A compound and an organic electroluminescent device

By optimizing the compound structure for the hole transport layer or injection layer of OLED devices, the problem of low luminescence efficiency of OLED devices is solved, efficient light extraction and low driving voltage are achieved, and higher performance OLED materials are met.

CN113149889BActive Publication Date: 2024-11-15FUYANG SINEVA MATERIAL TECHNOLOGY CO LTD +1
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202110216675.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-26
Publication Date
2024-11-15
Estimated Expiration
2041-02-26

AI Technical Summary

Technical Problem

The luminous efficiency of existing OLED devices is lower than the ideal level, mainly due to substrate mode loss, surface plasma effect and waveguide effect, light is limited to the light emitting device, and the light extraction material is single, the effect is poor, and it is difficult to meet higher Performance requirements.

Method used

A compound is provided for organic electroluminescent devices, and its structure optimized compound is used for a hole transport layer or an injection layer. By defining the structure of A, B and Z, the film forming performance and light transmittance are improved, and by The solution method is prepared to improve the dissolution performance and luminous efficiency of the material and reduce the driving voltage.

Benefits of technology

It achieves higher luminous efficiency and lower driving voltage, improves the light extraction efficiency and current efficiency of OLED devices, and is suitable for the development of higher performance OLED materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113149889B_ABST
    Figure CN113149889B_ABST
Patent Text Reader

Abstract

The present application relates to the field of electroluminescence, and discloses a compound and an organic electroluminescent device. The structural formula of the compound is shown in formula (I), #imgabs0# to reduce the driving voltage and current efficiency of the electroluminescent device, and at the same time provide a compound that can be used to prepare the transport layer of the electroluminescent device by a solution method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electroluminescence, and in particular to a compound and an organic electroluminescent device. Background Art

[0002] Currently, organic electroluminescent (OLED) display technology has been applied in smart phones, tablet computers and other fields, and will be further expanded to large-size application fields such as televisions. In the past 30 years of development, people have developed various OLED materials with excellent performance, and through different designs of device structures and optimization of device performance such as life and efficiency, the commercialization process of OLED has been accelerated, making OLED widely used in the display and lighting fields.

[0003] However, the huge gap between the external quantum efficiency and internal quantum efficiency of OLEDs has greatly restricted the development of OLEDs. One of the most important factors is that the efficiency of the device has not yet reached the ideal level. This is due to the mode loss of the substrate, the loss of the surface plasmon and the waveguide effect, which confines most of the light inside the light-emitting device, thereby reducing the luminous efficiency of the device. Improving the luminous efficiency of the device and using light extraction materials is one of the effective methods. The light extraction layer (Capping Layer, CPL) can effectively improve the light extraction efficiency of the device by reducing the surface plasma effect of the metal electrode and adjusting the light extraction direction and light extraction efficiency, thereby improving the luminous efficiency of the device. At present, the types of light extraction materials are relatively single, and the effects are not ideal. Developing more effective light extraction materials is one of the more severe challenges facing OLED workers.

[0004] In addition, the selection of light-emitting layer and other organic functional layer materials also has a significant impact on the current efficiency and driving voltage of the device, and functional layer materials with higher performance are still being explored.

[0005] Therefore, in order to meet people's higher requirements for OLED devices, the field is in urgent need of developing more types of OLED materials with higher performance. Summary of the invention

[0006] The present application discloses a compound and an organic electroluminescent device. The organic electroluminescent device using the material of the compound of the present application has a lower driving voltage and a higher current efficiency. At the same time, a compound capable of preparing a transport layer of the electroluminescent device by a solution method is provided.

