems, the first aspect of the present invention provides a cross-linked conductive adhesive, which is obtained by modifying a conductive agent, wherein the conductive agent is selected from a mixture of one or more of conductive carbon black, carbon nanotubes, graphene, and graphite; the conductive agent connects carbon chains through amide bonds, and at least two carbon chains are cross-linked through polyether.

[0006] In some embodiments, the cross-linked conductive adhesive has a structure as shown in Formula I: Wherein A is the conductive agent, R is selected from at least one of cyano, phenyl, carboxyl, and ester groups, x and y are integers greater than or equal to 100, and a is an integer greater than or equal to 3.

[0007] In some embodiments, the method for preparing a cross-linked conductive adhesive comprises the following steps:

[0008] S1: reacting the conductive agent with an oxidant to obtain a carboxylated conductive agent;

[0009] S2: reacting the carboxylated conductive agent with an acylating agent to obtain an acylated conductive agent;

[0010] S3: reacting the acylated conductive agent with a vinyl modifier to obtain a vinyl conductive agent;

[0011] S4: reacting the vinyl conductive agent with a vinyl monomer and an initiator to obtain a linear graft-modified conductive agent;

[0012] S5: reacting the linear graft modified conductive agent with a crosslinking agent to obtain a crosslinked conductive adhesive.

[0013] In some embodiments, in step S1, the mass ratio of the conductive agent to the oxidant is 1:(100-200), the reaction temperature is 80-100°C, and the reaction time is 18-36h; the oxidant is concentrated nitric acid, and the mass fraction of concentrated nitric acid is 60%-80%.

[0014] In some embodiments, in step S2, the mass ratio of the carboxylated conductive agent to the acylating agent is 1:(700-900), the reaction temperature is 60-75°C, the reaction time is 20-40h; and the acylating agent is thionyl chloride.

[0015] In some embodiments, in step S3, the mass ratio of the acylated conductive agent to the vinyl modifier is 1:(0.5-2), the reaction temperature is 60-80° C., and the reaction time is 50-80 h; the vinyl modifier is allylamine.

[0016] In some embodiments, in step S4, based on the total mass of the vinyl conductive agent, the vinyl monomer, and the initiator as 100%, the vinyl conductive agent accounts for 10%-15%, the initiator accounts for 0.1%-1%, and the rest is the vinyl monomer. The reaction temperature of the three is 60-100°C, and the reaction time is 36-72h; the vinyl monomer is selected from a mixture of one or more of acrylic acid, methyl acrylate, butyl acrylate, butyl methacrylate, styrene, and acrylonitrile; the initiator is selected from one of dibenzoyl peroxide, azobisisobutyronitrile, and ammonium persulfate.

[0017] In some embodiments, in step S5, based on the total mass of the linear grafted modified conductive agent and the cross-linking agent as 100%, the linear grafted modified conductive agent accounts for 85%-95%, the cross-linking agent accounts for 5%-15%, the reaction temperature of the two is 100-150°C, and the reaction time is 2-4h; the cross-linking agent is selected from a mixture of one or more of polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.

[0018] The second aspect of the present invention provides a negative electrode plate, including a current collector, at least one surface of the current collector is provided with a negative electrode active material layer; the negative electrode active material layer includes 2%-7% of the above-mentioned cross-linked conductive binder, 0.5%-1% of the dispersant, and the balance is the negative electrode active material; the negative electrode active material includes 60%-95% of the carbon material and 5%-40% of the silicon material by weight; the dispersant is lithium carboxymethyl cellulose and / or sodium carboxymethyl cellulose.

[0019] In some embodiments, the carbon material is selected from a mixture of one or more of artificial graphite, natural graphite, and hard carbon; the silicon material is selected from a mixture of one or more of silicon-carbon material, silicon oxide, and pure silicon.

[0020] The third aspect of the present invention provides a method for preparing the above-mentioned negative electrode sheet, comprising the following steps: wet mixing a linear graft modified conductive agent, a negative electrode active material, a cross-linking agent, and a dispersant to obtain a negative electrode slurry, coating the negative electrode slurry on at least one surface of a current collector, and drying, rolling, and vacuum high-temperature drying to obtain a negative electrode sheet.

[0021] A fourth aspect of the present invention provides a lithium-ion battery comprising the above-mentioned negative electrode plate.

