Spherical forsterite particles, method for producing the same, and resin composition containing the spherical forsterite particles
By developing spherical magnesium sterilite particles with an average particle size of 0.1 μm to 10 μm and a dielectric loss tangent of 0.0003 to 0.0025, and improving their crystallinity through thermal spraying and resintering processes, the high dielectric loss tangent in high-frequency communication is solved The problem is that the substrate material with low dielectric loss tangent is achieved, and the high frequency characteristics and the insulation and toughness of the material are improved.
Patent Information
- Application Number
- CN201980078752.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-11-29
- Filing Date
- 2019-11-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-11-27
AI Technical Summary
In the prior art, the dielectric loss tangent of the substrate material in high frequency communication is high, resulting in signal deterioration, and the existing insulating materials such as silica cannot effectively improve the high frequency characteristics, and the shape of spherical insulating particles decreases the toughness of the composite material.
Spherical magnesium sterilite particles with an average particle size of 0.1 μm to 10 μm and a tangent of dielectric loss of 0.0003 to 0.0025 were developed, and their crystallinity was improved through thermal spraying and resintering process, so that they were easily blended with the resin and formed a low medium. Loss tangent substrate material.
The substrate material with low dielectric loss tangent is achieved, which improves high frequency characteristics, reduces signal transmission losses, and maintains the high insulation and toughness of the material.
Smart Images

Figure BDA0003089693540000321 
Figure BDA0003089693540000331 
Figure BDA0003089693540000332
Abstract
Description
Technical Field
[0001] The present invention relates to spherical forsterite particles, a method for producing the same, and a resin composition containing the spherical forsterite particles. Background Art
[0002] The communication technology using microwaves requires high-capacity, high-speed data communication due to high frequency. For mobile phones, the communication standard 4G (3GHz to 4GHz) is moving towards 5G (28GHz), and the frequency is moving towards high frequency. In addition, for cars equipped with automatic driving devices, there are cars equipped with millimeter-wave radars with frequencies of around 24GHz to 76GHz, which are radars for identifying surrounding obstacles, and the number has increased in recent years.
[0003] Resins are used for insulation between wirings of printed circuit boards (PCBs) after components are installed. In order to improve the insulation of the resin, it is required to contain a material with the same thermal expansion coefficient as the resin and with high insulation as a filler. Forsterite is one of them.
[0004] The signal transmission speed increases with the increase in frequency, but the transmission loss also increases. The dielectric loss increases in proportion to the frequency (f), dielectric loss tangent (tanδ), and relative dielectric constant (εr).
[0005] The dielectric constant is a value indicating the magnitude of polarization, and the relative dielectric constant indicates the ratio of the dielectric constant of a medium to the dielectric constant in a vacuum, and both are values indicating the characteristic magnitude of a capacitor component.
[0006] When a dielectric is exposed to electromagnetic waves, it becomes polarized, and the alternation of the electromagnetic waves induces polarization reversal, and dielectric loss occurs during this reversal. The so-called dielectric loss tangent is that when an AC electric field is applied to a dielectric, part of the electrical energy in the dielectric is converted into heat and lost. The higher the frequency of the AC electric field, the more susceptible it is to influence. The loss caused by the dielectric loss tangent is called dielectric loss.
[0007] Therefore, in order to improve high frequency characteristics, a low relative dielectric constant material with low dielectric loss tangent is required. It is required to use a resin (composite insulating material) containing an insulating material as a filler for a printed wiring board, and to have a substrate material with low dielectric loss tangent brought about by the low relative dielectric constant material.
[0008] As a material used as such a filler, a representative known material is silicon dioxide, which has a low relative dielectric constant (about 4.5), but has a dielectric loss tangent of about 0.003 to 0.005, which does not bring about an improvement in high-frequency characteristics. In particular, the dielectric loss tangent contributes more to reducing dielectric loss than the relative dielectric constant, so as a material to replace silicon dioxide, a material with a low dielectric loss tangent such as forsterite is required.
[0009] As a method for producing forsterite fine particles, there is disclosed a method of drying a solution containing a water-soluble magnesium salt and colloidal silica in an amount of Mg / Si molar ratio of 2, and then calcining it at 800° C. to 1000° C. to obtain forsterite particles with a primary particle size of 1 nm to 200 nm (see Patent Document 1).
[0010] Furthermore, it is described that when an insulating material such as forsterite particles is mixed with a resin, if the particle shape is blocky or angular, the toughness of the composite insulating material decreases, and spherical insulating particles are contained (see Patent Document 2).
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Application Publication No. 2016-222517
[0014] Patent Document 2: Japanese Patent Application Publication No. 2003-002640 Summary of the invention
[0015] Problems to be solved by the invention
[0016] The present invention is proposed in view of such a situation, and its subject is to provide forsterite particles with low dielectric loss tangent. In addition, its subject is to provide a substrate material with low dielectric loss tangent in order to suppress the signal degradation caused by the insulator material of the substrate. In addition, its subject is: because forsterite particles have low dielectric loss tangent, spherical forsterite particles that are spherical and easy to be mixed with resin are combined with resin to make substrate materials, thereby providing a substrate with less transmission loss (dielectric loss) that improves dielectric properties.
[0017] An object of the present invention is to produce forsterite particles having a low dielectric loss tangent and a spherical particle shape, and to provide a substrate having improved high-frequency characteristics.
[0018] Methods for solving problems
[0019] That is, as a first aspect of the present invention, there are forsterite particles having an average particle size of 0.1 μm to 10 μm and a dielectric loss tangent of 0.0003 to 0.0025.
[0020] As a second aspect, the forsterite particles according to the first aspect have a sphericity of 1.0 to 3.3 as calculated by the following formula (3),
[0021] Sphericity = L s / N s Formula (3)
[0022] [In formula (3), L s represents the average particle size (μm) measured by a laser diffraction particle size distribution analyzer, N s This indicates the average primary particle size (μm) calculated by converting the specific surface area according to the measurement item of the nitrogen adsorption method.]
[0023] As a third aspect, the forsterite particles according to the first aspect or the second aspect, wherein the forsterite particles have a water adsorption amount calculated by the following formula (4) of 0.15% or less,
[0024] Moisture adsorption (%) = [(m1-m2) / m2] × 100 Formula (4)
[0025] [In formula (4), m1 represents the mass (g) of the forsterite particles after being dried at a temperature of 150°C for 24 hours and then placed at a temperature of 25°C and a humidity of 50% for 48 hours, and m2 represents the mass (g) of the forsterite particles after being dried at a temperature of 150°C for 24 hours.]
[0026] As a fourth aspect, the forsterite particles according to any one of the first to third aspects, wherein the MgO / SiO2 molar ratio is 1.90 to 2.10,
[0027] As a fifth aspect, the forsterite particles according to any one of the first to fourth aspects are provided, wherein the surface of the particles is coated with at least one hydrolyzable silane selected from the group consisting of hydrolyzable silanes represented by the following formula (1) and formula (2),
[0028] R l a Si(R 2 ) 4-a Formula (1)
[0029] 〔R 3 d Si(R 4 ) 3-d 〕2Y e Formula (2)
[0030] [In formula (1), R 1 is an acryloyloxy group, a methacryloyloxy group, an aryl group, an alkyl group, a glycidoxy group, or an alkylene group having 1 to 10 carbon atoms and containing these functional groups, and R 1 It is bonded to the Si atom via a Si-C bond, and a represents an integer of 1 to 3. 2 is a hydrolyzable group consisting of an atom or group selected from an alkoxy group, an acyloxy group, and a halogen atom, and at least one R 2 The hydrolyzed groups form MO-Si bonds on the surfaces of the metal oxide particles, where M represents a Si atom or a Mg atom.
[0031] In formula (2), R 3 is an alkyl group and is bonded to the silicon atom through a Si-C bond, R 4 is a hydrolyzable group consisting of an atom or group selected from an alkoxy group, an acyloxy group, and a halogen atom, and at least one R 4 The hydrolyzed group forms a MO-Si bond on the surface of the metal oxide particle, where M represents a Si atom or a Mg atom. Y represents an alkylene group, an arylene group, an NH group, or an oxygen atom, d represents an integer of 0 to 3, and e is an integer of 0 or 1. ],
[0032] As a sixth aspect, a method for producing forsterite particles according to any one of the first aspect to the fourth aspect comprises the following steps (A) to (C):
[0033] (A) step: a step of preparing forsterite particles by mixing a magnesium compound serving as a magnesium source and a silicon compound serving as a silicon source so that the molar ratio of magnesium to silicon (MgO / SiO2) is 1.90 to 2.10,
[0034] (B) step: a step of introducing the forsterite particles prepared in step (A) into a hydrocarbon combustion flame and recovering the forsterite particles,
[0035] Step (C): a step of calcining the forsterite particles obtained in step (B) at 700° C. to 1100° C.,
[0036] According to a seventh aspect, in the production method according to the sixth aspect, the magnesium compound serving as the magnesium source in step (A) is an inorganic magnesium compound or an organic magnesium salt.
[0037] As an eighth aspect, the production method according to the seventh aspect, wherein the inorganic magnesium compound is magnesium oxide, magnesium hydroxide, basic magnesium carbonate, magnesium hydrogen carbonate, magnesium carbonate, magnesium nitrate, or a mixture thereof.
[0038] As a ninth aspect, in the production method according to the seventh aspect, the magnesium organic acid salt is an aliphatic magnesium monocarboxylate having 1 to 4 carbon atoms, a halogenated aliphatic magnesium monocarboxylate having 1 to 4 carbon atoms, an aliphatic magnesium polycarboxylate having 1 to 4 carbon atoms, an aliphatic magnesium hydroxycarboxylate having 1 to 4 carbon atoms, an alkoxy magnesium carboxylate having 1 to 4 carbon atoms, an oxo magnesium carboxylate having 1 to 4 carbon atoms, or a mixture thereof.
[0039] As a tenth aspect, in the production method according to the sixth aspect, the silicon compound serving as the silicon source in the step (A) is silicon oxide, alkoxysilane, or a mixture thereof,
[0040] As an eleventh aspect, in the production method according to any one of the sixth aspect to the tenth aspect, the temperature in the combustion flame of the hydrocarbon in the step (B) is 1900° C. to 3000° C. in terms of theoretical temperature,
[0041] As a twelfth aspect, the production method according to any one of the sixth aspect to the eleventh aspect further comprises the step (D) of pulverizing the forsterite particles obtained in the step (C);
[0042] As a 13th aspect, the production method according to any one of the 6th aspect to the 12th aspect further comprises the step (E): coating the forsterite particles obtained in the step (C) with the hydrolyzable silane according to the 5th aspect,
[0043] According to a fourteenth aspect, there is provided a resin composition comprising a resin and the forsterite particles according to any one of the first aspect to the fifth aspect.
