Expanded and expandable granular materials
By preparing a mixture of silicate and alkaline compounds, the problem of difficult control of the properties of expanded natural perlite materials is solved, and high-performance expanded granular materials suitable for thermal insulation and building materials are prepared, which have low density, high-pressure strength and low thermal conductivity. characteristics.
Patent Information
- Application Number
- CN201980080629.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2039-12-06
AI Technical Summary
The chemical composition and physical properties of existing expanded natural perlite materials are difficult to control, resulting in unstable applications in thermal insulation and building materials, and they contain mineral impurities that affect performance.
Expanded particulate materials, including silicate glass and aluminosilicate materials, with controllable physical properties and chemical composition are prepared by forming a mixture containing silicate materials, alkaline compounds and water, solidifying, crushing and heating.
The prepared expanded granular material has low loose packing density, high compaction resistance and low thermal conductivity. It is suitable for thermal insulation, construction and gardening materials, and has low impurity content, which improves the performance stability and application breadth of the material.
Smart Images

Figure BDA0003100687540000411 
Figure BDA0003100687540000412 
Figure BDA0003100687540000421
Abstract
Description
Technical Field
[0001] The present invention relates to expanded and expandable particulate materials, methods of making expanded and expandable particulate materials, insulation products, building materials and horticultural or agricultural substrates comprising expanded particulate materials, and fire retardant materials comprising expandable particulate materials. Background Art
[0002] Expanded natural perlite is often used as a lightweight filling material, for example in insulation and building materials. The desired properties of expanded natural perlite products include low bulk density, low water absorption, low water retention and low thermal conductivity. However, such properties depend on the chemical composition of the crude perlite before expansion. In particular, the expansion of natural perlite is achieved by heating the natural perlite to remove the "bound" or "chemical" water present in the form of hydroxyls in the perlite matrix. Therefore, the degree of expansion achieved depends on the starting hydroxyl content. Since perlite is a naturally occurring material, the chemical composition, especially the hydroxyl content, is highly variable. Natural perlite typically contains other mineral impurities, such as quartz and feldspar. Therefore, a synthetic expandable granular material with controllable physical properties and a controlled chemical composition is needed. Summary of the invention
[0003] According to a first aspect, the present invention relates to a method of manufacturing an expanded particulate material, the method comprising:
[0004] forming a mixture comprising:
[0005] Silicate materials;
[0006] basic compounds; and
[0007] water;
[0008] curing the mixture to form a solid precursor;
[0009] comminuting and / or grinding the solid precursor to form an expandable particulate material; and
[0010] The expandable particulate material is heated to form an expanded particulate material.
[0011] According to a second aspect, the present invention relates to an expanded particulate material produced by a method according to the first aspect.
[0012] According to a third aspect, the present invention relates to an expanded granular material having:
[0013] The loose bulk density measured according to PI 200-77 (wherein "PI" refers to "Perlite Institute") is about 15 kg / m 3 About 450kg / m 3 , for example about 20kg / m 3 About 100kg / m3 , or about 20kg / m 3 About 30kg / m 3 , or about 20kg / m 3 About 40kg / m 3 , or about 55kg / m 3 About 100kg / m 3 , or about 70kg / m 3 About 100kg / m 3 ;
[0014] A compaction resistance of about 3 PSI to about 350 PSI at 2", such as about 3 PSI to about 200 PSI at 2", or about 3 PSI to about 100 PSI at 2", or about 3 PSI to about 10 PSI at 2", or about 30 PSI to about 80 PSI at 2", or about 40 PSI to about 75 PSI at 2", or about 5 PSI to about 20 PSI at 2" as measured by PI 306-80; and / or
[0015] The thermal conductivity (λ, λ value) measured according to EN 12667 is about 0.0300 W / mK to about 0.0700 W / mK, for example about 0.0320 W / mK to about 0.0420 W / mK, about 0.0350 W / mK to about 0.0400 W / mK, or about 0.0360 W / mK to about 0.0410 W / mK, or about 0.0320 W / mK to about 0.0340 W / mK, or about 0.042 W / mK to about 0.055 W / mK, or about 0.055 W / mK to about 0.070 W / mK.
[0016] According to a fourth aspect, the present invention relates to an expandable material comprising:
[0017] about 0.1 wt % to about 25 wt %, for example about 0.2 wt % to about 5 wt % X2O, wherein X is an alkali metal such as Na or Li;
[0018] About 0.1 wt % to about 30 wt %, such as about 1 wt % to about 20 wt % Al2O3;
[0019] From about 30 wt % to about 80 wt %, such as from about 40 wt % to about 60 wt % SiO 2 ; and
[0020] From about 10 wt % to about 40 wt %, such as from about 15 wt % to about 30 wt % H O;
[0021] Wherein the expandable material optionally comprises less than about 5 wt %, such as less than about 3.5 wt %, B 2 O 3 .
[0022] According to a fifth aspect, the present invention relates to a method for producing an expandable material, the method comprising:
[0023] (a) forming a mixture comprising:
[0024] Silicate materials;
[0025] basic compounds; and
[0026] water;
[0027] Wherein optionally:
[0028] (i) the mixture contains glass network forming elements, glass network intermediate elements and / or glass network modifying elements other than silicon;
[0029] (ii) the mixture further comprises reactive silica; and / or
[0030] (iii) the mixture comprises two different silicate materials; and
[0031] (b) curing the mixture to form the expandable material.
[0032] According to a sixth aspect, the invention relates to an expandable material manufactured according to the method of the fifth aspect.
[0033] According to a seventh aspect, the present invention relates to an insulation product, such as a bulk granular material for insulating a cavity wall, a filler for a sound-absorbing or heat-insulating panel, a sound-absorbing or heat-insulating panel, a granular filler for insulating a refrigerated or cryogenic container, or an insulated refrigerated or cryogenic container, comprising an expanded granular material according to the second or third aspect or an expanded granular material formed by expanding an expandable material according to the fourth or sixth aspect.
[0034] According to an eighth aspect, the present invention relates to a building material, such as a sheet such as a fiber cement sheet, a mortar or plaster such as a cementitious, gypsum-based and / or acrylic-based mortar or plaster, or concrete, comprising the expanded granular material according to the second or third aspect or the expanded granular material formed by expanding the expandable material according to the fourth or sixth aspect.
[0035] According to a ninth aspect, the present invention relates to a horticultural or agricultural substrate or substrate component comprising an expanded particulate material according to the second or third aspect or an expanded particulate material formed by expanding an expandable material according to the fourth or sixth aspect.
[0036] According to a tenth aspect, the present invention relates to a flame retardant material comprising an expandable material according to the fourth or sixth aspect or an expandable material manufactured by the method according to the fifth aspect.
[0037] According to an eleventh aspect, the present invention relates to the use of an expanded granular material according to the second or third aspect or an expanded granular material formed by expanding an expandable material according to the fourth or sixth aspect in an insulation product, such as a bulk material for insulating a cavity wall, an insulation board, or an insulation container such as a refrigerated or cryogenic container, or a building material, such as a sheet such as a fiber cement sheet, a mortar or plaster such as a cementitious, gypsum-based and / or acrylic-based mortar or plaster, or concrete, or a horticultural or agricultural matrix or matrix component. DETAILED DESCRIPTION
[0038] Surprisingly, it has been found that an expandable material can be made by forming a mixture comprising a silicate material, an alkaline compound and water, and curing the mixture. The expandable material (i.e., the cured mixture) can be expanded by heating to form an expanded material. Therefore, the cured mixture can be referred to as a solid precursor of an expandable material.
[0039] The expanded particulate material may be manufactured by pulverizing a solid precursor to form an expandable particulate material and heating the expandable particulate material to form the expanded particulate material. The expanded particulate material thus formed has been found to have beneficial physical properties, such as low loose bulk density, high resistance to compaction and abrasion and / or low thermal conductivity, which makes it suitable for use in insulation products, sound absorbing products, building materials, horticultural or agricultural applications, and as a flame retardant material. The expandable material manufactured has a low concentration of impurities and therefore is generally desirable to form expanded spherical particles having a high concentration (usually greater than 98%) of floaters, as explained in more detail below.
[0040] Starting mixture
[0041] The first step of forming the expandable or expandable material includes forming a mixture comprising: a silicate material; an alkaline compound; and water.
[0042] Silicate materials
[0043] In this specification and the appended claims, the term "silicate material" refers to a material containing silicon and oxygen in substantial proportions. Silicate materials include silicates, wherein the silicate is a material having the general formula (where 0≤x≤2) of the silicate anion family, which includes orthosilicate, metasilicate and pyrosilicate anions. Silicate materials also include silicate glasses, wherein silicate glasses are amorphous (i.e., non-crystalline) solid materials formed primarily of a covalently bonded network of silicon dioxide, i.e., materials often referred to simply as "glass". Silicate materials also include silicate minerals, wherein silicate minerals are rock-forming minerals that predominantly have silicate anions or are formed primarily of silicon dioxide.
[0044] Silicate materials include aluminosilicate materials. The term "aluminosilicate material" refers to a silicate material that contains aluminum in addition to silicon and oxygen. Therefore, aluminosilicate materials include aluminosilicates, aluminosilicate glasses, and aluminosilicate minerals.
[0045] Therefore, the silicate material in the mixture can be a silicate. The silicate material in the mixture can be an aluminosilicate. For example, the silicate material in the mixture can be sodium silicate, i.e. water glass, or sodium aluminosilicate.
[0046] The silicate material in the mixture can be a silicate glass. The silicate glass can mainly contain (e.g., consist of) silicon and oxygen. However, the silicate glass can also contain one or more elements in addition to silicon and oxygen. For example, in addition to silicon and oxygen, the silicate glass can contain aluminum, sodium, iron, chromium, lead, zinc, calcium, manganese, magnesium, barium, potassium, boron, fluorine, germanium, sulfur, selenium and / or tellurium.
[0047] The silicate glass may be selected from the group consisting of fused silica glass, soda-lime glass, borosilicate glass, lead oxide glass, aluminosilicate glass and silicon-germanium glass.
[0048] The silicate glass may include (eg be) native glass. Additionally or alternatively, the silicate glass may include (eg be) recycled glass, such as recycled cullet.
[0049] Unless otherwise stated, the particle size properties of particulate materials such as ground glass or minerals referred to herein (wherein the particle size is quoted as less than 300 μm) are measured in a known manner by wet Malvern laser light scattering (standard ISO 13320-1). In this technique, based on the application of Mie theory, the diffraction of a laser beam can be used to measure the size of particles in powders, suspensions and emulsions. Such machines, such as the Malvern Mastersizer S (supplied by Malverninstruments) provide measurement and mapping of the volume cumulative percentage of particles having a size less than a given esd value (referred to in the art as the "equivalent spherical diameter" (esd)). The average particle size d 50 is the value of the esd of particles determined in this way, where there are 50% by volume of particles with an equivalent spherical diameter smaller than d 50 Value particles.
[0050] When the particle size is expressed as being equal to or greater than 300 μm, the particle size is measured by applying a sieve particle size analysis. In particular, a representative sample of the material is taken with a sampler (300-400 mL) and weighed. The sample is placed on a sieve with an opening of 300 μm or more (a smaller sieve can be used for a finer sample). The sample is thrown onto the sieve with the largest opening (located above) and the lid is placed on top. The column with the sieve is shaken back and forth 30 times without losing contact with the ground (such as rolling). The column is then allowed to fall freely 4 times from a height of 10 cm. The column is rotated 90 ° and the procedure is repeated. The fraction below 300 microns is then analyzed using a laser particle analyzer.
[0051] The silicate glass may be provided in the form of ground silicate glass (i.e., silicate cullet). The ground silicate glass may have a maximum particle size of about 200 μm, such as about 150 μm, or about 100 μm, or about 80 μm, or about 70 μm, or about 65 μm. The ground silicate glass may have a d of not greater than about 100 μm, such as not greater than about 80 μm, or not greater than about 60 μm, or not greater than about 50 μm, or not greater than about 40 μm, or not greater than about 35 μm, or not greater than about 30 μm, or not greater than about 29 μm, or not greater than about 28 μm. 50 The ground silicate glass may have a d of not less than about 5 μm, for example not less than about 10 μm, or not less than about 15 μm, or not less than about 20 μm, or not less than about 25 μm, or not less than about 26 μm, or not less than about 27 μm, or not less than about 28 μm. 50 The ground silicate glass may have a d of about 5 μm to about 100 μm, for example about 10 μm to about 80 μm, or about 15 μm to about 50 μm, or about 20 μm to about 35 μm, or about 25 μm to about 30 μm, or about 26 μm to about 28 μm, or about 27 μm to about 28 μm, or about 27 μm to about 29 μm, or about 28 μm to about 29 μm. 50 .
[0052] The silicate glass may be ground soda-lime glass having a maximum particle size of about 200 μm, such as about 150 μm, or about 100 μm, or about 80 μm, or about 70 μm, or about 65 μm. The silicate glass may be d 50 Ground soda-lime glass of about 5 μm to about 100 μm, for example about 10 μm to about 80 μm, or about 15 μm to about 50 μm, or about 20 μm to about 35 μm, or about 25 μm to about 30 μm, or about 27 μm to about 29 μm, or about 28 μm to about 29 μm.
[0053] The silicate glass may be ground borosilicate glass having a maximum particle size of about 200 μm, such as about 150 μm, or about 100 μm, or about 80 μm, or about 70 μm. The silicate glass may be d 50 Ground borosilicate glass of about 5 μm to about 100 μm, for example, about 10 μm to about 80 μm, or about 15 μm to about 50 μm, or about 20 μm to about 35 μm, or about 25 μm to about 30 μm, or about 26 μm to about 28 μm, or about 27 μm to about 28 μm, or about 27 μm to about 29 μm.
[0054] It should be understood that throughout the specification and the appended claims, unless otherwise indicated, the elemental composition of a glass, mineral or mixture is expressed in terms of the oxide equivalents of the elements present, as is standard in the art. For example, the composition of a glass, mineral or mixture containing silicon, aluminum, iron, calcium, magnesium, potassium, sodium and / or boron is expressed in terms of the equivalent content of SiO2, Al2O3, Fe2O3, CaO, MgO, K2O, Na2O and / or B2O3, respectively. The elemental composition of a glass, mineral or mixture can be determined using energy dispersive X-ray fluorescence (EDXRF), for example using a Xepos instrument available from SPECTRO AIGBH. Similarly, the mineral content of a material can be determined using X-ray diffraction determination, for example using a SIEMENS D5000 diffractometer with CuKα1 (Ni filtered) radiation, over a 2θ range of 2° to 72° with a step size of 0.02° / second.
[0055] The silicate glass may contain not less than about 50 wt %, such as not less than about 60 wt %, or not less than about 70 wt %, or not less than about 75 wt %, or not less than about 78 wt % SiO2. The silicate glass may contain not more than about 100 wt %, such as not more than about 90 wt %, or not more than about 85 wt %, or not more than about 80 wt %, or not more than about 75 wt %, or not more than about 72 wt % SiO2. The silicate glass may contain from about 50 wt % to about 100 wt %, such as from about 60 wt % to about 90 wt %, or from about 70 wt % to about 80 wt %, or from about 70 wt % to about 75 wt %, or from about 70 wt % to about 72 wt %, or from about 75 wt % to about 80 wt %, or from about 78 wt % to about 80 wt % SiO2. The silicate glass may be a soda-lime glass containing about 50 wt % to about 95 wt %, such as about 60 wt % to about 90 wt %, or about 70 wt % to about 80 wt %, or about 70 wt % to about 75 wt %, or about 70 wt % to about 72 wt % SiO 2. The silicate glass may be a borosilicate glass containing 50 wt % to about 95 wt %, such as about 60 wt % to about 90 wt %, or about 70 wt % to about 80 wt %, or about 75 wt % to about 80 wt %, or about 78 wt % to about 80 wt % SiO 2.
[0056] The silicate glass may contain not less than about 0.1 wt %, such as not less than about 0.2 wt %, or not less than about 0.3 wt %, or not less than about 0.5 wt %, or not less than about 1.0 wt %, or not less than about 2.0 wt %, or not less than about 3.0 wt % Al2O3. The silicate glass may contain not more than about 10 wt %, such as not more than about 8.0 wt %, or not more than about 6.0 wt %, or not more than about 5.0 wt %, or not more than about 4.0 wt %, or not more than about 3.5 wt %, or not more than about 3.0 wt %, or not more than about 2.0 wt %, or not more than about 1.0 wt %, or not more than about 0.5 wt % Al2O3. The silicate glass may contain about 0.1 wt % to about 10 wt %, for example, about 0.2 wt % to about 8.0 wt %, or about 0.3 wt % to about 6.0 wt %, or about 0.3 wt % to about 0.5 wt %, or about 0.3 wt % to about 0.4 wt %, or about 2 wt % to about 6 wt %, or about 3 wt % to about 4 wt % of Al2O3. The silicate glass may be a soda-lime glass containing about 0.1 wt % to about 10 wt %, for example, about 0.2 wt % to about 8.0 wt %, or about 0.3 wt % to about 6.0 wt %, or about 0.3 wt % to about 0.5 wt %, or about 0.3 wt % to about 0.4 wt % of Al2O3. The silicate glass may be a borosilicate glass containing about 0.1 wt % to about 10 wt %, for example, about 0.2 wt % to about 8.0 wt %, or about 0.3 wt % to about 6.0 wt %, or about 2 wt % to about 6 wt %, or about 3 wt % to about 4 wt % of Al2O3.
[0057] The silicate glass may include not less than about 0.001 wt %, such as not less than about 0.005 wt %, or not less than about 0.01 wt %, or not less than about 0.02 wt %, or not less than about 0.03 wt %, or not less than about 0.03 wt %, or not less than about 0.04 wt %, or not less than about 0.05 wt %, or not less than about 0.06 wt %, or not less than about 0.07 wt %, or not less than about 0.08 wt % Fe2O3. The silicate glass may include not more than about 1.0 wt %, such as not more than about 0.5 wt %, or not more than about 0.1 wt %, or not more than about 0.09 wt %, or not more than about 0.08 wt %, or not more than about 0.07 wt %, or not more than about 0.06 wt % Fe2O3. The silicate glass may contain from about 0.001 wt % to about 1.0 wt %, for example, from about 0.005 wt % to about 0.5 wt %, or from about 0.01 wt % to about 0.1 wt %, or from about 0.04 wt % to about 0.08 wt %, or from about 0.05 wt % to about 0.07 wt %, or from about 0.05 wt % to about 0.1 wt %, or from about 0.06 wt % to about 0.1 wt %, or from about 0.07 wt % to about 0.09 wt % Fe O. The silicate glass may be a soda-lime glass containing from about 0.001 wt % to about 1.0 wt %, for example, from about 0.005 wt % to about 0.5 wt %, or from about 0.01 wt % to about 0.1 wt %, or from about 0.04 wt % to about 0.08 wt %, or from about 0.05 wt % to about 0.07 wt %. The silicate glass can be a borosilicate glass containing about 0.001 wt % to about 1.0 wt %, for example about 0.005 wt % to about 0.5 wt %, or about 0.01 wt % to about 0.1 wt %, or about 0.05 wt % to about 0.1 wt %, or about 0.06 wt % to about 0.1 wt %, or about 0.07 wt % to about 0.09 wt % Fe2O3.
[0058] The silicate glass may contain not less than about 0.01 wt %, such as not less than about 0.05 wt %, or not less than about 0.1 wt %, or not less than about 0.15 wt %, or not less than about 1 wt %, or not less than about 5 wt %, or not less than about 10 wt %, or not less than about 11 wt % CaO. The silicate glass may contain not more than about 20 wt %, such as not more than about 15 wt %, or not more than about 13 wt %, or not more than about 10 wt %, or not more than about 5 wt %, or not more than about 1 wt %, or not more than about 0.5 wt %, or not more than about 0.2 wt % CaO. The silicate glass may contain from about 0.01 wt % to about 20 wt %, for example, from about 0.05 wt % to about 15 wt %, or from about 0.1 wt % to about 13 wt %, or from about 10 wt % to about 20 wt %, or from about 10 wt % to about 15 wt %, or from about 11 wt % to about 13 wt %, or from about 0.05 wt % to about 1 wt %, or from about 0.1 wt % to about 1 wt %, or from about 0.1 wt % to about 0.2 wt % CaO. The silicate glass may be a soda-lime glass containing from about 0.01 wt % to about 20 wt %, for example, from about 0.05 wt % to about 15 wt %, or from about 0.1 wt % to about 13 wt %, or from about 10 wt % to about 20 wt %, or from about 10 wt % to about 15 wt %, or from about 11 wt % to about 13 wt % CaO. The silicate glass can be a borosilicate glass comprising about 0.01 wt % to about 20 wt %, for example about 0.05 wt % to about 15 wt %, or about 0.1 wt % to about 13 wt %, or about 0.05 wt % to about 1 wt %, or about 0.1 wt % to about 1 wt %, or about 0.1 wt % to about 0.2 wt % CaO.
[0059] The silicate glass may contain no more than about 10 wt %, such as no more than about 5 wt %, or no more than about 3 wt % MgO. The silicate glass may contain no less than about 1 wt %, such as no less than about 2 wt %, or no less than about 2.5 wt % MgO. The silicate glass may contain about 1 wt % to about 10 wt %, such as about 2 wt % to about 5 wt %, or about 2.5 wt % to about 3 wt % MgO. The silicate glass may be a soda-lime glass containing about 1 wt % to about 10 wt %, such as about 2 wt % to about 5 wt %, or about 2.5 wt % to about 3 wt % MgO. The silicate glass may be substantially free of MgO, i.e., the silicate glass may be substantially free of MgO. For example, the silicate glass may contain no more than 0.1 wt %, such as no more than 0.01 wt %, or no more than 0.001 wt % MgO. The silicate glass may be a borosilicate glass that is substantially free of MgO, for example, comprising no greater than 0.1 wt %, such as no greater than 0.01 wt %, or no greater than 0.001 wt % MgO.
[0060] The silicate glass may contain not less than about 0.001 wt %, such as not less than about 0.01 wt %, or not less than about 0.04 wt %, or not less than about 0.05 wt %, or not less than about 0.1 wt %, or not less than about 0.2 wt %, or not less than about 0.3 wt %, or not less than about 0.4 wt % K O. The silicate glass may contain not more than about 5 wt %, such as not more than about 1 wt %, or not more than about 0.5 wt %, or not more than about 0.45 wt %, or not more than about 0.2 wt %, or not more than about 0.1 wt %, or not more than about 0.06 wt % K O. The silicate glass may contain about 0.001 wt % to about 5 wt %, for example, about 0.01 wt % to about 1 wt %, or about 0.04 wt % to about 0.5 wt %, or about 0.04 wt % to about 0.1 wt %, or about 0.04 wt % to about 0.06 wt %, or about 0.1 wt % to about 1 wt %, or about 0.2 wt % to about 0.5 wt %, or about 0.4 wt % to about 0.5 wt % of K O. The silicate glass may be a soda-lime glass containing about 0.001 wt % to about 5 wt %, for example, about 0.01 wt % to about 1 wt %, or about 0.04 wt % to about 0.5 wt %, or about 0.04 wt % to about 0.1 wt %, or about 0.04 wt % to about 0.06 wt % of K O. The silicate glass may be a borosilicate glass comprising about 0.01 wt % to about 1 wt %, or about 0.04 wt % to about 0.5 wt %, or about 0.1 wt % to about 1 wt %, or about 0.2 wt % to about 0.5 wt %, or about 0.4 wt % to about 0.5 wt % K2O.
[0061] The silicate glass may include not less than about 1 wt %, such as not less than about 2 wt %, or not less than about 3 wt %, or not less than about 5 wt %, or not less than about 10 wt %. %, or not less than about 11 wt %, or not less than about 12 wt % Na2O. The silicate glass may include not more than about 20 wt %, such as not more than about 15 wt %, or not more than about 13 wt %, or not more than about 10 wt %, or not more than about 5 wt %, or not more than about 4 wt % Na2O. The silicate glass may include about 1 wt % to about 20 wt %, such as about 2 wt % to about 15 wt %, or about 3 wt % to about 13 wt %, or about 10 wt % to about 15 wt %, or about 11 wt % to about 13 wt %, or about 12 wt % to about 13 wt %, or about 1 wt % to about 5 wt %, or about 2 wt % to about 4 wt % Na2O. The silicate glass may be a soda-lime glass containing about 1 wt % to about 20 wt %, such as about 2 wt % to about 15 wt %, or about 3 wt % to about 13 wt %, or about 10 wt % to about 15 wt %, or about 11 wt % to about 13 wt %, or about 12 wt % to about 13 wt % of Na O. The silicate glass may be a borosilicate glass containing about 1 wt % to about 20 wt %, such as about 2 wt % to about 15 wt %, or about 3 wt % to about 13 wt %, or about 1 wt % to about 5 wt %, or about 2 wt % to about 4 wt % of Na O.
[0062] The silicate glass may contain not less than about 1 wt %, such as not less than about 5 wt %, or not less than about 10 wt %, or not less than about 13 wt % B2O3. The silicate glass may contain not more than about 25 wt %, such as not more than about 20 wt %, or not more than about 15 wt %, or not more than about 14 wt % B2O3. The silicate glass may contain from about 1 wt % to about 25 wt %, such as from about 5 wt % to about 20 wt %, or from about 10 wt % to about 15 wt %, or from about 13 wt % to about 14 wt % B2O3. The silicate glass may be a borosilicate glass containing from about 1 wt % to about 25 wt %, such as from about 5 wt % to about 20 wt %, or from about 10 wt % to about 15 wt %, or from about 13 wt % to about 14 wt % B2O3.
[0063] Silicate glass may be composed mainly of SiO2, Al2O3, Fe2O3, CaO, MgO, K2O, Na2O and / or B2O3. Silicate glass may contain at least 80 wt%, such as at least 90 wt%, or at least 95 wt%, or at least 98 wt%, or at least 99 wt% of SiO2, Al2O3, Fe2O3, CaO, MgO, K2O, Na2O and / or B2O3. Silicate glass may be soda-lime glass composed mainly of SiO2, Al2O3, Fe2O3, CaO, MgO, K2O and Na2O. Silicate glass may be borosilicate glass composed mainly of SiO2, Al2O3, Fe2O3, CaO, K2O, Na2O and B2O3.
[0064] The silicate glass may contain one or more elements or compounds other than SiO2, Al2O3, Fe2O3, CaO, MgO, K2O, Na2O, and / or B2O3. The silicate glass may contain not less than about 0.001 wt%, such as not less than about 0.01 wt%, or not less than about 0.05 wt%, or not less than about 0.1 wt% of water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)). The silicate glass may contain not more than about 1 wt%, such as not more than about 0.5 wt%, or not more than about 0.2 wt%, or not more than about 0.1 wt% of water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)). The silicate glass may contain about 0.001 wt % to about 1 wt %, e.g., about 0.01 wt % to about 0.5 wt %, or about 0.05 wt % to about 0.2 wt %, or about 0.1 wt % to about 0.2 wt % water and / or volatile matter (i.e., matter that contributes to “loss on ignition” (LOI)).