[0022] Based on the defects of silicon materials in negative electrode active materials, this application improves the binder in the negative electrode active material layer and proposes a cross-linked conductive binder. By in-situ grafting the conductive agent to the polymer binder, on the one hand, the dispersion ability of the conductive agent is improved, and on the other hand, the binder has better bonding force and better ionic conductivity. The three-dimensional cross-linked structure formed by cross-linking makes the conductive network more complete and the mechanical properties higher, while ensuring the flexibility of the pole piece, and realizing the long-term stability and electrode integrity of the silicon-containing negative electrode during the cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the description of the present application will be briefly introduced below.

[0024] Figure 1 It is a schematic diagram of the structure of a cylindrical lithium battery in this application;

[0025] Figure 2 It is a schematic diagram of the structure of the battery roll core in this application;

[0026] Figure 3 is a schematic diagram of the unfolding of the battery roll core in this application;

[0027] Figure 4 The figure is a comparison of the cycle performance test results of Example 3 of the present application and Comparative Examples 1 and 2.

[0028] Figure numerals: 1-positive terminal, 11-positive electrode column, 2-negative terminal, 3-steel shell, 4-battery roll core, 5-positive electrode sheet, 6-diaphragm, 7-negative electrode sheet. DETAILED DESCRIPTION

[0029] Examples of the present embodiment are described in detail below. The examples are only used to explain the present embodiment and are not to be construed as limiting the present embodiment.

[0030] In the description of this embodiment, "several" means one or more, "more" means more than two, "greater than", "less than", "exceed", etc. are understood to exclude the number, and "above", "below", "within", etc. are understood to include the number.

[0031] Figure 1 A schematic structural diagram of a cylindrical lithium battery in the present application is shown. The cylindrical lithium battery includes a cylindrical steel shell 3, the interior of which is used to accommodate a battery coil core 4; the top of the cylindrical lithium battery is a positive terminal 1, the bottom is a negative terminal 2, and a positive electrode column 11 is arranged on the positive terminal 1. Figure 2 The schematic diagram of the structure of the battery roll core 4 in this application is shown. Figure 3 The schematic diagram of the battery roll core in the present application is shown, and the positive electrode sheet 5, the negative electrode sheet 7 and the separator 6 are shown in FIG. Figure 3 As shown in the stacking, then winding to form Figure 2The battery winding core 4 is shown as being cylindrical.

[0032] The negative electrode plate includes a negative electrode coating area, and the negative electrode coating contains negative electrode active materials, mainly carbon materials, such as graphite. In order to increase the battery capacity of lithium-ion batteries, silicon materials can be introduced into the negative electrode active materials. However, the poor conductivity and volume expansion of silicon materials have hindered the application of silicon materials in lithium-ion batteries.

[0033] In order to solve the problems existing in silicon-containing negative electrodes, the first aspect of the present invention provides a cross-linked conductive binder obtained by modifying a conductive agent, wherein the conductive agent is selected from a mixture of one or more of conductive carbon black, carbon nanotubes, graphene, and graphite; the conductive agent connects carbon chains through amide bonds, and at least two carbon chains are cross-linked through polyether. Specifically, the cross-linked conductive binder has a structure as shown in Formula I, Formula I: Wherein A is the conductive agent, R is selected from at least one of cyano, phenyl, carboxyl, and ester, x and y are integers greater than or equal to 100, and a is an integer greater than or equal to 3. It can be understood that the R group depends on the vinyl monomer used for grafting modification, and when at least one vinyl monomer is used to participate in the reaction, the R group is a corresponding type.

[0034] The preparation method of the cross-linked conductive adhesive comprises the following steps:

[0035] S1: reacting the conductive agent with an oxidant to obtain a carboxylated conductive agent;

[0036] S2: reacting the carboxylated conductive agent with an acylating agent to obtain an acylated conductive agent;

[0037] S3: reacting the acylated conductive agent with a vinyl modifier to obtain a vinyl conductive agent;

[0038] S4: reacting the vinyl conductive agent with a vinyl monomer and an initiator to obtain a linear graft-modified conductive agent;

[0039] S5: reacting the linear graft modified conductive agent with a crosslinking agent to obtain a crosslinked conductive adhesive.

[0040] The preparation method of the cross-linked conductive adhesive in the present application first introduces active sites by chemically modifying the surface of the conductive agent, and then cross-linking the polymer monomers by in-situ polymerization growth through free radical polymerization on the surface of the conductive agent. This not only improves the dispersion ability of the conductive agent in the negative electrode slurry, but also the structure formed by the polymer coating the conductive agent makes the conductive network of the adhesive more complete.

[0041] In some embodiments, in step S1, the mass ratio of the conductive agent to the oxidant is 1:(100-200), the reaction temperature is 80-100°C, and the reaction time is 18-36h; the oxidant is concentrated nitric acid and / or concentrated sulfuric acid, and the mass fraction of concentrated nitric acid is 60%-80%.