[0044] According to a fifteenth aspect, in the resin composition according to the fourteenth aspect, the ratio of the resin to the forsterite particles is 1:0.001 to 1000 in terms of mass ratio, and
[0045] According to a sixteenth aspect, in the resin composition according to the fourteenth aspect or the fifteenth aspect, a dielectric loss tangent is 0.0003 to 0.01.
[0046] Effects of the Invention
[0047] The forsterite particles of the present invention have high crystallinity and low dielectric loss tangent, and therefore are easily blended with resins, and when used as a substrate material, a substrate having good high-frequency characteristics can be obtained.
[0048] The forsterite particles of the present invention have an average primary particle size of 0.1 μm to 10 μm and a dielectric loss tangent of 0.0003 to 0.0025. They are spherical particles with a specific sphericity and high crystallinity, and the integrated intensity of the diffraction peak at 2θ=52° to 53° measured by X-ray diffraction (CuKα) is 800 counts·deg or more, or 800 counts·deg to 2000 counts·deg, or 800 counts·deg to 1000 counts·deg.
[0049] In the present invention, the dielectric loss tangent immediately after step (A) is as high as 0.003 to 0.02, but the target low dielectric loss tangent of 0.0003 to 0.0025 is achieved by spheroidization by thermal spraying in step (B) and recovery of crystallinity by re-sintering (annealing) in step (C).
[0050] In the present invention, the molar ratio of MgO / SiO2 in the forsterite particles in step (A) is 1.90 to 2.10. Even after going through steps (B), (C), (D), and (E), the molar ratio does not change and is 1.90 to 2.10.
[0051] The forsterite particles of the present invention can be prepared by calcining a magnesium-containing silicon compound obtained by mixing a magnesium compound as a magnesium source and a silicon compound as a silicon source at a MgO / SiO2 molar ratio of 1.90 to 2.10 (preferably 2.0) to produce forsterite particles, and then thermally spraying the forsterite particles into a hydrocarbon combustion flame to form spherical forsterite particles. The forsterite particles used as the raw material before thermal spraying are crushed particles obtained by pulverization before being put into the combustion flame as a powder, but are changed into spherical forsterite particles by thermal spraying. DETAILED DESCRIPTION
[0052] The present invention provides forsterite particles having an average particle size of 0.1 μm to 10 μm and a dielectric loss tangent of 0.0003 to 0.0025.
[0053] As the value of the average particle size (μm), the average particle size (μm) measured by a laser diffraction particle size distribution analyzer can be applied.
[0054] The dielectric loss tangent value can be measured by a transmission path method, a resonator method, etc. As described later, in the measurement of the morphology of powder or film, the resonator method can be used to evaluate the values at 1 GHz and 10 GHz by a perturbation cavity resonator method.
[0055] The forsterite particles of the present invention have a sphericity calculated by the following formula (3) of 1.0 to 3.3.
[0056] Sphericity = L s / N s Formula (3)
[0057] [In formula (3), L s represents the average particle size (μm) measured by a laser diffraction particle size distribution analyzer, N s This indicates the average primary particle size (μm) calculated by converting the specific surface area according to the measurement item of the nitrogen adsorption method.]
[0058] The closer the sphericity is to 1.0, the more spherical the particle is. The sphericity of the forsterite particles obtained in the present invention may be 1.0 to 3.3.
[0059] The forsterite particles of the present invention have an integrated intensity of a diffraction peak at 2θ=52° to 53° measured by an X-ray diffraction method using CuKα rays of 800 counts·deg or more, or 800 to 2000 counts·deg, or 800 to 1000 counts·deg. 2θ=52° to 53° have characteristic peaks of diffracted X-rays originating from the (222) plane, (042) plane, and (321) plane that are unique to forsterite. Since the forsterite particles of the present invention have high crystallinity, their integrated intensities are in the range of 800 counts·deg or more, or 800 to 2000 counts·deg, or 800 to 1000 counts·deg when combined. In addition, in the measurement of X-ray diffraction at 2θ=52° to 53°, a range of plus or minus 0.5° can be included in consideration of the mechanical error range between the X-ray diffraction devices used for the measurement.
[0060] The forsterite particles obtained in the present invention are particles obtained by thermal spraying, so they are particles that are temporarily melted and spheroidized by raw materials, so that the amount of water adsorption is also low due to the small amount of hydroxyl groups present on the surface of the particles. When mixed with a resin based on these properties and used as a substrate material, high insulation can be maintained for a long time. The measurement of the amount of water adsorption due to the hydroxyl groups on the surface of the forsterite particles is calculated using, for example, about 100 g of forsterite particles according to the following formula (4).
[0061] Moisture adsorption (%) = [(m1-m2) / m2] × 100 Formula (4)
[0062] [In formula (4), m1 represents the mass (g) of the forsterite particles after being dried at a temperature of 150°C for 24 hours and then left at a temperature of 25°C and a humidity of 50% for 48 hours, and m2 represents the mass (g) of the forsterite particles after being dried at a temperature of 150°C for 24 hours.]
[0063] The moisture adsorption amount may be 0.15% or less, or 0.001% to 0.15%, or 0.01% to 0.15%.
[0064] The forsterite particles of the present invention may have a MgO / SiO2 molar ratio of 1.90 to 2.10. The forsterite particles have a MgO / SiO2 molar ratio of 2.0. Although it is preferred to use a MgO / SiO2 molar ratio of 2.0, even if the forsterite particles contain trace amounts of silicon dioxide, magnesium oxide, steatite, etc., as long as the same effect is exerted, it is also acceptable.
[0065] In the present invention, when forsterite particles are further hydrophobized to form a substrate material, a hydrolyzable silane compound may be reacted with the surface of the forsterite particles in order to exhibit high insulation properties.
[0066] The present invention also provides forsterite particles whose surfaces are coated with at least one hydrolyzable silane selected from the group consisting of hydrolyzable silane compounds represented by the following formula (1) and formula (2).
[0067] As these hydrolyzable silane compounds, at least one hydrolyzable silane compound selected from the group consisting of hydrolyzable silane compounds represented by the following formula (1) and formula (2) can be used.
[0068] R 1 a Si(R 2 ) 4-a Formula (1)
[0069] 〔R 3 d Si(R 4 ) 3-d 〕2Y e Formula (2)
[0070] In formula (1), R 1 is an acryloyloxy group, a methacryloyloxy group, an aryl group, an alkyl group, a glycidoxy group, or an alkylene group having 1 to 10 carbon atoms and containing these functional groups, and R 1 It is bonded to the Si atom via a Si-C bond, and a represents an integer of 1 to 3. 2 is a hydrolyzable group consisting of an atom or group selected from an alkoxy group, an acyloxy group, and a halogen atom, and at least one R 2 The hydrolyzed groups form MO-Si bonds on the surfaces of the metal oxide particles, where M represents a Si atom or a Mg atom.
[0071] In formula (2), R 3 is an alkyl group and is bonded to the silicon atom through a Si-C bond, R 4 is a hydrolyzable group consisting of an atom or group selected from an alkoxy group, an acyloxy group, and a halogen atom, and at least one R 4 The hydrolyzed groups form MO-Si bonds on the surfaces of the metal oxide particles, where M represents a Si atom or a Mg atom, Y represents an alkylene group, an arylene group, an NH group, or an oxygen atom, d represents an integer of 0 to 3, and e represents an integer of 0 or 1.
[0072] When there are multiple hydrolyzable groups in formula (1) and formula (2), the silanol groups generated by their hydrolysis can be combined in any proportion on the surface of the metal oxide particles (forsterite particle surface) to form MO-Si bonds. M represents Si atom or Mg atom. For example, when there are three hydrolyzable groups and three silanol groups are formed, three MO-Si bonds can be formed, two MO-Si bonds can be formed, or one MO-Si bond can be formed. The remaining silanol groups exist freely. In addition, the multiple hydrolyzable groups in the hydrolyzable silane compounds shown in formula (1) and formula (2) can be completely hydrolyzed, or some of them can remain as hydrolyzable groups in an unhydrolyzed state.
[0073] The alkyl group is a linear or branched alkyl group having 1 to 10 carbon atoms, and examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-butyl, The invention relates to 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1-dimethyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl and 1-ethyl-2-methyl-n-propyl, etc.
[0074] In addition, a cyclic alkyl group can also be used. For example, as a cyclic alkyl group having 1 to 10 carbon atoms, there can be mentioned a cyclopropyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, a cyclopentyl group, a 1-methyl-cyclobutyl group, a 2-methyl-cyclobutyl group, a 3-methyl-cyclobutyl group, a 1,2-dimethyl-cyclopropyl group, a 2,3-dimethyl-cyclopropyl group, a 1-ethyl-cyclopropyl group, a 2-ethyl-cyclopropyl group, a cyclohexyl group, a 1-methyl-cyclopentyl group, a 2-methyl-cyclopentyl group, a 3-methyl-cyclopentyl group, a 1-ethyl-cyclobutyl group, a 2-ethyl-cyclobutyl group, a 3-ethyl-cyclobutyl group, a 1,2-dimethyl-cyclobutyl group cyclopropyl, 1-ethyl-2-methyl-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl and 2-ethyl-3-methyl-cyclopropyl, etc.
[0075] Examples of the alkylene group include alkylene groups derived from the above-mentioned alkyl groups, for example, a methyl group may be a methylene group, an ethyl group may be an ethylene group, and a propyl group may be a propylene group.