[0065] The loss on ignition (LOI) of a material can be determined by heating a dry (ie, moisture-free) and pulverized sample of the material to 1050°C for 1 hour and measuring the weight loss upon heating.
[0066] The silicate glass can be a soda-lime glass comprising: about 60 wt % to about 80 wt % SiO2; about 0.1 wt % to about 1 wt % Al2O3; about 0.01 wt % to about 0.1 wt % Fe2O3; about 5 wt % to about 20 wt % CaO; about 1 wt % to about 5 wt % MgO; about 0.01 wt % to about 0.1 wt % K2O; about 5 wt % to about 20 wt % Na2O; and optionally about 0.01 wt % to about 0.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)).
[0067] The silicate glass can be a borosilicate glass comprising: about 70 wt % to about 90 wt % SiO2; about 1 wt % to about 10 wt % Al2O3; about 0.01 wt % to about 0.15 wt % Fe2O3; about 0.05 wt % to about 0.25 wt % CaO; about 0.1 wt % to about 1 wt % K2O; about 1 wt % to about 5 wt % Na2O; about 5 wt % to about 20 wt % B2O3; and optionally about 0.01 wt % to about 0.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)).
[0068] The silicate material in the mixture may be a silicate mineral.
[0069] For the purposes of this specification, the term "mineral" is not limited to crystalline materials, but also includes naturally occurring glasses (e.g., volcanic glasses such as obsidian or perlite), amorphous phases of minerals (e.g., metakaolin), sedimentary rocks (e.g., siliceous rock) and fossilized biomass (e.g., diatomaceous earth).
[0070] The silicate mineral in the mixture may be a naturally occurring silicate mineral. The silicate mineral in the mixture may be a naturally occurring silicate mineral that has been subjected to a physical and / or chemical treatment such as calcination or heat treatment, or the silicate mineral in the mixture may be a synthetic silicate mineral.
[0071] The silicate mineral may be an aluminosilicate mineral.
[0072] The silicate material may be volcanic glass.
[0073] The volcanic glass may contain not less than about 50 wt%, such as not less than about 60 wt%, or not less than about 65 wt%, or not less than about 70 wt%, or not less than about 75 wt% SiO2. The volcanic glass may contain not more than about 95 wt%, such as not more than about 90 wt%, or not more than about 85 wt%, or not more than about 80 wt%, or not more than about 75 wt%, or not more than about 70 wt% SiO2. The volcanic glass may contain from about 50 wt% to about 95 wt%, such as from about 60 wt% to about 90 wt%, or from about 60 wt% to about 80 wt%, or from about 60 wt% to about 70 wt%, or from about 70 wt% to about 80 wt% SiO2.
[0074] The volcanic glass may contain not less than about 5 wt %, such as not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt % Al2O3. The volcanic glass may contain not more than about 25 wt %, such as not more than about 20 wt %, or not more than about 15 wt %, or not more than about 12 wt % Al2O3. The volcanic glass may contain from about 5 wt % to about 25 wt %, such as from about 8 wt % to about 20 wt %, such as from about 8 wt % to about 12 wt %, or from about 12 wt % to about 15 wt % Al2O3.
[0075] The volcanic glass may contain not less than about 0.5 wt %, such as not less than about 1 wt %, or not less than about 2 wt % Fe2O3. The volcanic glass may contain not more than about 5 wt %, such as not more than about 3 wt %, or not more than about 2 wt % Fe2O3. The volcanic glass may contain from about 0.5 wt % to about 5 wt %, such as from about 1 wt % to about 3 wt %, or from about 2 wt % to about 3 wt %, or from about 1 wt % to about 2 wt % Fe2O3.
[0076] The volcanic glass may include not less than about 0.5 wt %, such as not less than about 0.8 wt % CaO. The volcanic glass may include not greater than about 5 wt %, such as not greater than about 3 wt %, or not greater than about 2 wt % CaO.
[0077] The volcanic glass can include from about 0.5 wt % to about 5 wt %, such as from about 0.8 wt % to about 3 wt %, or from about 0.8 wt % to about 2 wt % CaO.
[0078] The volcanic glass may contain not less than about 0.05 wt%, such as not less than about 0.1 wt%, or not less than about 0.2 wt%, or not less than about 0.5 wt%, or not less than about 1 wt%, or not less than about 1.2 wt% MgO. The volcanic glass may contain not more than about 10 wt%, such as not more than about 5 wt%, or not more than about 2 wt%, or not more than about 1 wt%, or not more than about 0.5 wt%, or not more than about 0.3 wt% MgO. The volcanic glass may contain from about 0.05 wt% to about 10 wt%, such as from about 0.1 wt% to about 5 wt%, or from about 0.2 wt% to about 2 wt%, or from about 0.2 wt% to about 1 wt%, or from about 0.2 wt% to about 0.5 wt%, or from about 0.2 wt% to about 0.3 wt%, or from about 1 wt% to about 5 wt%, or from about 1 wt% to about 2 wt% MgO.
[0079] The volcanic glass may contain not less than about 1 wt %, such as not less than about 2 wt %, or not less than about 3 wt %, or not less than about 4 wt % KO. The volcanic glass may contain not more than about 10 wt %, such as not more than about 8 wt %, or not more than about 6 wt %, or not more than about 5 wt % KO. The volcanic glass may contain from about 1 wt % to about 10 wt %, such as from about 2 wt % to about 8 wt %, or from about 3 wt % to about 6 wt %, or from about 4 wt % to about 5 wt % KO.
[0080] The volcanic glass may include not less than about 1 wt %, such as not less than about 2 wt %, or not less than about 3 wt % Na2O. The volcanic glass may include not more than about 10 wt %, such as not more than about 8 wt %, or not more than about 6 wt %, or not more than about 4 wt % Na2O. The volcanic glass may include from about 1 wt % to about 10 wt %, such as from about 2 wt % to about 8 wt %, or from about 3 wt % to about 6 wt %, or from about 3 wt % to about 4 wt % Na2O.
[0081] The volcanic glass may contain substantially no B 2 O 3. For example, the volcanic glass may contain less than 1 wt %, such as less than 0.1 wt % or less than 0.01 wt % B 2 O 3.
[0082] The volcanic glass may contain not less than about 1 wt %, such as not less than about 2 wt %, or not less than about 2.5 wt %, or not less than about 3 wt %, or not less than about 4 wt %, or not less than about 5 wt % chemically bound water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)). The volcanic glass may contain not more than about 10 wt %, such as not more than about 8 wt %, or not more than about 6 wt %, or not more than about 4 wt %, or not more than about 3 wt % chemically bound water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)). The volcanic glass may contain from about 1 wt % to about 10 wt %, such as from about 2 wt % to about 8 wt %, or from about 2 wt % to about 6 wt %, or from about 2 wt % to about 3 wt %, or from about 5 wt % to about 6 wt % chemically bound water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)).
[0083] The volcanic glass may contain: about 70 wt % to about 80 wt % SiO2; about 5 wt % to about 15 wt % Al2O3; about 0.5 wt % to about 1.5 wt % Fe2O3; about 0.5 wt % to about 2 wt % CaO; about 0.05 wt % to about 1 wt % MgO; about 1 wt % to about 10 wt % K2O; about 1 wt % to about 8 wt % Na2O; about 1 wt % to about 5 wt % chemically bonded water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)); and optionally less than about 1 wt % B2O3.
[0084] The volcanic glass may contain: about 65 wt % to about 75 wt % SiO2; about 8 wt % to about 17 wt % Al2O3; about 1 wt % to about 5 wt % Fe2O3; about 0.5 wt % to about 2 wt % CaO; about 0.5 wt % to about 5 wt % MgO; about 1 wt % to about 10 wt % K2O; about 1 wt % to about 8 wt % Na2O; about 3 wt % to about 8 wt % chemically bonded water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)); and optionally less than about 1 wt % B2O3.
[0085] The volcanic glass may have a d of not less than about 1 μm, such as not less than about 3 μm, or not less than about 5 μm, or not less than about 6 μm, or not less than about 10 μm, or not less than about 20 μm, or not less than about 25 μm, or not less than about 30 μm. 50 The volcanic glass may have a d of not greater than about 250 μm, such as not greater than about 200 μm, or not greater than about 150 μm, or not greater than about 100 μm, or not greater than about 80 μm, or not greater than about 60 μm, or not greater than about 50 μm, or not greater than about 40 μm, or not greater than about 35 μm, or not greater than about 30 μm, or not greater than about 15 μm, or not greater than about 10 μm, or not greater than about 8 μm, or not greater than about 7 μm. 50 The volcanic glass may have a d of about 1 μm to about 250 μm, for example about 1 μm to about 200 μm, or about 1 μm to about 150 μm, or about 1 μm to about 100 μm, or about 1 μm to about 80 μm, or about 1 μm to about 60 μm, or about 1 μm to about 50 μm, about 3 μm to about 40 μm, or about 5 μm to about 35 μm, or about 5 μm to about 10 μm, or about 5 μm to about 8 μm, or about 6 μm to about 7 μm, or about 20 μm to about 40 μm, or about 25 μm to about 35 μm. 50 .
[0086] The silicate material (e.g., silicate glass or silicate mineral) can be a perlite material. The perlite material can be perlite. The perlite material can be naturally occurring perlite, such as naturally occurring perlite ore. Naturally occurring perlite is an amorphous volcanic glass formed primarily of silicon dioxide, typically in combination with aluminum oxide, sodium oxide, potassium oxide, iron oxide, magnesium oxide, and / or calcium oxide. Perlite can be naturally formed by the hydration of obsidian. The perlite material can contain a small amount of crystalline phases, such as biotite, quartz, cristobalite, feldspar, or hydroxysodalite.
[0087] The perlite material can be unexpanded perlite, such as unexpanded natural perlite ore. The unexpanded perlite, such as unexpanded natural perlite ore, can have a water content greater than about 2% by weight. The unexpanded perlite, such as unexpanded natural perlite ore, can be unexpanded perlite derived from natural perlite ore tailings, such as unexpanded natural perlite ore. That is, the unexpanded perlite can be the perlite material (i.e., a byproduct) remaining after removing the more valuable portions from the unexpanded natural perlite ore. The natural perlite ore tailings can originate from different stages of perlite ore processing.
[0088] Perlite materials (e.g., unexpanded natural perlite ore) may contain not less than about 50% by weight, such as not less than about 60% by weight, or not less than about 65% by weight, or not less than about 70% by weight, or not less than about 75% by weight SiO2. Perlite materials (e.g., unexpanded natural perlite ore) may contain not more than about 95% by weight, such as not more than about 90% by weight, or not more than about 85% by weight, or not more than about 80% by weight, or not more than about 75% by weight, or not more than about 70% by weight SiO2. Perlite materials (e.g., unexpanded natural perlite ore) may contain from about 50% to about 95% by weight, such as from about 60% to about 90% by weight, or from about 60% to about 80% by weight, or from about 60% to about 70% by weight, or from about 70% to about 80% by weight SiO2.
[0089] Perlite materials (e.g., unexpanded natural perlite ore) may contain not less than about 5 wt%, such as not less than about 8 wt%, or not less than about 10 wt%, or not less than about 12 wt% Al2O3. Perlite materials (e.g., unexpanded natural perlite ore) may contain not more than about 25 wt%, such as not more than about 20 wt%, or not more than about 15 wt%, or not more than about 12 wt% Al2O3. Perlite materials (e.g., unexpanded natural perlite ore) may contain from about 5 wt% to about 25 wt%, such as from about 8 wt% to about 20 wt%, such as from about 8 wt% to about 12 wt%, or from about 12 wt% to about 15 wt% Al2O3.
[0090] Perlite materials (e.g., unexpanded natural perlite ore) may contain not less than about 0.5 wt%, such as not less than about 1 wt%, or not less than about 2 wt% Fe2O3. Perlite materials (e.g., unexpanded natural perlite ore) may contain not more than about 5 wt%, such as not more than about 3 wt%, or not more than about 2 wt% Fe2O3. Perlite materials (e.g., unexpanded natural perlite ore) may contain from about 0.5 wt% to about 5 wt%, such as from about 1 wt% to about 3 wt%, or from about 2 wt% to about 3 wt%, or from about 1 wt% to about 2 wt% Fe2O3.
[0091] Perlite materials (e.g., unexpanded natural perlite ore) may contain not less than about 0.5 wt %, such as not less than about 0.8 wt % CaO. Perlite materials (e.g., unexpanded natural perlite ore) may contain not more than about 5 wt %, such as not more than about 3 wt %, or not more than about 2 wt % CaO. Perlite materials (e.g., unexpanded natural perlite ore) may contain from about 0.5 wt % to about 5 wt %, such as from about 0.8 wt % to about 3 wt %, or from about 0.8 wt % to about 2 wt % CaO.
[0092] Perlite materials (e.g., unexpanded natural perlite ore) may contain not less than about 0.05 wt%, such as not less than about 0.1 wt%, or not less than about 0.2 wt%, or not less than about 0.5 wt%, or not less than about 1 wt%, or not less than about 1.2 wt% MgO. Perlite materials (e.g., unexpanded natural perlite ore) may contain no more than about 10 wt%, such as no more than about 5 wt%, or no more than about 2 wt%, or no more than about 1 wt%, or no more than about 0.5 wt%, or no more than about 0.3 wt% MgO. Perlite materials (e.g., unexpanded natural perlite ore) may contain from about 0.05 wt% to about 10 wt%, such as from about 0.1 wt% to about 5 wt%, or from about 0.2 wt% to about 2 wt%, or from about 0.2 wt% to about 1 wt%, or from about 0.2 wt% to about 0.5 wt%, or from about 0.2 wt% to about 0.3 wt%, or from about 1 wt% to about 5 wt%, or from about 1 wt% to about 2 wt% MgO.
[0093] The perlite material (e.g., unexpanded natural perlite ore) may contain not less than about 1 wt%, such as not less than about 2 wt%, or not less than about 3 wt%, or not less than about 4 wt% KO. The perlite material (e.g., unexpanded natural perlite ore) may contain not more than about 10 wt%, such as not more than about 8 wt%, or not more than about 6 wt%, or not more than about 5 wt% KO. The perlite material (e.g., unexpanded natural perlite ore) may contain from about 1 wt% to about 10 wt%, such as from about 2 wt% to about 8 wt%, or from about 3 wt% to about 6 wt%, or from about 4 wt% to about 5 wt% KO.
[0094] The perlite material (e.g., unexpanded natural perlite ore) may contain not less than about 1 wt %, such as not less than about 2 wt %, or not less than about 3 wt % Na O. The perlite material (e.g., unexpanded natural perlite ore) may contain not more than about 10 wt %, such as not more than about 8 wt %, or not more than about 6 wt %, or not more than about 4 wt % Na O. The perlite material (e.g., unexpanded natural perlite ore) may contain from about 1 wt % to about 10 wt %, such as from about 2 wt % to about 8 wt %, or from about 3 wt % to about 6 wt %, or from about 3 wt % to about 4 wt % Na O.
[0095] The perlite material (e.g., unexpanded natural perlite ore) may contain substantially no B2O3. For example, the perlite material (e.g., unexpanded natural perlite ore) may contain less than 1 wt%, such as less than 0.1 wt% or less than 0.01 wt% B2O3.
[0096] Perlite material (e.g., unexpanded natural perlite ore) may contain not less than about 1 wt%, such as not less than about 2 wt%, or not less than about 2.5 wt%, or not less than about 3 wt%, or not less than about 4 wt%, or not less than about 5 wt% chemically bound water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)). Perlite material (e.g., unexpanded natural perlite ore) may contain not more than about 10 wt%, such as not more than about 8 wt%, or not more than about 6 wt%, or not more than about 4 wt%, or not more than about 3 wt% chemically bound water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)). Perlite material (e.g., unexpanded natural perlite ore) may contain from about 1 wt % to about 10 wt %, e.g., from about 2 wt % to about 8 wt %, or from about 2 wt % to about 6 wt %, or from about 2 wt % to about 3 wt %, or from about 5 wt % to about 6 wt % chemically bound water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)).
[0097] Perlite material (e.g., unexpanded natural perlite ore) may contain: about 70 wt % to about 80 wt % SiO2; about 5 wt % to about 15 wt % Al2O3; about 0.5 wt % to about 1.5 wt % Fe2O3; about 0.5 wt % to about 2 wt % CaO; about 0.05 wt % to about 1 wt % MgO; about 1 wt % to about 10 wt % K2O; about 1 wt % to about 8 wt % Na2O; about 1 wt % to about 5 wt % chemically bonded water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)); and optionally less than about 1 wt % B2O3.
[0098] Perlite material (e.g., unexpanded natural perlite ore) may contain: about 65 wt % to about 75 wt % SiO2; about 8 wt % to about 17 wt % Al2O3; about 1 wt % to about 5 wt % Fe2O3; about 0.5 wt % to about 2 wt % CaO; about 0.5 wt % to about 5 wt % MgO; about 1 wt % to about 10 wt % K2O; about 1 wt % to about 8 wt % Na2O; about 3 wt % to about 8 wt % chemically bonded water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)); and optionally less than about 1 wt % B2O3.
[0099] Perlite material (e.g., unexpanded natural perlite ore, such as perlite tailings) may contain: about 67 wt% to about 76 wt% SiO2; about 10 wt% to about 14 wt% Al2O3; about 1 wt% to about 2.5 wt% Fe2O3; about 1 wt% to about 1.5 wt% CaO; about 0.25 wt% to about 1.5 wt% MgO; about 3 wt% to about 5 wt% K2O; about 3.5 wt% to about 4 wt% Na2O; from about 51 wt% to about 5 wt% chemically combined water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)); and optionally less than about 1 wt% B2O3.
[0100] The perlite material (e.g., unexpanded natural perlite ore) may have a d of not less than about 1 μm, such as not less than about 3 μm, or not less than about 5 μm, or not less than about 6 μm, or not less than about 10 μm, or not less than about 20 μm, or not less than about 25 μm, or not less than about 30 μm. 50 The perlite material (e.g., unexpanded natural perlite ore) may have a d of not greater than about 250 μm, e.g., not greater than about 200 μm, or not greater than about 150 μm, or not greater than about 100 μm, or not greater than about 80 μm, or not greater than about 60 μm, or not greater than about 50 μm, or not greater than about 40 μm, or not greater than about 35 μm, or not greater than about 32 μm, or not greater than about 30 μm, or not greater than about 15 μm, or not greater than about 10 μm, or not greater than about 8 μm, or not greater than about 7 μm. 50The perlite material (e.g., unexpanded natural perlite ore) may have a d of about 1 μm to about 250 μm, for example, about 1 μm to about 200 μm, or about 1 μm to about 150 μm, or about 1 μm to about 100 μm, or about 1 μm to about 80 μm, or about 1 μm to about 60 μm, or about 1 μm to about 50 μm, about 3 μm to about 40 μm, or about 5 μm to about 32 μm, or about 5 μm to about 35 μm, or about 5 μm to about 10 μm, or about 5 μm to about 8 μm, or about 6 μm to about 7 μm, or about 20 μm to about 40 μm, or about 25 μm to about 35 μm. 50 .
[0101] Perlite material (e.g., unexpanded natural perlite ore, such as perlite tailings) may have a d 50 and comprises: from about 67 wt % to about 76 wt % SiO2; from about 10 wt % to about 14 wt % Al2O3; from about 1 wt % to about 2.5 wt % Fe2O3; from about 1 wt % to about 1.5 wt % CaO; from about 0.25 wt % to about 1.5 wt % MgO; from about 3 wt % to about 5 wt % K2O; from about 3.5 wt % to about 4 wt % Na2O; from about 51 wt % to about 5 wt % chemically combined water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI)); and optionally less than about 1 wt % B2O3.
[0102] The silicate material (e.g., silicate mineral) can be a phyllosilicate mineral. The phyllosilicate mineral can be a clay mineral, i.e., a hydrated aluminum phyllosilicate mineral. The silicate material (e.g., silicate mineral) can be selected from: halloysite, kaolin, illite, montmorillonite, nontronite, beidellite, vermiculite, talc, sepiolite, palygorskite, pyrophyllite. The silicate material (e.g., silicate mineral) can be kaolin, such as calcined kaolin (i.e., metakaolin). The silicate material (e.g., silicate mineral) can be bentonite or any other clay mineral containing smectite. The silicate material (e.g., silicate mineral) can be bentonite tailings, such as Na-bentonite tailings or Ca-bentonite tailings.
[0103] The silicate material (eg, silicate mineral) may be diatomaceous earth or a mineral containing diatomaceous earth, such as a mineral containing diatomaceous earth and a clay mineral (in any relative proportions).
[0104] Silicate materials (e.g., silicates, silicate glasses, or silicate minerals) may contain not less than about 30 wt%, such as not less than about 40 wt%, or not less than about 50 wt%, or not less than about 60 wt% SiO2. Silicate materials (e.g., silicates, silicate glasses, or silicate minerals) may contain up to about 100 wt%, such as not more than about 99 wt%, or not more than about 95 wt%, or not more than about 90 wt%, or not more than about 85 wt%, or not more than about 80 wt%, or not more than about 70 wt%, or not more than about 60 wt% SiO2. Silicate materials (e.g., silicates, silicate glasses, or silicate minerals) may contain from about 30 wt% to about 100 wt%, such as from about 40 wt% to about 99 wt%, or from about 50 wt% to about 95 wt%, or from about 60 wt% to about 90 wt%, or from about 60 wt% to about 85 wt% SiO2.
[0105] The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not less than about 0.1 wt %, such as not less than about 0.5 wt %, or not less than about 1 wt %, or not less than about 2 wt % Na O. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not more than about 40 wt %, such as not more than about 30 wt %, or not more than about 20 wt %, or not more than about 15 wt % Na O. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain from about 0.1 wt % to about 40 wt %, such as from about 0.5 wt % to about 30 wt %, or from about 1 wt % to about 30 wt %, or from about 2 wt % to about 15 wt % Na O.
[0106] The silicate material (e.g., a silicate, a silicate glass, or a silicate mineral) may contain substantially 0 wt % KO. The silicate material (e.g., a silicate, a silicate glass, or a silicate mineral) may contain not less than about 0.01 wt % KO. The silicate material (e.g., a silicate, a silicate glass, or a silicate mineral) may contain not more than about 20 wt %, such as not more than about 15 wt %, or not more than about 10 wt %, or not more than about 6 wt % KO. The silicate material (e.g., a silicate, a silicate glass, or a silicate mineral) may contain from about 0 wt % to about 20 wt %, such as from about 0 wt % to about 15 wt %, or from about 0.01 wt % to about 10 wt %, or from about 0.01 wt % to about 6 wt % KO.
[0107] The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain substantially 0 wt % CaO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not less than about 0.05 wt % CaO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not more than about 20 wt %, such as not more than about 15 wt % CaO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain from about 0 wt % to about 20 wt %, such as from about 0.05 wt % to about 15 wt % CaO.
[0108] The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain substantially 0 wt% Al2O3. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not less than about 0.1 wt% Al2O3. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not more than about 20 wt%, such as not more than about 15 wt% Al2O3. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain from about 0 wt% to about 20 wt%, such as from about 0.1 wt% to about 15 wt% Al2O3.
[0109] The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain substantially 0 wt % B2O3. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not less than about 0.01 wt %, such as not less than about 0.05 wt %, or not less than about 0.1 wt % B2O3. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not more than about 20 wt %, such as not more than about 15 wt %, or not more than about 10 wt % B2O3. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain from about 0 wt % to about 20 wt %, such as from about 0 wt % to about 15 wt %, or from about 0.01 wt % to about 10 wt %, or from about 0.1 wt % to about 10 wt % B2O3.
[0110] The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain substantially 0 wt % PbO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not less than about 0.01 wt %, such as not less than about 0.05 wt %, or not less than about 0.1 wt % PbO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not more than about 20 wt %, such as not more than about 15 wt %, or not more than about 10 wt % PbO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain from about 0 wt % to about 20 wt %, such as from about 0 wt % to about 15 wt %, or from about 0.01 wt % to about 10 wt %, or from about 0.1 wt % to about 10 wt % PbO.
[0111] The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain substantially 0 wt % MgO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not less than about 0.01 wt %, such as not less than about 0.05 wt %, or not less than about 0.1 wt % MgO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not more than about 10 wt %, such as not more than about 5 wt %, or not more than about 2 wt % MgO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain from about 0 wt % to about 10 wt %, such as from about 0 wt % to about 5 wt %, or from about 0.01 wt % to about 2 wt %, or from about 0.1 wt % to about 2 wt % MgO.
[0112] The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain substantially 0 wt % BaO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not less than about 0.01 wt %, such as not less than about 0.05 wt %, or not less than about 0.1 wt % BaO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain not more than about 10 wt %, such as not more than about 5 wt %, or not more than about 2 wt % BaO. The silicate material (e.g., silicate, silicate glass, or silicate mineral) may contain from about 0 wt % to about 10 wt %, such as from about 0 wt % to about 5 wt %, or from about 0.01 wt % to about 2 wt %, or from about 0.1 wt % to about 2 wt % BaO.
[0113] The silicate material (e.g., a silicate, a silicate glass, or a silicate mineral) may include: about 50 wt. % to about 95 wt. %, for example, about 60 wt. % to about 85 wt. % SiO2; about 1 wt. % to about 30 wt. %, for example, about 2 wt. % to about 15 wt. % Na2O; about 0 wt. % to about 15 wt. %, for example, about 0.01 wt. % to about 6 wt. % K2O; about 0 wt. % to about 20 wt. %, for example, about 0.05 wt. % to about 15 wt. % CaO; about 0 wt. % to about 20 wt. %, for example, about 0.1 wt. % to about 15 wt. % Al2O3; not more than about 20 wt. %, for example, less than about 15 wt. % B2O3; not more than about 20 wt. %, for example, less than about 15 wt. % PbO; not more than about 10 wt. %, for example, less than about 5 wt. % MgO; and not more than about 10 wt. %, for example, less than about 5 wt. % BaO.
[0114] The silicate material can be crystalline, or the silicate material can be amorphous. The silicate material can include not less than 25% by weight, such as not less than about 50% by weight, or not less than about 75% by weight, or not less than about 90% by weight of amorphous material. For example, the silicate material can include about 25% by weight to about 100% by weight, such as about 50% by weight to about 100% by weight, or about 75% by weight to about 100% by weight, or about 90% by weight to about 100% by weight of amorphous material.
[0115] Basic compounds
[0116] A basic compound is a compound of an alkali metal or an alkaline earth metal. Thus, the basic compound may be an alkali metal compound or an alkaline earth metal compound.