[0042] Step S1: Treat the conductive agent with a strong oxidant to introduce carboxyl active sites on the surface of the conductive agent, providing a reaction basis for subsequent modification treatment. By controlling the mass ratio of the conductive agent to the oxidant, the reaction temperature, the reaction time and other conditions, it is ensured that the surface of the conductive agent has sufficient reaction sites to improve the reactivity of the conductive agent.

[0043] In some embodiments, in step S2, the mass ratio of the carboxylated conductive agent to the acylating agent is 1:(700-900), the reaction temperature is 60-75°C, and the reaction time is 20-40h; the acylating agent is thionyl chloride (SOCl2).

[0044] In some embodiments, in step S3, the mass ratio of the acylated conductive agent to the vinyl modifier is 1:(0.5-2), the reaction temperature is 60-80° C., and the reaction time is 50-80 h; the vinyl modifier is allylamine.

[0045] Step S2 and step S3 sequentially perform acylation reaction and vinyl reaction on the conductive agent to introduce vinyl groups on the surface of the conductive agent to provide unsaturated bonds for subsequent grafting modification. By controlling the mass ratio of reactants, reaction temperature, and reaction time, the reaction sites on the carboxylated conductive agent are converted into carbon-carbon double bonds to the greatest extent, thereby increasing the number of grafted long chains on the surface of the conductive agent.

[0046] In some embodiments, in step S4, based on the total mass of the vinyl conductive agent, the vinyl monomer, and the initiator as 100%, the vinyl conductive agent accounts for 10%-15%, the initiator accounts for 0.1%-1%, and the rest is the vinyl monomer. The reaction temperature of the three is 60-100°C, and the reaction time is 36-72h; the vinyl monomer is selected from a mixture of one or more of acrylic acid, methyl acrylate, butyl acrylate, butyl methacrylate, styrene, and acrylonitrile; the initiator is selected from one of dibenzoyl peroxide, azobisisobutyronitrile, and ammonium persulfate.

[0047] In step S4, the vinyl monomer is polymerized in situ on the surface of the conductive agent by free radical polymerization with the vinyl conductive agent under the action of the initiator to obtain a conductive agent grafted with a polymerized long chain. The chain length grafted on the surface of the conductive agent is adjusted by limiting the amount of the vinyl monomer, the reaction temperature, the reaction time and other conditions. If the chain length is short, it is difficult to provide a sufficient number of active groups to ensure the bonding force, and it is also impossible to form an effective coating on the conductive agent, thereby affecting the dispersibility of the conductive agent in the negative electrode plate coating; if the chain length is too long, it will affect the strength of the three-dimensional structure after cross-linking, resulting in poor mechanical properties of the conductive adhesive. The vinyl monomer is preferably acrylic acid, so that a linear polyacrylic acid long chain is grafted on the surface of the conductive agent. Polyacrylic acid (PAA) has a high density of -COOH polar groups and has a strong interfacial adhesion with the hydroxyl groups on the silicon surface. PAA belongs to line bonding, has a higher degree of anchoring to the particles, and has a stronger cohesive force on the pole piece.

[0048] However, the linear chain properties of polymer binders make them easy to slide during the continuous volume expansion and contraction of silicon-containing negative electrodes, thereby reducing the stability and integrity of the electrode during the cycle. In addition, PAA materials are relatively brittle, and the flexibility of the coated electrode is poor. The prior art has a solution of adding styrene-butadiene rubber (SBR) for compound use. However, SBR has fewer polar groups than PAA, and compound use will inevitably cause weakening of the bonding force.

[0049] In some embodiments, in step S5, based on the total mass of the linear grafted modified conductive agent and the cross-linking agent as 100%, the linear grafted modified conductive agent accounts for 85%-95%, the cross-linking agent accounts for 5%-15%, the reaction temperature of the two is 100-150°C, and the reaction time is 2-4h; the cross-linking agent is selected from a mixture of one or more of polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.

[0050] Step 5 is a cross-linking reaction, which converts the linear structure into a mesh structure. The three-dimensional (3D) cross-linked network can enhance the mechanical properties of the linear binder to achieve long-term cycling stability and good electrode integrity of the electrode during the cycle. The polyacrylic acid retains the number of carboxyl groups, ensuring excellent bonding performance. Using cross-linkers such as polyethylene glycol as polymer soft segments to adjust the mechanical properties of polyacrylic acid can also improve the brittleness of PAA, enhance elasticity, and thus enhance the flexibility of the negative electrode sheet.