[0076] Examples of the alkenyl group include an alkenyl group having 2 to 10 carbon atoms, such as vinyl, 1-propenyl, 2-propenyl, 1-methyl-1-vinyl, 1-butenyl, 2-butenyl, 3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylvinyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 1-n-propylvinyl, 1-methyl-1-butenyl, 1-methyl-2-butenyl, 1-methyl-3-butenyl, 2-ethyl-2-propenyl, 2-methyl-1-butenyl, 2-methyl-2-butenyl, 2-methyl-3-butenyl, 1-butylene, 3-methyl-1-butylene, 3-methyl-2-butylene, 3-methyl-3-butylene, 1,1-dimethyl-2-propenyl, 1-isopropylvinyl, 1,2-dimethyl-1-propenyl, 1,2-dimethyl-2-propenyl, 1-cyclopentenyl, 2-cyclopentenyl, 3-cyclopentenyl, 1-hexenyl, 2-hexenyl, 3-hexenyl, 4-hexenyl, 5-hexenyl, 1-methyl-1-pentenyl, 1-methyl-2-pentenyl, 1-methyl-3-pentenyl, 1-methyl-4-pentenyl, 1-n-butylvinyl, 2-methyl-1-pentenyl, 2-methyl-2-pentenyl, 2-methyl-3-pentenyl 1,2-dimethyl-2-butenyl, 1,2-dimethyl-3-butenyl, 1,2-dimethyl-1-butenyl, 1,2-dimethyl-2-butenyl, 1,2-dimethyl-3-butenyl, 1-methyl-2-ethyl-2-propenyl, 1-sec-butylvinyl, 1,3- -dimethyl-1-butenyl, 1,3-dimethyl-2-butenyl, 1,3-dimethyl-3-butenyl, 1-isobutylvinyl, 2,2-dimethyl-3-butenyl, 2,3-dimethyl-1-butenyl, 2,3-dimethyl-2-butenyl, 2,3-dimethyl-3-butenyl, 2-isopropyl-2-propenyl, 3,3-dimethyl-1-butenyl, 1-ethyl-1-butenyl, 1-ethyl-2-butenyl, 1-ethyl-3-butenyl, 1-n-propyl-1-propenyl, 1-n-propyl-2-propenyl, 2-ethyl-1-butenyl, 2-ethyl-2-butenyl, 2-ethyl-3-butenyl, 1,1,2-Trimethyl-2-propenyl, 1-tert-butylvinyl, 1-methyl-1-ethyl-2-propenyl, 1-ethyl-2-methyl-1-propenyl, 1-ethyl-2-methyl-2-propenyl, 1-isopropyl-1-propenyl, 1-isopropyl-2-propenyl, 1-methyl-2-cyclopentenyl, 1-methyl-3-cyclopentenyl, 2-methyl-1-cyclopentenyl, 2-methyl-2-cyclopentenyl cyclopentenyl, 2-methyl-3-cyclopentenyl, 2-methyl-4-cyclopentenyl, 2-methyl-5-cyclopentenyl, 2-methylene-cyclopentyl, 3-methyl-1-cyclopentenyl, 3-methyl-2-cyclopentenyl, 3-methyl-3-cyclopentenyl, 3-methyl-4-cyclopentenyl, 3-methyl-5-cyclopentenyl, 3-methylene-cyclopentyl, 1-cyclohexenyl, 2-cyclohexenyl and 3-cyclohexenyl, etc.
[0077] Examples of the aryl group include aryl groups having 6 to 20 carbon atoms, such as phenyl, o-methylphenyl, m-methylphenyl, p-methylphenyl, o-chlorophenyl, m-chlorophenyl, p-chlorophenyl, o-fluorophenyl, p-mercaptophenyl, o-methoxyphenyl, p-methoxyphenyl, p-aminophenyl, p-cyanophenyl, α-naphthyl, β-naphthyl, o-biphenyl, m-biphenyl, p-biphenyl, 1-anthryl, 2-anthryl, 9-anthryl, 1-phenanthryl, 2-phenanthryl, 3-phenanthryl, 4-phenanthryl and 9-phenanthryl.
[0078] Examples of the organic group having an epoxy group include a glycidoxymethyl group, a glycidoxyethyl group, a glycidoxypropyl group, a glycidoxybutyl group, and an epoxycyclohexyl group.
[0079] Examples of the organic group having an acryloyl group include an acryloylmethyl group, an acryloylethyl group, and an acryloylpropyl group.
[0080] Examples of the organic group having a methacryloyl group include a methacryloylmethyl group, a methacryloylethyl group, and a methacryloylpropyl group.
[0081] Examples of the organic group having a mercapto group include ethylmercapto, butylmercapto, hexylmercapto, and octylmercapto.
[0082] Examples of the organic group having a cyano group include a cyanoethyl group and a cyanopropyl group.
[0083] Examples of the alkoxy group having 1 to 10 carbon atoms include alkoxy groups having a linear, branched, or cyclic alkyl group having 1 to 10 carbon atoms, such as a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, an n-pentoxy group, a 1-methyl-n-butoxy group, a 2-methyl-n-butoxy group, a 3-methyl-n-butoxy group, a 1,1-dimethyl-n-propoxy group, a 1,2-dimethyl-n-propoxy group, a 2,2-dimethyl-n-propoxy group, a 1-ethyl-n-propoxy group, an n-hexyloxy group, a 1-methyl-n-pentoxy group, a 2-methyl-n-pentoxy group 1-ethyl-n-butoxy, 2-ethyl-n-butoxy, 1,1,2-trimethyl-n-propoxy, 1,2,2-trimethyl-n-propoxy, 1-ethyl-1-methyl-n-propoxy and 1-ethyl-2-methyl-n-propoxy. Examples of cyclic alkoxy groups include cyclopropyloxy, Cyclobutyloxy, 1-methyl-cyclopropyloxy, 2-methyl-cyclopropyloxy, cyclopentyloxy, 1-methyl-cyclobutyloxy, 2-methyl-cyclobutyloxy, 3-methyl-cyclobutyloxy, 1,2-dimethyl-cyclopropyloxy, 2,3-dimethyl-cyclopropyloxy, 1-ethyl-cyclopropyloxy, 2-ethyl-cyclopropyloxy, cyclohexyloxy, 1-methyl-cyclopentyloxy, 2-methyl-cyclopentyloxy, 3-methyl-cyclopentyloxy, 1-ethyl-cyclobutyloxy, 2-ethyl-cyclobutyloxy, 3-ethyl-cyclobutyloxy, 1,2-dimethyl-cyclobutyloxy, 1,3-dimethyl-cyclobutyloxy, 2, 2-dimethyl-cyclobutyloxy, 2,3-dimethyl-cyclobutyloxy, 2,4-dimethyl-cyclobutyloxy, 3,3-dimethyl-cyclobutyloxy, 1-n-propyl-cyclopropyloxy, 2-n-propyl-cyclopropyloxy, 1-isopropyl-cyclopropyloxy, 2-isopropyl-cyclopropyloxy, 1,2,2-trimethyl-cyclopropyloxy, 1,2,3-trimethyl-cyclopropyloxy, 2,2,3-trimethyl-cyclopropyloxy, 1-ethyl-2-methyl-cyclopropyloxy, 2-ethyl-1-methyl-cyclopropyloxy, 2-ethyl-2-methyl-cyclopropyloxy and 2-ethyl-3-methyl-cyclopropyloxy, etc.
[0084] Examples of the acyloxy group having 2 to 20 carbon atoms include methylcarbonyloxy, ethylcarbonyloxy, n-propylcarbonyloxy, isopropylcarbonyloxy, n-butylcarbonyloxy, isobutylcarbonyloxy, sec-butylcarbonyloxy, tert-butylcarbonyloxy, n-pentylcarbonyloxy, 1-methyl-n-butylcarbonyloxy, 2-methyl-n-butylcarbonyloxy, 3-methyl-n-butylcarbonyloxy, 1,1-dimethyl-n-propylcarbonyloxy, 1,2-dimethyl-n-propylcarbonyloxy, 2,2-dimethyl-n-propylcarbonyloxy, 1-ethyl-n-propylcarbonyloxy, n-hexylcarbonyloxy, 1-methyl-n-pentylcarbonyloxy, 2-methyl-n-pentylcarbonyloxy, 3-methyl-n-pentylcarbonyloxy, carbonyloxy, 4-methyl-n-pentylcarbonyloxy, 1,1-dimethyl-n-butylcarbonyloxy, 1,2-dimethyl-n-butylcarbonyloxy, 1,3-dimethyl-n-butylcarbonyloxy, 2,2-dimethyl-n-butylcarbonyloxy, 2,3-dimethyl-n-butylcarbonyloxy, 3,3-dimethyl-n-butylcarbonyloxy, 1-ethyl-n-butylcarbonyloxy, 2-ethyl-n-butylcarbonyloxy, 1,1,2-trimethyl-n-propylcarbonyloxy, 1,2,2-trimethyl-n-propylcarbonyloxy, 1-ethyl-1-methyl-n-propylcarbonyloxy, 1-ethyl-2-methyl-n-propylcarbonyloxy, phenylcarbonyloxy, and tosylcarbonyloxy, etc.