[0117] The basic compound can be an alkaline salt. The alkaline salt is a basic salt of an alkali metal or an alkaline earth metal. Therefore, the alkaline salt can be an alkali metal salt or an alkaline earth metal salt. The alkaline salt can be a hydroxide, a carbonate or a silicate of an alkali metal or an alkaline earth metal, i.e., the alkaline salt can be an alkaline hydroxide, an alkaline carbonate or an alkaline silicate. The alkaline salt can be an alkaline hydroxide, an alkaline carbonate or an alkaline silicate. The alkaline salt can be selected from: sodium hydroxide (NaOH), lithium hydroxide (LiOH), potassium hydroxide (KOH), sodium carbonate (Na2CO3), lithium carbonate (Li2CO3), potassium carbonate (Na2CO3), sodium silicate (Na2SiO3, Na4SiO4 or Na6Si2O7), lithium silicate (Li2SiO3, Lia4SiO4 or Lia6Si2O7), potassium silicate (K2SiO3, K4SiO4 or K6Si2O7).
[0118] In certain embodiments, the basic salt is a sodium salt, such as sodium hydroxide.
[0119] In certain embodiments, the basic salt is a lithium salt, such as lithium hydroxide.
[0120] In certain embodiments, the alkaline salt is a mixture of sodium and lithium salts, such as a mixture of sodium hydroxide and lithium hydroxide. The ratio of the weight % sodium salt to the weight % lithium salt in the mixture may be not less than about 1, for example, not less than about 1.5. The ratio of the weight % of the sodium salt to the weight % of the lithium salt in the mixture may be not greater than about 20, for example, not greater than about 15, or not greater than about 10. The ratio of the weight % of the sodium salt to the weight % of the lithium salt in the mixture may be from about 1 to about 20, for example, from about 1.5 to about 15, or from about 1.5 to about 10. For example, the ratio of the weight % sodium hydroxide to the weight % lithium hydroxide in the mixture may be not less than about 1, for example, not less than about 1.5. The ratio of the weight % of sodium hydroxide to the weight % of lithium hydroxide in the mixture may be not greater than about 20, for example, not greater than about 15, or not greater than about 10. The ratio of the weight % of sodium hydroxide to the weight % of lithium hydroxide in the mixture may be from about 1 to about 20, for example, from about 1.5 to about 15, or from about 1.5 to about 10. Thus, the basic salts may be described as mixed basic salts, for example sodium / lithium salts or sodium / potassium salts such as sodium / lithium silicate or sodium / potassium silicate.
[0121] water
[0122] The water in the mixture may contain one or more impurities, such as dissolved minerals. The water in the mixture may include not less than about 95% by weight, such as not less than about 96% by weight, or not less than about 97% by weight, or not less than about 98% by weight, or not less than about 99% by weight, or not less than about 99.5% by weight of H2O. The water in the mixture may include substantially 100% by weight of H2O. The water in the mixture may include not more than about 99.999% by weight, such as not more than about 99.99% by weight, or not more than about 99.9% by weight, or not more than about 99.5% by weight, or not more than about 99% by weight of H2O. The water in the mixture may include about 95% by weight to about 100% by weight, such as about 96% by weight to about 99.999% by weight, or about 98% by weight to about 99.99% by weight, or about 99% by weight to about 99.9% by weight, or about 95% by weight to about 99.5% by weight, or about 95% by weight to about 99% by weight of H2O.
[0123] Reactive Silica
[0124] In addition to the silicate material, the mixture may include reactive silica. When present, the reactive silica has a different chemical composition and / or physical structure (eg, crystalline, microcrystalline, nanocrystalline, or amorphous phase, microstructure, particle morphology, or shape) than the silicate material.
[0125] The reactive silica may be in the form of a high surface area (i.e., particle) of silica. For example, the reactive silica may have a surface area of not less than about 50 m 2 / g, or not less than about 100m 2 / g, or not less than about 200m 2 / g, or not less than about 300m 2 The reactive silica may have a specific surface area (eg, BET specific surface area) of not more than about 1000 m 2 / g, for example not more than about 800m 2 / g or not more than about 600m 2 The reactive silica may have (for example, include) a specific surface area (for example, a BET specific surface area) of about 50 m / g. 2 / g to about 1000m 2 / g, for example, about 100m 2 / g to about 1000m 2 / g, or about 200m 2 / g to about 1000m 2 / g, or about 300m 2 / g to about 1000m 2 / g, or about 50m 2 / g to about 800m 2 / g, or about 200m 2 / g to about 800m 2 / g, or about 100m 2 / g to about 800m 2 / g, or about 300m 2 / g to about 800m 2 / g, or about 50m 2 / g to about 600m 2 / g, or about 600m 2 / g to about 600m 2 / g, or about 100m 2 / g to about 600m 2 / g, or about 300m 2 / g to about 600m 2 / g of specific surface area (for example, BET specific surface area) (for example, containing silica particles having the above specific surface area).
[0126] The reactive silica may be in the form of mid-surface-area (i.e., particles) of silica. For example, the reactive silica may have a particle size of not less than about 5 m 2 / g, or not less than about 8m2 / g, or not less than about 10m 2 / g, or not less than about 12m 2 / g, or not less than about 15m 2 The reactive silica may have a specific surface area (eg, BET specific surface area) of not more than about 100 m / g. 2 / g, for example not more than about 75m 2 / g, or not more than about 50m 2 / g, or not more than about 30m 2 / g of silica particles (eg, containing silica particles having the above-mentioned specific surface area). The reactive silica may have a specific surface area of about 5 m 2 / g to about 100m 2 / g, for example about 8m 2 / g to about 100m 2 / g, or about 10m 2 / g to about 100m 2 / g, or about 12m 2 / g to about 100m 2 / g, or about 15m 2 / g to about 100m 2 / g, or about 5m 2 / g to about 75m 2 / g, or about 8m 2 / g to about 75m 2 / g, or about 10m 2 / g to about 75m 2 / g, or about 12m 2 / g to about 75m 2 / g, or about 15m 2 / g to about 75m 2 / g, or about 5m 2 / g to about 50m 2 / g, or about 8m 2 / g to about 50m 2 / g, or about 10m 2 / g to about 50m 2 / g, or about 12m 2 / g to about 50m 2 / g, or about 15m 2 / g to about 50m 2 / g, or about 5m 2 / g to about 30m 2 / g, or about 8m 2 / g to about 30m 2 / g, or about 10m2 / g to about 30m 2 / g, or about 12m 2 / g to about 30m 2 / g, or about 15m 2 / g to about 30m 2 / g of specific surface area (for example, BET specific surface area) (for example, containing silica particles having the above specific surface area).
[0127] The reactive silica may be a low-surface area (ie, particle) form of silica. For example, the reactive silica may have a particle size of not less than about 1 m 2 / g or not less than about 2m 2 / g specific surface area (eg, BET specific surface area) (eg, comprising silica particles having the above specific surface area). The reactive silica may have a specific surface area of not more than about 10 m 2 / g, for example not more than about 5m 2 / g or not more than about 3m 2 / g specific surface area (eg, BET specific surface area) (eg, comprising silica particles having the above specific surface area). The reactive silica may have a specific surface area of about 1 m 2 / g to about 10m 2 / g, for example about 1m 2 / g to about 5m 2 / g, or about 1m 2 / g to about 3m 2 / g, or about 2m 2 / g to about 10m 2 / g, or about 2m 2 / g to about 5m 2 / g, or about 2m 2 / g to about 3m 2 / g of specific surface area (for example, BET specific surface area) (for example, containing silica particles having the above specific surface area).
[0128] The reactive silica can be predominantly (e.g., completely) amorphous. The reactive silica can be (e.g., by volume) at least about 50%, such as at least about 60%, or at least about 70%, or at least about 80%, or at least about 90%, or at least about 95% amorphous.
[0129] The reactive silica may include (e.g., be) silica fume. Silica fume, also known as microsilica, is an amorphous polymorph of silicon dioxide. Silica fume may be provided in the form of a powder, such as a powder of spherical particles. The silica fume particles may have a d of not less than about 10 nm, such as not less than about 50 nm, or not less than about 100 nm, or not less than about 200 nm, or not less than about 500 nm. 50The silica fume particles may have a d of not greater than about 5 μm, or not greater than about 1 μm, or not greater than about 900 nm, or not greater than about 800 nm, or not greater than about 600 nm, or not greater than about 500 nm, or not greater than about 400 nm, or not greater than about 300 nm, or not greater than about 200 nm. 50 The silica fume particles may have a d of about 10 nm to about 5 μm, such as about 50 nm to about 1 μm, or about 100 nm to about 500 nm, or about 100 nm to about 200 nm. 50 .
[0130] Additionally or alternatively, the reactive silica may comprise (e.g., be) fumed silica. Fumed silica, also known as pyrogenic silica, comprises branched, chain-like aggregates of amorphous silica primary particles. The silica primary particles may have a d of not less than about 1 nm, or not less than about 5 nm, or not less than about 10 nm. 50 The silica primary particles may have a d of no greater than about 1 μm, or no greater than about 500 nm, or no greater than about 100 nm, or no greater than about 50 nm. 50 . d of silica primary particles 50 The d may be about 1 nm to about 1 μm, for example, about 5 nm to about 500 nm, or about 10 nm to about 100 nm, or about 10 nm to about 50 nm. 50 .
[0131] Additionally or alternatively, the reactive silica may comprise (eg, be) silica gel, natural volcanic glass, perlite material, or burned organic matter, such as rice husk ash.
[0132] Glass network forming elements
[0133] The mixture may contain glass network forming elements other than silicon. The glass network forming elements other than silicon in the mixture may be provided by a silicate material.
[0134] Glass network forming elements are those elements whose oxides can spontaneously form a covalently bonded glass network structure (eg, conforming to the Zachariasen rule for glass network formation). Glass network forming elements include silicon, boron, germanium, and phosphorus.
[0135] Thus, the glass network forming element present in the mixture other than silicon may be boron. For example, the silicate material may be a silicate glass as a boron-containing glass such as a borosilicate glass. Additionally or alternatively, the mixture may contain one or more other boron sources, such as boric acid or one or more borates (e.g. borax, i.e. sodium borate).
[0136] Alternatively, the glass network forming element other than silicon present in the mixture may be germanium. For example, the silicate material may be a silicate glass which is a germanium-containing glass such as silica-germania glass.
[0137] Alternatively, the glass network forming element other than silicon present in the mixture may be phosphorus. For example, the silicate material may be a silicate glass as a phosphorus-containing glass. Additionally or alternatively, the mixture may contain one or more other phosphorus sources, such as phosphoric acid or one or more phosphates.
[0138] Glass Network Intermediate Elements
[0139] The mixture may include one or more glass network intermediate elements. One or more glass network intermediate elements in the mixture may be provided by a silicate material.
[0140] Glass network intermediate elements are those elements whose oxides do not spontaneously form a glass network structure, but when combined with other glass network forming elements, can act similarly to glass network formers. Glass network intermediates include titanium, aluminum, zirconium, beryllium, magnesium and zinc. The silicate material can be a silicate glass containing one or more glass network intermediate elements such as titanium, aluminum, zirconium, beryllium, magnesium or zinc. For example, the silicate glass can be an aluminum-containing glass, such as an aluminosilicate glass.
[0141] Glass network modification elements
[0142] The mixture may contain one or more glass network modifying elements.The one or more glass network modifying elements present in the mixture may be provided by a silicate material and / or an alkaline compound.
[0143] Glass network modifying elements are those elements whose oxides alone or in combination with glass network forming elements do not form a glass network structure. When present in the glass, the glass network modifying elements destroy or modify the glass network structure. The glass network modifying elements are usually present in the glass in the form of ions; the charge of the glass network modifying ions is compensated by nearby non-bridging oxygen atoms covalently bonded to nearby glass network forming elements.
[0144] Glass network modifying elements include calcium, lead, lithium, sodium and potassium. The silicate material may be a silicate glass containing one or more glass network modifying elements such as calcium, lead, lithium, sodium or potassium.
[0145] mixture
[0146] The mixture may contain not less than about 5 wt %, for example not less than about 10 wt %, or not less than about 20 wt %, or not less than about 30 wt %, or not less than about 40 wt %, or not less than about 50 wt % of silicate material. The mixture may contain not more than about 90 wt %, for example not more than about 80 wt %, or not more than about 70 wt %, or not more than about 60 wt % of silicate material. The mixture may contain from about 5 wt % to about 90 wt %, for example from about 10 wt % to about 90 wt %, or from about 20 wt % to about 90 wt %, or from about 30 wt % to about 90 wt %, or from about 40 wt % to about 90 wt %, or from about 50 wt % to about 90 wt %, or from about 5 wt % to about 80 wt %, or from about 10 wt % to about 80 wt %, or from about 20 wt % to about 80 wt %, or from about 30 wt % to about 80 wt %, or from about 40 wt % to about 80 wt %, or from about 50 wt % to about 80 wt %, Or about 5 wt % to about 70 wt %, or about 10 wt % to about 70 wt %, or about 20 wt % to about 70 wt %, or about 30 wt % to about 70 wt %, or about 40 wt % to about 70 wt %, or about 50 wt % to about 70 wt %, or about 5 wt % to about 60 wt %, or about 10 wt % to about 60 wt %, or about 20 wt % to about 60 wt %, or about 30 wt % to about 60 wt %, or about 40 wt % to about 60 wt %, or about 50 wt % to about 60 wt % of silicate material.
[0147] The mixture may contain not less than about 5 wt %, such as not less than about 10 wt %, or not less than about 20 wt %, or not less than about 30 wt %, or not less than about 40 wt %, or not less than about 50 wt % of amorphous silicate material. The mixture may contain not more than about 90 wt %, such as not more than about 80 wt %, or not more than about 70 wt %, or not more than about 60 wt % of amorphous silicate material. The mixture may contain from about 5 wt % to about 90 wt %, such as from about 10 wt % to about 90 wt %, or from about 20 wt % to about 90 wt %, or from about 30 wt % to about 90 wt %, or from about 40 wt % to about 90 wt %, or from about 50 wt % to about 90 wt %, or from about 5 wt % to about 80 wt %, or from about 10 wt % to about 80 wt %, or from about 20 wt % to about 80 wt %, or from about 30 wt % to about 80 wt %, or from about 40 wt % to about 80 wt %, or from about 50 wt % to about 80 wt %, or From about 5 wt % to about 70 wt %, or from about 10 wt % to about 70 wt %, or from about 20 wt % to about 70 wt %, or from about 30 wt % to about 70 wt %, or from about 40 wt % to about 70 wt %, or from about 50 wt % to about 70 wt %, or from about 5 wt % to about 60 wt %, or from about 10 wt % to about 60 wt %, or from about 20 wt % to about 60 wt %, or from about 30 wt % to about 60 wt %, or from about 40 wt % to about 60 wt %, or from about 50 wt % to about 60 wt % of amorphous silicate material.
[0148] The mixture may contain not less than about 5 wt %, such as not less than about 10 wt %, or not less than about 20 wt %, or not less than about 30 wt %, or not less than about 40 wt %, or not less than about 50 wt % of aluminosilicate material. The mixture may contain not more than about 90 wt %, such as not more than about 80 wt %, or not more than about 70 wt %, or not more than about 60 wt % of aluminosilicate material. The mixture may contain from about 5 wt % to about 90 wt %, such as from about 10 wt % to about 90 wt %, or from about 20 wt % to about 90 wt %, or from about 30 wt % to about 90 wt %, or from about 40 wt % to about 90 wt %, or from about 50 wt % to about 90 wt %, or from about 5 wt % to about 80 wt %, or from about 10 wt % to about 80 wt %, or from about 20 wt % to about 80 wt %, or from about 30 wt % to about 80 wt %, or from about 40 wt % to about 80 wt %, or from about 50 wt % to about 80 wt %, Or about 5 wt % to about 70 wt %, or about 10 wt % to about 70 wt %, or about 20 wt % to about 70 wt %, or about 30 wt % to about 70 wt %, or about 40 wt % to about 70 wt %, or about 50 wt % to about 70 wt %, or about 5 wt % to about 60 wt %, or about 10 wt % to about 60 wt %, or about 20 wt % to about 60 wt %, or about 30 wt % to about 60 wt %, or about 40 wt % to about 60 wt %, or about 50 wt % to about 60 wt % of aluminosilicate material.
[0149] The mixture may contain not less than about 5% by weight, for example not less than about 10% by weight, or not less than about 20% by weight, or not less than about 30% by weight, or not less than about 40% by weight, or not less than about 50% by weight of silicate. The mixture may contain not more than about 90% by weight, for example not more than about 80% by weight, or not more than about 70% by weight, or not more than about 60% by weight of silicate. The mixture may contain from about 5% by weight to about 90% by weight, for example from about 10% by weight to about 90% by weight, or from about 20% by weight to about 90% by weight, or from about 30% by weight to about 90% by weight, or from about 40% by weight to about 90% by weight, or from about 50% by weight to about 90% by weight, or from about 5% by weight to about 80% by weight, or from about 10% by weight to about 80% by weight, or from about 20% by weight to about 80% by weight, or from about 30% by weight to about 80% by weight, or from about 40% by weight to about 80% by weight, or from about 50% by weight to about 80% by weight , or about 5 wt % to about 70 wt %, or about 10 wt % to about 70 wt %, or about 20 wt % to about 70 wt %, or about 30 wt % to about 70 wt %, or about 40 wt % to about 70 wt %, or about 50 wt % to about 70 wt %, or about 5 wt % to about 60 wt %, or about 10 wt % to about 60 wt %, or about 20 wt % to about 60 wt %, or about 30 wt % to about 60 wt %, or about 40 wt % to about 60 wt %, or about 50 wt % to about 60 wt % of silicate.
[0150] The mixture may contain not less than about 5% by weight, for example not less than about 10% by weight, or not less than about 20% by weight, or not less than about 30% by weight, or not less than about 40% by weight, or not less than about 50% by weight of aluminosilicate. The mixture may contain not more than about 90% by weight, for example not more than about 80% by weight, or not more than about 70% by weight, or not more than about 60% by weight of aluminosilicate. The mixture may contain from about 5% by weight to about 90% by weight, for example from about 10% by weight to about 90% by weight, or from about 20% by weight to about 90% by weight, or from about 30% by weight to about 90% by weight, or from about 40% by weight to about 90% by weight, or from about 50% by weight to about 90% by weight, or from about 5% by weight to about 80% by weight, or from about 10% by weight to about 80% by weight, or from about 20% by weight to about 80% by weight, or from about 30% by weight to about 80% by weight, or from about 40% by weight to about 80% by weight, or from about 50% by weight to about 80% by weight , or about 5 wt % to about 70 wt %, or about 10 wt % to about 70 wt %, or about 20 wt % to about 70 wt %, or about 30 wt % to about 70 wt %, or about 40 wt % to about 70 wt %, or about 50 wt % to about 70 wt %, or about 5 wt % to about 60 wt %, or about 10 wt % to about 60 wt %, or about 20 wt % to about 60 wt %, or about 30 wt % to about 60 wt %, or about 40 wt % to about 60 wt %, or about 50 wt % to about 60 wt % of aluminosilicate.
[0151] The mixture may contain not less than about 5 wt %, such as not less than about 10 wt %, or not less than about 20 wt %, or not less than about 30 wt %, or not less than about 40 wt %, or not less than about 50 wt % of silicate glass. The mixture may contain not more than about 90 wt %, such as not more than about 80 wt %, or not more than about 70 wt %, or not more than about 60 wt % of silicate glass. The mixture may contain from about 5 wt % to about 90 wt %, such as from about 10 wt % to about 90 wt %, or from about 20 wt % to about 90 wt %, or from about 30 wt % to about 90 wt %, or from about 40 wt % to about 90 wt %, or from about 50 wt % to about 90 wt %, or from about 5 wt % to about 80 wt %, or from about 10 wt % to about 80 wt %, or from about 20 wt % to about 80 wt %, or from about 30 wt % to about 80 wt %, or from about 40 wt % to about 80 wt %, or from about 50 wt % to about 80 wt %, Or about 5 wt % to about 70 wt %, or about 10 wt % to about 70 wt %, or about 20 wt % to about 70 wt %, or about 30 wt % to about 70 wt %, or about 40 wt % to about 70 wt %, or about 50 wt % to about 70 wt %, or about 5 wt % to about 60 wt %, or about 10 wt % to about 60 wt %, or about 20 wt % to about 60 wt %, or about 30 wt % to about 60 wt %, or about 40 wt % to about 60 wt %, or about 50 wt % to about 60 wt % silicate glass.
[0152] The mixture may include not less than about 5 wt %, such as not less than about 10 wt %, or not less than about 20 wt %, or not less than about 30 wt %, or not less than about 40 wt %, or not less than about 50 wt % of aluminosilicate glass. The mixture may include not more than about 90 wt %, such as not more than about 80 wt %, or not more than about 70 wt %, or not more than about 60 wt % of aluminosilicate glass. The mixture may include from about 5 wt % to about 90 wt %, such as from about 10 wt % to about 90 wt %, or from about 20 wt % to about 90 wt %, or from about 30 wt % to about 90 wt %, or from about 40 wt % to about 90 wt %, or from about 50 wt % to about 90 wt %, or from about 5 wt % to about 80 wt %, or from about 10 wt % to about 80 wt %, or from about 20 wt % to about 80 wt %, or from about 30 wt % to about 80 wt %, or from about 40 wt % to about 80 wt %, or from about 50 wt % to about 80 wt %, Or about 5 wt % to about 70 wt %, or about 10 wt % to about 70 wt %, or about 20 wt % to about 70 wt %, or about 30 wt % to about 70 wt %, or about 40 wt % to about 70 wt %, or about 50 wt % to about 70 wt %, or about 5 wt % to about 60 wt %, or about 10 wt % to about 60 wt %, or about 20 wt % to about 60 wt %, or about 30 wt % to about 60 wt %, or about 40 wt % to about 60 wt %, or about 50 wt % to about 60 wt % of aluminosilicate glass.
[0153] The mixture may contain not less than about 5 wt %, such as not less than about 10 wt %, or not less than about 20 wt %, or not less than about 30 wt %, or not less than about 40 wt %, or not less than about 50 wt % of borosilicate glass. The mixture may contain not more than about 90 wt %, such as not more than about 80 wt %, or not more than about 70 wt %, or not more than about 60 wt % of borosilicate glass. The mixture may contain from about 5 wt % to about 90 wt %, such as from about 10 wt % to about 90 wt %, or from about 20 wt % to about 90 wt %, or from about 30 wt % to about 90 wt %, or from about 40 wt % to about 90 wt %, or from about 50 wt % to about 90 wt %, or from about 5 wt % to about 80 wt %, or from about 10 wt % to about 80 wt %, or from about 20 wt % to about 80 wt %, or from about 30 wt % to about 80 wt %, or from about 40 wt % to about 80 wt %, or from about 50 wt % to about 80 wt %, Or about 5 wt % to about 70 wt %, or about 10 wt % to about 70 wt %, or about 20 wt % to about 70 wt %, or about 30 wt % to about 70 wt %, or about 40 wt % to about 70 wt %, or about 50 wt % to about 70 wt %, or about 5 wt % to about 60 wt %, or about 10 wt % to about 60 wt %, or about 20 wt % to about 60 wt %, or about 30 wt % to about 60 wt %, or about 40 wt % to about 60 wt %, or about 50 wt % to about 60 wt % of borosilicate glass.
[0154] For example, the mixture may include not less than about 5 wt %, such as not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt %, or not less than about 13 wt %, or not less than about 14 wt % of borosilicate glass. The mixture may include not more than about 50 wt %, such as not more than about 30 wt %, or not more than about 25 wt %, or not more than about 20 wt %, or not more than about 17 wt %, or not more than about 16 wt %, or not more than about 15 wt %, or not more than about 14 wt % of borosilicate glass. The mixture may include from about 5 wt % to about 50 wt %, such as from about 5 wt % to about 30 wt %, or from about 5 wt % to about 25 wt %, or from about 10 wt % to about 20 wt %, or from about 12 wt % to about 16 wt %, or from about 12 wt % to about 14 wt %, or from about 13 wt % to about 14 wt %, or from about 14 wt % to about 16 wt %, or from about 14 wt % to about 15 wt % of borosilicate glass.
[0155] The mixture may contain not less than about 5% by weight, such as not less than about 10% by weight, or not less than about 20% by weight, or not less than about 30% by weight, or not less than about 40% by weight, or not less than about 50% by weight of silicate minerals. The mixture may contain not more than about 90% by weight, such as not more than about 80% by weight, or not more than about 70% by weight, or not more than about 60% by weight of silicate minerals. The mixture may contain from about 5% by weight to about 90% by weight, such as from about 10% by weight to about 90% by weight, or from about 20% by weight to about 90% by weight, or from about 30% by weight to about 90% by weight, or from about 40% by weight to about 90% by weight, or from about 50% by weight to about 90% by weight, or from about 5% by weight to about 80% by weight, or from about 10% by weight to about 80% by weight, or from about 20% by weight to about 80% by weight, or from about 30% by weight to about 80% by weight, or from about 40% by weight to about 80% by weight, or from about 50% by weight to about 80% by weight, Or about 5 wt % to about 70 wt %, or about 10 wt % to about 70 wt %, or about 20 wt % to about 70 wt %, or about 30 wt % to about 70 wt %, or about 40 wt % to about 70 wt %, or about 50 wt % to about 70 wt %, or about 5 wt % to about 60 wt %, or about 10 wt % to about 60 wt %, or about 20 wt % to about 60 wt %, or about 30 wt % to about 60 wt %, or about 40 wt % to about 60 wt %, or about 50 wt % to about 60 wt % of silicate minerals.
[0156] The mixture may contain not less than about 5% by weight, such as not less than about 10% by weight, or not less than about 20% by weight, or not less than about 30% by weight, or not less than about 40% by weight, or not less than about 50% by weight of aluminosilicate minerals. The mixture may contain not more than about 90% by weight, such as not more than about 80% by weight, or not more than about 70% by weight, or not more than about 60% by weight of aluminosilicate minerals. The mixture may contain from about 5% by weight to about 90% by weight, such as from about 10% by weight to about 90% by weight, or from about 20% by weight to about 90% by weight, or from about 30% by weight to about 90% by weight, or from about 40% by weight to about 90% by weight, or from about 50% by weight to about 90% by weight, or from about 5% by weight to about 80% by weight, or from about 10% by weight to about 80% by weight, or from about 20% by weight to about 80% by weight, or from about 30% by weight to about 80% by weight, or from about 40% by weight to about 80% by weight, or from about 50% by weight to about 80% by weight, Or about 5 wt % to about 70 wt %, or about 10 wt % to about 70 wt %, or about 20 wt % to about 70 wt %, or about 30 wt % to about 70 wt %, or about 40 wt % to about 70 wt %, or about 50 wt % to about 70 wt %, or about 5 wt % to about 60 wt %, or about 10 wt % to about 60 wt %, or about 20 wt % to about 60 wt %, or about 30 wt % to about 60 wt %, or about 40 wt % to about 60 wt %, or about 50 wt % to about 60 wt % of aluminosilicate minerals.