[0051] The second aspect of the present invention provides a negative electrode plate, including a current collector, at least one surface of the current collector is provided with a negative electrode active material layer; the negative electrode active material layer includes 2%-7% of the above-mentioned cross-linked conductive binder, 0.5%-1% of the dispersant, and the remainder is the negative electrode active material; the negative electrode active material includes 60%-95% of the carbon material and 5%-40% of the silicon material; the dispersant is lithium carboxymethyl cellulose (CMC-Li) and / or sodium carboxymethyl cellulose (CMC-Na).

[0052] In some embodiments, the carbon material is selected from a mixture of one or more of artificial graphite, natural graphite, and hard carbon; the silicon material is selected from a mixture of one or more of silicon-carbon material, silicon oxide, and pure silicon. In the present application, the silicon-carbon material may be a carbon-coated silicon material, and the coated silicon material may be crystalline silicon or amorphous silicon. Silicon oxide may be represented by the chemical formula SiO x Indicates, where 0<x≤2, can be obtained from the market, and silicon oxide can also be further treated with carbon coating. Generally speaking, carbon coating can improve the conductivity and stability of silicon materials, and the method of carbon coating can be any method known to those skilled in the art, such as chemical vapor deposition, physical vapor deposition, solution method, etc.

[0053] The third aspect of the present invention provides a method for preparing the above-mentioned negative electrode sheet, comprising the following steps: wet mixing a linear graft modified conductive agent, a negative electrode active material, a cross-linking agent, and a dispersant to obtain a negative electrode slurry, applying the negative electrode slurry to at least one surface of a current collector, and drying, cold pressing, and vacuum high-temperature drying to obtain a negative electrode sheet.

[0054] The step S5 of the cross-linked conductive adhesive of the present application can be selectively completed in the preparation process of the negative electrode plate, that is, the linear grafted modified conductive agent and the cross-linking agent undergo a cross-linking reaction during the high-temperature vacuum drying process of the plate, and finally a negative electrode plate containing the cross-linked conductive adhesive is obtained. This can further simplify the production steps, and cross-linking is formed during the drying process of the negative electrode active coating, which can obtain a more uniform three-dimensional structure and improve the conductive and mechanical properties of the adhesive.

[0055] A fourth aspect of the present invention provides a lithium ion battery, comprising the above-mentioned negative electrode sheet. The preparation method of the lithium ion battery in the present application comprises the following steps:

[0056] (1) Making a positive electrode sheet: taking a positive electrode active material, conductive carbon black, and a binder polyvinylidene fluoride (PVDF) and stirring them in N-methylpyrrolidone to mix them evenly, coating them on an aluminum foil, drying them, and rolling them to obtain a positive electrode sheet;

[0057] (2) Preparation of electrolyte: dissolving lithium salt LiPF6 in an organic solvent to prepare an electrolyte with a concentration of 1 mol / L;

[0058] (3) Assembly: stack the positive electrode sheet, the separator, and the negative electrode sheet in order, weld the positive and negative electrode tabs to obtain an electrode assembly, and place the electrode assembly in an outer packaging aluminum-plastic film to obtain a lithium-ion soft-pack battery.

[0059] The present invention will be further explained with reference to the following examples.

[0060] Example 1

[0061] Example 1 provides a negative electrode sheet, and the preparation method thereof includes the following steps (it can be understood that the mass of the reactants provided in each step of this embodiment is exemplary, and each step can be repeated to provide sufficient reactants for the next step):

[0062] (1) Carboxylation modification of conductive agent

[0063] First, 1g carbon nanotubes (CNT) and 210g (i.e., 150mL) of concentrated HNO3 (mass fraction 67%) solution were added to a round-bottomed bottle and reacted at 100°C for 24h. After cooling to room temperature, the mixture was diluted with 240mL of deionized water and vacuum filtered. The solid was then washed with deionized water until the pH value of the filtrate reached 7, and then the filtered solid was dispersed in 160mL HCl (2mol / L) for 10 hours and vacuum dried at 100°C for 10h to obtain a carboxylic acid functional group conductive agent (CNT-COOH).

[0064] (2) Acylation modification of carbon nanotubes

[0065] 1 g CNT-COOH, 800 g SOCl2 and 25 mL N,N-dimethylformamide (DMF) were added to a round-bottom flask, stirred at 75 °C for 30 h and then vacuum filtered. The solid was then washed with anhydrous tetrahydrofuran (THF) until the filtrate was colorless and then vacuum dried at 50 °C for 1 h to obtain acylated carbon nanotubes (CNT-COCl).