[0085] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0086] Examples of the silicon-containing compound represented by formula (1) include tetramethoxysilane, tetrachlorosilane, tetraacetoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetraisopropoxysilane, tetra-n-butoxysilane, tetraacetoxysilane, methyltrimethoxysilane, methyltrichlorosilane, methyltriacetoxysilane, methyltripropoxysilane, methyltriacetoxysilane, methyltributoxysilane, methyltripropoxysilane, methyltripentoxysilane, methyltriphenoxysilane, methyltripenyloxysilane, methyltriphenethoxysilane, and glycidoxysilane. Methyltrimethoxysilane, glycidoxymethyltriethoxysilane, α-glycidoxyethyltrimethoxysilane, α-glycidoxyethyltriethoxysilane, β-glycidoxyethyltrimethoxysilane, β-glycidoxyethyltriethoxysilane, α-glycidoxypropyltrimethoxysilane, α-glycidoxypropyltriethoxysilane, β-glycidoxypropyltrimethoxysilane, β-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyl Oxypropyltripropoxysilane, γ-glycidoxypropyltributoxysilane, γ-glycidoxypropyltriphenoxysilane, α-glycidoxybutyltrimethoxysilane, α-glycidoxybutyltriethoxysilane, β-glycidoxybutyltriethoxysilane, γ-glycidoxybutyltrimethoxysilane, γ-glycidoxybutyltriethoxysilane, δ-glycidoxybutyltrimethoxysilane, δ-glycidoxybutyltriethoxysilane, (3,4-epoxycyclohexyl)methyltrimethoxysilane, (3,4-epoxycyclohexyl)methyl Triethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltriproxylsilane, β-(3,4-epoxycyclohexyl)ethyltributoxysilane, β-(3,4-epoxycyclohexyl)ethyltriphenoxysilane, γ-(3,4-epoxycyclohexyl)propyltrimethoxysilane, γ-(3,4-epoxycyclohexyl)propyltriethoxysilane, δ-(3,4-epoxycyclohexyl)butyltrimethoxysilane, δ-(3,4-epoxycyclohexyl)ethyltriproxylsilane,4-Epoxycyclohexyl)butyltriethoxysilane, glycidoxymethylmethyldimethoxysilane, glycidoxymethylmethyldiethoxysilane, α-glycidoxyethylmethyldimethoxysilane, α-glycidoxyethylmethyldiethoxysilane, β-glycidoxyethylmethyldimethoxysilane, β-glycidoxyethylethyldimethoxysilane, α-glycidoxypropylmethyldimethoxysilane, α-glycidoxypropylmethyldiethoxysilane, β-glycidoxypropylmethyldimethoxysilane, β-glycidoxypropylethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropylmethyldipropoxysilane, γ-cyclohexyl)butyltriethoxysilane, glycidoxymethylmethyldimethoxysilane, α-glycidoxypropylmethyldiethoxysilane, β-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropylmethyldipropoxysilane, γ-cyclohexyl)butyltriethoxysilane, γ-Glycidoxypropylmethyldibutyloxysilane, γ-Glycidoxypropylmethyldiphenoxysilane, γ-Glycidoxypropylethyldimethoxysilane, γ-Glycidoxypropylethyldiethoxysilane, γ-Glycidoxypropylvinyldimethoxysilane, γ-Glycidoxypropylvinyldiethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, vinyltrimethoxysilane, vinyltrichlorosilane, vinyltriacetoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane, methoxyphenyltrimethoxysilane, methoxyphenyltriethoxysilane, methoxyphenyltriacetoxysilane, methoxyphenyltrichlorosilane, methoxybenzyltrimethoxysilane, methoxybenzyltriethoxysilane, methoxybenzyl triacetoxysilane, methoxybenzyl trichlorosilane, methoxyphenethyl trimethoxysilane, methoxyphenethyl triethoxysilane, methoxyphenethyl triacetoxysilane, methoxyphenethyl trichlorosilane, ethoxyphenyl trimethoxysilane, ethoxyphenyl triethoxysilane, ethoxyphenyl triacetoxysilane, ethoxyphenyl trichlorosilane, ethoxybenzyl trimethoxysilane, ethoxybenzyl triethoxysilane, ethoxybenzyl triacetoxysilane, ethoxybenzyl trichlorosilane, isopropoxyphenyl trimethoxysilane, isopropoxyphenyl triethoxysilane, isopropoxyphenyl triacetoxysilane, isopropoxyphenyl trichlorosilane, isopropoxybenzyl trimethoxysilane, isopropoxybenzyl triethoxysilane, isopropoxybenzyl triacetoxysilane Oxysilane, isopropoxybenzyltrichlorosilane, tert-butoxyphenyltrimethoxysilane, tert-butoxyphenyltriethoxysilane, tert-butoxyphenyltriacetoxysilane, tert-butoxyphenyltrichlorosilane, tert-butoxybenzyltrimethoxysilane, tert-butoxybenzyltriethoxysilane, tert-butoxybenzyltriacetoxysilane, tert-butoxybenzyltrichlorosilane, methoxynaphthyltrimethoxysilane, methoxynaphthyltriethoxysilane, methoxynaphthyltriacetoxysilane, methoxynaphthyltrichlorosilane, ethoxynaphthyltrimethoxysilane, ethoxynaphthyltriethoxysilane, ethoxynaphthyltriacetoxysilane, ethoxynaphthyltrichlorosilane, γ-chloropropyltrimethoxysilane, γ-chloropropyltriethoxysilane, γ-chloropropyltriacetoxysilane, 3,3,3-Trifluoropropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, β-cyanoethyltriethoxysilane, chloromethyltrimethoxysilane, chloromethyltriethoxysilane, dimethyldimethoxysilane, phenylmethyldimethoxysilane, dimethyldiethoxysilane, phenylmethyldiethoxysilane, γ-chloropropylmethyldimethoxysilane, γ-chloropropylmethyldiethoxysilane, dimethyldiacetoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptomethyldiethoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane, etc.
[0087] As the silicon-containing compound represented by formula (2), for example, methylenebistrimethoxysilane, methylenebistrichlorosilane, methylenebistriacetoxysilane, ethylenebistriethoxysilane, ethylenebistrichlorosilane, ethylenebistriacetoxysilane, propylenebistriethoxysilane, butylenebistrimethoxysilane, phenylenebistrimethoxysilane, phenylenebistriethoxysilane, phenylenebismethyldiethoxysilane, phenylenebismethyldimethoxysilane, naphthylenebistrimethoxysilane, bistrimethoxydisilane, bistriethoxydisilane, bisethyldiethoxydisilane, bismethyldimethoxydisilane, hexamethyldisilane, hexamethyldisilazane, hexamethyldisiloxane, and the like.
[0088] In the hydrolysis of the alkoxysilyl group, the acyloxysilyl group or the halosilyl group, 0.5 mol to 100 mol, preferably 1 mol to 10 mol of water is used per 1 mol of the hydrolyzable group.
[0089] Furthermore, the hydrolysis catalyst can be used in an amount of 0.001 to 10 mol, preferably 0.001 to 1 mol, per 1 mol of the hydrolyzable group.
[0090] The reaction temperature for hydrolysis and surface coating is usually 20°C to 80°C.
[0091] The hydrolysis may be complete or partial, that is, unhydrolyzed monomers may remain in the hydrolyzate.
[0092] The hydrolysis can be carried out by adding water and heating. In addition, a catalyst can be used when the surface is coated by hydrolysis.
[0093] Nitric acid is used as a hydrolysis catalyst. In addition to nitric acid, a metal chelate, an organic acid, an inorganic acid, an organic base, or an inorganic base may be used in combination.
[0094] When coating is performed by a silane compound, it can also be performed in a dry manner, but the forsterite particles can be dispersed in water or an organic solvent. The dispersion can be performed by replacing the aqueous medium solvent with an organic solvent. The solvent replacement can be performed by evaporation or ultrafiltration. As organic solvents, methanol, ethanol, isopropanol, butanol, diacetone alcohol, methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, methyl isobutyl methanol, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monobutyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxylate, ethyl hydroxylate, methyl 2-hydroxy-3-methylbutyrate, 3- Methyl methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol dipropyl ether, propylene glycol dibutyl ether, ethyl lactate, propyl lactate, lactic acid Isopropyl, butyl lactate, isobutyl lactate, methyl formate, ethyl formate, propyl formate, isopropyl formate, butyl formate, isobutyl formate, pentyl formate, isoamyl formate, methyl acetate, ethyl acetate, pentyl acetate, isoamyl acetate, hexyl acetate, methyl propionate, ethyl propionate, propyl propionate, isopropyl propionate, butyl propionate, isobutyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, isopropyl butyrate, butyl butyrate, isobutyl butyrate, ethyl hydroxyacetate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxy-2-methylpropionate, methyl 2-hydroxy-3-methylbutyrate, methoxyethyl ethyl acetate, ethyl ethoxylate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-methoxybutyl acetate, 3-methoxypropyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, 3-methyl-3-methoxybutyl butyrate, methyl acetoacetate, methyl propyl ketone, methyl butyl ketone, 2-heptanone, 3-heptanone, 4-heptanone, N,N-dimethylformamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpyrrolidone, 4-methyl-2-pentanol, and γ-butyrolactone, etc.
[0095] These solvents may be used alone or in combination of two or more.
[0096] The method for producing forsterite particles of the present invention comprises the following steps (A) to (C):
[0097] (A) step: a step of preparing forsterite particles by mixing a magnesium compound serving as a magnesium source and a silicon compound serving as a silicon source so that the molar ratio of magnesium to silicon (MgO / SiO2) is 1.90 to 2.10,
[0098] (B) step: a step of introducing the forsterite particles prepared in step (A) into a hydrocarbon combustion flame and recovering the forsterite particles,
[0099] Step (C): a step of calcining the forsterite particles obtained in step (B) at 700°C to 1100°C.
[0100] As the magnesium compound serving as the magnesium source in the step (A), an inorganic magnesium compound or an organic magnesium salt may be used.
[0101] As the inorganic magnesium compound, for example, magnesium oxide, magnesium hydroxide, basic magnesium carbonate, magnesium hydrogen carbonate, magnesium carbonate, magnesium nitrate, or a mixture thereof can be used.
[0102] As the magnesium organic acid salt, for example, magnesium formate, magnesium acetate, magnesium propionate, magnesium butyrate, magnesium isobutyrate, magnesium valerate, magnesium acrylate, magnesium crotonate, magnesium halogenated aliphatic monocarboxylates having 1 to 4 carbon atoms such as magnesium monochloroacetate, magnesium dichloroacetate, magnesium trichloroacetate, magnesium malonate, magnesium succinate, magnesium adipate, magnesium maleate, magnesium aliphatic polycarboxylates having 1 to 4 carbon atoms such as magnesium glycolate, magnesium lactate, magnesium glycerate, magnesium malate, magnesium tartrate, magnesium citrate, magnesium gluconate, magnesium alkoxycarboxylates having 1 to 4 carbon atoms such as magnesium methoxyacetate, magnesium ethoxyacetate, magnesium oxocarboxylates having 1 to 4 carbon atoms such as magnesium acetoacetate, or a mixture thereof can be used.
[0103] As the silicon compound serving as the silicon source in step (A), silicon oxide, alkoxysilane, or a mixture thereof can be used.
[0104] As silicon oxide, for example, colloidal silica, silica gel, fumed silica, aerosil, precipitated silica, fused silica, silica, etc. can be used. As for the particle size, the average primary particle size thereof can be within the range of 10 nm to 100 μm.
[0105] As the alkoxysilane of the silicon compound serving as the silicon source, for example, tetramethoxysilane, tetraethoxysilane, or a hydrolyzate or hydrolysis-condensate thereof, or a mixture thereof can be used. Silica particles obtained by hydrolyzing / condensing an alkoxysilane can be used.