[0157] The mixture may contain not less than about 5% by weight, such as not less than about 10% by weight, or not less than about 20% by weight, or not less than about 30% by weight, or not less than about 40% by weight, or not less than about 50% by weight of volcanic glass. The mixture may contain not more than about 90% by weight, such as not more than about 80% by weight, or not more than about 70% by weight, or not more than about 60% by weight of volcanic glass. The mixture may contain from about 5% to about 90% by weight, such as from about 10% to about 90% by weight, or from about 20% to about 90% by weight, or from about 30% to about 90% by weight, or from about 40% to about 90% by weight, or from about 50% to about 90% by weight, or from about 5% to about 80% by weight, or from about 10% to about 80% by weight, or from about 20% to about 80% by weight, or from about 30% to about 80% by weight, or from about 40% to about 80% by weight, or from about 50% to about 80% by weight , or about 5 wt % to about 70 wt %, or about 10 wt % to about 70 wt %, or about 20 wt % to about 70 wt %, or about 30 wt % to about 70 wt %, or about 40 wt % to about 70 wt %, or about 50 wt % to about 70 wt %, or about 5 wt % to about 60 wt %, or about 10 wt % to about 60 wt %, or about 20 wt % to about 60 wt %, or about 30 wt % to about 60 wt %, or about 40 wt % to about 60 wt %, or about 50 wt % to about 60 wt % of volcanic glass.
[0158] For example, the mixture may include not less than about 20% by weight, such as not less than about 25% by weight, or not less than about 28% by weight, or not less than about 30% by weight, or not less than about 34% by weight of volcanic glass. The mixture may include no more than about 50% by weight, such as no more than about 45% by weight, or no more than about 40% by weight, or no more than about 35% by weight, or no more than about 30% by weight of volcanic glass. The mixture may include from about 20% to about 50% by weight, such as from about 25% to about 45% by weight, or from about 25% to about 35% by weight, or from about 25% to about 30% by weight, or from about 28% to about 30% by weight, or from about 30% to about 40% by weight, or from about 34% to about 35% by weight of volcanic glass.
[0159] The mixture may contain not less than about 5% by weight, such as not less than about 10% by weight, or not less than about 20% by weight, or not less than about 30% by weight, or not less than about 40% by weight, or not less than about 50% by weight of perlite material. The mixture may contain not more than about 90% by weight, such as not more than about 80% by weight, or not more than about 70% by weight, or not more than about 60% by weight of perlite material. The mixture may contain from about 5% to about 90% by weight, such as from about 10% to about 90% by weight, or from about 20% to about 90% by weight, or from about 30% to about 90% by weight, or from about 40% to about 90% by weight, or from about 50% to about 90% by weight, or from about 5% to about 80% by weight, or from about 10% to about 80% by weight, or from about 20% to about 80% by weight, or from about 30% to about 80% by weight, or from about 40% to about 80% by weight, or from about 50% to about 80% by weight, Or about 5 wt % to about 70 wt %, or about 10 wt % to about 70 wt %, or about 20 wt % to about 70 wt %, or about 30 wt % to about 70 wt %, or about 40 wt % to about 70 wt %, or about 50 wt % to about 70 wt %, or about 5 wt % to about 60 wt %, or about 10 wt % to about 60 wt %, or about 20 wt % to about 60 wt %, or about 30 wt % to about 60 wt %, or about 40 wt % to about 60 wt %, or about 50 wt % to about 60 wt % of perlite material.
[0160] For example, the mixture may include not less than about 20% by weight, such as not less than about 25% by weight, or not less than about 28% by weight, or not less than about 30% by weight, or not less than about 34% by weight of perlite material. The mixture may include no more than about 50% by weight, such as no more than about 45% by weight, or no more than about 40% by weight, or no more than about 35% by weight, or no more than about 30% by weight of perlite material. The mixture may include from about 20% to about 50% by weight, such as from about 25% to about 45% by weight, or from about 25% to about 35% by weight, or from about 25% to about 30% by weight, or from about 28% to about 30% by weight, or from about 30% to about 40% by weight, or from about 34% to about 35% by weight of perlite material.
[0161] The mixture may contain not less than about 20% by weight, such as not less than about 25% by weight, or not less than about 28% by weight, or not less than about 30% by weight, or not less than about 34% by weight of unexpanded natural perlite ore. The mixture may contain no more than about 50% by weight, such as no more than about 45% by weight, or no more than about 40% by weight, or no more than about 35% by weight, or no more than about 30% by weight of unexpanded natural perlite ore. The mixture may contain from about 20% to about 50% by weight, such as from about 25% to about 45% by weight, or from about 25% to about 35% by weight, or from about 25% to about 30% by weight, or from about 28% to about 30% by weight, or from about 30% to about 40% by weight, or from about 34% to about 35% by weight of unexpanded natural perlite ore.
[0162] The mixture may include not less than about 5 wt %, for example not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt %, or not less than about 15 wt %, or not less than about 17 wt % of the basic compound. The mixture may include no more than about 30 wt %, for example no more than about 25 wt %, or no more than about 20 wt %, or no more than about 18 wt %, or no more than about 17 wt %, or no more than about 15 wt % or no more than about 14 wt % of the basic compound. The mixture may contain from about 5 wt % to about 30 wt %, for example from about 5 wt % to about 25 wt %, or from about 5 wt % to about 20 wt %, or from about 8 wt % to about 20 wt %, or from about 8 wt % to about 18 wt %, or from about 10 wt % to about 15 wt %, or from about 12 wt % to about 15 wt %, or from about 12 wt % to about 14 wt %, or from about 10 wt % to about 14 wt %, or from about 14 wt % to about 18 wt %, or from about 15 wt % to about 17 wt %, or from about 16 wt % to about 20 wt % of the basic compound.
[0163] The mixture may contain not less than about 5 wt %, such as not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt %, or not less than about 15 wt %, or not less than about 17 wt % of the alkaline hydroxide. The mixture may contain no more than about 30 wt %, such as no more than about 25 wt %, or no more than about 20 wt %, or no more than about 18 wt %, or no more than about 17 wt %, or no more than about 15 wt %, or no more than about 14 wt % of the alkaline hydroxide. The mixture may contain from about 5 wt % to about 30 wt %, for example from about 5 wt % to about 25 wt %, or from about 5 wt % to about 20 wt %, or from about 8 wt % to about 20 wt %, or from about 8 wt % to about 18 wt %, or from about 10 wt % to about 15 wt %, or from about 12 wt % to about 15 wt %, or from about 12 wt % to about 14 wt %, or from about 10 wt % to about 14 wt %, or from about 14 wt % to about 18 wt %, or from about 15 wt % to about 17 wt %, or from about 16 wt % to about 20 wt % of the alkaline hydroxide.
[0164] The mixture can include not less than about 5 wt %, for example not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt %, or not less than about 15 wt %, or not less than about 17 wt % of the alkaline carbonate. The mixture can include no more than about 30 wt %, for example no more than about 25 wt %, or no more than about 20 wt %, or no more than about 18 wt %, or no more than about 17 wt %, or no more than about 15 wt % or no more than about 14 wt % of the alkaline carbonate. The mixture may contain from about 5 wt % to about 30 wt %, for example from about 5 wt % to about 25 wt %, or from about 5 wt % to about 20 wt %, or from about 8 wt % to about 20 wt %, or from about 8 wt % to about 18 wt %, or from about 10 wt % to about 15 wt %, or from about 12 wt % to about 15 wt %, or from about 12 wt % to about 14 wt %, or from about 10 wt % to about 14 wt %, or from about 14 wt % to about 18 wt %, or from about 15 wt % to about 17 wt %, or from about 16 wt % to about 20 wt % of the alkaline carbonate.
[0165] The mixture may contain not less than about 5 wt %, such as not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt %, or not less than about 15 wt %, or not less than about 17 wt % of the alkali silicate. The mixture may contain no more than about 30 wt %, such as no more than about 25 wt %, or no more than about 20 wt %, or no more than about 18 wt %, or no more than about 17 wt %, or no more than about 15 wt %, or no more than about 14 wt % of the alkali silicate. The mixture may contain from about 5% to about 30% by weight, for example from about 5% to about 25% by weight, or from about 5% to about 20% by weight, or from about 8% to about 20% by weight, or from about 8% to about 18% by weight, or from about 10% to about 15% by weight, or from about 12% to about 15% by weight, or from about 12% to about 14% by weight, or from about 10% to about 14% by weight, or from about 14% to about 18% by weight, or from about 15% to about 17% by weight, or from about 16% to about 20% by weight of the alkali silicate.
[0166] For example, the mixture may contain not less than about 5 wt %, such as not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt %, or not less than about 15 wt %, or not less than about 17 wt % of sodium hydroxide, lithium hydroxide, and / or potassium hydroxide. The mixture may contain no more than about 30 wt %, such as no more than about 25 wt %, or no more than about 20 wt %, or no more than about 18 wt %, or no more than about 17 wt %, or no more than about 15 wt %, or no more than about 14 wt % of sodium hydroxide, lithium hydroxide, and / or potassium hydroxide. The mixture may contain from about 5 wt % to about 30 wt %, for example from about 5 wt % to about 25 wt %, or from about 5 wt % to about 20 wt %, or from about 8 wt % to about 20 wt %, or from about 8 wt % to about 18 wt %, or from about 10 wt % to about 15 wt %, or from about 12 wt % to about 15 wt %, or from about 12 wt % to about 14 wt %, or from about 10 wt % to about 14 wt %, or from about 14 wt % to about 18 wt %, or from about 15 wt % to about 17 wt %, or from about 16 wt % to about 20 wt % of sodium hydroxide, lithium hydroxide and / or potassium hydroxide.
[0167] The mixture may include not less than about 5% by weight, such as not less than about 8% by weight, or not less than about 10% by weight, or not less than about 12% by weight, or not less than about 15% by weight, or not less than about 17% by weight of sodium carbonate, lithium carbonate and / or potassium carbonate. The mixture may include no more than about 30% by weight, such as no more than about 25% by weight, or no more than about 20% by weight, or no more than about 18% by weight, or no more than about 17% by weight, or no more than about 15% by weight or no more than about 14% by weight of sodium carbonate, lithium carbonate and / or potassium carbonate. The mixture may contain from about 5 wt % to about 30 wt %, for example from about 5 wt % to about 25 wt %, or from about 5 wt % to about 20 wt %, or from about 8 wt % to about 20 wt %, or from about 8 wt % to about 18 wt %, or from about 10 wt % to about 15 wt %, or from about 12 wt % to about 15 wt %, or from about 12 wt % to about 14 wt %, or from about 10 wt % to about 14 wt %, or from about 14 wt % to about 18 wt %, or from about 15 wt % to about 17 wt %, or from about 16 wt % to about 20 wt % of sodium carbonate, lithium carbonate and / or potassium carbonate.
[0168] The mixture may contain not less than about 5 wt %, such as not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt %, or not less than about 15 wt %, or not less than about 17 wt % of sodium silicate, lithium silicate and / or potassium silicate. The mixture may contain no more than about 30 wt %, such as no more than about 25 wt %, or no more than about 20 wt %, or no more than about 18 wt %, or no more than about 17 wt %, or no more than about 15 wt %, or no more than about 14 wt % of sodium silicate, lithium silicate and / or potassium silicate. The mixture may contain from about 5 wt % to about 30 wt %, for example from about 5 wt % to about 25 wt %, or from about 5 wt % to about 20 wt %, or from about 8 wt % to about 20 wt %, or from about 8 wt % to about 18 wt %, or from about 10 wt % to about 15 wt %, or from about 12 wt % to about 15 wt %, or from about 12 wt % to about 14 wt %, or from about 10 wt % to about 14 wt %, or from about 14 wt % to about 18 wt %, or from about 15 wt % to about 17 wt %, or from about 16 wt % to about 20 wt % of sodium silicate, lithium silicate and / or potassium silicate.
[0169] The mixture may include not less than about 15 wt %, for example not less than about 20 wt %, or not less than about 22 wt %, or less than about 25 wt % water. The mixture may include no more than about 45 wt %, for example no more than about 40 wt %, or no more than about 35 wt %, or no more than about 30 wt % water. The mixture may include about 15 wt % to about 45 wt %, for example about 20 wt % to about 40 wt %, or about 20 wt % to about 30 wt %, or about 25 wt % to about 30 wt % water.
[0170] The mixture may comprise two different silicate materials.
[0171] For example, the mixture may include silicate glass (e.g., aluminosilicate glass) and silicate minerals (e.g., aluminosilicate minerals). The mixture may include not less than about 5% by weight, such as not less than about 8% by weight, or not less than about 10% by weight, or not less than about 12% by weight, or not less than about 15% by weight, or not less than about 20% by weight of silicate glass (e.g., aluminosilicate glass). The mixture may include not more than about 50% by weight, such as not more than about 40% by weight, or not more than about 30% by weight, or not more than about 25% by weight, or not more than about 20% by weight, or not more than about 16% by weight of silicate glass (e.g., aluminosilicate glass). The mixture may include from about 5% by weight to about 50% by weight, such as from about 8% by weight to about 40% by weight, or from about 10% by weight to about 30% by weight, or from about 10% by weight to about 20% by weight, or from about 12% by weight to about 16% by weight of silicate glass (e.g., aluminosilicate glass). In addition, the mixture may include not less than about 10% by weight, such as not less than about 15% by weight, or not less than about 20% by weight, or not less than about 25% by weight of silicate minerals (e.g., aluminosilicate minerals). The mixture may include not more than about 60% by weight, such as not more than about 50% by weight, or not more than about 45% by weight, or not more than about 40% by weight, or not more than about 35% by weight of silicate minerals (e.g., aluminosilicate minerals). The mixture may include about 10% by weight to about 60% by weight, such as about 15% by weight to about 50% by weight, or about 20% by weight to about 45% by weight, or about 25% by weight to about 45% by weight, or about 25% by weight to about 30% by weight of silicate minerals (e.g., aluminosilicate minerals).
[0172] Alternatively, the mixture may include a first silicate glass (e.g., a first aluminosilicate glass) and a second silicate glass (e.g., a second aluminosilicate glass). The mixture may include not less than about 5% by weight, such as not less than about 8% by weight, or not less than about 10% by weight, or not less than about 12% by weight, or not less than about 15% by weight, or not less than about 20% by weight of the first silicate glass (e.g., the first aluminosilicate glass). The mixture may include not more than about 50% by weight, such as not more than about 40% by weight, or not more than about 30% by weight, or not more than about 25% by weight, or not more than about 20% by weight, or not more than about 16% by weight of the first silicate glass (e.g., the first aluminosilicate glass). The mixture may include from about 5% by weight to about 50% by weight, such as from about 8% by weight to about 40% by weight, or from about 10% by weight to about 30% by weight, or from about 10% by weight to about 20% by weight, or from about 12% by weight to about 16% by weight of the first silicate glass (e.g., the first aluminosilicate glass). In addition, the mixture may include not less than about 5 wt %, such as not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt %, or not less than about 15 wt %, or not less than about 20 wt % of the second silicate glass (e.g., the second aluminosilicate glass). The mixture may include not more than about 50 wt %, such as not more than about 40 wt %, or not more than about 30 wt %, or not more than about 25 wt %, or not more than about 20 wt %, or not more than about 16 wt % of the second silicate glass (e.g., the second aluminosilicate glass). The mixture may include from about 5 wt % to about 50 wt %, such as from about 8 wt % to about 40 wt %, or from about 10 wt % to about 30 wt %, or from about 10 wt % to about 20 wt %, or from about 12 wt % to about 16 wt % of the second silicate glass (e.g., the second aluminosilicate glass).
[0173] One of the two different silicate materials can be selected from: perlite material, such as unexpanded natural perlite ore with a water content greater than about 2% by weight; phyllosilicate minerals, such as bentonite, kaolin or calcined kaolin; diatomaceous earth. Additionally or alternatively, one of the two different silicate materials can be selected from: fused silica glass, soda-lime glass, borosilicate glass, lead oxide glass, aluminosilicate glass, silicon germanium glass.
[0174] For example, a mixture may contain:
[0175] A first silicate material selected from:
[0176] Volcanic glass, such as perlite material, such as unexpanded natural perlite ore having a water content greater than about 2% by weight;
[0177] Phyllosilicate minerals such as bentonite, kaolin or calcined kaolin; and diatomaceous earth; or combinations thereof; and
[0178] The second silicate material is selected from:
[0179] Fused silica glass, soda-lime glass, borosilicate glass, lead oxide glass, aluminosilicate glass, silicon-germanium glass.
[0180] The mixture may include a first silicate material and a second silicate material, the first silicate material being a perlite material, the second silicate material being selected from the group consisting of fused silica glass, soda-lime glass, borosilicate glass, lead oxide glass, aluminosilicate glass, and silicon-germanium glass.
[0181] The mixture may include a perlite material, such as an unexpanded natural perlite ore having a water content greater than about 2% by weight, and a silicate glass in addition to the perlite material. For example, the mixture may include a perlite material, such as an unexpanded natural perlite ore having a water content greater than about 2% by weight, and a borosilicate glass.
[0182] The first silicate material and the second silicate material may both be silicate glasses. For example, the mixture may include two different silicate glasses selected from the group consisting of: fused silica glass, soda-lime glass, borosilicate glass, lead oxide glass, aluminosilicate glass, silicon-germanium glass. The mixture may include borosilicate glass and soda-lime glass.
[0183] The mixture may contain three or more different silicate materials. For example, the mixture may contain a first silicate glass, a second silicate glass different from the first silicate glass, and a silicate mineral different from the first and second silicate glasses. For example, the mixture may contain: a first and a second silicate glass selected from: used silica glass, soda-lime glass, borosilicate glass, lead oxide glass, aluminosilicate glass, silicon germanium glass; and a silicate mineral selected from: volcanic glass, such as a perlite material, such as an unexpanded natural perlite ore having a water content greater than about 2% by weight; a phyllosilicate mineral, such as bentonite, kaolin, or calcined kaolin; diatomaceous earth; or a combination thereof (e.g., diatomaceous mudstone (moler) (i.e., clay diatomaceous earth containing both clay minerals and diatomaceous earth)). The mixture may contain borosilicate glass, soda-lime glass, and a perlite material (e.g., an unexpanded natural perlite ore having a water content greater than about 2% by weight).
[0184] It should be understood that whenever a mixture is described as comprising a silicate material (e.g., a silicate glass or a silicate mineral) and a perlite material, the silicate material (e.g., a silicate glass or a silicate mineral) is not a perlite material. Similarly, when a mixture is described as comprising both a silicate glass and a silicate mineral, the silicate glass and the silicate mineral are not the same material, i.e., the silicate glass and the silicate mineral differ in chemical composition and / or physical structure, e.g., crystalline phase or amorphous phase and / or microstructure.
[0185] The mixture may contain not less than about 1 wt %, such as not less than about 5 wt %, or not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt %, or not less than about 14 wt %, or not less than about 20 wt %, or not less than about 30 wt %, or not less than about 35 wt %, or not less than about 40 wt % of reactive silica. The mixture may contain no more than about 60 wt %, such as no more than about 50 wt %, or no more than about 45 wt %, or no more than about 40 wt %, or no more than about 30 wt %, or no more than about 20 wt %, or no more than about 18 wt %, or no more than about 15 wt % of reactive silica. The mixture may contain from about 1 wt % to about 60 wt %, for example from about 5 wt % to about 50 wt %, or from about 5 wt % to about 45 wt %, or from about 5 wt % to about 25 wt %, or from about 5 wt % to about 20 wt %, or from about 8 wt % to about 20 wt %, or from about 8 wt % to about 18 wt %, or from about 8 wt % to about 12 wt %, or from about 10 wt % to about 18 wt %, or from about 12 wt % to about 18 wt %, or from about 14 wt % to about 15 wt %, or from about 20 wt % to about 60 wt %, or from about 30 wt % to about 50 wt %, or from about 35 wt % to about 45 wt % of reactive silica.
[0186] For example, the mixture may include not less than about 1 wt %, such as not less than about 5 wt %, or not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt %, or not less than about 14 wt %, or not less than about 20 wt %, or not less than about 30 wt %, or not less than about 35 wt %, or not less than about 40 wt % silica fume. The mixture may include no more than about 60 wt %, such as no more than about 50 wt %, or no more than about 45 wt %, or no more than about 40 wt %, or no more than about 30 wt %, or no more than about 20 wt %, or no more than about 18 wt %, or no more than about 15 wt % silica fume. The mixture may contain from about 1 wt % to about 60 wt %, for example from about 5 wt % to about 50 wt %, or from about 5 wt % to about 45 wt %, or from about 5 wt % to about 25 wt %, or from about 5 wt % to about 20 wt %, or from about 8 wt % to about 20 wt %, or from about 8 wt % to about 18 wt %, or from about 8 wt % to about 12 wt %, or from about 10 wt % to about 18 wt %, or from about 12 wt % to about 18 wt %, or from about 14 wt % to about 15 wt %, or from about 20 wt % to about 60 wt %, or from about 30 wt % to about 50 wt %, or from about 35 wt % to about 45 wt % silica fume.
[0187] Alternatively, the mixture may contain not less than about 1 wt %, such as not less than about 5 wt %, or not less than about 8 wt %, or not less than about 10 wt %, or not less than about 12 wt %, or not less than about 14 wt %, or not less than about 20 wt %, or not less than about 30 wt %, or not less than about 35 wt %, or not less than about 40 wt % of fumed silica. The mixture may contain no more than about 60 wt %, such as no more than about 50 wt %, or no more than about 45 wt %, or no more than about 40 wt %, or no more than about 30 wt %, or no more than about 20 wt %, or no more than about 18 wt %, or no more than about 15 wt % of fumed silica. The mixture may contain from about 1 wt % to about 60 wt %, for example from about 5 wt % to about 50 wt %, or from about 5 wt % to about 45 wt %, or from about 5 wt % to about 25 wt %, or from about 5 wt % to about 20 wt %, or from about 8 wt % to about 20 wt %, or from about 8 wt % to about 18 wt %, or from about 8 wt % to about 12 wt %, or from about 10 wt % to about 18 wt %, or from about 12 wt % to about 18 wt %, or from about 14 wt % to about 15 wt %, or from about 20 wt % to about 60 wt %, or from about 30 wt % to about 50 wt %, or from about 35 wt % to about 45 wt % fumed silica.
[0188] The mixture may contain: from about 5 wt % to about 80 wt %, for example from about 10 wt % to about 70 wt %, or from about 10 wt % to about 20 wt %, or from about 20 wt % to about 70 wt %, or from about 30 wt % to about 70 wt %, or from about 40 wt % to about 70 wt %, or from about 50 wt % to about 70 wt % of silicate material; from about 5 wt % to about 30 wt %, for example from about 5 wt % to about 20 wt % of alkaline compound; and from about 20 wt % to about 40 wt %, for example from about 20 wt % to about 30 wt % of water.
[0189] For example, the mixture may be composed of: about 40% to about 80% by weight, such as about 50% to about 70% by weight of silicate materials; about 5% to about 30% by weight, such as about 5% to about 20% by weight of alkaline compounds; and about 20% to about 50% by weight, such as about 20% to about 40% by weight of water. The mixture may be composed of: about 40% to about 80% by weight, such as about 50% to about 70% by weight of silicate glass (e.g., borosilicate glass); about 5% to about 30% by weight, such as about 5% to about 20% by weight of alkaline compounds; and about 20% to about 50% by weight, such as about 20% to about 40% by weight of water.
[0190] The mixture may include: about 5 wt % to about 80 wt %, for example, about 10 wt % to about 70 wt %, or about 10 wt % to about 50 wt %, or about 10 wt % to about 30 wt % of silicate material; about 10 wt % to about 60 wt %, for example, about 15 wt % to about 50 wt % of reactive silica other than silicate material; about 5 wt % to about 30 wt %, for example, about 5 wt % to about 25 wt % of a basic compound; and about 20 wt % to about 40 wt %, for example, about 20 wt % to about 35 wt % of water.
[0191] For example, the mixture may be composed of: about 5 wt % to about 80 wt %, for example, about 10 wt % to about 70 wt %, or about 10 wt % to about 50 wt %, or about 10 wt % to about 30 wt % of silicate glass (e.g., borosilicate glass and / or soda-lime glass); about 10 wt % to about 60 wt %, for example, about 15 wt % to about 50 wt % of reactive silica; about 5 wt % to about 30 wt %, for example, about 5 wt % to about 25 wt % of an alkaline compound; and about 20 wt % to about 40 wt %, for example, about 20 wt % to about 35 wt % of water.
[0192] The mixture may include: about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of the first silicate material; about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of the second silicate material; about 5 wt % to about 30 wt %, for example, about 5 wt % to about 25 wt % of the alkaline compound; and about 20 wt % to about 40 wt %, for example, about 20 wt % to about 35 wt % of water.
[0193] The mixture may include: about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of a first silicate glass (e.g., borosilicate glass); about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of a second silicate glass (e.g., soda-lime glass); about 5 wt % to about 30 wt %, for example, about 5 wt % to about 25 wt % of an alkaline compound; and about 20 wt % to about 40 wt %, for example, about 20 wt % to about 35 wt % of water.
[0194] The mixture may contain: about 5 wt % to about 50 wt %, for example about 5 wt % to about 40 wt % of silicate glass (e.g., borosilicate and / or soda-lime glass); about 5 wt % to about 50 wt %, for example about 5 wt % to about 40 wt % of silicate minerals other than silicate glass; about 5 wt % to about 30 wt %, for example about 5 wt % to about 25 wt % of alkaline compounds; and about 20 wt % to about 40 wt %, for example about 20 wt % to about 35 wt % of water.
[0195] The mixture may include: about 5% to about 50% by weight, for example, about 5% to about 40% by weight of perlite material (e.g., unexpanded natural perlite ore having a water content greater than about 2% by weight); about 5% to about 50% by weight, for example, about 5% to about 40% by weight of silicate glass other than perlite material (e.g., borosilicate and / or soda-lime glass); about 5% to about 30% by weight, for example, about 5% to about 25% by weight of an alkaline compound; and about 20% to about 40% by weight, for example, about 20% to about 35% by weight of water.
[0196] The mixture may include: about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of the first silicate material; about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of the second silicate material; about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of reactive silica other than the first and second silicate materials; about 5 wt % to about 30 wt %, for example, about 5 wt % to about 25 wt % of a basic compound; and about 20 wt % to about 40 wt %, for example, about 20 wt % to about 35 wt % of water.
[0197] The mixture may include: about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of a first silicate glass; about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of a second silicate glass; about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of reactive silica; about 5 wt % to about 30 wt %, for example, about 5 wt % to about 25 wt % of an alkaline compound; and about 20 wt % to about 40 wt %, for example, about 20 wt % to about 35 wt % of water.
[0198] The mixture may include: about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of silicate glass; about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of silicate minerals; about 5 wt % to about 50 wt %, for example, about 5 wt % to about 40 wt % of reactive silica; about 5 wt % to about 30 wt %, for example, about 5 wt % to about 25 wt % of alkaline compounds; and about 20 wt % to about 40 wt %, for example, about 20 wt % to about 35 wt % of water.