[0066] (3) Vinyl modification of carbon nanotubes

[0067] First, 1 g of CNT-COCl was dispersed in 300 mL of DMF under a nitrogen atmosphere. After stirring at 80 °C for 1 hour, 1 g of allylamine dissolved in 50 mL of DMF was slowly added to the mixture and the reaction was stirred for 72 hours before vacuum filtration. The solid was then washed three times with anhydrous THF and finally dried under vacuum at 50 °C for 5 hours to obtain vinylated carbon nanotubes (CNT-CH=CH2).

[0068] (4) Preparation of CNT-g-PAA

[0069] First, 0.5 g of CNT-CH=CH2 was dispersed in 100 mL of deionized water under a nitrogen atmosphere, and then 6.8 g of acrylic acid monomer and 18 mg of initiator ammonium persulfate were added and mixed evenly. After reacting at 80°C for 48 h, vacuum filtration was performed, and the solid was washed three times with deionized water. Finally, vacuum drying was performed at 60°C for 10 h to obtain polyacrylic acid grafted carbon nanotubes CNT-g-PAA.

[0070] (5) Preparation of negative electrode sheet containing CNT-g-PAA-PEG

[0071] 82.8g of artificial graphite, 9.2g of silicon carbon (carbon-coated silicon oxide), 6g of CNT-g-PAA, 1g of crosslinking agent polyethylene glycol (PEG) and 1g of CMC-Na were dispersed in 150g of deionized water for wet mixing, wherein the mass ratio of artificial graphite to silicon carbon was 90:10, and the mass ratio of negative electrode active material (i.e. the sum of artificial graphite and silicon carbon), conductive binder CNT-g-PAA and crosslinking agent PEG was 92:6:1. The planetary centrifugal mixer was operated at a speed of 800 rpm for 1h and 2000 rpm for 2h to make the dispersion uniform and obtain the negative electrode slurry. The dispersed negative electrode slurry was coated on the current collector copper foil, and the electrode was dried at 60℃, cold pressed and placed in a vacuum oven at 120℃ for 3h. PAA and PEG underwent crosslinking reaction during the high-temperature vacuum drying process to obtain a negative electrode electrode containing a crosslinked conductive binder CNT-g-PAA-PEG.

[0072] Example 2

[0073] Example 2 provides a negative electrode plate, which differs from Example 1 in that the raw materials used in step (5) are: 84.6g artificial graphite, 9.4g silicon carbon, 4.3g CNT-g-PAA, 0.7g cross-linking agent polyethylene glycol (PEG) and 1g CMC-Na, wherein the mass ratio of artificial graphite and silicon carbon is 90:10, and the mass ratio of negative electrode active material, conductive binder CNT-g-PAA and cross-linking agent PEG is 94:4.3:0.7.

[0074] Example 3

[0075] Example 3 provides a negative electrode plate, which differs from Example 1 in that the raw materials used in step (5) are: 85.5g artificial graphite, 9.5g silicon carbon, 3.4g CNT-g-PAA, 0.6g cross-linking agent polyethylene glycol (PEG) and 1g CMC-Na, wherein the mass ratio of artificial graphite and silicon carbon is 90:10, and the mass ratio of negative electrode active material, conductive binder CNT-g-PAA and cross-linking agent PEG is 95:3.4:0.6.

[0076] Example 4

[0077] Example 4 provides a negative electrode plate, which differs from Example 1 in that the raw materials used in step (5) are: 87.3g artificial graphite, 9.7g silicon carbon, 1.7g CNT-g-PAA, 0.3g cross-linking agent polyethylene glycol (PEG) and 1g CMC-Na, wherein the mass ratio of artificial graphite and silicon carbon is 90:10, and the mass ratio of negative electrode active material, conductive binder CNT-g-PAA and cross-linking agent PEG is 97:1.7:0.3.

[0078] Example 5

[0079] Example 5 provides a negative electrode plate, which differs from Example 1 in that the raw materials used in step (5) are: 87.4g artificial graphite, 4.6g silicon carbon, 6g CNT-g-PAA, 1g cross-linking agent polyethylene glycol (PEG) and 1g CMC-Na, wherein the mass ratio of artificial graphite to silicon carbon is 95:5, and the mass ratio of negative electrode active material, conductive binder CNT-g-PAA and cross-linking agent PEG is 92:6:1.

[0080] Example 6

[0081] Example 6 provides a negative electrode plate, which differs from Example 1 in that the raw materials used in step (5) are: 78.2 g artificial graphite, 13.8 g silicon carbon, 6 g CNT-g-PAA, 1 g cross-linking agent polyethylene glycol (PEG) and 1 g CMC-Na, wherein the mass ratio of artificial graphite to silicon carbon is 85:15, and the mass ratio of negative electrode active material, conductive binder CNT-g-PAA and cross-linking agent PEG is 92:6:1.