[0007] In order to achieve the above objectives, this application provides the following technical solutions:

[0008] A compound, the structural formula of the compound is as shown in formula (I),

[0009]

[0010] Wherein, m, n are selected from 0, 1;

[0011] Ar1 and Ar2 are each independently selected from an arylene group consisting of carbon and hydrogen containing 6 to 60 carbon atoms, and the hydrogen in Ar1 and Ar2 can be replaced by an aliphatic alkyl group having 1 to 30 carbon atoms, an aliphatic alkoxy group, an aryl group consisting of carbon and hydrogen containing 6 to 60 carbon atoms, or a -N(R1R2) group;

[0012] A and B are each independently selected from hydrogen or II-1 to II-6, and A and B are not H at the same time,

[0013]

[0014] In II-1 to II-6, the Sp2 hybridized carbon atom is connected to Ar1 or Ar2 in formula (I), and when m or n is selected from 0, the Sp2 hybridized carbon atom is connected to N in formula (I);

[0015] X and Y are each independently selected from one of O, S, NR or C(R1R2), and R, R1 and R2 are each independently selected from an alkyl group containing 1 to 30 carbon atoms or an aryl group consisting of carbon and hydrogen containing 6 to 60 carbon atoms;

[0016] Rings M, N, and P consist of sp2-hybridized carbon and hydrogen atoms and may be present or absent;

[0017] The hydrogen in A and B can be replaced by an aliphatic alkyl group of 1 to 30 carbon atoms, an aliphatic alkoxy group, or an aromatic group composed of carbon and hydrogen containing 6 to 60 carbon atoms;

[0018] Z is independently selected from at least one of an alkyl group or an alkoxy group containing 1 to 30 carbon atoms, and the carbon atom in Z is connected to the N atom in formula (I), and the hydrogen in Z can be replaced by an aromatic group consisting of carbon and hydrogen and having 6 to 60 carbon atoms;

[0019] One or more hydrogen groups in formula (I) may be replaced by deuterium, cyano or fluorine.

[0020] Wherein, when M, N, and P exist, it means that the rings M, N, and P can form an aromatic condensed ring compound with the adjacent aromatic ring, and the rings M, N, and P contain 4 to 10 carbon atoms.

[0021] Furthermore, Ar1 and Ar2 are each independently selected from at least one of phenyl, naphthyl, anthracenyl, phenanthryl, 9,9-dialkyl-substituted fluorenyl, biphenyl, binaphthyl, anthracenyl, bifluorenyl, terphenyl, triphenylene, fluoranthene, triphenylene or hydrogenated benzanthryl.

[0022] Furthermore, the combination of Ar1 and Ar2 is selected from a combination of two of: phenyl, naphthyl, anthracenyl, 9,9-dialkyl-substituted fluorenyl, and triphenylene.

[0023] Further, A and B are each independently selected from at least one of a carbazolyl group, a benzocarbazolyl group, a dibenzocarbazolyl group, a dibenzothiophenyl group, a naphthobenzothiophenyl group, a dinaphthothiophenyl group, a dibenzofuranyl group, a naphthobenzofuranyl group, a dinaphthofuranyl group, an indenofluorenyl group, a benzoindenofluorenyl group, an indenocarbazolyl group, a benzoindenocarbazolyl group, an indolecarbazolyl group, a benzoindolecarbazolyl group, an indenobenzofuranyl group, and an indenobenzothiophenyl group.

[0024] Furthermore, R, R1 and R2 are each independently selected from an alkyl group containing 1 to 30 carbon atoms or an aryl group consisting of carbon and hydrogen having 6 to 20 carbon atoms, and the hydrogen in the aryl group consisting of carbon and hydrogen having 6 to 20 carbon atoms can be replaced by an alkyl group having 1 to 30 carbon atoms.

[0025] Wherein, X and Y are each independently selected from one of O, S, NR or C(R1R2), taking X and Y as an example, each independently selected from C(R1R2), and A or B is an indenofluorenyl For example, the structure of A or B is as follows: The four R1s may be the same or different.

[0026] Furthermore, Z is selected from one of methyl, ethyl, propyl, butyl, pentyl or hexyl.