[0199] The mixture may include: about 5% to about 50% by weight, for example, about 5% to about 40% by weight of perlite material (e.g., unexpanded natural perlite ore having a water content greater than about 2% by weight); about 5% to about 50% by weight, for example, about 5% to about 40% by weight of silicate glass other than perlite material (e.g., borosilicate and / or soda-lime glass); about 5% to about 50% by weight, for example, about 5% to about 40% by weight of reactive silica other than the first and second silicate materials; about 5% to about 30% by weight, for example, about 5% to about 25% by weight of an alkaline compound; and about 20% to about 40% by weight, for example, about 20% to about 35% by weight of water.
[0200] The mixture may include: about 5 wt % to about 25 wt %, for example, about 10 wt % to about 20 wt % silicate glass; about 1 wt % to about 50 wt %, for example, about 5 wt % to about 45 wt % reactive silica; about 5 wt % to about 30 wt %, for example, about 10 wt % to about 20 wt % alkaline compound; about 20 wt % to about 40 wt %, for example, about 20 wt % to about 30 wt % water; and optionally about 20 wt % to about 55 wt %, for example, about 25 wt % to about 50 wt % perlite material. For example, the mixture may include: about 5 wt % to about 25 wt %, for example, about 10 wt % to about 20 wt % borosilicate glass; about 5 wt % to about 20 wt %, for example, about 10 wt % to about 45 wt % silica fume; about 5 wt % to about 20 wt %, for example, about 10 wt % to about 20 wt % sodium hydroxide and / or lithium hydroxide; about 20 wt % to about 40 wt %, for example, about 20 wt % to about 30 wt % water; and optionally about 20 wt % to about 55 wt %, for example, about 25 wt % to about 50 wt % unexpanded natural perlite ore.
[0201] The mixture may include: about 5 wt % to about 25 wt %, for example, about 10 wt % to about 20 wt % of silicate glass; about 20 wt % to about 50 wt %, for example, about 25 wt % to about 45 wt % of perlite material; about 5 wt % to about 20 wt %, for example, about 10 wt % to about 15 wt % of reactive silica; about 5 wt % to about 20 wt %, for example, about 10 wt % to about 17 wt % of alkaline compounds; and about 20 wt % to about 40 wt %, for example, about 20 wt % to about 30 wt % of water. For example, the mixture may include: about 5 wt % to about 25 wt %, for example, about 10 wt % to about 20 wt % borosilicate glass; about 20 wt % to about 50 wt %, for example, about 25 wt % to about 45 wt % unexpanded natural perlite ore; about 5 wt % to about 20 wt %, for example, about 10 wt % to about 15 wt % silica fume; about 5 wt % to about 20 wt %, for example, about 10 wt % to about 17 wt % sodium hydroxide and / or lithium hydroxide; and about 20 wt % to about 40 wt %, for example, about 20 wt % to about 30 wt % water.
[0202] The mixture may include (e.g., consist essentially of or consist of): about 10% to about 15% by weight silicate glass; about 35% to about 45% by weight reactive silica; about 15% to about 20% by weight alkaline compound; and about 25% to about 35% by weight water. For example, the mixture may include (e.g., consist essentially of or consist of): about 10% to about 15% by weight borosilicate glass; about 35% to about 45% by weight silica fume; about 15% to about 20% by weight sodium hydroxide and / or lithium hydroxide; and about 25% to about 35% by weight water.
[0203] The mixture may include (e.g., consist essentially of or consist of): about 30% to about 40% by weight of perlite material; about 10% to about 20% by weight of silicate glass; about 5% to about 15% by weight of reactive silica; about 10% to about 15% by weight of an alkaline compound; and about 20% to about 30% by weight of water. For example, the mixture may include (e.g., consist essentially of or consist of): about 30% to about 40% by weight of unexpanded natural perlite ore; about 10% to about 20% by weight of borosilicate glass; about 5% to about 15% by weight of silica fume; about 10% to about 15% by weight of sodium hydroxide and / or lithium hydroxide; and about 20% to about 30% by weight of water.
[0204] The mixture may include (e.g., consist essentially of or consist of): about 25% to about 35% by weight of perlite material; about 10% to about 20% by weight of silicate glass; about 10% to about 20% by weight of reactive silica; about 10% to about 20% by weight of an alkaline compound; and about 20% to about 30% by weight of water. For example, the mixture may include (e.g., consist essentially of or consist of): about 25% to about 35% by weight of unexpanded natural perlite ore; about 10% to about 20% by weight of borosilicate glass; about 10% to about 20% by weight of silica fume; about 10% to about 20% by weight of sodium hydroxide and / or lithium hydroxide; and about 20% to about 30% by weight of water.
[0205] The mixture may include (e.g., consist essentially of or consist of): about 20% to about 50% by weight of silicate minerals; about 10% to about 20% by weight of silicate glass; about 5% to about 45% by weight of reactive silica; about 5% to about 30% by weight of alkaline compounds; and about 15% to about 40% by weight of water. For example, the mixture may include (e.g., consist essentially of or consist of): about 20% to about 50% by weight of perlite material; about 10% to about 20% by weight of borosilicate and / or soda-lime glass; about 5% to about 45% by weight of silica fume; about 5% to about 30% by weight of sodium hydroxide and / or lithium hydroxide; and about 15% to about 40% by weight of water. The mixture may include (e.g., consist essentially of or consist of): about 20 weight percent to about 50 weight percent perlite material; about 10 weight percent to about 20 weight percent borosilicate and / or soda-lime glass; about 5 weight percent to about 45 weight percent silica fume; about 5 weight percent to about 20 weight percent sodium hydroxide; about 0 weight percent to about 10 weight percent lithium hydroxide; and about 15 weight percent to about 40 weight percent water.
[0206] The mixture may include not less than about 0.01 wt %, such as not less than about 0.1 wt %, or not less than about 1 wt % of glass network forming elements other than silicon. The mixture may include not more than about 20 wt %, such as not more than about 15 wt %, or not more than about 10 wt %, or not more than about 5 wt %, or not more than about 3 wt %, or not more than about 1 wt % of glass network forming elements other than silicon. The mixture may include from about 0.01 wt % to about 10 wt %, such as from about 0.01 wt % to about 5 wt %, or from about 0.01 wt % to about 3 wt %, or from about 0.01 wt % to about 1 wt % of glass network forming elements other than silicon.
[0207] For example, the mixture may include not less than about 0.01 wt %, such as not less than about 0.1 wt %, or not less than about 1 wt % boron. The mixture may include not more than about 20 wt %, such as not more than about 15 wt %, or not more than about 10 wt %, or not more than about 5 wt %, or not more than about 3 wt %, or not more than about 1 wt % boron. The mixture may include from about 0.01 wt % to about 10 wt %, such as from about 0.01 wt % to about 5 wt %, or from about 0.01 wt % to about 3 wt %, or from about 0.01 wt % to about 1 wt % boron.
[0208] The mixture may include an amount of boron such that the cured mixture (ie, solid precursor or expandable material) and / or the expanded material includes less than about 5.0 wt %, such as less than about 3.5 wt %, B2O3.
[0209] The mixture may include not less than about 0.01 wt %, such as not less than about 0.1 wt %, or not less than about 1 wt % of the glass network intermediate element. The mixture may include not more than about 20 wt %, such as not more than about 15 wt %, or not more than about 10 wt %, or not more than about 5 wt %, or not more than about 3 wt %, or not more than about 1 wt % of the glass network intermediate element. The mixture may include from about 0.01 wt % to about 10 wt %, such as from about 0.01 wt % to about 5 wt %, or from about 0.01 wt % to about 3 wt %, or from about 0.01 wt % to about 1 wt % of the glass network intermediate element.
[0210] The mixture may include not less than about 0.01 wt %, such as not less than about 0.1 wt %, or not less than about 1 wt % of the glass network modifier. The mixture may include not more than about 20 wt %, such as not more than about 15 wt %, or not more than about 10 wt %, or not more than about 5 wt %, or not more than about 3 wt %, or not more than about 1 wt % of the glass network modifier. The mixture may include from about 0.01 wt % to about 10 wt %, such as from about 0.01 wt % to about 5 wt %, or from about 0.01 wt % to about 3 wt %, or from about 0.01 wt % to about 1 wt % of the glass network modifier.
[0211] The ratio of the total weight % of reactive silica in the mixture to the total weight % of silicate glass in the mixture, i.e.:
[0212]
[0213] The ratio of the total weight % of reactive silica in the mixture to the total weight % of silicate glass in the mixture may be not less than about 1, or not less than about 1.5, or not less than about 2, or not less than about 2.5, or not less than about 3. The ratio of the total weight % of reactive silica in the mixture to the total weight % of silicate glass in the mixture may be not greater than about 4, or not greater than about 3.5, or not greater than about 3. The ratio of the total weight % of reactive silica in the mixture to the total weight % of silicate glass in the mixture may be from about 1 to about 4, or from about 1.5 to about 3.5, or from about 2 to about 3. The ratio of the total weight % of reactive silica in the mixture to the total weight % of silicate glass in the mixture may be about 2. The ratio of the total weight % of reactive silica in the mixture to the total weight % of silicate glass in the mixture may be about 3.
[0214] It can be the ratio of the total weight % of silica fume in the mixture to the total weight % of borosilicate glass in the mixture, that is:
[0215]
[0216] The ratio of the total weight % of silica fume in the mixture to the total weight % of borosilicate glass in the mixture may be not less than about 1, or not less than about 1.5, or not less than about 2, or not less than about 2.5, or not less than about 3. The ratio of the total weight % of silica fume in the mixture to the total weight % of borosilicate glass in the mixture may be not greater than about 4, or not greater than about 3.5, or not greater than about 3. The ratio of the total weight % of silica fume in the mixture to the total weight % of borosilicate glass in the mixture may be from about 1 to about 4, or from about 1.5 to about 3.5, or from about 2 to about 3. The ratio of the total weight % of silica fume in the mixture to the total weight % of borosilicate glass in the mixture may be about 2. The ratio of the total weight % of silica fume in the mixture to the total weight % of borosilicate glass in the mixture may be about 3.
[0217] The ratio of the combined total weight % of reactive silica and silicate minerals in the mixture to the total weight % of silicate glass in the mixture, i.e.:
[0218]
[0219] The ratio of the total weight % of the reactive silica and silicate minerals in the mixture to the total weight % of the silicate glass in the mixture may be not greater than about 4, or not greater than about 3.5, or not greater than about 3. The ratio of the total weight % of the reactive silica and silicate minerals in the mixture to the total weight % of the silicate glass in the mixture may be from about 2 to about 4, or from about 2.5 to about 3.5. The ratio of the total weight % of the reactive silica and silicate minerals in the mixture to the total weight % of the silicate glass in the mixture may be about 3.
[0220] It can be the ratio of the combined total weight % of silica fume and perlite materials in the mixture to the total weight % of borosilicate glass in the mixture, that is:
[0221]
[0222] Not less than about 2, for example, not less than about 2.5, or not less than about 3. The ratio of the combined total weight % of silica fume and perlite materials in the mixture to the total weight % of borosilicate glass in the mixture may be not greater than about 4, or not greater than about 3.5, or not greater than about 3. The ratio of the combined total weight % of silica fume and perlite materials in the mixture to the total weight % of borosilicate glass in the mixture may be from about 2 to about 4, or from about 2.5 to about 3.5. The ratio of the combined total weight % of silica fume and perlite materials in the mixture to the total weight % of borosilicate glass in the mixture may be about 3.
[0223] The ratio of the total weight % of reactive silica in the mixture to the total weight % of silicate minerals in the mixture may be not less than about 0.1, or not less than about 0.2, or not less than about 0.3.
[0224] The ratio of the total weight % of silicon in the mixture to the total weight % of sodium in the mixture (i.e., the Si / Na ratio) is not less than about 1, or not less than about 1.2, or not less than about 1.4, or not less than about 1.5. The Si / Na ratio may be not greater than about 4, or not greater than about 3.5, or not greater than about 3, or not greater than about 2.9. The Si / Na ratio may be from about 1 to about 4, for example, from about 1.2 to about 3.5, or from about 1.4 to about 3, or from about 1.5 to about 2.9.
[0225] Expandable materials
[0226] The solidified mixture (i.e., solid precursor or expandable material) may contain not less than about 0.01 wt%, such as not less than about 0.1 wt%, or not less than about 0.2 wt%, or not less than about 0.3 wt%, or not less than about 0.4 wt%, or not less than about 1 wt%, or not less than about 1.5 wt%, or not less than about 2 wt%, or not less than about 3 wt% X2O, wherein X is an alkali metal such as Na or Li. The solidified mixture (i.e., solid precursor or expandable material) may contain not more than about 25 wt%, such as not more than about 20 wt%, or not more than about 15 wt%, or not more than about 10 wt%, or not more than about 5 wt%, or not more than about 3 wt%, or not more than about 2 wt%, or not more than about 1 wt%, or not more than about 0.6 wt% X2O, wherein X is an alkali metal such as Na or Li. The solidified mixture (i.e., solid precursor or expandable material) may contain from about 0.01 wt % to about 25 wt %, such as from about 0.01 wt % to about 20 wt %, or from about 0.01 wt % to about 15 wt %, or from about 0.01 wt % to about 10 wt %, or from about 0.1 wt % to about 20 wt %, or from about 0.1 wt % to about 15 wt %, or from about 0.1 wt % to about 10 wt %, or from about 1 wt % to about 20 wt %, or from about 1 wt % to about 15 wt %, or from about 1 wt % to about 10 wt %. % to about 10 wt %, or about 3 wt % to about 20 wt %, or about 3 wt % to about 15 wt %, or about 3 wt % to about 10 wt %, or about 0.1 wt % to about 5 wt %, or about 0.2 wt % to about 5 wt %, or about 0.2 wt % to about 1 wt %, or about 0.4 wt % to about 1 wt %, or about 0.4 wt % to about 0.6 wt %, or about 1 wt % to about 3 wt %, or about 1 wt % to about 2 wt % of X2O, wherein X is an alkali metal such as Na or Li.
[0227] For example, the solidified mixture (i.e., the solid precursor or the expandable material) may contain not less than about 0.01 wt %, such as not less than about 0.1 wt %, or not less than about 0.2 wt %, or not less than about 0.3 wt %, or not less than about 0.4 wt %, or not less than about 1 wt %, or not less than about 1.5 wt %, or not less than about 2 wt %, or not less than about 3 wt % of Na O. The solidified mixture (i.e., the solid precursor or the expandable material) may contain not more than about 25 wt %, such as not more than about 20 wt %, or not more than about 15 wt %, or not more than about 10 wt %, or not more than about 5 wt %, or not more than about 3 wt %, or not more than about 2 wt %, or not more than about 1 wt %, or not more than about 0.6 wt % of Na O. The solidified mixture (i.e., solid precursor or expandable material) may contain about 0.01 wt % to about 25 wt %, for example, about 0.01 wt % to about 20 wt %, or about 0.01 wt % to about 15 wt %, or about 0.01 wt % to about 10 wt %, or about 0.1 wt % to about 20 wt %, or about 0.1 wt % to about 15 wt %, or about 0.1 wt % to about 10 wt %, or about 1 wt % to about 20 wt %, or about 1 wt % to about 15 wt %, or about 1 wt % to about 10 wt %, or about 3 wt % to about 20 wt %, or about 3 wt % to about 15 wt %, or about 3 wt % to about 10 wt %, or about 0.1 wt % to about 5 wt %, or about 0.2 wt % to about 5 wt %, or about 0.2 wt % to about 1 wt %, or about 0.4 wt % to about 1 wt %, or about 0.4 wt % to about 0.6 wt %, or about 1 wt % to about 3 wt %, or about 1 wt % to about 2 wt % Na2O.
[0228] The solidified mixture (i.e., solid precursor or expandable material) may contain not less than about 0.01 wt %, such as not less than about 0.1 wt %, or not less than about 0.2 wt %, or not less than about 0.3 wt %, or not less than about 0.4 wt %, or not less than about 1 wt %, or not less than about 1.5 wt %, or not less than about 2 wt %, or not less than about 3 wt % Li O. The solidified mixture (i.e., solid precursor or expandable material) may contain not more than about 25 wt %, such as not more than about 20 wt %, or not more than about 15 wt %, or not more than about 10 wt %, or not more than about 5 wt %, or not more than about 3 wt %, or not more than about 2 wt %, or not more than about 1 wt %, or not more than about 0.6 wt % Li O. The solidified mixture (i.e., solid precursor or expandable material) may contain about 0.01 wt % to about 25 wt %, for example, about 0.01 wt % to about 20 wt %, or about 0.01 wt % to about 15 wt %, or about 0.01 wt % to about 10 wt %, or about 0.1 wt % to about 20 wt %, or about 0.1 wt % to about 15 wt %, or about 0.1 wt % to about 10 wt %, or about 1 wt % to about 20 wt %, or about 1 wt % to about 15 wt %, or about 1 wt % to about 10 wt %, or about 3 wt % to about 20 wt %, or about 3 wt % to about 15 wt %, or about 3 wt % to about 10 wt %, or about 0.1 wt % to about 5 wt %, or about 0.2 wt % to about 5 wt %, or about 0.2 wt % to about 1 wt %, or about 0.4 wt % to about 1 wt %, or about 0.4 wt % to about 0.6 wt %, or about 1 wt % to about 3 wt %, or about 1 wt % to about 2 wt % Li2O.
[0229] The solidified mixture (i.e., solid precursor or expandable material) may contain not less than about 0.1 wt%, such as not less than about 0.2 wt%, or not less than about 0.4 wt%, or not less than about 1 wt%, or not less than about 2 wt%, or not less than about 3 wt%, or not less than about 4 wt% Al2O3. The solidified mixture (i.e., solid precursor or expandable material) may contain not more than about 30 wt%, such as not more than about 25 wt%, or not more than about 20 wt%, or not more than about 15 wt%, or not more than about 10 wt%, or not more than about 8 wt%, or not more than about 6 wt%, or not more than about 5 wt%, or not more than about 4 wt%, or not more than about 1 wt%, or not more than about 0.8 wt% Al2O3. The solidified mixture (i.e., solid precursor or expandable material) may contain about 0.1 wt % to about 30 wt %, for example, about 0.1 wt % to about 25 wt %, or about 0.1 wt % to about 20 wt %, or about 0.1 wt % to about 15 wt %, or about 0.2 wt % to about 10 wt %, or about 0.4 wt % to about 1 wt %, or about 0.4 wt % to about 0.8 wt %, or about 1 wt % to about 5 wt %, or about 2 wt % to about 5 wt %, or about 2 wt % to about 4 wt %, or about 4 wt % to about 5 wt % Al2O3.
[0230] The solidified mixture (i.e., solid precursor or expandable material) may contain not less than about 30% by weight, such as not less than about 35% by weight, or not less than about 40% by weight, or not less than about 45% by weight of SiO2. The solidified mixture (i.e., solid precursor or expandable material) may contain not more than about 80% by weight, such as not more than about 70% by weight, or not more than about 60% by weight, or not more than about 55% by weight, or not more than about 50% by weight of SiO2. The solidified mixture (i.e., solid precursor or expandable material) may contain from about 30% by weight to about 80% by weight, such as from about 30% by weight to about 70% by weight, or from about 30% by weight to about 60% by weight, or from about 35% by weight to about 55% by weight, or from about 40% by weight to about 50% by weight of SiO2.
[0231] The solidified mixture (i.e., solid precursor or expandable material) may contain not less than about 0.001 wt%, such as not less than about 0.01 wt%, or not less than about 0.05 wt%, or not less than about 0.1 wt%, or not less than about 0.2 wt%, or not less than about 0.3 wt% Fe2O3. The solidified mixture (i.e., solid precursor or expandable material) may contain no more than about 1 wt%, or no more than about 0.5 wt%, or no more than about 0.4 wt%, or no more than about 0.1 wt% Fe2O3. The solidified mixture (i.e., solid precursor or expandable material) may contain from about 0.001 wt% to about 1 wt%, such as from about 0.01 wt% to about 0.5 wt%, or from about 0.05 wt% to about 0.5 wt%, or from about 0.05 wt% to about 0.1 wt%, or from about 0.3 wt% to about 0.5 wt%, or from about 0.3 wt% to about 0.4 wt% Fe2O3.
[0232] The solidified mixture (i.e., solid precursor or expandable material) may contain not less than about 0.01 wt %, such as not less than about 0.05 wt %, or not less than about 0.1 wt %, or not less than about 0.15 wt %, or not less than about 0.2 wt %, or not less than about 0.3 wt %, or not less than about 0.4 wt %, or not less than about 0.5 wt % CaO. The solidified mixture (i.e., solid precursor or expandable material) may contain no more than about 2 wt %, such as no more than about 1 wt %, or no more than about 0.8 wt %, or no more than about 0.6 wt %, or no more than about 0.5 wt %, or no more than about 0.2 wt % CaO. The solidified mixture (i.e., solid precursor or expandable material) may contain about 0.01 wt % to about 2 wt %, for example, about 0.05 wt % to about 1 wt %, or about 0.1 wt % to about 0.8 wt %, or about 0.15 wt % to about 0.2 wt %, or about 0.3 wt % to about 0.6 wt %, or about 0.3 wt % to about 0.5 wt %, or about 0.5 wt % to about 0.6 wt % CaO.
[0233] The solidified mixture (i.e., solid precursor or expandable material) may contain not less than about 0.001 wt%, such as not less than about 0.005 wt%, or not less than about 0.01 wt%, or not less than about 0.05 wt% MgO. The solidified mixture (i.e., solid precursor or expandable material) may contain no more than about 1 wt%, or no more than about 0.5 wt%, or no more than about 0.1 wt% MgO. The solidified mixture (i.e., solid precursor or expandable material) may contain from about 0.001 wt% to about 1 wt%, such as from about 0.005 wt% to about 0.5 wt%, or from about 0.01 wt% to about 0.1 wt%, or from about 0.05 wt% to about 0.1 wt% MgO.
[0234] The solidified mixture (i.e., solid precursor or expandable material) may contain not less than about 0.05 wt %, such as not less than about 0.1 wt %, or not less than about 0.15 wt %, or not less than about 0.2 wt %, or not less than about 0.5 wt %, or not less than about 1 wt %, or not less than about 1.2 wt % of K 2 O. The solidified mixture (i.e., solid precursor or expandable material) may contain not more than about 5 wt %, such as not more than about 3 wt %, or not more than about 2 wt %, or not more than about 1.6 wt %, or not more than about 1 wt %, or not more than about 0.5 wt % of K 2 O. The solidified mixture (i.e., solid precursor or expandable material) may contain about 0.05 wt % to about 5 wt %, for example, about 0.1 wt % to about 3 wt %, or about 0.15 wt % to about 2 wt %, or about 0.15 wt % to about 1 wt %, or about 0.15 wt % to about 0.5 wt %, or about 0.5 wt % to about 3 wt %, or about 0.5 wt % to about 2 wt %, or about 1 wt % to about 2 wt %, or about 1.2 wt % to about 1.6 wt % K2O.
[0235] The solidified mixture (i.e., solid precursor or expandable material) may contain not less than about 0.1 wt%, such as not less than about 0.5 wt%, or not less than about 1 wt%, or not less than about 1.5 wt% B2O3. The solidified mixture (i.e., solid precursor or expandable material) may contain not more than about 5 wt%, such as not more than about 3.5 wt%, or not more than about 3 wt%, or not more than about 2.5 wt% B2O3. The solidified mixture (i.e., solid precursor or expandable material) may contain from about 0.1 wt% to about 5 wt%, such as from about 0.5 wt% to about 3.5 wt%, or from about 1 wt% to about 2.5 wt% B2O3.
[0236] The solidified mixture (i.e., solid precursor or expandable material) may contain not less than about 10% by weight, such as not less than about 15% by weight, or not less than about 20% by weight, or not less than about 25% by weight of water and / or volatile matter (i.e., substances that contribute to "loss on ignition" (LOI)). The solidified mixture (i.e., solid precursor or expandable material) may contain no more than about 50% by weight, such as no more than about 40% by weight, or no more than about 30% by weight of water and / or volatile matter (i.e., substances that contribute to "loss on ignition" (LOI)). The solidified mixture (i.e., solid precursor or expandable material) may contain from about 10% by weight to about 50% by weight, such as from about 15% by weight to about 40% by weight, or from about 20% by weight to about 30% by weight, or from about 25% by weight to about 40% by weight, or from about 25% by weight to about 30% by weight of water and / or volatile matter (i.e., substances that cause "loss on ignition" (LOI)).
[0237] The solidified mixture (i.e., solid precursor or expandable material) may contain: about 0.1 wt.% to about 25 wt.%, for example, about 0.2 wt.% to about 5 wt.%, X2O, wherein X is an alkali metal such as Na or Li; about 0.1 wt.% to about 30 wt.%, for example, about 0.2 wt.% to about 20 wt.%, Al2O3; about 30 wt.% to about 80 wt.%, for example, about 40 wt.% to about 60 wt.%, SiO2; about 10 wt.% to about 40 wt.%, for example, about 15 wt.% to about 30 wt.%, H2O; and optionally not more than about 5 wt.%, for example not more than about 3.5 wt.%, B2O3.
[0238] The solidified mixture (i.e., solid precursor or expandable material) may include: about 0.1 wt % to about 25 wt %, for example, about 0.2 wt % to about 5 wt % X2O, wherein X is an alkali metal such as Na or Li; about 0.1 wt % to about 30 wt %, for example, about 0.2 wt % to about 10 wt % Al2O3; about 30 wt % to about 80 wt %, for example, about 40 wt % to about 60 wt % SiO2; about 0.01 wt % to about 2 wt %, for example, about 0.05 wt % to about 1 wt % SiO2; about 0.1 wt % to about 2 wt %, for example, about 0.2 wt % to about 5 wt % X2O, wherein X is an alkali metal such as Na or Li; about 0.1 wt % to about 30 wt %, for example, about 0.2 wt % to about 10 wt % Al2O3; about 30 wt % to about 80 wt %, for example, about 40 wt % to about 60 wt % SiO2; about 0.01 wt % to about 2 wt %, for example, about 0.05 wt % to about 1 wt % % Fe2O3; about 0.01 wt. % to about 1 wt. %, for example, about 0.05 wt. % to about 0.8 wt. % CaO; not more than about 1 wt. %, for example, not more than about 0.5 wt. % MgO; about 0.05 wt. % to about 3 wt. %, for example, about 0.1 wt. % to about 2 wt. % K2O; about 10 wt. % to about 40 wt. %, for example, about 15 wt. % to about 30 wt. % H2O; and optionally not more than about 5 wt. %, for example, not more than about 3.5 wt. % B2O3.
[0239] The solidified mixture (i.e., solid precursor or expandable material) may be amorphous (i.e., non-crystalline). The solidified mixture (i.e., solid precursor or expandable material) may comprise (e.g., be formed from) an inorganic polymer network, i.e., an inorganic polymer network incorporating water, e.g., in the form of hydroxyl groups. The solidified mixture (i.e., solid precursor or expandable body) may therefore be described as a synthetic perlite material, e.g., synthetic perlite.