[0106] The magnesium compound serving as the magnesium source and the silicon compound serving as the silicon source may be mixed in a dry or wet manner. In the case of dry mixing, the powders may be uniformly mixed by a mixer or the like. In the case of wet mixing, the powder of one party may be mixed in an aqueous medium of the other party, or the two aqueous media may be mixed using a mixing dispersing machine such as a dispersing machine. As for colloidal silica, a silica sol may be used as an aqueous medium, and may be used as the above-mentioned aqueous medium.
[0107] The forsterite particles used in the present invention can be prepared by mixing a magnesium compound serving as a magnesium source and a silicon compound serving as a silicon source in a manner such that the MgO / SiO2 molar ratio is 1.90 to 2.10 (preferably 2.0) and calcining to prepare the forsterite particles as a raw material, and prepare the raw material used in the step (B) described later. In addition, commercially available forsterite particles can be used as a starting material to prepare the raw material used in the step (B) described later.
[0108] When the magnesium compound that will become the magnesium source and the silicon compound that will become the silicon source are mixed and fired to synthesize the forsterite particles that will become the raw material of the present invention, it is preferred to perform the firing at a temperature of 800° C. to 1800° C. and a firing time of about 1 hour to 10 hours. The forsterite particles obtained in the step (A) are non-spherical particles, and can be crushed to form fine non-spherical (crushed) powders for thermal spraying in the step (B).
[0109] In the present invention, even after the (B) step, the crushed particles can be sphericalized while maintaining the particle size. The particle size of the (A) step can be close to the particle size of the spherical particles obtained in the (C) step. Therefore, the particle size of the crushed forsterite in the (A) step can be set in the range of 0.1 μm to 10 μm.
[0110] (B) process is a process of making non-spherical (crushed) forsterite particles into spherical forsterite particles by thermal spraying. It is a process of putting the forsterite particles modulated in the (A) process into the combustion flame of hydrocarbons. In these thermal spraying methods, raw materials can be put into the combustion flame of the burner, so that the raw materials are melted and spheroidized by surface tension in the middle of falling by gravity. Therefore, the forsterite of crushed particles put into the combustion flame of hydrocarbons is spheroidized by surface tension in the middle of melting and falling by gravity to generate spherical forsterite particles. The resulting spherical forsterite particles are particles with few surface silanol groups, low specific surface area, and difficulty in fusion due to surface melting. When the crushed forsterite particles are put into the combustion flame, it can be either an aqueous solution or a powder, but in order to promote melting, it is preferred to directly put the powdered forsterite particles into the combustion flame.
[0111] The burner can use air (oxygen concentration 20.9%), oxygen-enriched air (oxygen concentration greater than 20.9% and less than 100%), and oxygen (oxygen concentration 100%) as the gas (combustion gas) for burning hydrocarbons. Burners for burning hydrocarbons include air burners (theoretical temperature 1800°C), oxygen-enriched air burners (theoretical temperature 1800°C to 2800°C), and oxygen burners (theoretical temperature 2800°C to 3000°C). However, since the melting point of forsterite is 1880°C to 1900°C, the theoretical temperature in the combustion flame of hydrocarbons in step (B) is preferably 1900°C to 3000°C, and it is preferred to use an oxygen burner.
[0112] The raw material input to the burner can be a method of directly inputting the aqueous medium of the raw material forsterite particles into the burner, or since the raw material forsterite particles themselves can be treated as powder, the latter powder can be directly input into the burner in the present invention. For the combustion furnace, the powder of the raw material forsterite particles is input into the flame generated by hydrocarbon gas (using, for example, standard 13A industrial city gas, propane gas as a hydrocarbon source.) and combustion gas (oxygen). The forsterite particles melted and vaporized and condensed in the upper part of the combustion furnace become spherical and cooled in the process of falling to the lower part of the combustion furnace. The post-combustion gas containing forsterite particles induced to the lower part of the combustion furnace is diluted and cooled by the external air, and due to the suction of the above-mentioned gas by a fan, it is discharged to the outside of the furnace through a cyclone separator dust collector and a filter device. By setting a cyclone separator and a filter in the middle of the piping, the spherical forsterite particles can be separated. The recovery rate can be set in the range of 40% to 90%.
[0113] The combustion amount in the furnace depends on the size of the device, but can be set within the range of 50,000 kcal / hour to 200,000 kcal / hour, for example, and can be set to 120,000 kcal / hour, for example. The supply rate of raw material powder into the furnace is within the range of 1 kg to 20 kg / hour, for example, and can be set to 7.5 kg / hour.
[0114] In the step (C), the crystallinity is improved by calcining the forsterite particles obtained in the step (B) at 700°C to 1100°C. The forsterite particles have the following characteristics: due to the production by thermal spraying, the surface area is small, the amount of surface hydroxyl groups is small, so the moisture absorption is low, and it is difficult for the particles to fuse with each other. The re-calcining temperature in the step (C) is appropriately 700°C to 1100°C. If it is below 700°C, sufficient crystallinity cannot be obtained, and if it is above 1100°C, the particles are easily fused. The forsterite particles have high crystallinity, especially at a calcining temperature of 800°C to 1100°C, or 800°C to 1000°C, especially 800°C to 900°C, and the forsterite particles can obtain a low dielectric loss tangent value of 0.0011 or less, for example, 0.0009 to 0.0011, so it is preferred.
[0115] The forsterite particles used as the raw material of step (A) are crushed particles, and the integrated intensity of the diffraction peak at 2θ=52° to 53° measured by an X-ray diffraction method using CuKα rays is 800 counts·deg or less, and the dielectric loss tangent has a value of about 0.003 to 0.02.
[0116] In the step (B), the crystallinity is reduced due to rapid cooling when falling from the combustion flame, so if it is left as it is, it does not have an appropriate dielectric loss tangent value. The spherical forsterite particles obtained in the step (B) have an integrated intensity of a diffraction peak of 2θ=52° to 53° measured by an X-ray diffraction method using CuKα rays of less than 700 counts·deg, and a dielectric loss tangent of about 0.005 to 0.015.
[0117] By adding the step (C), the crystallinity of the spherical forsterite particles is restored, and the integrated intensity of the diffraction peak at 2θ=52° to 53° measured by the X-ray diffraction method using CuKα rays becomes 800 counts·deg or more, and the dielectric loss tangent is 0.0003 to 0.0025. As mentioned above, the re-sintering temperature is appropriately 700°C to 1100°C, and if it is below 700°C, sufficient crystallinity cannot be obtained, and if it is above 1100°C, the particles are easily fused.
[0118] As described above, in the (C) step, the forsterite particles have high crystallinity, particularly at a sintering temperature of 800°C to 1100°C, or 800°C to 1000°C, particularly 800°C to 900°C, and can obtain a dielectric loss tangent value of 0.0011 or less, for example, 0.0008 to 0.0011, and are therefore preferred.
[0119] In addition, in the thermal spraying of the forsterite particles in the process (A) of the present invention, the shape of the particles changes from non-spherical (crushed) to spherical, but spherical particles are obtained while maintaining the particle size. The dielectric loss tangent of the forsterite particles also changes in proportion to the size of the particle size. For small particles, the dielectric loss tangent becomes high, but in the present invention, even through the process (B), the particle size does not change, so the dielectric loss tangent can also be maintained at a low state.
[0120] In addition, it has the following characteristics: the surface area is small due to the production by thermal spraying, the number of hydroxyl groups bonded to Si atoms and Mg atoms existing on the surface is small, so the moisture absorption is low, and the particles are unlikely to fuse with each other.
[0121] The forsterite particles that have been subjected to the step (C) may be subjected to a slight pulverization step (D) in order to eliminate slight adhesion.
[0122] Furthermore, in order to further hydrophobize the surface of the forsterite particles, the surface may be coated with the above-mentioned hydrolyzable silane.
[0123] In the present invention, the forsterite particles can be mixed with a resin to manufacture a substrate material. The resin is mixed by mixing the forsterite particles in a molten resin and kneading. The mixing uses an intermittent mixer, a continuous mixer, a twin-screw extruder, etc. In addition, when using a resin dissolved in a solvent, the forsterite particles are added / mixed to a solvent obtained by dissolving the resin, and varnishing is obtained, and the varnish is applied or impregnated on a substrate and then heat-treated and light-irradiated to solidify.
[0124] As the substrate resin, for example, polytetrafluoroethylene (PTFE), oligomeric polyphenylene ether resin (OPE), polyphenylene ether resin (PPE), polyethylene resin (PE), bismaleimide triazine resin (BT), liquid crystal resin (LCP), polysulfone resin (PS), polyethersulfone resin (PES), polycarbonate resin (PC), polyimide resin (PI), epoxy resin (EP), polyarylate resin (PA), phenol resin (PN), etc. It is also desirable that the relative dielectric constant and dielectric loss tangent of the substrate resin are low, and polytetrafluoroethylene (PTFE), oligomeric polyphenylene ether resin (OPE), polyphenylene ether resin (PPE), bismaleimide triazine resin (BT), and liquid crystal resin (LCP) can obtain a substrate with a low dielectric loss tangent.
[0125] The substrate resin can be used in a ratio of the resin to the forsterite particles in a mass ratio of 1:0.001 to 1000, 1:0.01 to 300, or 1:0.1 to 100.
[0126] The dielectric loss tangent of the substrate resin obtained by mixing the resin and the forsterite particles may be in the range of 0.0003 to 0.01.
[0127] The mixing of forsterite particles into the substrate resin is affected by the thermal expansion and hydrophilicity of the resin, and therefore, in addition to forsterite particles, particles such as silica particles and cordierite particles, glass cloth, etc. may be included unless the above characteristics are impaired.
[0128] Example
[0129] (Evaluation method)
[0130] Determination of average particle size
[0131] The particle size distribution was measured using a laser diffraction particle size distribution analyzer (trade name: MASTERSIZER2000) (manufactured by Malvern).
[0132] ·Determination of dielectric loss tangent
[0133] Using a cavity resonator fixture for measuring frequencies of 1 GHz and 10 GHz (manufactured by Keycom Co., Ltd.), a PTFE sample tube (length 30 mm, inner diameter 3 mm (for 1 GHz), 1 mm (for 10 GHz)) was filled with the powder sample, and then measured using a vector network analyzer FieldFox N6626A (manufactured by KEYSIGHT TECHNOLOGIES).