[0027] Furthermore, the compound is selected from one of the following structures:

[0028]

[0029]

[0030]

[0031]

[0032]

[0033] An organic electroluminescent device, comprising the compound of the present application.

[0034] Furthermore, the material of the hole transport layer or hole injection layer of the organic electroluminescent device is the compound of the present application.

[0035] Furthermore, the compounds of the present application can be used to prepare hole transport layers or hole injection layers of electroluminescent devices by a solution method.

[0036] The technical solution of this application produces the following beneficial effects:

[0037] The present application provides a compound shown in Formula I, which improves the film-forming properties and light transmittance of the material by limiting the structures of A and B, and by limiting the structure of Z, so that the material is applied to HTL, EBL, and Host materials, which is more improved than the existing materials. At the same time, the change in the structure of the compound correspondingly changes the solubility of the material in the organic solvent. After the solvent, the solution of this compound can obtain an organic solvent with good viscosity performance. After the solvent evaporates, the film-forming properties of the remaining organic material are excellent, so that this material is more suitable for preparation using a solution method when used to prepare OLED devices. At the same time, the change in the structure of the compound improves the HOMO and LOMO energy levels of the material, so that the material described in the present application, as a hole injection layer (HIL) material or a hole transport layer (HTL) material, has a higher luminous efficiency and a lower driving voltage when applied to OLED devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The mass spectrum test diagram of compound HT-F01-1 in the preparation of compound C-49;

[0039] Figure 2 This is the mass spectrum test diagram of compound C-49. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0041] It should be noted that: in this application, if there is no special description, all the embodiments and preferred implementation methods mentioned herein can be combined with each other to form a new technical solution. In this application, if there is no special description, all the technical features and preferred features mentioned herein can be combined with each other to form a new technical solution. In this application, if there is no special description, percentage (%) or part refers to the weight percentage or weight part relative to the composition. In this application, if there is no special description, the components or their preferred components involved can be combined with each other to form a new technical solution. In this application, unless otherwise specified, the numerical range "a-b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "6-22" means that all real numbers between "6-22" have been listed in this article, and "6-22" is just an abbreviation of these numerical combinations. The "range" disclosed in this application can be one or more lower limits and one or more upper limits in the form of lower limits and upper limits. In this application, unless otherwise specified, each reaction or operation step can be carried out sequentially or not in sequence. Preferably, the reaction method in this article is carried out sequentially.

[0042] Unless otherwise specified, the professional and scientific terms used herein are the same as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the described content may also be applied to the present application.

[0043] Synthesis of Compound A-1

[0044]

[0045] In a 250 ml autoclave, 3.98 g (0.01 mol) of 3-(4-bromophenyl)-9-phenyl-9H-carbazole, 30 ml of toluene, 150 ml of N,N-dimethylformamide, 0.1 g of cuprous iodide, and 5.52 g of potassium carbonate were added, and the temperature was lowered to 0°C, and 0.9 g (0.02 mol) of ethylamine was added. After nitrogen replacement at 0°C, the temperature was raised to 100°C in a sealed manner for 8 hours to react. Although the amount of ethylamine was much greater than that of 3-(4-bromophenyl)-9-phenyl-9H-carbazole when the materials were added, because the boiling point of ethylamine was low, after the temperature was raised, most of the ethylamine would exist in the closed space above the reactor in the form of gas, and only a small amount would participate in the reaction in the solution. The temperature was lowered, and the reaction solution was poured into a mixture of toluene and water for separation. The organic layer was washed with water until neutral, concentrated to dryness, and separated by silica gel column chromatography with petroleum ether: ethyl acetate: dichloromethane = 9:1:1 (volume ratio) as eluent to obtain 1.1 g of the compound shown in A--1 with a yield of 32%.

[0046] The obtained compound A-1 was subjected to mass spectrometry and the m / z of the molecule was determined to be 679.