[0240] method
[0241] The method may include dissolving the alkaline compound in water to form an alkaline aqueous solution. The dissolution of the alkaline compound in water may be an exothermic process. The method may include adding a silicate material to the alkaline aqueous solution and stirring. Adding the silicate material to the alkaline aqueous solution may include adding any other input material to the alkaline aqueous solution, including any silicate glass, silicate mineral and / or reactive silica. The method may include stirring the mixture, typically for 1 to 10 minutes, to form a paste. The heat generated when the alkaline compound dissolves may contribute to the dissolution of other input materials.
[0242] The method may include shaping the mixture prior to curing.
[0243] The mixture can be cured in an oven. The mixture can be cured at a temperature of no more than about 250°C, such as from about 20°C to about 200°C, or from about 20°C to about 150°C, or from about 20°C to about 120°C, or from about 50°C to about 120°C, or from about 50°C to about 110°C, or from about 70°C to about 100°C. The mixture can be cured for no less than about 1 hour, such as no less than about 2 hours, or no less than about 4 hours, or no less than about 6 hours, or no less than about 8 hours, or no less than about 10 hours, or no less than about 12 hours, or no less than about 24 hours. The mixture can be cured for no more than about 72 hours, such as no more than about 48 hours, or no more than about 24 hours. The mixture can be cured for about 1 hour to about 72 hours, such as from about 2 hours to about 48 hours, or from about 4 hours to about 24 hours, or from about 4 hours to about 12 hours, or from about 12 hours to about 72 hours, or from about 24 hours to about 72 hours.
[0244] During curing, the mixture may undergo polymerization to form an inorganic polymer network. The polymerization of the mixture may be similar to geopolymerisation. In geopolymerisation, aluminosilicate materials polymerise after base activation to form a rigid three-dimensional framework of SiO4 and AlO4 tetrahedra linked by shared oxygens. The form of the resulting framework (i.e. poly(sialate), poly(sialate-siloxy) or poly(sialate-disiloxy)) depends on the ratio of SiO2 to Al2O3 in the initial mixture. However, the inorganic polymer network formed during the curing of the mixture of the present invention is generally less rigid and more linear than geopolymers and incorporates large amounts of water.
[0245] The solid precursor may be comminuted after solidification to form a particulate material (i.e., a particulate expandable material). The method may include sieving the solid precursor (i.e., the particulate material) after comminuting. The method may include comminuting (and optionally sieving) the solid precursor to obtain a particle size (e.g., d 50 ) is not less than about 10 μm, such as not less than about 50 μm, or not less than about 100 μm, or not less than about 250 μm, or not less than about 500 μm, or not less than about 750 μm, or not less than about 1 mm. The method may include comminuting (and optionally sieving) the solid precursor to obtain an average particle size (e.g., d 50) is not greater than about 10 mm, such as not greater than about 8 mm, or not greater than about 6 mm, or not greater than about 4 mm, 2 mm, or not greater than about 1.5 mm, or not greater than about 1 mm. The method may include comminuting (and optionally sieving) the solid precursor to obtain a particle size (e.g., d ) of about 10 μm to about 10 mm, or about 10 μm to about 8 mm, or about 10 μm to about 6 mm, or about 10 μm to about 4 mm, or about 10 μm to about 2 mm. 50 ) of granular material (i.e., granular expandable material), or about 100μm to about 2mm, or about 500μm to about 1mm, or about 250μm to about 750μm, or about 500μm to about 1.5mm, or about 750μm to about 1.5mm.
[0246] The method may include more than one comminution and / or screening step. For example, the method may include: comminuting a solid precursor in a first comminution step to form a particulate material having a first particle size; determining the first particle size; and then comminuting the particulate material in a second comminution step to form a particulate material having a second particle size, the second particle size being lower than the first particle size.
[0247] The method may include heating the particulate material (i.e., particulate expandable material) to form an expanded particulate material. The method may include heating the particulate material (i.e., particulate expandable material) to a temperature of not more than about 1100°C, for example, not more than about 1000°C, or not more than about 900°C, or not more than about 700°C, or not more than about 600°C. The method may include heating the particulate material (i.e., particulate expandable material) to a temperature of not less than about 200°C, for example, not less than about 300°C, or not less than about 400°C. The method may include heating the particulate material (i.e., particulate expandable material) to a temperature of about 200°C to about 1100°C, for example, about 200°C to about 1000°C, or about 200°C to about 900°C, or about 300°C to about 700°C, or about 300°C to about 700°C, or about 400°C to about 600°C.
[0248] The method may comprise heating the particulate material (i.e., particulate expandable material) in a furnace, for example in a furnace selected from the group consisting of an infrared (IR) furnace, an electrically heated furnace, a natural gas or LPG expansion furnace, a muffle furnace (e.g., a laboratory muffle furnace), or a fluidized bed (FB) reactor. The furnace may be a horizontal furnace, a vertical furnace, or an inclined furnace. The method may comprise heating the particulate material (i.e., particulate expandable material) in a fluidized bed reactor.
[0249] The method may include comminuting (and optionally sieving) the solid precursor to obtain a particle size (e.g., d 50) is not less than about 500 μm, for example, not less than about 1 mm or not less than about 2 mm, and the particulate material (i.e., particulate expandable material) is heated in an infrared (IR) furnace to form an expanded particulate material. An example of an infrared (IR) furnace includes an Elstein HTS (125×125 mm) ceramic infrared panel radiator, which operates at 64 kW / m and has a maximum operating temperature of 860° C. The infrared (IR) furnace may include a steel vibration plate for vibrating the particulate material during heating. An exemplary mechanical vibration element can be obtained from Italvibras G. Silingardi SpA, for example, model M3 / 45-SO2, series: AA, CFKN 0.44 / 0.64, RPM 3000 / 3800.
[0250] The method may include comminuting (and optionally sieving) the solid precursor to obtain a particle size (e.g., d 50 ) a particulate material (i.e., a particulate expandable material) not larger than about 500 μm, and heating the particulate material (i.e., the particulate expandable material) in an electric furnace (e.g., a vertical electric furnace) to form an expanded particulate material.
[0251] nature
[0252] The expanded particulate material may have a particle size of not less than about 15 kg / m 3 , for example not less than about 20 kg / m 3 , or not less than about 30kg / m 3 , or not less than about 40kg / m 3 , or not less than about 50kg / m 3 , or not less than about 55kg / m 3 , or not less than about 60kg / m 3 , or not less than about 65kg / m 3 , or not less than about 70kg / m 3 The expanded particulate material may have a loose bulk density of not more than about 450 kg / m 3 , for example not more than about 400 kg / m 3 , or not more than about 350kg / m 3 , or not more than about 300kg / m 3 , or not more than about 250kg / m 3 , or not more than about 200kg / m 3 , or not more than about 150kg / m 3 , or not more than about 100kg / m 3 , or not more than about 80kg / m 3 , or not more than about 70kg / m3 , or not more than about 60kg / m 3 , or not more than about 50kg / m 3 , or not more than about 40kg / m 3 Loose bulk density.
[0253] The expanded particulate material may have a particle size of about 15 kg / m 3 About 450kg / m 3 , for example about 15kg / m 3 About 400kg / m 3 , or about 15kg / m 3 About 350kg / m 3 , or about 15kg / m 3 About 300kg / m 3 , or about 15kg / m 3 About 250kg / m 3 , or about 15kg / m 3 About 200kg / m 3 , or about 15kg / m 3 About 150kg / m 3 , or about 15kg / m 3 About 100kg / m 3 , or about 15kg / m 3 About 80kg / m 3 , or about 15kg / m 3 About 70kg / m 3 , or about 15kg / m 3 About 60kg / m 3 , or about 15kg / m 3 About 50kg / m 3 , or about 15kg / m 3 About 40kg / m 3 Loose bulk density.
[0254] The expanded particulate material may have a particle size of about 20 kg / m 3 About 450kg / m 3 , for example about 20kg / m 3 About 400kg / m 3 , or about 20kg / m 3 About 350kg / m 3 , or about 20kg / m 3 About 300kg / m 3 , or about 20kg / m 3 About 250kg / m 3 , or about 20kg / m3 About 200kg / m 3 , or about 20kg / m 3 About 150kg / m 3 , or about 20kg / m 3 About 100kg / m 3 , or about 20kg / m 3 About 80kg / m 3 , or about 20kg / m 3 About 70kg / m 3 , or about 20kg / m 3 About 60kg / m 3 , or about 20kg / m 3 About 50kg / m 3 , or about 20kg / m 3 About 40kg / m 3 Loose bulk density.
[0255] The expanded particulate material may have a particle size of about 30 kg / m 3 About 450kg / m 3 , for example about 30kg / m 3 About 400kg / m 3 , or about 30kg / m 3 About 350kg / m 3 , or about 30kg / m 3 About 300kg / m 3 , or about 30kg / m 3 About 250kg / m 3 , or about 30kg / m 3 About 200kg / m 3 , or about 30kg / m 3 About 150kg / m 3 , or about 30kg / m 3 About 100kg / m 3 , or about 30kg / m 3 About 80kg / m 3 , or about 30kg / m 3 About 70kg / m 3 , or about 30kg / m 3 About 60kg / m 3 , or about 30kg / m 3 About 50kg / m 3 , or about 30kg / m 3 About 40kg / m 3 Loose bulk density.
[0256] The expanded particulate material may have a particle size of about 40 kg / m 3 About 450kg / m 3 , for example about 40kg / m 3 About 400kg / m 3 , or about 40kg / m 3 About 350kg / m 3 , or about 40kg / m 3 About 300kg / m 3 , or about 40kg / m 3 About 250kg / m 3 , or about 40kg / m 3 About 200kg / m 3 , or about 40kg / m 3 About 150kg / m 3 , or about 40kg / m 3 About 100kg / m 3 , or about 40kg / m 3 About 80kg / m 3 , or about 40kg / m 3 About 70kg / m 3 , or about 40kg / m 3 About 60kg / m 3 , or about 40kg / m 3 About 50kg / m 3 , or about 40kg / m 3 About 40kg / m 3 Loose bulk density.
[0257] The expanded particulate material may have a particle size of about 50 kg / m 3 About 450kg / m 3 , for example about 50kg / m 3 About 400kg / m 3 , or about 50kg / m 3 About 350kg / m 3 , or about 50kg / m 3 About 300kg / m 3 , or about 50kg / m 3 About 250kg / m 3 , or about 50kg / m 3 About 200kg / m 3 , or about 50kg / m 3 About 150kg / m 3 , or about 50kg / m 3 About 100kg / m 3, or about 50kg / m 3 About 80kg / m 3 , or about 50kg / m 3 About 70kg / m 3 , or about 50kg / m 3 About 60kg / m 3 , or about 50kg / m 3 About 50kg / m 3 , or about 50kg / m 3 About 40kg / m 3 Loose bulk density.
[0258] The expanded particulate material may have a particle size of about 55 kg / m 3 About 450kg / m 3 , for example about 55kg / m 3 About 400kg / m 3 , or about 55kg / m 3 About 350kg / m 3 , or about 55kg / m 3 About 300kg / m 3 , or about 55kg / m 3 About 250kg / m 3 , or about 55kg / m 3 About 200kg / m 3 , or about 55kg / m 3 About 150kg / m 3 , or about 55kg / m 3 About 100kg / m 3 , or about 55kg / m 3 About 80kg / m 3 , or about 55kg / m 3 About 70kg / m 3 , or about 55kg / m 3 About 60kg / m 3 , or about 55kg / m 3 About 50kg / m 3 , or about 55kg / m 3 About 40kg / m 3 Loose bulk density.
[0259] The expanded particulate material may have a particle size of about 60 kg / m 3 About 450kg / m 3 , for example about 60kg / m 3 About 400kg / m 3 , or about 60kg / m3 About 350kg / m 3 , or about 60kg / m 3 About 300kg / m 3 , or about 60kg / m 3 About 250kg / m 3 , or about 60kg / m 3 About 200kg / m 3 , or about 60kg / m 3 About 150kg / m 3 , or about 60kg / m 3 About 100kg / m 3 , or about 60kg / m 3 About 80kg / m 3 , or about 60kg / m 3 About 70kg / m 3 , or about 60kg / m 3 About 60kg / m 3 , or about 60kg / m 3 About 50kg / m 3 , or about 60kg / m 3 About 40kg / m 3 Loose bulk density.
[0260] The expanded particulate material may have a particle size of about 65 kg / m 3 About 450kg / m 3 , for example about 65kg / m 3 About 400kg / m 3 , or about 65kg / m 3 About 350kg / m 3 , or about 65kg / m 3 About 300kg / m 3 , or about 65kg / m 3 About 250kg / m 3 , or about 65kg / m 3 About 200kg / m 3 , or about 65kg / m 3 About 150kg / m 3 , or about 65kg / m 3 About 100kg / m 3 , or about 65kg / m 3 About 80kg / m 3 , or about 65kg / m 3 About 70kg / m 3 , or about 65kg / m 3 About 60kg / m3 , or about 65kg / m 3 About 50kg / m 3 , or about 65kg / m 3 About 40kg / m 3 Loose bulk density.
[0261] The expanded particulate material may have a particle size of about 70 kg / m 3 About 450kg / m 3 , for example about 70kg / m 3 About 400kg / m 3 , or about 70kg / m 3 About 350kg / m 3 , or about 70kg / m 3 About 300kg / m 3 , or about 70kg / m 3 About 250kg / m 3 , or about 70kg / m 3 About 200kg / m 3 , or about 70kg / m 3 About 150kg / m 3 , or about 70kg / m 3 About 100kg / m 3 , or about 70kg / m 3 About 80kg / m 3 , or about 70kg / m 3 About 70kg / m 3 , or about 70kg / m 3 About 60kg / m 3 , or about 70kg / m 3 About 50kg / m 3 , or about 70kg / m 3 About 40kg / m 3 Loose bulk density.
[0262] The loose bulk density of a material can be measured by sampling the material with a sampler (750-1000 mL), pouring the sample into a weighed cylinder, taking care not to disturb the sample to cause sedimentation. The weight and volume of the sample are then recorded and the loose bulk density is calculated according to the following formula:
[0263] Loose bulk density [kg / m 3 ]=1000xweight[g] / volume[mL]
[0264] In addition to or as an alternative to any of the loose bulk densities described above, the expanded particulate material may have a resistance to compaction of not less than about 3 PSI at 2", e.g., not less than about 5 PSI at 2", or not less than about 10 PSI at 2", or not less than about 20 PSI at 2", or not less than about 30 PSI at 2", or not less than about 40 PSI at 2", as measured in accordance with PI 306-80. The expanded particulate material may have a resistance to compaction of not greater than about 350 PSI at 2", for example, not greater than about 300 PSI at 2", or not greater than about 250 PSI at 2", or not greater than about 200 PSI at 2", or not greater than about 100 PSI at 2", or not greater than about 90 PSI at 2", or not greater than about 80 PSI at 2", or not greater than about 75 PSI, or not greater than about 50 PSI, or not greater than about 40 PSI, or not greater than about 30 PSI, or not greater than about 20 PSI, or not greater than about 15 PSI, or not greater than about 10 PSI, as measured according to PI 306-80.
[0265] The expanded particulate material may have a resistance to compaction of about 3 PSI to about 350 PSI at 2", for example, about 3 PSI to about 300 PSI at 2", or about 3 PSI to about 250 PSI at 2", or about 3 PSI to about 200 PSI at 2", or about 3 PSI to about 100 PSI at 2", or about 3 PSI to about 90 PSI at 2", or about 3 PSI to about 80 PSI at 2", or about 3 PSI to about 75 PSI at 2", or about 3 PSI to about 50 PSI at 2", or about 3 PSI to about 40 PSI at 2", or about 3 PSI to about 30 PSI at 2", or about 3 PSI to about 20 PSI at 2", or about 3 PSI to about 15 PSI at 2", or about 3 PSI to about 10 PSI at 2", as measured according to PI 306-80.
[0266] The expanded particulate material may have a resistance to compaction of about 5 PSI to about 350 PSI at 2", for example, about 5 PSI to about 300 PSI at 2", or about 5 PSI to about 250 PSI at 2", or about 5 PSI to about 200 PSI at 2", or about 5 PSI to about 100 PSI at 2", or about 5 PSI to about 90 PSI at 2", or about 5 PSI to about 80 PSI at 2", or about 5 PSI to about 75 PSI at 2", or about 5 PSI to about 50 PSI at 2", or about 5 PSI to about 40 PSI at 2", or about 5 PSI to about 30 PSI at 2", or about 5 PSI to about 20 PSI at 2", or about 5 PSI to about 15 PSI at 2", or about 5 PSI to about 10 PSI at 2", as measured according to PI 306-80.
[0267] The expanded particulate material may have a resistance to compaction of about 10 PSI to about 350 PSI at 2", for example, about 10 PSI to about 300 PSI at 2", or about 10 PSI to about 250 PSI at 2", or about 10 PSI to about 200 PSI at 2", or about 10 PSI to about 100 PSI at 2", or about 10 PSI to about 90 PSI at 2", or about 10 PSI to about 80 PSI at 2", or about 10 PSI to about 75 PSI at 2", or about 10 PSI to about 50 PSI at 2", or about 10 PSI to about 40 PSI at 2", or about 10 PSI to about 30 PSI at 2", or about 10 PSI to about 20 PSI at 2", or about 10 PSI to about 15 PSI at 2", or about 10 PSI to about 10 PSI at 2", as measured according to PI 306-80.
[0268] The expanded particulate material may have a resistance to compaction of about 20 PSI to about 350 PSI at 2", for example, about 20 PSI to about 300 PSI at 2", or about 20 PSI to about 250 PSI at 2", or about 20 PSI to about 200 PSI at 2", or about 20 PSI to about 100 PSI at 2", or about 20 PSI to about 90 PSI at 2", or about 20 PSI to about 80 PSI at 2", or about 20 PSI to about 75 PSI at 2", or about 20 PSI to about 50 PSI at 2", or about 20 PSI to about 40 PSI at 2", or about 20 PSI to about 30 PSI at 2", or about 20 PSI to about 20 PSI at 2", or about 20 PSI to about 15 PSI at 2", or about 20 PSI to about 10 PSI at 2", as measured according to PI 306-80.
[0269] The expanded particulate material may have a resistance to compaction of about 30 PSI to about 350 PSI at 2", for example, about 30 PSI to about 300 PSI at 2", or about 30 PSI to about 250 PSI at 2", or about 30 PSI to about 200 PSI at 2", or about 30 PSI to about 100 PSI at 2", or about 30 PSI to about 90 PSI at 2", or about 30 PSI to about 80 PSI at 2", or about 30 PSI to about 75 PSI at 2", or about 30 PSI to about 50 PSI at 2", or about 30 PSI to about 40 PSI at 2", or about 30 PSI to about 30 PSI at 2", or about 30 PSI to about 30 PSI at 2", or about 30 PSI to about 20 PSI at 2", or about 30 PSI to about 15 PSI at 2", or about 30 PSI to about 10 PSI at 2", as measured according to PI 306-80.
[0270] The expanded particulate material may have a resistance to compaction of about 40 PSI to about 3500 PSI at 2", for example, about 40 PSI to about 300 PSI at 2", or about 40 PSI to about 250 PSI at 2", or about 40 PSI to about 200 PSI at 2", or about 40 PSI to about 100 PSI at 2", or about 40 PSI to about 90 PSI at 2", or about 40 PSI to about 80 PSI at 2", or about 40 PSI to about 75 PSI at 2", or about 40 PSI to about 50 PSI at 2", or about 40 PSI to about 40 PSI at 2", or about 40 PSI to about 40 PSI at 2", or about 40 PSI to about 30 PSI at 2", or about 40 PSI to about 20 PSI at 2", or about 40 PSI to about 15 PSI at 2", or about 40 PSI to about 10 PSI at 2", as measured according to PI 306-80.
[0271] Additionally or alternatively, the expanded granular material may have a compaction resistance of not less than about 0.5 PSI at 1", e.g., not less than about 1 PSI at 1", or not less than about 2 PSI at 1", or not less than about 2.5 PSI at 1", as measured according to PI 306-80. The expanded granular material may have a compaction resistance of not more than about 50 PSI at 1", e.g., not more than about 40 PSI at 1", or not more than about 30 PSI at 1", as measured according to PI 306-80. The expanded granular material may have a compaction resistance of from about 0.5 PSI to about 50 PSI at 1", e.g., from about 1 PSI to about 40 PSI at 1", or from about 2 PSI to about 40 PSI at 1", or from about 2.5 PSI to about 30 PSI at 1", as measured according to PI 306-80.
[0272] The compaction resistance of a material can be measured by taking a representative sample of about 500 mL of the material with a sampler. The sample is placed in the container of a computer-controlled hydraulic press. Shake the container 25 times to settle the sample. Then add another 250 mL of material to the container. The sample is settled again by shaking it 25 more times. Then the sample is placed flat on the top of the container. The sample is pressed at a speed of 20 mm / min and a maximum load of 6800 N (or 2800 N for very lightweight samples) under an automatic hydraulic press. The computer continuously records the load and displacement of the sample and plots the data into a graph. Once the maximum load is reached, the instrument calculates the total displacement and the zero deformation point. The load / displacement data is exported, and the corresponding load values (B) for 1 inch (i.e. 1") and 2 inches (i.e. 2") displacements (plus the zero deformation point, i.e. 1 inch deformation distance (mm) = 25.4 + zero deformation point (mm)) are used to calculate the compaction resistance according to the following formula:
[0273] Compaction resistance [PSI] = (B [N] / A [m2 ])*0.000145037738007
[0274] Where A is the cross-sectional area of the vessel.
[0275] In addition to or as an alternative to the above loose bulk density and / or compaction resistance, the expanded particulate material may have a thermal conductivity (i.e., λ, λ value) of not less than about 0.0300 W / mK, for example not less than about 0.0310 W / mK, or not less than about 0.0320 W / mK, or not less than about 0.0330 W / mK, or not less than about 0.0340 W / mK, or not less than about 0.0350 W / mK, or not less than about 0.0360 W / mK, measured according to EN 12667. 12667 measured at not more than about 0.0700 W / mK, for example, not more than about 0.0600 W / mK, or not more than about 0.0500 W / mK, or not more than about 0.0490 W / mK, or not more than about 0.0480 W / mK, or not more than about 0.0470 W / mK, or not more than about 0.0460 W / mK, or not more than about 0.0450 W / mK, or not more than about 0.0440 W / mK, or not more than about 0.0 .0430W / mK, or not greater than about 0.0420W / mK, or not greater than about 0.0410W / mK, or not greater than about 0.0400W / mK, or not greater than about 0.0390W / mK, or not greater than about 0.0380W / mK, or not greater than about 0.0370W / mK, or not greater than about 0.0360W / mK, or not greater than about 0.0350W / mK, or not greater than about 0.0340W / mK.
[0276] The expanded particulate material may have a thermal conductivity measured according to EN 12667 of, for example, about 0.0300 W / mK to about 0.0700 W / mK, or about 0.0300 W / mK to about 0.0600 W / mK, or about 0.0300 W / mK to about 0.0500 W / mK, about 0.0300 W / mK to about 0.0490 W / mK, or about 0.0300 W / mK to about 0.0480 W / mK, or about 0.0300 W / mK to about 0.0470 W / mK, or about 0.0300 W / mK to about 0.0460 W / mK, or about 0.0300 W / mK to about 0.0450 W / mK, or about 0.0300 W / mK to about 0.0440 W / mK, or about 0.0300 W / mK to about 0.0430 W / mK, or about 0.0300 W / mK to about 0.0440 W / mK, or about 0.0300 W / mK to about 0.0450 W / mK, About 0.0420 W / mK, or about 0.0300 W / mK to about 0.0410 W / mK, or about 0.0300 W / mK to about 0.0400 W / mK, or about 0.0300 W / mK to about 0.0390 W / mK, or 0.0300 W / mK to about 0.0380 W / mK, or about 0.0300 W / mK to about 0.0370 W / mK , or thermal conductivity (i.e., λ, λ value) of 0.0300 W / mK to about 0.0380 W / mK, or about 0.0300 W / mK to about 0.0360 W / mK, or about 0.0300 W / mK to about 0.0380 W / mK, or about 0.0300 W / mK to about 0.0380 W / mK, or about 0.0300 W / mK to about 0.0380 W / mK, or about 0.0300 W / mK to about 0.0340 W / mK.
[0277] The expanded particulate material may have a relative humidity of about 0.0310 W / mK to about 0.0500 W / mK, for example about 0.0310 W / mK to about 0.0490 W / mK, or about 0.0310 W / mK to about 0.0480 W / mK, or about 0.0310 W / mK to about 0.0470 W / mK, or about 0.0310 W / mK to about 0.0460 W / mK, measured according to EN 12667. / mK, or about 0.0310W / mK to about 0.0450W / mK, or about 0.0310W / mK to about 0.0440W / mK, or about 0.0310W / mK to about 0.0430W / mK, or about 0.0310W / mK to about 0.0420W / mK, or about 0.0310W / mK to about 0.0410W / mK, or about 0.0310 W / mK to about 0.0400 W / mK, or about 0.0310 W / mK to about 0.0390 W / mK, or about 0.0310 W / mK to about 0.0380 W / mK, or about 0.0310 W / mK to about 0.0370 W / mK, or 0.0310 W / mK to about 0.0380 W / mK, or about 0.0 The thermal conductivity (i.e., λ, λ value) of about 0.0310 W / mK to about 0.0360 W / mK, or about 0.0310 W / mK to about 0.0380 W / mK, or about 0.0310 W / mK to about 0.0350 W / mK, or 0.0310 W / mK to about 0.0380 W / mK, or about 0.0310 W / mK to about 0.0340 W / mK.
[0278] The expanded particulate material may have a relative humidity of about 0.0320 W / mK to about 0.0500 W / mK, for example about 0.0320 W / mK to about 0.0490 W / mK, or about 0.0320 W / mK to about 0.0480 W / mK, or about 0.0320 W / mK to about 0.0470 W / mK, or about 0.0320 W / mK to about 0.0460 W / mK, measured according to EN 12667. / mK, or about 0.0320W / mK to about 0.0450W / mK, or about 0.0320W / mK to about 0.0440W / mK, or about 0.0320W / mK to about 0.0430W / mK, or about 0.0320W / mK to about 0.0420W / mK, or about 0.0320W / mK to about 0.0410W / mK, or about 0.0320 W / mK to about 0.0400 W / mK, or about 0.0320 W / mK to about 0.0390 W / mK, or about 0.0320 W / mK to about 0.0380 W / mK, or about 0.0320 W / mK to about 0.0370 W / mK, or 0.0320 W / mK to about 0.0380 W / mK, or about 0.0 The thermal conductivity (i.e., λ, λ value) is about 0.0320 W / mK to about 0.0360 W / mK, or about 0.0320 W / mK to about 0.0380 W / mK, or about 0.0320 W / mK to about 0.0350 W / mK, or 0.0320 W / mK to about 0.0380 W / mK, or about 0.0320 W / mK to about 0.0340 W / mK.