[0134] · Determination of specific surface area based on BET method
[0135] The surface area was measured using a surface area measuring device based on the BET method (trade name Monosorb (manufactured by Quantachrome Instruments)) using the 1-point method (relative pressure 0.3) of the BET method. The average primary particle size was calculated by (3 / (3.2(g / cm 3 )×Specific surface area based on BET method (m 2 / g)))×2(μm) is calculated.
[0136] ·XRD (powder X-ray diffraction) measurement
[0137] The X-ray diffraction apparatus MiniFlex600 (manufactured by Rigaku Corporation) was used for measurement at a tube voltage of 40 kV and a tube current of 15 mA. The integrated intensity was calculated as counts·deg (or cps·deg) by processing the above measured data using comprehensive powder X-ray analysis software PDXL2.
[0138] Determination of moisture adsorption rate
[0139] The powder sample was weighed in a magnetic crucible and dried in a dryer at 150°C for 24 hours. After weighing the mass after drying, the sample was kept in a constant temperature and humidity chamber set at 25°C and 50% for 48 hours and the mass was measured again. The water absorption (%) was calculated according to the following formula (4).
[0140] Moisture adsorption (%) = [(m1-m2) / m2] × 100 Formula (4)
[0141] [In formula (4), m1 represents the mass (g) of the forsterite particles after being dried at a temperature of 150°C for 24 hours and then left at a temperature of 25°C and a humidity of 50% for 48 hours, and m2 represents the mass (g) of the forsterite particles after being dried at a temperature of 150°C for 24 hours.]
[0142] (Synthesis of forsterite powder)
[0143] (Production Example 1)
[0144] As step (A), basic magnesium carbonate powder (manufactured by Kamishima Chemical Co., Ltd.) and silica sol (trade name: SNOTEX XS, manufactured by Nissan Chemical Co., Ltd.) are mixed and dried in a molar ratio of MgO:SiO2=2:1, the dried product is crushed with a chopper, and then calcined at 1200°C for 2 hours in an electric furnace to prepare forsterite powder.
[0145] The powder obtained above was further pulverized by a dry jet mill at a pressure of 0.64 MPa to prepare a pulverized forsterite powder (average particle size: 2.3 μm).
[0146] (Synthesis of spherical forsterite powder)
[0147] (Example 1)
[0148] As step (B), the pulverized forsterite powder prepared in manufacturing example 1 was fed into the flame of an oxygen burner (theoretical temperature: 3000° C.) using propane gas as fuel and setting the combustion amount to 120,000 kcal at a supply rate of 7.5 kg / h to perform thermal spraying, and spherical thermal sprayed forsterite powder was obtained in the cyclone separator recovery section. As step (C), the powder obtained in step (B) was calcined at 700° C. for 2 hours using an electric furnace to prepare forsterite powder.
[0149] The powder obtained by calcining maintained a spherical shape, and had an average particle size of 5.9 μm. The dielectric loss tangent was 0.0015 at a measurement frequency of 1 GHz and was 0.0017 at a measurement frequency of 10 GHz.
[0150] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 2.4 μm, and the sphericity calculated from the ratio to the above average particle size was 2.5.
[0151] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 894 counts·deg, and the water adsorption rate was 0.06%.
[0152] (Example 2)
[0153] In Example 1, forsterite powder was prepared by carrying out the same operation as in Example 1 except that the firing temperature in the electric furnace was changed to 800° C. as in the step (C).
[0154] The powder obtained by calcining maintained a spherical shape, and had an average particle size of 6.0 μm. The dielectric loss tangent was 0.0009 at a measurement frequency of 1 GHz and was 0.0008 at a measurement frequency of 10 GHz.
[0155] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 2.6 μm, and the sphericity calculated from the ratio to the above average particle size was 2.3.
[0156] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 917 counts·deg, and the water adsorption rate was 0.07%.
[0157] (Example 3)
[0158] In Example 1, forsterite powder was prepared by carrying out the same operation as in Example 1 except that the firing temperature in the electric furnace was changed to 900° C. as the step (C).
[0159] The powder obtained by calcining maintained a spherical shape, and had an average particle size of 7.1 μm. The dielectric loss tangent was 0.0015 at a measurement frequency of 1 GHz and was 0.0011 at a measurement frequency of 10 GHz.
[0160] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 2.6 μm, and the sphericity calculated from the ratio to the above average particle size was 2.7.
[0161] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 905 counts·deg, and the water adsorption rate was 0.07%.
[0162] (Example 4)
[0163] In Example 1, forsterite powder was prepared by carrying out the same operation as in Example 1 except that the firing temperature in the electric furnace was changed to 1000° C. as the step (C).
[0164] The powder obtained by sintering maintained a spherical shape, although some aggregation of particles was observed due to sintering. The average particle size was 6.3 μm, and the dielectric loss tangent was 0.0020 at a measurement frequency of 1 GHz and 0.0012 at a measurement frequency of 10 GHz.
[0165] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 2.6 μm, and the sphericity calculated from the ratio to the above average particle size was 2.4.
[0166] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 899 counts·deg, and the water adsorption rate was 0.06%.
[0167] (Example 5)
[0168] In Example 1, forsterite powder was prepared by carrying out the same operation as in Example 1 except that the firing temperature in the electric furnace was changed to 1100° C. as the step (C).
[0169] The powder obtained by sintering maintained a spherical shape, although some aggregation of particles was observed during sintering. The average particle size was 9.8 μm, and the dielectric loss tangent was 0.0024 at a measurement frequency of 1 GHz and 0.0013 at a measurement frequency of 10 GHz.
[0170] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 3.0 μm, and the sphericity calculated from the ratio to the above average particle size was 3.3.
[0171] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 891 counts·deg, and the water adsorption rate was 0.03%.
[0172] (Comparative Example 1)
[0173] In Production Example 1, as step (C), the forsterite powder obtained by calcining at 1200° C. for 2 hours in an electric furnace had an average particle size as large as 13.0 μm, and a dielectric loss tangent of 0.0015 at a measurement frequency of 1 GHz and 0.0012 at 10 GHz.
[0174] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 1.6 μm, and the sphericity calculated from the ratio to the above average particle size was 8.6.
[0175] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 877 counts·deg, and the water adsorption rate was 0.12%.
[0176] (Comparative Example 2)
[0177] Thermal spraying in step (B) and re-firing in step (C) were not performed in Example 1. The average particle size of the pulverized forsterite powder obtained by pulverization using a dry jet mill was 2.3 μm, and the dielectric loss tangent was 0.0032 at a measurement frequency of 1 GHz and 0.0042 at 10 GHz.
[0178] The primary particle size (BET particle size) calculated from the BET surface area was 0.9 μm, and the sphericity calculated from the ratio to the above average particle size was 2.6.
[0179] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 818 counts·deg, and the water adsorption rate was 0.26%.
[0180] (Comparative Example 3)
[0181] In Example 1, the thermal sprayed forsterite powder obtained after the thermal spraying in step (B) was not subjected to re-sintering in step (C). The average particle size of the spherical thermal sprayed forsterite powder obtained was 4.2 μm, and the dielectric loss tangent was 0.0050 at a measurement frequency of 1 GHz and 0.0054 at 10 GHz.
[0182] The primary particle size (BET particle size) calculated from the BET surface area was 2.3 μm, and the sphericity calculated from the ratio to the above average particle size was 1.8.
[0183] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 670, and the water adsorption rate was 0.16%.
[0184] (Comparative Example 4)
[0185] In Example 1, the burner used for the thermal spraying treatment was changed to an air burner (theoretical temperature: 1800° C.) and the powder supply rate was set to 5.0 kg / h. The thermal sprayed forsterite powder was obtained in the same manner as in Example 1. The obtained powder had significant agglomeration of particles, an average particle size of 7.6 μm, and a dielectric loss tangent of 0.0043 at a measurement frequency of 1 GHz and 0.0047 at 10 GHz.
[0186] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 2.2, and the sphericity calculated from the ratio to the above average particle size was 3.5.
[0187] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 870 counts·deg, and the water adsorption rate was 0.07%.
[0188] (Comparative Example 5)
[0189] As the step (C), the thermally sprayed forsterite powder obtained in Comparative Example 2 without the step (B) was calcined at 800° C. for 2 hours using an electric furnace to prepare forsterite powder. The obtained powder had significant agglomeration of particles, an average particle size of 10.2 μm, and a dielectric loss tangent of 0.0017 at a measurement frequency of 1 GHz and 0.0019 at 10 GHz.
[0190] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 2.3 μm, and the sphericity calculated from the ratio to the above average particle size was 4.4.
[0191] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 872 counts·deg, and the water adsorption rate was 0.06%.
[0192] (Comparative Example 6)
[0193] In Example 1, forsterite powder was prepared by carrying out the same operation as in Example 1 except that the firing temperature in the electric furnace was changed to 1200° C. in the step (C).
[0194] The powder obtained by calcining was found to be significantly aggregated with each other during sintering and did not maintain a spherical shape. The average particle size was 12.5 μm, and the dielectric loss tangent was 0.0021 at a measurement frequency of 1 GHz and 0.0017 at a measurement frequency of 10 GHz.
[0195] The primary particle size (BET particle size) calculated from the BET surface area was 3.5 μm, and the sphericity calculated from the ratio to the above average particle size was 3.6.
[0196] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 874, and the water adsorption rate was 0.06%.
[0197] The results of Examples 1 to 5 and Comparative Examples 1 to 6 are shown in the table below. In Examples 1 to 5, the average particle size was 4.2 μm to 9.8 μm, and the dielectric loss tangent was 0.0008 to 0.0024 at the measurement frequencies of 1 GHz and 10 GHz, showing excellent properties as a filler for high-frequency applications. In addition, the sphericity calculated from the ratio of the primary particle size (BET particle size) calculated from the BET surface area to the average particle size was 2.3 to 3.3, showing a good value for use as a filler.
[0198] Furthermore, the integrated intensity of the diffraction peak at 52-53° in XRD measurement (CuKα1) was as high as 891 counts·deg to 917 counts·deg, confirming that it has sufficient crystallinity for the performance of the characteristics of forsterite itself. In addition, the water adsorption rate also showed a low value of 0.03% to 0.07%, which is good as a filler for high-frequency applications.