[0047] The obtained compound A-1 was subjected to NMR detection, and the data analysis was as follows: 1HNMR (500MHz, CDCl3): δ8.55 (m, 2H), 8.19 (d, 2H), 7.67–7.48 (m, 20H), 7.34 (m, 4H), 7.19–7.07 (m, 4H), 3.59 (m, 2H), 1.16 (s, 3H).

[0048] Synthesis of compound C-1

[0049]

[0050] In a 250 ml three-necked flask, under nitrogen protection, 100 ml of dry toluene, 5.5 g (0.0138 mol) of 3-(4-bromophenyl)-9-phenyl-9H-carbazole, 0.595 g (0.006 mol) of cyclohexylamine, 0.11 g (0.00012 mol) of Pd2(dba)3 (tridibenzylideneacetone dipalladium), 0.48 g (0.00024 mol) of a toluene solution containing 10% tri-tert-butylphosphine, and 1.61 g (0.0168 mol) of sodium tert-butoxide were added. The mixture was heated to reflux for 4 hours, cooled, and separated by adding water. The organic layer was concentrated to dryness and separated by silica gel column chromatography. The mixture was eluted with petroleum ether: ethyl acetate: dichloromethane = 9:1:0.2 (volume ratio) to obtain 3.3 g of the compound shown in C-1 with a yield of 75%.

[0051] The compound shown in C-1 was detected by mass spectrometry, and the m / z of the product was 733.

[0052] Synthesis of compound C-49

[0053]

[0054] (1) Synthesis of HT-F01-1

[0055] In a 1000 ml three-necked flask, under nitrogen protection, add 280 ml of dry toluene, 19.6 g of 4'bromo-N,N-diphenyl-[1,1'-biphenyl]-4-amine, 6.3 g of cyclohexylamine, 0.55 g of Pd2(dba)3 (tridibenzylideneacetone dipalladium), 2.44 g of a toluene solution containing 10% tri-tert-butylphosphine, and 6.38 g of sodium tert-butoxide. Heat to reflux for 2 hours, cool, add water to separate, decolorize the organic layer with a silica gel column, concentrate to dryness, and crystallize with methanol to obtain 16.2 g of the compound shown in HT-F01-1.

[0056] The compound shown in HT-F01-1 was detected by mass spectrometry, and the product m / z was 418. The mass spectrum is shown in Figure 1 .

[0057] (2) Synthesis of C-49

[0058] In a 250 ml three-necked flask, under nitrogen protection, add 80 ml of dry toluene, 3.48 g of 3-(4-bromophenyl)-9-phenylcarbazole, 3.66 g of HT-F01-1, 0.08 g of Pd2(dba)3 (tridibenzylideneacetone dipalladium), 0.35 g of a toluene solution of 10% tri-tert-butylphosphine, and 1.09 g of sodium tert-butoxide. Heat to reflux for 6 hours, cool, add water to separate, dry the organic layer, separate on a silica gel column, and elute with petroleum ether: ethyl acetate: dichloromethane = 9:1:0.5 (volume ratio) to obtain 4.2 g of compound C-49.

[0059] The compound shown in C-49 was detected by mass spectrometry, and the product m / z was 735. The mass spectrum is shown in Figure 2 .

[0060] Other compounds of the present application can be synthesized by referring to the above reaction steps and using methods well known in the art.

[0061] Device Embodiment

[0062] The electroluminescent devices will be prepared using the compounds of the present application and existing compounds respectively to further illustrate the performance of the compounds of the present application.

[0063] The specific structures of several materials used in the following device embodiments and comparative examples of this application are as follows:

[0064]

[0065] Device Example 1

[0066] In the examples, the compounds of the present application are selected as hole transport materials in organic electroluminescent devices. In comparative examples 1 to 2, NPB and HT-3 are selected as hole transport materials in organic electroluminescent devices, respectively.