[0279] The expanded particulate material may have a relative humidity of about 0.0330 W / mK to about 0.0500 W / mK, for example about 0.0330 W / mK to about 0.0490 W / mK, or about 0.0330 W / mK to about 0.0480 W / mK, or about 0.0330 W / mK to about 0.0470 W / mK, or about 0.0330 W / mK to about 0.0460 W / mK, measured according to EN 12667. / mK, or about 0.0330W / mK to about 0.0450W / mK, or about 0.0330W / mK to about 0.0440W / mK, or about 0.0330W / mK to about 0.0430W / mK, or about 0.0330W / mK to about 0.0420W / mK, or about 0.0330W / mK to about 0.0410W / mK, or about 0.0330 W / mK to about 0.0400 W / mK, or about 0.0330 W / mK to about 0.0390 W / mK, or about 0.0320 W / mK to about 0.0380 W / mK, or about 0.0330 W / mK to about 0.0370 W / mK, or 0.0330 W / mK to about 0.0380 W / mK, or about 0.0 The thermal conductivity (i.e., λ, λ value) is from about 0.0330 W / mK to about 0.0360 W / mK, or from about 0.0330 W / mK to about 0.0380 W / mK, or from about 0.0330 W / mK to about 0.0350 W / mK, or from 0.0330 W / mK to about 0.0380 W / mK, or from about 0.0330 W / mK to about 0.0340 W / mK.
[0280] The expanded particulate material may have a relative humidity of about 0.0340 W / mK to about 0.0500 W / mK, for example about 0.0340 W / mK to about 0.0490 W / mK, or about 0.0340 W / mK to about 0.0480 W / mK, or about 0.0340 W / mK to about 0.0470 W / mK, or about 0.0340 W / mK to about 0.0460 W / mK, measured according to EN 12667. K, or from about 0.0340 W / mK to about 0.0450 W / mK, or from about 0.0340 W / mK to about 0.0440 W / mK, or from about 0.0340 W / mK to about 0.0430 W / mK, or from about 0.0340 W / mK to about 0.0420 W / mK, or from about 0.0340 W / mK to about 0.0410 W / mK, or from about 0.0340 W / mK to about 0.0400 W / mK, or from about 0.0340 W / mK to about 0.0390 W / mK, or from about 0.0320 W / mK to about 0.0380 W / mK, or from about 0.0340 W / mK to about 0.0370 W / mK, or from 0.0340 W / mK to about 0.0380 W / mK, or from about ...90 W / mK, or from about 0.0320 W / mK to about 0.0380 W / mK, or from about 0.0340 W / mK to about 0.0370 W / mK, or from about The thermal conductivity (i.e., λ, λ value) of about 0.0340 W / mK to about 0.0360 W / mK, or 0.0340 W / mK to about 0.0380 W / mK, or about 0.0340 W / mK to about 0.0350 W / mK, or 0.0340 W / mK to about 0.0380 W / mK, or about 0.0340 W / mK to about 0.0340 W / mK.
[0281] The expanded particulate material may have a relative humidity of about 0.0350 W / mK to about 0.0500 W / mK, for example about 0.0350 W / mK to about 0.0490 W / mK, or about 0.0350 W / mK to about 0.0480 W / mK, or about 0.0350 W / mK to about 0.0470 W / mK, or about 0.0350 W / mK to about 0.0460 W / mK, measured according to EN 12667. K, or from about 0.0350 W / mK to about 0.0450 W / mK, or from about 0.0350 W / mK to about 0.0440 W / mK, or from about 0.0350 W / mK to about 0.0430 W / mK, or from about 0.0350 W / mK to about 0.0420 W / mK, or from about 0.0350 W / mK to about 0.0410 W / mK, or from about 0.0350 W / mK to about 0.0400 W / mK, or from about 0.0350 W / mK to about 0.0390 W / mK, or from about 0.0320 W / mK to about 0.0380 W / mK, or from about 0.0350 W / mK to about 0.0370 W / mK, or from 0.0350 W / mK to about 0.038 ... about 0 The thermal conductivity (i.e., λ, λ value) of about 0.0350 W / mK to about 0.0360 W / mK, or 0.0350 W / mK to about 0.0380 W / mK, or about 0.0350 W / mK to about 0.0350 W / mK, or 0.0350 W / mK to about 0.0380 W / mK, or about 0.0350 W / mK to about 0.0340 W / mK.
[0282] The expanded particulate material may have a relative humidity of about 0.0360 W / mK to about 0.0500 W / mK, for example about 0.0360 W / mK to about 0.0490 W / mK, or about 0.0360 W / mK to about 0.0480 W / mK, or about 0.0360 W / mK to about 0.0470 W / mK, or about 0.0360 W / mK to about 0.0460 W / mK, measured according to EN 12667. / mK, or about 0.0360W / mK to about 0.0450W / mK, or about 0.0360W / mK to about 0.0440W / mK, or about 0.0360W / mK to about 0.0430W / mK, or about 0.0360W / mK to about 0.0420W / mK, or about 0.0360W / mK to about 0.0410W / mK, or about 0.0360 W / mK to about 0.0400 W / mK, or about 0.0360 W / mK to about 0.0390 W / mK, or about 0.0320 W / mK to about 0.0380 W / mK, or about 0.0360 W / mK to about 0.0370 W / mK, or about 0.0360 W / mK to about 0.0380 W / mK, or about 0.0. The thermal conductivity (i.e., λ, λ value) of about 0.0360 W / mK to about 0.0360 W / mK, or 0.0360 W / mK to about 0.0380 W / mK, or about 0.0360 W / mK to about 0.0350 W / mK, or 0.0360 W / mK to about 0.0380 W / mK, or about 0.0360 W / mK to about 0.0340 W / mK.
[0283] The expanded particulate material may have a thermal conductivity (ie, lambda, λ value) measured according to EN 12667 of about 0.042 W / mK to about 0.055 W / mK, or about 0.055 W / mK to about 0.070 W / mK.
[0284] For example, the expanded particulate material may have a particle size of about 15 kg / m 3 About 450kg / m 3 , for example about 20kg / m 3 About 100kg / m 3 , or about 20kg / m 3 About 30kg / m 3 , or about 20kg / m 3 About 40kg / m 3 , or about 55kg / m 3 About 100kg / m 3 , or about 70kg / m 3 About 100kg / m 3A loose bulk density of about 3 PSI to about 100 PSI at 2" as measured according to PI306-80, for example, about 3 PSI to about 10 PSI at 2", or about 30 PSI to about 80 PSI at 2", or about 40 PSI to about 75 PSI at 2", or about 5 PSI to about 20 PSI at 2"; and / or a compaction resistance of about 30 PSI to about 100 PSI at 2" as measured according to PI306-80, for example, about 30 PSI to about 80 PSI at 2", or about 40 PSI to about 75 PSI at 2", or about 5 PSI to about 20 PSI at 2"; and / or a compaction resistance of about 30 PSI to about 100 PSI at 2" as measured according to EN The thermal conductivity measured by 12667 is about 0.0300 W / mK to about 0.0700 W / mK, for example, about 0.0320 W / mK to about 0.0420 W / mK, about 0.0350 W / mK to about 0.0400 W / mK, or about 0.0360 W / mK to about 0.0410 W / mK, or about 0.0320 W / mK to about 0.0340 W / mK, or about 0.042 W / mK to about 0.055 W / mK, or about 0.055 W / mK to about 0.070 W / mK.
[0285] The thermal conductivity of the material can be measured using a Netzsch HFM436 / 3 lambda heat flow meter. The material samples were kept under standard laboratory conditions before the measurements were made. The loose-filled samples were placed in a custom frame consisting of a 30×30×2.5 cm XPS sheet with internal dimensions of 15×15 cm, with a thin plastic film on the bottom to hold the loose-filled sample in place. The average temperature and the temperature difference between the cold and hot plates were both set to 10°C.
[0286] The expanded particulate material may have:
[0287] (a) Approximately 18 kg / m2 measured according to PI 200-77 3 About 30kg / m 3 The loose bulk density;
[0288] (b) a compaction resistance of about 4 PSI to about 8 PSI at 2" as measured in accordance with PI 306-80; and / or
[0289] (c) Thermal conductivity of about 0.0300 W / mK to about 0.0400 W / mK measured according to EN 12667.
[0290] The expanded particulate material may have:
[0291] (a) Approximately 50 kg / m2 measured according to PI 200-77 3 About 100kg / m 3 The loose bulk density;
[0292] (b) a compaction resistance of from about 30 PSI to about 80 PSI at 2" as measured in accordance with PI 306-80; and / or
[0293] (c) Thermal conductivity of about 0.0350 W / mK to about 0.0450 W / mK measured according to EN 12667.
[0294] The expanded particulate material may have:
[0295] (a) Approximately 70 kg / m2 measured according to PI 200-77 3 About 105kg / m 3 The loose bulk density;
[0296] (b) a compaction resistance of about 40 PSI to about 75 PSI at 2" as measured in accordance with PI 306-80; and / or
[0297] (c) Thermal conductivity of about 0.0350 W / mK to about 0.0450 W / mK measured according to EN 12667.
[0298] The expanded particulate material may have:
[0299] (a) Approximately 20 kg / m2 measured according to PI 200-77 3 About 40kg / m 3 The loose bulk density;
[0300] (b) a compaction resistance of about 5 PSI to about 15 PSI at 2" as measured in accordance with PI 306-80; and / or
[0301] (c) Thermal conductivity of about 0.0310 W / mK to about 0.0350 W / mK measured according to EN 12667.
[0302] The expanded particulate material may be formed from a mixture comprising:
[0303] one or more silicate materials and / or reactive silica comprising: about 44 wt % to about 54 wt % SiO2; about 0.1 wt % to about 1 wt % Na2O; about 0.1 wt % to about 1 wt % Al2O3; less than about 0.2 wt % Fe2O3; about 0.05 wt % to about 0.5 wt % CaO; less than about 0.1 wt % MgO; about 0.05 wt % to about 0.5 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.1 to about 1 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0304] basic compounds; and
[0305] water;
[0306] And the expanded granular material has:
[0307] (a) Approximately 18 kg / m2 measured according to PI 200-77 3 About 30kg / m 3 The loose bulk density;
[0308] (b) a compaction resistance of about 4 PSI to about 8 PSI at 2" as measured in accordance with PI 306-80; and / or
[0309] (c) Thermal conductivity of about 0.0300 W / mK to about 0.0400 W / mK measured according to EN 12667.
[0310] The expanded particulate material may be formed from a mixture comprising:
[0311] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 3 wt % to about 6 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0312] basic compounds; and
[0313] water;
[0314] And the expanded granular material has:
[0315] (a) Approximately 50 kg / m2 measured according to PI 200-77 3 About 100kg / m 3 The loose bulk density;
[0316] (b) a compaction resistance of from about 30 PSI to about 80 PSI at 2" as measured in accordance with PI 306-80; and / or
[0317] (c) Thermal conductivity of about 0.0350 W / mK to about 0.0450 W / mK measured according to EN 12667.
[0318] The expanded particulate material may be formed from a mixture comprising:
[0319] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 3 wt % to about 6 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0320] basic compounds; and
[0321] water;
[0322] And the expanded granular material has:
[0323] (a) Approximately 70 kg / m2 measured according to PI 200-77 3 About 105kg / m 3 The loose bulk density;
[0324] (b) a compaction resistance of about 40 PSI to about 75 PSI at 2" as measured in accordance with PI 306-80; and / or
[0325] (c) Thermal conductivity of about 0.0350 W / mK to about 0.0450 W / mK measured according to EN 12667.
[0326] The expanded particulate material may be formed from a mixture comprising:
[0327] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 2.5 wt % to about 4.5 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0328] basic compounds; and
[0329] water;
[0330] And the expanded granular material has:
[0331] (a) Approximately 20 kg / m2 measured according to PI 200-77 3About 40kg / m 3 The loose bulk density;
[0332] (b) a compaction resistance of about 5 PSI to about 15 PSI at 2" as measured in accordance with PI 306-80; and / or
[0333] (c) Thermal conductivity of about 0.0310 W / mK to about 0.0350 W / mK measured according to EN 12667.
[0334] The expanded particulate material may be formed from a mixture comprising: about 10 wt % to about 15 wt % borosilicate glass; about 35 wt % to about 45 wt % silica fume; about 15 wt % to about 20 wt % sodium hydroxide; and about 25 wt % to about 32 wt % water; and the expanded particulate material has:
[0335] (a) Approximately 18 kg / m2 measured according to PI 200-77 3 About 30kg / m 3 The loose bulk density;
[0336] (b) a compaction resistance of about 4 PSI to about 8 PSI at 2" as measured in accordance with PI 306-80; and / or
[0337] (c) Thermal conductivity of about 0.0300 W / mK to about 0.0400 W / mK measured according to EN 12667.
[0338] The expanded particulate material may be formed from a mixture comprising: about 12 wt % to about 18 wt % borosilicate glass; about 5 wt % to about 15 wt % silica fume; about 10 wt % to about 15 wt % sodium hydroxide; and about 20 wt % to about 30 wt % water; and the expanded particulate material has:
[0339] (a) Approximately 50 kg / m2 measured according to PI 200-77 3 About 100kg / m 3 The loose bulk density;
[0340] (b) a compaction resistance of from about 30 PSI to about 80 PSI at 2" as measured in accordance with PI 306-80; and / or
[0341] (c) Thermal conductivity of about 0.0350 W / mK to about 0.0450 W / mK measured according to EN 12667.
[0342] The expanded particulate material may be formed from a mixture comprising: about 12 wt % to about 18 wt % borosilicate glass; about 5 wt % to about 10 wt % silica fume; about 8 wt % to about 16 wt % sodium hydroxide; and about 20 wt % to about 32 wt % water; and the expanded particulate material has:
[0343] (a) Approximately 70 kg / m2 measured according to PI 200-77 3 About 105kg / m 3 The loose bulk density;
[0344] (b) a compaction resistance of about 40 PSI to about 75 PSI at 2" as measured in accordance with PI 306-80; and / or
[0345] (c) Thermal conductivity of about 0.0350 W / mK to about 0.0450 W / mK measured according to EN 12667.
[0346] The expanded particulate material may be formed from a mixture comprising: about 10 wt % to about 20 wt % borosilicate glass; about 10 wt % to about 20 wt % silica fume; about 10 wt % to about 20 wt % sodium hydroxide; and about 20 wt % to about 30 wt % water; and the expanded particulate material has:
[0347] (a) Approximately 20 kg / m2 measured according to PI 200-77 3 About 40kg / m 3 The loose bulk density;
[0348] (b) a compaction resistance of about 5 PSI to about 15 PSI at 2" as measured in accordance with PI 306-80; and / or
[0349] (c) Thermal conductivity of about 0.0310 W / mK to about 0.0350 W / mK measured according to EN 12667.
[0350] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of about 0.125 mm to about 1 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0351] one or more silicate materials and / or reactive silica comprising: about 44 wt % to about 54 wt % SiO2; about 0.1 wt % to about 1 wt % Na2O; about 0.1 wt % to about 1 wt % Al2O3; less than about 0.2 wt % Fe2O3; about 0.05 wt % to about 0.5 wt % CaO; less than about 0.1 wt % MgO; about 0.05 wt % to about 0.5 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.1 to about 1 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0352] basic compounds; and
[0353] water;
[0354] The expanded granular material has:
[0355] (a) Approximately 18 kg / m2 measured according to PI 200-77 3 About 30kg / m 3 The loose bulk density;
[0356] (b) a compaction resistance of about 4 PSI to about 8 PSI at 2" as measured in accordance with PI 306-80; and / or
[0357] (c) Thermal conductivity of about 0.0300 W / mK to about 0.0400 W / mK measured according to EN 12667.
[0358] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of less than or equal to about 2 mm (as determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0359] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 3 wt % to about 6 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0360] basic compounds; and
[0361] water;
[0362] The expanded granular material has:
[0363] (a) Approximately 50 kg / m2 measured according to PI 200-77 3 About 100kg / m 3 The loose bulk density;
[0364] (b) a compaction resistance of from about 30 PSI to about 80 PSI at 2" as measured in accordance with PI 306-80; and / or
[0365] (c) Thermal conductivity of about 0.0350 W / mK to about 0.0450 W / mK measured according to EN 12667.
[0366] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of about 0.1 mm to about 1 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0367] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 3 wt % to about 6 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0368] basic compounds; and
[0369] water;
[0370] The expanded particulate material has:
[0371] (a) Approximately 70 kg / m2 measured according to PI 200-77 3 About 105kg / m 3 The loose bulk density;
[0372] (b) a compaction resistance of about 40 PSI to about 75 PSI at 2" as measured in accordance with PI 306-80; and / or
[0373] (c) Thermal conductivity of about 0.0350 W / mK to about 0.0450 W / mK measured according to EN 12667.
[0374] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of less than about 1 mm (as determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0375] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 2.5 wt % to about 4.5 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0376] basic salts; and
[0377] water;
[0378] The expanded particulate material has:
[0379] (a) Approximately 20 kg / m2 measured according to PI 200-77 3 About 40kg / m 3 The loose bulk density;
[0380] (b) a compaction resistance of about 5 PSI to about 15 PSI at 2" as measured in accordance with PI 306-80; and / or
[0381] (c) Thermal conductivity of about 0.0310 W / mK to about 0.0350 W / mK measured according to EN 12667.
[0382] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of about 0.5 mm to about 1 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0383] one or more silicate materials and / or reactive silica comprising: about 44 wt % to about 54 wt % SiO2; about 0.1 wt % to about 1 wt % Na2O; about 0.1 wt % to about 1 wt % Al2O3; less than about 0.2 wt % Fe2O3; about 0.05 wt % to about 0.5 wt % CaO; less than about 0.1 wt % MgO; about 0.05 wt % to about 0.5 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.1 to about 1 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0384] basic compounds; and
[0385] water;
[0386] The expanded particulate material has:
[0387] (a) Approximately 18 kg / m2 measured according to PI 200-77 3 About 25kg / m 3 The loose bulk density;
[0388] (b) a compaction resistance of about 4 PSI to about 8 PSI at 2" as measured in accordance with PI 306-80; and / or
[0389] (c) Thermal conductivity of about 0.0320 W / mK to about 0.0360 W / mK measured according to EN 12667.
[0390] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of about 0.125 mm to about 0.5 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0391] one or more silicate materials and / or reactive silica comprising: about 44 wt % to about 54 wt % SiO2; about 0.1 wt % to about 1 wt % Na2O; about 0.1 wt % to about 1 wt % Al2O3; less than about 0.2 wt % Fe2O3; about 0.05 wt % to about 0.5 wt % CaO; less than about 0.1 wt % MgO; about 0.05 wt % to about 0.5 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.1 to about 1 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0392] basic compounds; and
[0393] water;
[0394] The expanded particulate material has:
[0395] (a) Approximately 25 kg / m2 measured according to PI 200-77 3 About 30kg / m 3 The loose bulk density;
[0396] (b) a compaction resistance of about 4 PSI to about 8 PSI at 2" as measured in accordance with PI 306-80; and / or
[0397] (c) Thermal conductivity of about 0.0310 W / mK to about 0.0350 W / mK measured according to EN 12667.
[0398] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of about 0.3 mm to about 2 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0399] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 3 wt % to about 6 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0400] basic compounds; and
[0401] water;
[0402] The expanded particulate material has:
[0403] (a) Approximately 55 kg / m2 measured according to PI 200-77 3 About 65kg / m 3 The loose bulk density;
[0404] (b) a compaction resistance of about 35 PSI to about 40 PSI at 2" as measured in accordance with PI 306-80; and / or
[0405] (c) Thermal conductivity of about 0.0360 W / mK to about 0.0400 W / mK measured according to EN 12667.
[0406] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of less than about 0.3 mm (as determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0407] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 3 wt % to about 6 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0408] basic compounds; and
[0409] water;
[0410] The expanded particulate material has:
[0411] (a) Approximately 90 kg / m2 measured according to PI 200-77 3 About 100kg / m 3 The loose bulk density;
[0412] (b) a compaction resistance of from about 70 PSI to about 80 PSI at 2" as measured in accordance with PI 306-80; and / or
[0413] (c) Thermal conductivity of about 0.0370 W / mK to about 0.0420 W / mK measured according to EN 12667.
[0414] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of about 0.5 mm to about 1 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0415] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 3 wt % to about 6 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0416] basic compounds; and
[0417] water;
[0418] The expanded granular material has:
[0419] (a) Approximately 75 kg / m2 measured according to PI 200-77 3 About 85kg / m 3 The loose bulk density;
[0420] (b) a compaction resistance of from about 40 PSI to about 50 PSI at 2" as measured in accordance with PI 306-80; and / or
[0421] (c) Thermal conductivity of about 0.0370 W / mK to about 0.0410 W / mK measured according to EN 12667.
[0422] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of about 0.125 mm to about 0.5 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0423] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 3 wt % to about 6 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0424] basic compounds; and
[0425] water;
[0426] The expanded granular material has:
[0427] (a) Approximately 78 kg / m2 measured according to PI 200-77 3 About 86kg / m 3 The loose bulk density;
[0428] (b) a compaction resistance of from about 60 PSI to about 74 PSI at 2" as measured in accordance with PI 306-80; and / or
[0429] (c) Thermal conductivity of about 0.0360 W / mK to about 0.0420 W / mK measured according to EN 12667.
[0430] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of about 0.1 mm to about 1 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0431] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 3 wt % to about 6 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0432] basic compounds; and
[0433] water;
[0434] The expanded granular material has:
[0435] (a) Approximately 70 kg / m2 measured according to PI 200-77 3 About 105kg / m 3 The loose bulk density;
[0436] (b) a compaction resistance of from about 60 PSI to about 75 PSI at 2" as measured in accordance with PI 306-80; and / or
[0437] (c) Thermal conductivity of about 0.0360 W / mK to about 0.0430 W / mK measured according to EN 12667.
[0438] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of about 0.5 mm to about 1 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0439] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 2.5 wt % to about 4.5 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0440] basic compounds; and
[0441] water;
[0442] The expanded particulate material has:
[0443] (a) Approximately 20 kg / m2 measured according to PI 200-77 3 About 30kg / m 3 The loose bulk density;
[0444] (b) a compaction resistance of about 5 PSI to about 10 PSI at 2" as measured in accordance with PI 306-80; and / or
[0445] (c) Thermal conductivity of about 0.0310 W / mK to about 0.0360 W / mK measured according to EN 12667.
[0446] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of about 0.125 mm to about 0.5 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0447] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 2.5 wt % to about 4.5 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0448] basic compounds; and
[0449] water;
[0450] The expanded granular material has:
[0451] (a) Approximately 25 kg / m2 measured according to PI 200-77 3 About 35kg / m 3 The loose bulk density;
[0452] (b) a compaction resistance of about 5 PSI to about 15 PSI at 2" as measured in accordance with PI 306-80; and / or
[0453] (c) Thermal conductivity of about 0.0310 W / mK to about 0.0350 W / mK measured according to EN 12667.
[0454] The expanded particulate material may be formed by heating an expandable particulate material having a particle size of less than about 0.3 mm (as determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising:
[0455] one or more silicate materials and / or reactive silica comprising: about 42 wt % to about 52 wt % SiO2; about 1.2 wt % to about 2.4 wt % Na2O; about 2.5 wt % to about 4.5 wt % Al2O3; about 0.1 wt % to about 1 wt % Fe2O3; about 0.1 wt % to about 1 wt % CaO; less than about 0.2 wt % MgO; about 1 wt % to about 2 wt % K2O; about 1 wt % to about 3 wt % B2O3; and about 0.5 to about 1.5 wt % water and / or volatile matter (i.e., matter that contributes to "loss on ignition" (LOI));
[0456] Alkali salts; and
[0457] water;
[0458] The expanded particulate material has:
[0459] (a) Approximately 30 kg / m2 measured according to PI 200-77 3 About 40kg / m 3 The loose bulk density;
[0460] (b) a compaction resistance of about 8 PSI to about 16 PSI at 2" as measured in accordance with PI 306-80; and / or
[0461] (c) Thermal conductivity of about 0.0300 W / mK to about 0.0350 W / mK measured according to EN 12667.
[0462] The expanded particulate material can be formed by heating an expandable particulate material having a particle size of about 0.5 mm to about 1 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising: about 10 wt % to about 15 wt % borosilicate glass; about 35 wt % to about 45 wt % silica fume; about 15 wt % to about 20 wt % sodium hydroxide; and about 25 wt % to about 32 wt % water; and wherein the expanded particulate material has:
[0463] (a) Approximately 18 kg / m2 measured according to PI 200-77 3 About 25kg / m 3 The loose bulk density;
[0464] (b) a compaction resistance of about 4 PSI to about 8 PSI at 2" as measured in accordance with PI 306-80; and / or
[0465] (c) Thermal conductivity of about 0.0320 W / mK to about 0.0360 W / mK measured according to EN 12667.
[0466] The expanded particulate material can be formed by heating an expandable particulate material having a particle size of about 0.125 mm to about 0.5 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising: about 10 wt % to about 15 wt % borosilicate glass; about 35 wt % to about 45 wt % silica fume; about 15 wt % to about 20 wt % sodium hydroxide; and about 25 wt % to about 32 wt % water; and wherein the expanded particulate material has:
[0467] (a) Approximately 25 kg / m2 measured according to PI 200-77 3 About 30kg / m3 The loose bulk density;
[0468] (b) a compaction resistance of about 4 PSI to about 8 PSI at 2" as measured in accordance with PI 306-80; and / or
[0469] (c) Thermal conductivity of about 0.0310 W / mK to about 0.0350 W / mK measured according to EN 12667.
[0470] The expanded particulate material can be formed by heating an expandable particulate material having a particle size of about 0.3 mm to about 2 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising: about 12 wt % to about 18 wt % borosilicate glass; about 5 wt % to about 15 wt % silica fume; about 10 wt % to about 15 wt % sodium hydroxide; and about 20 wt % to about 30 wt % water; and the expanded particulate material has:
[0471] (a) Approximately 55 kg / m2 measured according to PI 200-77 3 About 65kg / m 3 The loose bulk density;
[0472] (b) a compaction resistance of about 35 PSI to about 40 PSI at 2" as measured in accordance with PI 306-80; and / or
[0473] (c) Thermal conductivity of about 0.0360 W / mK to about 0.0400 W / mK measured according to EN 12667.