[0199] On the other hand, in Comparative Examples 1 to 6, it was confirmed that the average particle size was as large as 10 μm or more (Comparative Examples 1, 5, and 6), and the dielectric loss tangent was as high as 0.0026 or more even when the average particle size was small (Comparative Examples 2, 3, and 4), which cannot be said to be excellent properties as a filler for high-frequency applications. In addition, the sphericity calculated from the ratio of the primary particle size (BET particle size) calculated from the BET surface area to the average particle size did not satisfy 1.0 to 3.3, and sometimes showed a value suggesting that particle aggregation was progressing (Comparative Examples 1, 4, 5, and 6), which was not good for use as a filler.
[0200] Furthermore, the integrated intensity of the diffraction peak at 52-53° in the XRD measurement (CuKα) was as low as 850 counts·deg or less, confirming that it did not have sufficient crystallinity for the expression of the characteristics of forsterite itself (Comparative Example 3). Even when the integrated intensity was 850-1000, the agglomeration of particles occurred, which was not suitable as a filler for high-frequency applications. In addition, the water adsorption rate also showed a high value of more than 0.1% (Comparative Examples 1, 2, and 3), which was not suitable as a filler for high-frequency applications.
[0201] (Example 6)
[0202] In Example 1, as the forsterite powder used for thermal spraying, forsterite trade name FF-200·M-40 (average particle size 2.5 μm) manufactured by Marusu Yoshinoya Kaisha was used, and spherical thermal sprayed forsterite powder was obtained in the same manner as in Example 1. The obtained powder was calcined at 800° C. for 2 hours using an electric furnace to prepare forsterite powder.
[0203] The powder obtained by calcining maintained a spherical shape, and had an average particle size of 5.6 μm. The dielectric loss tangent was 0.0008 at a measurement frequency of 1 GHz and was 0.0009 at a measurement frequency of 10 GHz.
[0204] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 2.3 μm, and the sphericity calculated from the ratio to the above average particle size was 2.4.
[0205] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 873 counts·deg, and the water adsorption rate was 0.05%.
[0206] (Example 7)
[0207] In Example 6, the same operation was carried out except that the calcination temperature in the electric furnace was changed to 900° C. to prepare forsterite powder.
[0208] The powder obtained by calcining maintained a spherical shape, and had an average particle size of 6.3 μm. The dielectric loss tangent was 0.0009 at a measurement frequency of 1 GHz and was 0.0010 at a measurement frequency of 10 GHz.
[0209] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 2.3 μm, and the sphericity calculated from the ratio to the above average particle size was 2.8.
[0210] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 870 counts·deg, and the water adsorption rate was 0.05%.
[0211] (Example 8)
[0212] In Example 6, the same operation was carried out except that the sintering temperature in the electric furnace was changed to 1000° C. to prepare forsterite powder.
[0213] The powder obtained by sintering maintained a spherical shape, although some aggregation of particles was observed due to sintering. The average particle size was 5.7 μm, and the dielectric loss tangent was 0.0009 at a measurement frequency of 1 GHz and 0.0010 at a measurement frequency of 10 GHz.
[0214] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 2.3 μm, and the sphericity calculated from the ratio to the above average particle size was 2.5.
[0215] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 865 counts·deg, and the water adsorption rate was 0.07%.
[0216] (Example 9)
[0217] In Example 6, the same operation was carried out except that the calcination temperature in the electric furnace was changed to 1100° C. to prepare forsterite powder.
[0218] The powder obtained by sintering maintained a spherical shape, although some aggregation of particles was observed due to sintering. The average particle size was 6.1 μm, and the dielectric loss tangent was 0.0011 at a measurement frequency of 1 GHz and 0.0011 at a measurement frequency of 10 GHz.
[0219] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 2.5 μm, and the sphericity calculated from the ratio to the above average particle size was 2.4.
[0220] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα1) was 882 counts·deg, and the water adsorption rate was 0.05%.
[0221] (Comparative Example 7)
[0222] In Example 6, thermal spraying in step (B) was not performed, and the purchased forsterite manufactured by Marusu Yokogaku Co., Ltd., trade name FF-200·M-40, had an average particle size of 4.3 μm and a dielectric loss tangent of 0.0115 at a measurement frequency of 1 GHz and 0.0198 at 10 GHz.
[0223] The primary particle size (BET particle size) calculated from the BET surface area was 0.1 μm, and the sphericity calculated from the ratio to the above average particle size was 31.9.
[0224] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 791 counts·deg, and the water adsorption rate was 0.40%.
[0225] (Comparative Example 8)
[0226] In Example 6, after thermal spraying in step (B), sintering in step (C) was not performed. The average particle size of the obtained spherical thermal sprayed forsterite powder was 5.2 μm, and the dielectric loss tangent was 0.0095 at a measurement frequency of 1 GHz and 0.0130 at 10 GHz.
[0227] The primary particle size (BET particle size) calculated from the BET surface area was 2.4 μm, and the sphericity calculated from the ratio to the above average particle size was 2.2.
[0228] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 361 counts·deg, and the water adsorption rate was 0.09%.
[0229] The results of Examples 6 to 9 and Comparative Examples 7 and 8 are shown in the table below. In Examples 6 to 9, the average particle size was 5.6 μm to 6.3 μm, and the dielectric loss tangent was 0.0008 to 0.0011 at the measurement frequencies of 1 GHz and 10 GHz, showing excellent properties as a filler for high-frequency applications. In addition, the sphericity calculated from the ratio of the average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method to the average particle size was 2.4 to 2.8, showing a good value for use as a filler.
[0230] Furthermore, the integrated intensity of the diffraction peak at 52-53° in XRD measurement (CuKα) is as high as 870 counts·deg to 882 counts·deg, confirming that it has sufficient crystallinity for the expression of the characteristics of forsterite itself. In addition, the water adsorption rate is as low as 0.05% to 0.07%, which is good as a filler for high-frequency applications.
[0231] On the other hand, in Comparative Examples 7 and 8, it was confirmed that the dielectric loss tangent was as high as 0.0026 or more, which cannot be said to be excellent characteristics as a filler for high-frequency applications.
[0232] Furthermore, the water adsorption rate was as high as 0.1% or more (Comparative Example 7), and was not suitable as a filler for high-frequency applications.
[0233] (Surface treatment of spherical forsterite particles)
[0234] (Example 10)
[0235] The forsterite powder obtained in Example 2 was added to 2-propanol in such a manner that the concentration of the forsterite powder became 20% by mass, and water was further added in such a manner that the water concentration became 1%. Among them, phenyltrimethoxysilane was added in such a manner that it became 0.01% by mass ratio relative to the forsterite powder, and then heated while stirring in a container, and heated for 5 hours under reflux conditions to perform surface treatment. After cooling, the contents were transferred to a flat container, and after removing the solvent, they were dried at 150°C for one night (about 12 hours) to prepare a surface-treated forsterite powder.
[0236] The average particle size of the obtained powder was 6.0 μm, and the dielectric loss tangent was 0.0007 at a measurement frequency of 1 GHz and was 0.0006 at a measurement frequency of 10 GHz.
[0237] The average primary particle size (particle size based on the BET method) calculated from the specific surface area based on the BET method was 2.2 μm, and the sphericity calculated from the ratio to the above average particle size was 2.7.
[0238] Furthermore, the integrated intensity of the diffraction peak at 52 to 53° in XRD measurement (CuKα) was 917 cps·deg, and the water adsorption rate was 0.05%.
[0239] (Resin composition containing spherical forsterite particles)
[0240] (Polymer solution formulation example 1)
[0241] 31.6 g of OPE-2St2200 / toluene (OPE, toluene solution, concentration 63% by mass), a low molecular weight polyphenylene ether manufactured by Mitsubishi Gas Chemical Co., Ltd., and 20.0 g of polystyrene-poly(ethylene-butylene) block-polystyrene (PSEBS, manufactured by Shigma-Aldrich, weight average molecular weight 118,000) were mixed in a mass ratio of OPE:PSEBS=50:50, and then diluted with 148.3 g of toluene so that the polymer concentration became 20% by mass, and stirred at room temperature to prepare 200 g of a mother polymer solution.
[0242] (Example 11)
[0243] After adding 0.4 g of the forsterite powder prepared in Example 6 to 8.0 g of the mother polymer solution prepared in Formulation Example 1 (polymer concentration 20% by mass), 1.6 g of toluene was added so that the solid content concentration became 20% by mass, and the mixture was stirred and mixed at room temperature for 1 hour to prepare a polymer / forsterite mixed solution. The polymer / forsterite ratio was 80 / 20 by mass.
[0244] The prepared mixed solution was cast on a cellulose release film and dried at 100° C. to remove the solvent. Thereafter, the mixed solution was peeled from the cellulose release film and heated at 200° C. for 2 hours to be cured to prepare a composite film (thickness: about 30 μm).
[0245] A test piece with a width of 30 mm and a length of 60 to 70 mm was cut from the modulated composite film, formed into a cylindrical shape, and filled into a PTFE tube with a length of 30 mm and an inner diameter of 3 mm. The dielectric loss tangent at a frequency of 1 GHz measured by the perturbation cavity resonance method was 0.0014.
[0246] (Example 12)
[0247] After adding 0.8 g of the forsterite powder prepared in Example 6 to 6.0 g of the mother polymer solution prepared in Formulation Example 1 (polymer concentration 20% by mass), 3.2 g of toluene was added so that the solid content concentration became 20% by mass, and the mixture was stirred and mixed at room temperature for 1 hour to prepare a polymer / forsterite mixed solution. The polymer / forsterite ratio was 60 / 40 by mass.
[0248] Using the prepared mixed solution, a composite film was prepared in the same manner as in Example 11, and the dielectric loss tangent at a frequency of 1 GHz was measured by a perturbation cavity resonance method to find that it was 0.0014.
[0249] (Example 13)
[0250] After adding 1.2 g of the forsterite powder prepared in Example 6 to 4.0 g of the mother polymer solution prepared in Formulation Example 1 (polymer concentration 20% by mass), 4.8 g of toluene was added so that the solid content concentration became 20% by mass, and the mixture was stirred and mixed at room temperature for 1 hour to prepare a polymer / forsterite mixed solution. The polymer / forsterite ratio was 40 / 60 by mass.
[0251] Using the prepared mixed solution, a composite film was prepared in the same manner as in Example 11, and the dielectric loss tangent at a frequency of 1 GHz was measured by a perturbation cavity resonance method to find that it was 0.0013.