[0067] The structure of the organic electroluminescent device is: ITO / HIL02 (100nm) / hole transport material (40nm) / EM1 (30nm) / TPBI (30nm) / LiF (0.5nm) / Al (150nm).

[0068] The preparation process of organic electroluminescent device is as follows:

[0069] The glass substrate coated with an ITO transparent conductive layer (as an anode) is ultrasonically treated in a cleaning agent, then rinsed in deionized water, ultrasonically degreased in a mixed solvent of acetone and ethanol, baked in a clean environment until the water is completely removed, cleaned with ultraviolet light and ozone, and bombarded with a low-energy cation beam to improve the properties of the surface and enhance the binding ability with the hole injection layer;

[0070] The glass substrate was placed in a vacuum chamber and evacuated to 1×10 -5 ~9×10 -3 Pa, vacuum evaporate HIL02 on the anode as a hole injection layer, the evaporation rate is 0.1nm / s, and the evaporation film thickness is 100nm;

[0071] The compound of the present application and comparative materials NPB and HT-3 were vacuum-deposited on the hole injection layer as a hole transport layer, respectively, with a deposition rate of 0.1 nm / s and a deposition film thickness of 40 nm;

[0072] Vacuum evaporate EM1 on the hole transport layer as the organic light-emitting layer of the device, with an evaporation rate of 0.1 nm / s and a total evaporation film thickness of 30 nm;

[0073] Vacuum evaporation of TPBI on the organic light-emitting layer as the electron transport layer of the organic electroluminescent device; the evaporation rate is 0.1nm / s, and the total evaporation film thickness is 30nm;

[0074] 0.5 nm of LiF and 150 nm of Al were vacuum-deposited on the electron transport layer to serve as an electron injection layer and a cathode.

[0075] The brightness, driving voltage and current efficiency of the prepared organic electroluminescent device were measured.

[0076] The performance of the organic electroluminescent device is shown in Table 1. The test was conducted using the OLED-1000 multi-channel accelerated aging life and light color performance analysis system produced by Hangzhou Yuanfang.

[0077] Table 1

[0078] Hole transport materials <![CDATA[Required brightness cd / m 2 > Drive voltage V Current efficiency cd / A NPB 1000 6.31 1.56 HT-3 1000 5.61 1.39 A-1 1000 5.58 1.69 C-1 1000 5.11 1.66 A-17 1000 5.0 1.59 A-38 1000 5.31 1.61 C-49 1000 5.33 1.71 A-55 1000 4.90 1.69 B-57 1000 5.22 1.91

[0079] It can be seen from the data in Table 1 that the driving voltage of the electroluminescent device obtained using the compounds of the present application is lower than the voltage of the electroluminescent device prepared using the compounds NPB and HT-3, and the driving voltage of the electroluminescent device obtained using the compounds of the present application is lower than the current efficiency of the electroluminescent device prepared using the comparative compounds NPB and HT-3, and the current efficiency is higher than the current efficiency of the electroluminescent device prepared using the compounds NPB and HT-3. It can be seen from the data in Table 1 that the driving voltage of the electroluminescent device obtained using the compounds provided by the present application can also be below 5.6V, and at the same time, the current efficiency can reach above 1.59cd / A.

[0080] Device Example 2

[0081] In the embodiment, the compound of the present application is selected as the hole transport material in the organic electroluminescent device. In the comparative example, NPB and HT-3 are selected as the hole transport materials in the organic electroluminescent device, respectively. In this embodiment, the hole transport layer is prepared by a solution method.

[0082] The structure of the organic electroluminescent device is: ITO / HIL02 (100 nm) / hole transport material / EM1 (30 nm) / TPBI (30 nm) / LiF (0.5 nm) / Al (150 nm). The thickness of the hole transport material is indicated in Table 2.