[0082] Example 7

[0083] Example 7 provides a negative electrode plate, which differs from Example 1 in that the raw materials used in step (5) are: 64.4 g artificial graphite, 27.6 g silicon carbon, 6 g CNT-g-PAA, 1 g cross-linking agent polyethylene glycol (PEG) and 1 g CMC-Na, wherein the mass ratio of artificial graphite to silicon carbon is 70:30, and the mass ratio of negative electrode active material, conductive binder CNT-g-PAA and cross-linking agent PEG is 92:6:1.

[0084] Example 8

[0085] Example 8 provides a negative electrode plate, which differs from Example 1 in that the raw materials used in step (5) are: 55.2 g artificial graphite, 36.8 g silicon carbon, 6 g CNT-g-PAA, 1 g cross-linking agent polyethylene glycol (PEG) and 1 g CMC-Na, wherein the mass ratio of artificial graphite and silicon carbon is 60:40, and the mass ratio of negative electrode active material, conductive binder CNT-g-PAA and cross-linking agent PEG is 92:6:1.

[0086] Example 9

[0087] Example 9 provides a negative electrode sheet, which differs from Example 1 in that the raw materials used in step (5) are: 82.8g artificial graphite, 9.2g silicon carbon, 6.5g CNT-g-PAA, 0.5g cross-linking agent polyethylene glycol (PEG) and 1g CMC-Na are dispersed in 150g deionized water for wet mixing, wherein the mass ratio of artificial graphite and silicon carbon is 90:10, and the mass ratio of negative electrode active material, electrode conductive binder CNT-g-PAA and cross-linking agent PEG is 92:6.5:0.5.

[0088] Example 10

[0089] Example 10 provides a negative electrode plate, which differs from Example 9 in that the cross-linking agent polyethylene glycol (PEG) is replaced by polypropylene glycol (PPG), and the obtained cross-linked electrode conductive binder is CNT-g-PAA-PPG.

[0090] Comparative Example 1

[0091] Comparative Example 1 provides a negative electrode sheet, which differs from Example 3 in that no cross-linking agent is added in step (5), and the raw materials used are: 85.5 g of artificial graphite, 9.5 g of silicon carbon, 4 g of CNT-g-PAA and 1 g of CMC-Na, wherein the mass ratio of artificial graphite to silicon carbon is 90:10, and the mass ratio of negative electrode active material to conductive binder CNT-g-PAA is 95:4.

[0092] Comparative Example 2

[0093] Comparative Example 2 provides a negative electrode sheet, and the preparation method thereof comprises the following steps:

[0094] 85.5g of artificial graphite, 9.5g of silicon carbon, 0.5g of carbon nanotubes, 3.5g of polyacrylic acid (Mw ~ 50000) and 1g of CMC-Na were dispersed in 150g of deionized water for wet mixing, wherein the mass ratio of artificial graphite to silicon carbon was 90:10. The planetary centrifugal mixer was operated at a speed of 800 rpm for 1h and 2000 rpm for 2h to make the dispersion uniform and obtain the negative electrode slurry. The dispersed negative electrode slurry was coated on the current collector copper foil, and the pole piece was dried at 60°C, cold pressed and placed in a vacuum oven at 120°C for 3h to obtain the negative electrode pole piece.

[0095] Performance Evaluation

[0096] Test 1: Cycle performance test

[0097] The negative electrode sheets provided in the above embodiments are assembled into a battery for testing, and the preparation method is as follows:

[0098] (1) Preparation of positive electrode sheet: positive electrode active material (lithium nickel cobalt manganese oxide), conductive carbon black, and binder polyvinylidene fluoride (PVDF) are mixed in N-methylpyrrolidone at a mass ratio of 96:1:3, and then coated on a 12 μm aluminum foil, dried, and rolled to obtain a positive electrode sheet;

[0099] (2) preparing an electrolyte: mixing ethylene carbonate (EC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 15:15:20:50 to obtain an organic solvent, and then dissolving fully dried lithium salt LiPF6 in the mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L;

[0100] (3) Assembly: stack the positive electrode sheet, separator, and negative electrode sheet in order, weld the positive and negative electrode tabs, and obtain an electrode assembly. The separator is a 15 μm thick polyethylene porous separator, the number of layers of the positive electrode current collector is 1, and the number of layers of the negative electrode current collector is 2. Place the electrode assembly in an outer packaging aluminum-plastic film to obtain a lithium-ion soft-pack battery.