[0252] (Comparative Example 9)
[0253] In Example 11, without adding forsterite powder, the mother polymer solution prepared in Formulation Example 1 was used to prepare a polymer film in the same manner, and the dielectric loss tangent at a frequency of 1 GHz was measured by a perturbation cavity resonance method and found to be 0.0015.
[0254] (Comparative Example 10)
[0255] After adding 0.4 g of the forsterite powder prepared in Comparative Example 1 to 8.0 g of the mother polymer solution prepared in Formulation Example 1 (polymer concentration 20% by mass), 1.6 g of toluene was added so that the solid content concentration became 20% by mass, and the mixture was stirred and mixed at room temperature for 1 hour to prepare a polymer / forsterite mixed solution. The polymer / forsterite ratio was 80 / 20 by mass.
[0256] Using the prepared mixed solution, a composite film was prepared in the same manner as in Example 11, and the dielectric loss tangent at a frequency of 1 GHz was measured by a perturbation cavity resonance method to find that it was 0.0015.
[0257] (Comparative Example 11)
[0258] To 6.0 g of the mother polymer solution prepared in Formulation Example 1 (polymer concentration 20% by mass), 0.8 g of the forsterite powder prepared in Comparative Example 1 was added, and then 3.2 g of toluene was added so that the solid content concentration became 20% by mass. The mixture was stirred and mixed at room temperature for 1 hour to prepare a polymer / forsterite mixed solution.
[0259] The prepared mixed solution was used to prepare a composite film in the same manner as in Example 11, and the dielectric loss tangent at a frequency of 1 GHz was measured by a perturbation cavity resonance method and found to be 0.0015. The polymer / forsterite ratio was 60 / 40 by mass.
[0260] (Comparative Example 12)
[0261] After adding 1.2 g of the forsterite powder prepared in Comparative Example 1 to 4.0 g of the mother polymer solution prepared in Formulation Example 1 (polymer concentration 20% by mass), 4.8 g of toluene was added so that the solid content concentration became 20% by mass, and the mixture was stirred and mixed at room temperature for 1 hour to prepare a polymer / forsterite mixed solution. The polymer / forsterite ratio was 40 / 60 by mass.
[0262] Using the prepared mixed solution, a composite film was prepared in the same manner as in Example 11, and the dielectric loss tangent at a frequency of 1 GHz was measured by a perturbation cavity resonance method to find that it was 0.0015.
[0263] The results of Examples 11 to 13 and Comparative Examples 9 to 12 are shown in the table below. As is clear from the table below, the dielectric loss tangent of the polymer / forsterite composite film blended with the forsterite powder of the present invention is 0.0015 (Comparative Example 9), and the dielectric loss tangent shows a value as low as 0.0013 to 0.0014 (Examples 11 to 13), compared to the dielectric loss tangent of 0.0015 of the polymer film alone (Comparative Example 9). The dielectric loss tangent of the polymer / forsterite composite film blended with the forsterite powder of the present invention is confirmed to reduce the dielectric loss tangent by blending the forsterite powder of the present invention, and it can be confirmed that it exhibits excellent characteristics as a filler for high-frequency applications. On the other hand, when the forsterite powder prepared in Comparative Example 1 is used, the dielectric loss tangent of the polymer / forsterite composite film is 0.0015 (Comparative Examples 10 to 12), and the dielectric loss tangent reduction effect of blending the forsterite powder cannot be confirmed.
[0264] [Table 1]
[0265] Table 1
[0266]
[0267] [Table 2]
[0268] Table 2
[0269]
[0270] [Table 3]
[0271] Table 3
[0272]
[0273] [Table 4]
[0274] Table 4
[0275]
[0276] [Table 5]
[0277] Table 5
[0278]
[0279] [Table 6]
[0280] Table 6 (In Table 6, P represents the mass part of the polymer, and F represents the mass part of forsterite.)
[0281]
[0282] [Table 7]
[0283] Table 7 (In Table 7, P represents the mass part of the polymer, and F represents the mass part of forsterite.)
[0284]
[0285] Industrial Availability
[0286] Providing forsterite particles with low dielectric loss tangent can provide a substrate material with low dielectric loss tangent in order to suppress signal degradation caused by the insulating material of the substrate. Since forsterite particles have low dielectric loss tangent, by making the resin contain spherical forsterite particles that are easy to mix with the resin to make a substrate material, it is possible to provide a substrate with improved dielectric properties and low transmission loss. Forsterite with low dielectric loss tangent and spherical particle shape can be manufactured to provide a substrate with improved high-frequency characteristics.
Claims
1. A forsterite particle having an average particle size of 0.1 μm to 10 μm and a dielectric loss tangent of 0.0003 to 0.0025, wherein the dielectric loss tangent is evaluated by measuring the values at 1 GHz and 10 GHz by a perturbation cavity resonator method in a resonator method, The sphericity of the forsterite particles calculated according to the following formula (3) is 1.0 to 3.
3. Sphericity = L s / N s Formula (3) In formula (3), L s It represents the average particle size measured by a laser diffraction particle size distribution analyzer, N s It represents the average primary particle size calculated by converting the specific surface area according to the measurement item of the nitrogen adsorption method, L s and N s The unit is μm. The moisture adsorption amount of the forsterite particles calculated according to the following formula (4) is 0.15% or less. Moisture adsorption (%) = [(m1-m2) / m2] × 100 Formula (4) In formula (4), m1 represents the mass of the forsterite particles after being dried at a temperature of 150°C for 24 hours and then placed at a temperature of 25°C and a humidity of 50% for 48 hours, and m2 represents the mass of the forsterite particles after being dried at a temperature of 150°C for 24 hours. The units of m1 and m2 are both g. The forsterite particles have an integrated intensity of a diffraction peak at 2θ=52° to 53° obtained by X-ray diffraction measurement using CuKα radiation of 800 counts·deg or more.
2. The forsterite particles according to claim 1, wherein the MgO / SiO2 molar ratio is 1.90 to 2.
10.
3. The forsterite particles according to claim 1 or 2, wherein the surface of the particles is coated with at least one hydrolyzable silane selected from the group consisting of the hydrolyzable silanes represented by the following formula (1) and formula (2), R 1 a Si(R 2 ) 4-a Formula (1) 〔R 3 d Si(R 4 ) 3-d 〕2Y e Formula (2) In formula (1), R 1is an acryloyloxy group, a methacryloyloxy group, an aryl group, an alkyl group, a glycidoxy group, or an alkylene group having 1 to 10 carbon atoms and containing these functional groups, and R 1 Combined with Si atom through Si-C bond, a represents an integer of 1 to 3; R 2 is a hydrolyzable group consisting of an atom or group selected from an alkoxy group, an acyloxy group, and a halogen atom, and at least one R 2 The hydrolyzed groups form MO-Si bonds on the surface of metal oxide particles, where M represents Si atom or Mg atom; In formula (2), R 3 is an alkyl group and is bonded to the silicon atom through a Si-C bond, R 4 is a hydrolyzable group consisting of an atom or group selected from an alkoxy group, an acyloxy group, and a halogen atom, and at least one R 4 The hydrolyzed group forms a MO-Si bond on the surface of the metal oxide particle, where M represents a Si atom or a Mg atom; Y represents an alkylene group, an arylene group, an NH group, or an oxygen atom; d represents an integer of 0 to 3, and e is an integer of 0 or 1.
4. The method for producing forsterite particles according to claim 1 or 2, comprising the following steps (A) to (C): (A) step: a step of preparing forsterite particles by mixing a magnesium compound serving as a magnesium source and a silicon compound serving as a silicon source so that the molar ratio of magnesium to silicon (MgO / SiO2) is 1.90 to 2.10, (B) step: a step of introducing the forsterite particles prepared in step (A) into a hydrocarbon combustion flame and recovering the forsterite particles, Step (C): a step of calcining the forsterite particles obtained in step (B) at 700°C to 1100°C. 5 . The production method according to claim 4 , wherein the magnesium compound serving as the magnesium source in step (A) is an inorganic magnesium compound or an organic magnesium salt.
6. The production method according to claim 5, wherein the inorganic magnesium compound is magnesium oxide, magnesium hydroxide, basic magnesium carbonate, magnesium hydrogen carbonate, magnesium carbonate, magnesium nitrate, or a mixture thereof.
7. The production method according to claim 5, wherein the magnesium organic acid salt is an aliphatic magnesium monocarboxylate having 1 to 4 carbon atoms, a halogenated magnesium monocarboxylate having 1 to 4 carbon atoms, an aliphatic magnesium polycarboxylate having 1 to 4 carbon atoms, an aliphatic magnesium hydroxycarboxylate having 1 to 4 carbon atoms, an alkoxy magnesium carboxylate having 1 to 4 carbon atoms, an oxo magnesium carboxylate having 1 to 4 carbon atoms, or a mixture thereof. 8 . The production method according to claim 4 , wherein the silicon compound serving as the silicon source in step (A) is silicon oxide, alkoxysilane, or a mixture thereof.
9. The production method according to claim 4 or 5, wherein the temperature in the combustion flame of hydrocarbons in step (B) is 1900°C to 3000°C in terms of theoretical temperature. 10 . The production method according to claim 4 or 5 , further comprising the step (D) of pulverizing the forsterite particles obtained in the step (C). 11 . The production method according to claim 4 or 5 , further comprising the step (E) of coating the forsterite particles obtained in the step (C) with the hydrolyzable silane according to claim 3 . 12 . A resin composition comprising a resin and the forsterite particles according to claim 1 . 13 . The resin composition according to claim 12 , wherein the ratio of the resin to the forsterite particles is 1:0.001 to 1000 in terms of mass ratio.
14. The resin composition according to claim 12 or 13, wherein the dielectric loss tangent is 0.0003 to 0.01, wherein the dielectric loss tangent is evaluated by measuring the values at 1 GHz and 10 GHz by a perturbation-mode cavity resonator method in a resonator method.
Citation Information
Patent Citations
Magnesium-containing oxide powder
JP2003002640A
Method for producing forsterite fine particles
JP2016222517A
Method for production of forsterite powder, forsterite powder, sintered forsterite, ceramic insulator composition, and laminated ceramic electronic element
CN101346310A
Production method for forsterite fine particles
CN105980333A
Silane-treated forsterite fine particles and production method therefor, and organic solvent dispersion of the silane-treated forsterite fine particles and production method therefor
CN106573788A