[0083] The preparation process of organic electroluminescent device is as follows:

[0084] The glass substrate coated with an ITO transparent conductive layer (as an anode) is ultrasonically treated in a cleaning agent, then rinsed in deionized water, ultrasonically degreased in a mixed solvent of acetone and ethanol, baked in a clean environment until the water is completely removed, cleaned with ultraviolet light and ozone, and bombarded with a low-energy cation beam to improve the properties of the surface and enhance the binding ability with the hole injection layer;

[0085] The glass substrate was placed in a vacuum chamber and evacuated to 1×10 -5 ~9×10 -3 Pa, vacuum evaporate HIL02 on the anode as a hole injection layer, the evaporation rate is 0.1nm / s, and the evaporation film thickness is 100nm;

[0086] The glass substrate on which the hole injection layer has been evaporated was transferred to a glove box filled with nitrogen, and solutions of the compound of the present application and the comparative compound were spin-coated on the hole injection layer, respectively. The solvent was chlorobenzene: anisole = 1: 1 (volume ratio), the spin coating speed was 1000 rpm, and the time was 60 seconds. Then, the glass substrate was heated at 80° C. for 2 hours, and the solvent was removed in vacuo. The concentration of the compound of the present application and the comparative compound in the solvent was adjusted to obtain a hole transport layer with a thickness of 46 to 55 nm. The film thickness of the spin-coated hole transport layer was measured by a step profiler (model Amibios XP-2 surface profiler), and is listed in Table 2 below.

[0087] Transfer the glass substrate on which the hole transport layer has been spin-coated in the previous step into a vacuum chamber, and vacuum evaporate EM1 on the hole transport layer as the organic light-emitting layer of the device. The evaporation rate is 0.1 nm / s, and the total evaporation film thickness is 30 nm.

[0088] Vacuum evaporation of TPBI on the organic light-emitting layer as the electron transport layer of the organic electroluminescent device; the evaporation rate is 0.1nm / s, and the total evaporation film thickness is 30nm;

[0089] 0.5 nm of LiF and 150 nm of Al were vacuum-deposited on the electron transport layer to serve as an electron injection layer and a cathode.

[0090] The brightness, driving voltage and current efficiency of the prepared organic electroluminescent device were measured.

[0091] The performance of the organic electroluminescent device is shown in Table 2. The test was conducted using the OLED-1000 multi-channel accelerated aging life and light color performance analysis system produced by Hangzhou Yuanfang.

[0092] Table 2

[0093]

[0094] From the data in Table 2, it can be seen that the driving voltage of the electroluminescent device obtained using the compounds of the present application is lower than the voltage of the electroluminescent device prepared using the compounds NPB and HT-3, and the driving voltage of the electroluminescent device obtained using the compounds of the present application is lower than the current efficiency of the electroluminescent device prepared using the comparative compounds NPB and HT-3, and the current efficiency is higher than the current efficiency of the electroluminescent device prepared using the comparative compounds NPB and HT-3. From the data in Table 2, it can be seen that using the compounds provided by the present application, after preparing the hole transport layer using the solution method, the driving voltage of the obtained electroluminescent device can also be below 5.2V, and at the same time, the current efficiency can reach above 1.26cd / A.

[0095] Obviously, those skilled in the art can make various changes and modifications to the embodiments of the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.

Claims

1. A compound, characterized in that The compound is selected from one of the following structures:

2. An organic electroluminescent device, characterized in that: The organic electroluminescent device comprises the compound according to claim 1.

3. The organic electroluminescent device according to claim 2, characterized in that: The material of the hole transport layer or hole injection layer of the organic electroluminescent device is the compound according to claim 1.

Citation Information

Patent Citations

  • Light-emitting element, light-emitting device, display device, electronic device and lighting device

    CN103579515A

  • Organic electroluminescent device

    CN106612616A

  • Dibenzo-hexatomic ring-cored compound and application thereof to organic electroluminescent device

    CN109574926A

  • Nitrogen-containing compound, electronic component, and electronic device

    CN111892505A

  • Electrophotographic sensitive body

    JP1987250459A