[0101] The lithium-ion soft-pack battery was charged and discharged at room temperature of 25°C. The first cycle of constant current and constant voltage charging: 0.1CCC (constant current) to 4.2V, CV (constant voltage) to 0.01C; standing for 10 minutes, constant current discharge: 0.1C to 2.5V. Then repeat the constant current charging: 1C to 4.2V, CV to 0.01C; standing for 10 minutes, constant current discharge: 1C to 2.5V. After 500 cycles, the capacity retention rate of the lithium-ion soft-pack battery was recorded. The results are shown in Table 1. The comparison between Example 3 and Comparative Examples 1 and 2 is shown in Figure 4 .

[0102] Test 2: Peel strength test

[0103] The rolled negative electrode sheet is made into an electrode strip (400mm*15mm), and double-sided tape is pasted on a flat thin steel plate. One end of the electrode strip to be tested is pasted on the double-sided tape, and the electrode strip is rolled with a pressure roller. The unpasted end of the electrode strip is bent upward and clamped on the upward traction end of the tensile testing machine to perform a 180° peeling test; the stage in the tensile force curve where the tensile force changes by no more than 10% is taken as the stable peeling section, and the average tensile force of the stable peeling section is divided by the electrode width to calculate the peeling strength of the battery electrode. The results are shown in Table 1.

[0104] Table 1

[0105]

[0106] As shown in Table 1 above, the cycle capacity retention rate and negative electrode sheet peeling strength of Example 1 are excellent. This is because the conductive agent carbon nanotubes are in-situ grafted onto the polymer binder, which improves the dispersibility of the conductive agent in the negative electrode slurry, and the structure of the polymer-coated carbon nanotubes makes the conductive network of the adhesive more complete. The three-dimensional cross-linked network formed by using polyethylene glycol as a polymer soft segment cross-linking agent enhances the mechanical properties of the linear binder modified by polyacrylic acid grafting, inhibits the volume expansion of the active material during the charge and discharge process, so as to achieve long-term cycle stability and good electrode integrity of the silicon anode during the cycle process.

[0107] In Example 1-4, as the content of the cross-linked binder increases, the bonding force between the active material and the active material (i.e., artificial graphite and silicon carbon), and between the active material and the current collector increases, and the peel strength of the pole piece gradually increases. In Example 5-8, as the content of silicon carbon increases, during the long cycle charge and discharge process, the volume expansion of the silicon base intensifies the particle breakage, and a new SEI film is formed on the surface of the silicon base, resulting in further volume expansion, loss of active lithium, and slippage of the active material particles. The bonding performance of the binder is weakened, and the cycle performance decreases. However, under the action of the cross-linked binder, the cycle performance of the battery can still be maintained at more than 63%, meeting the use requirements. In Example 9-10, the reduction in the content of the cross-linking agent leads to a reduction in the three-dimensional cross-linking network density of the cross-linked dry electrode binder, and a reduction in the mechanical properties of the binder. Comparative Example 1 Compared with Example 3, PAA has a linear structure and its mechanical strength is weaker than that of the cross-linked PAA-PEG. The linear chain properties of the polymer binder make it easy for the polymer chains to slip during the continuous volume expansion and contraction of the Si electrode during the cycle, thereby reducing the stability and integrity of the electrode during the cycle. Therefore, the cycle capacity retention rate and peel strength are lower than those of Example 3; in Comparative Example 2, the carbon nanotubes are not modified. During the mixing process, the carbon nanotubes are not easy to disperse and are easy to agglomerate in the negative electrode slurry, so that a complete conductive network cannot be formed, polarization increases, and it is difficult to maintain a high capacity retention rate under high-rate long cycles. It can be concluded from Table 1 above that the capacity retention rate of the lithium-ion battery in the embodiment of the present application for 500 cycles is between 63-90%, preferably between 70-90%, and the negative electrode sheet peel strength is between 6.4-13.1N / m, preferably between 9.2-13.1N / m.

[0108] In the description of this specification, reference to the terms "some embodiments", "an example", or similar descriptions means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment are included in at least one embodiment or example. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0109] Although examples of the present embodiment have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present embodiment, and the scope of the present embodiment is defined by the claims and their equivalents.

Claims

1. A cross-linked conductive adhesive, characterized in that: The cross-linked conductive adhesive is obtained by modifying a conductive agent, wherein the conductive agent is selected from a mixture of one or more of conductive carbon black, carbon nanotubes, graphene, and graphite; the conductive agent connects carbon chains via amide bonds, and at least two of the carbon chains are cross-linked via polyether.

2. The cross-linked conductive adhesive according to claim 1, characterized in that: The cross-linked conductive adhesive has a structure as shown in Formula I: Wherein A is the conductive agent, R is selected from at least one of cyano, phenyl, carboxyl, and ester groups, x and y are integers greater than or equal to 100, and a is an integer greater than or equal to 3.

3. The cross-linked conductive adhesive according to claim 1 or 2, characterized in that: The preparation method of the cross-linked conductive adhesive comprises the following steps: S1: reacting the conductive agent with an oxidant to obtain a carboxylated conductive agent; S2: reacting the carboxylated conductive agent with an acylating agent to obtain an acylated conductive agent; S3: reacting the acylated conductive agent with a vinyl modifier to obtain a vinyl conductive agent; S4: reacting the vinyl conductive agent with a vinyl monomer and an initiator to obtain a linear graft modified conductive agent; S5: reacting the linear graft modified conductive agent with a crosslinking agent to obtain the crosslinked conductive adhesive.

4. The cross-linked conductive adhesive according to claim 3, characterized in that: In the step S1, the mass ratio of the conductive agent to the oxidant is 1:(100-200), the reaction temperature is 80-100°C, and the reaction time is 18-36h; the oxidant is concentrated nitric acid, and the mass fraction of the concentrated nitric acid is 60%-80%.

5. The cross-linked conductive adhesive according to claim 4, characterized in that: In the step S2, the mass ratio of the carboxylated conductive agent to the acylating agent is 1:(700-900), the reaction temperature is 60-75° C., and the reaction time is 20-40 h; the acylating agent is thionyl chloride.

6. The cross-linked conductive adhesive according to claim 5, characterized in that: In the step S3, the mass ratio of the acylated conductive agent to the vinyl modifier is 1:(0.5-2), the reaction temperature is 60-80°C, and the reaction time is 50-80h; the vinyl modifier is allylamine.

7. The cross-linked conductive adhesive according to claim 6, characterized in that: In the step S4, based on the total mass of the vinyl conductive agent, the vinyl monomer and the initiator being 100%, the vinyl conductive agent accounts for 10%-15%, the initiator accounts for 0.1%-1%, and the rest is the vinyl monomer. The reaction temperature of the three is 60-100°C, and the reaction time is 36-72h; the vinyl monomer is selected from a mixture of one or more of acrylic acid, methyl acrylate, butyl acrylate, butyl methacrylate, styrene, and acrylonitrile; the initiator is selected from one of dibenzoyl peroxide, azobisisobutyronitrile, and ammonium persulfate.

8. The cross-linked conductive adhesive according to claim 7, characterized in that: In the step S5, based on the total mass of the linear graft modified conductive agent and the cross-linking agent as 100%, the linear graft modified conductive agent accounts for 85%-95%, the cross-linking agent accounts for 5%-15%, the reaction temperature of the two is 100-150° C., and the reaction time is 2-4 hours; the cross-linking agent is selected from a mixture of one or more of polyethylene glycol, polypropylene glycol, and polytetrahydrofuran diol.

9. A negative electrode plate, characterized in that: A current collector is included, wherein at least one surface of the current collector is provided with a negative electrode active material layer; In terms of weight percentage, the negative electrode active material layer comprises 2%-7% of the cross-linked conductive binder according to any one of claims 1 to 8, 0.5%-1% of a dispersant, and the balance is negative electrode active material; The negative electrode active material comprises 60%-95% of carbon material and 5%-40% of silicon material by weight percentage; The dispersant is lithium carboxymethyl cellulose and / or sodium carboxymethyl cellulose.

10. The negative electrode sheet according to claim 9, characterized in that: The carbon material is selected from a mixture of one or more of artificial graphite, natural graphite and hard carbon; the silicon material is selected from a mixture of one or more of silicon-carbon material, silicon oxide and pure silicon.

11. A method for preparing a negative electrode sheet according to claim 9 or 10, characterized in that: The following steps are involved: The linear graft modified conductive agent, the negative electrode active material, the crosslinking agent and the dispersant are wet mixed to obtain a negative electrode slurry, the negative electrode slurry is coated on at least one surface of the current collector, and the negative electrode sheet is obtained after drying, rolling and vacuum high temperature drying.

12. A lithium ion battery, characterized in that: Comprising the negative electrode sheet according to claim 9 or 10.

Citation Information

Cited By

  • Lithium ion battery and method for predicting, regulating and controlling diaphragm resistance of lithium ion battery

    CN119627034A

  • Conductive binder and preparation method thereof, electrode slurry, electrode and lithium ion battery

    CN122381740A

  • Conductive binder and method for producing the same, electrode slurry, electrode, and lithium ion battery

    CN122381740B