[0474] The expanded particulate material can be formed by heating an expandable particulate material having a particle size of less than about 0.3 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising: about 12 wt % to about 18 wt % borosilicate glass; about 5 wt % to about 15 wt % silica fume; about 10 wt % to about 15 wt % sodium hydroxide; and about 20 wt % to about 30 wt % water; and the expanded particulate material has:
[0475] (a) Approximately 90 kg / m2 measured according to PI 200-77 3 About 100kg / m 3 The loose bulk density;
[0476] (b) a compaction resistance of from about 70 PSI to about 80 PSI at 2" as measured in accordance with PI 306-80; and / or
[0477] (c) Thermal conductivity of about 0.0370 W / mK to about 0.0420 W / mK measured according to EN 12667.
[0478] The expanded particulate material can be formed by heating an expandable particulate material having a particle size of about 0.5 mm to about 1 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising: about 12 wt % to about 18 wt % borosilicate glass; about 5 wt % to about 10 wt % silica fume; about 8 wt % to about 16 wt % sodium hydroxide; and about 20 wt % to about 32 wt % water; wherein the expanded particulate material has:
[0479] (a) Approximately 75 kg / m2 measured according to PI 200-77 3 About 85kg / m 3 The loose bulk density;
[0480] (b) a compaction resistance of from about 40 PSI to about 50 PSI at 2" as measured in accordance with PI 306-80; and / or
[0481] (c) Thermal conductivity of about 0.0370 W / mK to about 0.0410 W / mK measured according to EN 12667.
[0482] The expanded particulate material can be formed by heating an expandable particulate material having a particle size of about 0.125 mm to about 0.5 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising: about 12 wt % to about 18 wt % borosilicate glass; about 5 wt % to about 10 wt % silica fume; about 8 wt % to about 16 wt % sodium hydroxide; and about 20 wt % to about 32 wt % water; wherein the expanded particulate material has:
[0483] (a) Approximately 78 kg / m2 measured according to PI 200-77 3 About 86kg / m 3 The loose bulk density;
[0484] (b) a compaction resistance of from about 60 PSI to about 74 PSI at 2" as measured in accordance with PI 306-80; and / or
[0485] (c) Thermal conductivity of about 0.0360 W / mK to about 0.0420 W / mK measured according to EN 12667.
[0486] The expanded particulate material can be formed by heating an expandable particulate material having a particle size of about 0.1 mm to about 1 mm (determined by particle size determination by sieving), the expandable particulate material being formed from a mixture comprising: about 12 wt % to about 18 wt % borosilicate glass; about 5 wt % to about 10 wt % silica fume; about 8 wt % to about 16 wt % sodium hydroxide; and about 20 wt % to about 32 wt % water; wherein the expanded particulate material has:
[0487] (a) Approximately 70 kg / m2 measured according to PI 200-77 3 About 105kg / m 3 The loose bulk density;
[0488] (b) a compaction resistance of from about 60 PSI to about 75 PSI at 2" as measured in accordance with PI 306-80; and / or
[0489] (c) Thermal conductivity of about 0.0360 W / mK to about 0.0430 W / mK measured according to EN 12667.
[0490] The expanded particulate material can be formed by heating an expandable particulate material having a particle size of about 0.5 mm to about 1 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising: about 10 wt % to about 20 wt % borosilicate glass; about 10 wt % to about 20 wt % silica fume; about 10 wt % to about 20 wt % sodium hydroxide; and about 20 wt % to about 30 wt % water; wherein the expanded particulate material has:
[0491] (a) Approximately 20 kg / m2 measured according to PI 200-77 3 About 30kg / m 3 The loose bulk density;
[0492] (b) a compaction resistance of about 5 PSI to about 10 PSI at 2" as measured in accordance with PI 306-80; and / or
[0493] (c) Thermal conductivity of about 0.0310 W / mK to about 0.0360 W / mK measured according to EN 12667.
[0494] The expanded particulate material can be formed by heating an expandable particulate material having a particle size of about 0.125 mm to about 0.5 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising: about 10 wt % to about 20 wt % borosilicate glass; about 10 wt % to about 20 wt % silica fume; about 10 wt % to about 20 wt % sodium hydroxide; and about 20 wt % to about 30 wt % water; wherein the expanded particulate material has:
[0495] (a) Approximately 25 kg / m2 measured according to PI 200-77 3 About 35kg / m 3 The loose bulk density;
[0496] (b) a compaction resistance of about 5 PSI to about 15 PSI at 2" as measured in accordance with PI 306-80; and / or
[0497] (c) Thermal conductivity of about 0.0310 W / mK to about 0.0350 W / mK measured according to EN 12667.
[0498] The expanded particulate material can be formed by heating an expandable particulate material having a particle size of less than about 0.3 mm (determined by granulometry by sieving), the expandable particulate material being formed from a mixture comprising: about 10 wt % to about 20 wt % borosilicate glass; about 10 wt % to about 20 wt % silica fume; about 10 wt % to about 20 wt % sodium hydroxide; and about 20 wt % to about 30 wt % water; wherein the expandable particulate material has:
[0499] (a) Approximately 30 kg / m2 measured according to PI 200-77 3 About 40kg / m 3 The loose bulk density;
[0500] (b) a compaction resistance of about 8 PSI to about 16 PSI at 2" as measured in accordance with PI 306-80; and / or
[0501] (c) Thermal conductivity of about 0.0300 W / mK to about 0.0350 W / mK measured according to EN 12667.
[0502] The expanded particulate material may have a water absorption rate (in grams of water absorbed per gram of the expanded particulate material) of not less than about 0.1 g / g, such as not less than about 0.2 g / g, or not less than about 0.5 g / g, or not less than about 1 g / g. The expanded particulate material may have a water absorption rate (in grams of water absorbed per gram of the expanded particulate material) of not more than about 15 g / g, such as not more than about 10 g / g. The expanded particulate material may have a water absorption rate (in grams of water absorbed per gram of the expanded particulate material) of about 0.1 g / g to about 15 g / g, such as about 0.2 g / g to about 15 g / g, or about 0.5 g / g to about 10 g / g, or about 1 g / g to about 10 g / g.
[0503] The water absorption of granular materials can be measured by first accurately measuring 500 ml of granular material and recording the weight of the sample. The 500 ml sample is transferred to a 500 ml cylinder with a very fine screen at the bottom, which is enough to keep the granular material in the cylinder, but also allows water to pass through. The cylinder is tapped 10 times to allow the material to settle. 250 g of water is weighed and poured into the cylinder with the granular material. Start the timer and measure the mass of water that passes through the material and leaves the cylinder after 3, 5, 7, 10 and 30 minutes. The water absorption of the granular material is then the mass of water that does not flow out of the cylinder (i.e. the mass of water absorbed) / the mass of the granular material in the cylinder (expressed in g / g).
[0504] The expanded particulate material may have a water repellency of not less than about 40%, such as not less than about 50%, or not less than about 60%, or not less than about 65%. The water repellency of the expanded particulate material may be not more than about 95%, such as not more than about 90%. The water repellency of the expanded particulate material may be from about 40% to about 95%, such as from about 50% to about 95%, or from about 60% to about 95%, or from about 65% to about 90%.
[0505] The water repellency of material can be measured by taking a representative sample of the material with a sampler (500mL) and weighing the sample. Use a funnel to transfer the sample to a graduated cylinder with a perforated bottom. Make the graduated cylinder fall ten times from a height of about 7.5cm to allow the sample to settle. 250g of deionized water is slowly poured into the graduated cylinder together with the sample to avoid water loss or cavitation in the sample. Every 3 minutes, 5 minutes, 7 minutes, 10 minutes and 30 minutes, the water passing through the sample is collected in a weighing glass beaker below the graduated cylinder, and the water in the glass beaker is weighed. When 30 minutes are over, the graduated cylinder is tilted 45 ° to allow any remaining water to drip out of the graduated cylinder. Then the water absorption rate of 30 minutes is calculated according to the following equation:
[0506]
[0507] Where W H2O,30min is the mass of water collected after 30 minutes and A(g) is the mass of 500 ml of granular material.
[0508] The expanded particulate material may contain not less than about 95%, such as not less than about 97% or not less than about 99% floating matter. The expanded particulate material may contain up to 100% floating matter. The expanded particulate material may contain from about 95% to about 100%, such as from about 97% to about 100%, or from about 99% to about 100% floating matter.
[0509] The Imhoff cone is used to determine the amount of floating objects in a material sample. Specifically, 600 mL of deionized water is poured into an Imhoff cone fixed vertically in a stand. Another 50 mL of deionized water containing 20 drops of bromothymol blue or methylene blue indicator is added to the cone. The indicator is used to facilitate reading the cone with the color it gives to the water. Take a 300 mL representative sample of the material to be studied with a sampler. Record the exact volume (A mL) and weight (Bg) of the sample and add the sample to the cone. Add another 300 mL of deionized water to the cone on the sample, so that a total of 950 mL of water is in the Imhoff cone. The sample and water are stirred 20 times with a rod. Rinse the walls and rods on the top of the cone with 50 mL of deionized water (so that a total of 1000 mL of water is present in the cone) to rinse any particles adhering to it into the cone. Allow the cone and its contents to stand for 45 minutes. Thereafter, the cone volume (C_mL) corresponding to the level of dark particles (i.e., "sinks") at the bottom of the cone was recorded. The cone volume (DmL) corresponding to the level of total sediment at the bottom of the cone was also recorded. The percentages of "sinks", "shattered", and "floaters" were then determined according to the following equations:
[0510]
[0511]
[0512]
[0513] The expanded granular material may have a pH of not less than about 8, e.g., not less than about 9, or not less than about 9.5, measured according to PI 202-77. The expanded granular material may have a pH of not more than about 12, e.g., not more than about 115, measured according to PI 202-77. The expanded granular material may have a pH of about 8 to about 12, e.g., about 9 to about 11, or about 9.5 to about 11, measured according to PI 202-77. The pH of the expanded granular material can be determined by mixing 0.5 g of the granular material with 50 mL of deionized water and stirring at room temperature for 30 minutes. During the last 2 minutes of stirring, the pH value is measured (e.g., using a pH probe) and recorded.
[0514] The skeleton density of the expanded particulate material may be not less than about 0.4 g / cm 3 , for example not less than about 0.5 g / cm 3 , or not less than about 0.6 g / cm 3 The skeletal density of the expanded particulate material may be no greater than about 2 g / cm 3 , for example not more than about 1.8 g / cm 3 , or not more than about 1.6 g / cm 3The skeletal density of the expanded particulate material may be about 0.4 g / cm 3 About 2g / cm 3 , for example about 0.5 g / cm 3 To about 1.8g / cm 3 , or about 0.6 g / cm 3 To about 1.6g / cm 3 The skeletal density of a porous material (ie, the absolute density of a porous material determined using a volume excluding the volume of any pores in the porous material and the volume of any void spaces between particles) can be measured using, for example, a stereopycnometer available from Quantachrome.
[0515] application
[0516] The expanded particulate material can be used as an insulation product or in an insulation product. The insulation product can be a cavity wall insulation material, such as a cavity wall bulk particulate insulation material. The insulation product can be an insulation board or a filler for an insulation board. The insulation product can be an acoustic ceiling or a filler for an acoustic ceiling. The insulation product can be an insulation container such as a refrigerated or cryogenic container or a particulate material for insulation of a container such as a cryogenic or cryogenic container. The expanded particulate material can have (a) an average particle size (e.g., d ) less than about 1.25 mm. 50 ) and / or (b) about 30kg / m 3 About 100kg / m 3 Expanded granular materials with a loose bulk density are particularly suitable for such applications.
[0517] The expanded particulate material can be used as a building material or in a building material. The building material can be a fiber cement sheet. The building material can be concrete. For example, the expanded particulate material can be used as a lightweight aggregate material in concrete. The expanded particulate material has (a) an average particle size (e.g., d) greater than or equal to about 500 μm, such as about 500 μm to about 6 mm, such as about 2 mm to about 6 mm. 50 ), and / or (b) about 10 kg / m 3 About 100kg / m 3 Expanded granular materials with a loose bulk density are particularly suitable for such applications.
[0518] The building material may be a mortar or plaster, such as a cementitious, gypsum-based and / or acrylic-based mortar or plaster. 50 ), and / or (b) about 80 kg / m 3 About 450kg / m 3 , for example about 80kg / m 3About 350kg / m 3 Expanded granular materials with a loose bulk density are particularly suitable for such applications.
[0519] The expanded particulate material can be used in coatings such as paints. It has (a) an average particle size (e.g., d) of less than about 0.5 mm, such as less than about 0.2 mm. 50 ), and / or (b) about 80 kg / m 3 About 450kg / m 3 , for example about 80kg / m 3 About 350kg / m 3 Expanded granular materials with a loose bulk density are particularly suitable for such applications.
[0520] The expanded particulate material can be used as or in a horticultural or agricultural substrate. The horticultural or agricultural substrate can consist essentially of the expanded particulate material. For example, the horticultural or agricultural substrate can consist of the expanded particulate material, or the horticultural or agricultural substrate can comprise the expanded particulate material and one or more other materials, such as organic matter or soil.
[0521] The expandable particulate material can be used as or in a flame retardant functional material. The flame retardant functional material can be a flame retardant filling material.
[0522] Numbered paragraphs
[0523] For the avoidance of doubt, this application relates to the subject matter described in the following numbered paragraphs:
[0524] 1. A method for manufacturing an expanded granular material, the method comprising: forming a mixture comprising a silicate material, an alkaline compound and water; solidifying the mixture to form a solid precursor; crushing and / or grinding the solid precursor to form an expandable granular material; and heating the expandable granular material to form an expanded granular material.
[0525] 2. The method of numbered paragraph 1, wherein the mixture comprises glass network forming elements other than silicon, glass network intermediate elements and / or glass network modifying elements, and optionally wherein: the glass network forming elements other than silicon are selected from: boron, germanium and phosphorus; the glass network intermediate elements are selected from: titanium, aluminum, zirconium, beryllium, magnesium and zinc; and / or the glass network modifying elements are selected from: calcium, lead, lithium, sodium and potassium.
[0526] 3. The method according to numbered paragraph 1 or numbered paragraph 2, wherein the mixture further comprises reactive silica, such as silica fume and / or fumed silica.
[0527] 4. A method according to any one of the preceding numbered paragraphs, wherein the mixture comprises two different silicate materials, for example, wherein the mixture comprises: a silicate glass, such as an aluminosilicate glass, and a silicate mineral, such as an aluminosilicate mineral; or wherein the mixture comprises: a first silicate glass, such as a first aluminosilicate glass; and a second silicate glass, such as a second aluminosilicate glass.
[0528] 5. A method according to numbered paragraph 4, wherein one of the two different silicate materials is selected from: volcanic glass, such as a perlite material, such as an unexpanded natural perlite ore having a water content greater than about 2 weight percent; a phyllosilicate mineral, such as bentonite, kaolin or calcined kaolin; diatomaceous earth; or a combination thereof.
[0529] 6. The method according to numbered paragraph 4 or numbered paragraph 5, wherein one of the two different silicate materials is a silicate glass selected from the following: fused silica glass, soda-lime glass, borosilicate glass, lead oxide glass, aluminosilicate glass, and silicon-germanium glass.
[0530] 7. The method of numbered paragraph 6, wherein the silicate glass is recycled glass, for example in the form of recycled cullet.
[0531] 8. A method according to any one of the preceding numbered paragraphs, wherein the alkaline compound is an alkaline salt, for example: an alkaline hydroxide, such as sodium hydroxide, lithium hydroxide or potassium hydroxide; an alkaline carbonate, such as sodium carbonate, lithium carbonate or potassium carbonate; or an alkaline silicate, such as sodium silicate, lithium silicate or potassium silicate; or a mixed alkaline salt, such as sodium silicate / lithium silicate or sodium silicate / potassium silicate.
[0532] 9. A method according to any one of the preceding numbered paragraphs, wherein the mixture comprises: from about 10 wt % to about 90 wt %, for example from about 15 wt % to about 80 wt %, or from about 20 wt % to about 70 wt % of a silicate material; from about 5 wt % to about 25 wt %, from about 10 wt % to about 20 wt % of an alkaline compound; and from about 15 wt % to about 50 wt %, for example from about 20 wt % to about 40 wt % of water.
[0533] 10. The method of numbered paragraph 9, wherein the mixture comprises from about 5 wt % to about 75 wt %, for example from about 5 wt % to about 50 wt %, or from about 5 wt % to about 40 wt % reactive silica.
[0534] 11. A method according to numbered paragraph 9 or numbered paragraph 10, wherein the mixture comprises: about 5 weight percent to about 50 weight percent, for example, about 10 weight percent to about 40 weight percent, of the first silicate material; and about 5 weight percent to about 50 weight percent, for example, about 10 weight percent to about 40 weight percent, of the second silicate material.
[0535] 12. A method according to numbered paragraph 11, wherein: the first silicate material is a silicate glass, such as an aluminosilicate glass, and the second silicate material is a silicate mineral, such as an aluminosilicate mineral; or the first silicate material is a first silicate glass, such as a first aluminosilicate glass, and the second silicate material is a second silicate glass, such as a second aluminosilicate glass.
[0536] 13. A method according to numbered paragraph 9, wherein the silicate material includes: about 50 wt% to about 95 wt%, for example, about 60 wt% to about 85 wt% SiO2; about 1 wt% to about 30 wt%, for example, about 2 wt% to about 15 wt% Na2O; about 0 wt% to about 15 wt%, for example, about 0.01 wt% to about 6 wt% K2O; about 0 wt% to about 20 wt%, for example, about 0.05 wt% to about 15 wt% CaO; about 0 wt% to about 20 wt%, for example, about 0.1 wt% to about 15 wt% Al2O3; not more than about 20 wt%, for example, less than about 15 wt% B2O3; not more than about 20 wt%, for example, less than about 15 wt% PbO; not more than about 10 wt%, for example, less than about 5 wt% MgO; and not more than about 10 wt%, for example, less than about 5 wt% BaO.
[0537] 14. A method according to any of the preceding numbered paragraphs, wherein the mixture comprises boron in an amount such that the expanded particulate material comprises less than about 5.0 wt. %, such as less than about 3.5 wt. % B2O3.
[0538] 15. A method according to any of the preceding numbered paragraphs, wherein the step of curing the mixture to form the solid precursor comprises curing the mixture at a temperature of no greater than about 250°C, for example no greater than about 120°C, or from about 20°C to about 250°C, or from about 20°C to about 120°C, or from about 50°C to about 110°C, or from about 70°C to about 100°C.
[0539] 16. A method according to any of the preceding numbered paragraphs, wherein the step of heating the granular material to form the expanded granular material includes heating the granular material to a temperature of not greater than about 1100°C, for example not greater than about 700°C, or from about 300°C to about 900°C, or from about 300°C to about 700°C, or from about 400°C to about 600°C.
[0540] 17. A method according to any of the preceding numbered paragraphs, wherein the step of heating the particulate material to form an expanded particulate material comprises heating the particulate material in an infrared furnace, an electrically heated furnace, a natural gas or LPG expansion furnace, a muffle furnace or a fluidized bed reactor.
[0541] 18. A method according to any of the preceding numbered paragraphs, wherein the expanded particulate material has: a particle size of about 15 kg / m 3 About 450kg / m 3 , for example about 20kg / m 3 About 100kg / m 3 , or about 20kg / m 3 About 30kg / m 3 , or about 20kg / m 3 About 40kg / m 3 , or about 55kg / m 3 About 100kg / m 3 , or about 70kg / m 3 About 100kg / m 3 a loose bulk density of about 3 PSI to about 350 PSI at 2", measured according to PI 306-80, for example, about 3 PSI to about 200 PSI at 2", or about 3 PSI to about 100 PSI at 2", or about 3 PSI to about 10 PSI at 2", or about 30 PSI to about 80 PSI at 2", or about 40 PSI to about 75 PSI at 2", or about 5 PSI to about 20 PSI at 2"; and / or a compaction resistance according to EN 12667 measured thermal conductivity (λ, λ value) of about 0.0300 W / mK to about 0.0700 W / mK, for example, about 0.0320 W / mK to about 0.0420 W / mK, about 0.0350 W / mK to about 0.0400 W / mK, or about 0.0360 W / mK to about 0.0410 W / mK, or about 0.0320 W / mK to about 0.0340 W / mK, or about 0.042 W / mK to about 0.055 W / mK, or about 0.055 W / mK to about 0.070 W / mK.
[0542] 19. Expanded particulate material produced by the method according to any one of the preceding numbered paragraphs.
[0543] 20. An expanded granular material having: a particle size of about 15 kg / m 3 About 450kg / m 3 , for example about 20kg / m 3 About 100kg / m 3 , or about 20kg / m3 About 30kg / m 3 , or about 20kg / m 3 About 40kg / m 3 , or about 55kg / m 3 About 100kg / m 3 , or about 70kg / m 3 About 100kg / m 3 a loose bulk density of about 3PSI to about 350PSI at 2", measured according to PI306-80, for example, about 3PSI to about 200PSI at 2", or about 3PSI to about 100PSI at 2", or about 3PSI to about 10PSI at 2", or about 30PSI to about 80PSI at 2", or about 40PSI to about 75PSI at 2", or about 5PSI to about 20PSI at 2"; and / or a compaction resistance of about 5PSI to about 20PSI at 2" as measured according to EN 12667 measured thermal conductivity of about 0.0300 W / mK to about 0.0700 W / mK, for example, about 0.0320 W / mK to about 0.0420 W / mK, about 0.0350 W / mK to about 0.0400 W / mK, or about 0.0360 W / mK to about 0.0410 W / mK, or about 0.0320 W / mK to about 0.0340 W / mK, or about 0.042 W / mK to about 0.055 W / mK, or about 0.055 W / mK to about 0.070 W / mK.
[0544] 21. An expanded particulate material according to numbered paragraph 20, wherein the expanded particulate material comprises: about 8 wt% to about 30 wt%, for example about 13 wt% to about 22 wt% X2O, X being an alkali metal such as Na or Li; about 0 wt% to about 15 wt%, for example about 5 wt% to about 9 wt% Al2O3; and about 50 wt% to about 80 wt%, for example about 60 wt% to about 75 wt% SiO2; and optionally about 0 wt% to about 10 wt%, for example about 0.5 wt% to about 5 wt% H2O.
[0545] 22. The expanded particulate material of numbered paragraph 21, wherein the expanded particulate material comprises less than about 5 wt%, such as less than about 3.5 wt%, B2O3.
[0546] 23. An expanded granular material as described in any of numbered paragraphs 20-22, wherein the expanded granular material is formed by expanding a precursor obtained by curing a mixture comprising a silicate material, an alkaline compound and water; optionally wherein: (a) the mixture comprises glass network forming elements, glass network intermediate elements and / or glass network modifying elements other than silicon; (b) the mixture further comprises reactive silica; and / or (c) the mixture comprises two different silicate materials.
[0547] 24. An expanded granular material according to section (c) of paragraph number 23, wherein: (i) one of the two different silicate materials is selected from: volcanic glass, such as perlite material, such as unexpanded natural perlite ore having a water content greater than about 2% by weight; phyllosilicate minerals, such as bentonite, kaolin or calcined kaolin; diatomaceous earth; or any combination thereof; and / or (ii) one of the two different silicate materials is a silicate glass selected from the following: fused quartz glass, soda-lime glass, borosilicate glass, lead oxide glass, aluminosilicate glass, silicon germanium glass.
[0548] 25. An expandable material comprising: about 0.1 wt % to about 25 wt %, for example about 0.2 wt % to about 5 wt % X2O, wherein X is an alkali metal, such as Na or Li; about 0.1 wt % to about 30 wt %, for example about 0.2 wt % to about 20 wt % Al2O3; about 30 wt % to about 80 wt %, for example about 40 wt % to about 60 wt % SiO2; and about 10 wt % to about 30 wt %, for example about 15 wt % to about 30 wt % H2O; wherein the expandable material optionally comprises less than about 5 wt %, for example less than about 3.5 wt % B2O3.
[0549] 26. The expandable material of numbered paragraph 25, wherein the expandable material is substantially amorphous.
[0550] 27. The expandable material of numbered paragraph 25 or numbered paragraph 26, wherein the expandable material is granular and optionally has a particle size of about 10 μm to about 2 cm.
[0551] 28. A method for making an expandable material, the method comprising: (a) forming a mixture comprising a silicate material, an alkaline compound and water; wherein optionally: (i) the mixture comprises a glass network forming element, a glass network intermediate element and / or a glass network modifying element other than silicon; (ii) the mixture further comprises reactive silica; and / or (iii) the mixture comprises two different silicate materials; and (b) curing the mixture to form the expandable material.
[0552] 29. The method of numbered paragraph 28, further comprising comminuting the expandable material.
[0553] 30. An expandable material made according to the method of numbered paragraph 28 or numbered paragraph 29.
[0554] 31. An insulation product, such as a bulk material for insulating a cavity wall, a filler for an insulation board, an insulation board, a filler for a ceiling tile such as an acoustic ceiling tile, a ceiling tile such as an acoustic ceiling tile, a granular material for insulating a refrigerated or cryogenic container, or an insulated refrigerated or cryogenic container, comprising an expanded granular material as described in any of numbered paragraphs 19 to 24 or an expanded granular material formed by expanding an expandable material as described in any of numbered paragraphs 25 to 27 or 30.
[0555] 30. A building material, such as a sheet such as a fiber cement sheet, a mortar or plaster such as a cementitious, gypsum-based and / or acrylic-based mortar or plaster, or concrete, comprising the expanded particulate material of any one of numbered paragraphs 19 to 24 or an expanded particulate material formed by expanding the expandable material of any one of numbered paragraphs 25 to 27 or 30.
[0556] 31. A horticultural or agricultural substrate or substrate component comprising the expanded particulate material of any of numbered paragraphs 19 to 24 or an expanded particulate material formed by expanding the expandable material of any of numbered paragraphs 25 to 27 or 30.
[0557] 32. A flame retardant functional material comprising the expandable particulate material described in any one of numbered paragraphs 25 to 27 or the expandable particulate material manufactured according to the method described in any one of numbered paragraphs 28 to 30.
[0558] 33. Use of the expanded granular material of any of numbered paragraphs 19 to 24, or the expanded granular material formed by expanding the expandable material of any of numbered paragraphs 25 to 27 or 30, in an insulation product, such as bulk material for insulating cavity walls, filler for insulation panels, filler for sound-absorbing ceilings, granular material for insulating refrigerated or cryogenic containers, or building materials, such as sheets such as fiber cement sheets, mortars or plasters such as cementitious, gypsum-based and / or acrylic-based mortars or plasters, or concrete, or horticultural or agricultural substrates or substrate components.
[0559] Example
[0560] In the following examples, expandable and expandable materials were prepared using silicate raw materials whose chemical compositions (expressed in weight % of equivalent oxide content) are shown in Table 1. The particle size of each silicate raw material, expressed as d 50(μm) is expressed.
[0561] Table 1.
[0562]
[0563] *Values are expressed as weight %
[0564] **Values are expressed in μm
[0565] Typically, expandable materials are prepared by inorganic polymerization of silicate raw materials in alkaline aqueous solutions. Granules of alkaline salts (e.g., sodium hydroxide or lithium hydroxide) are dissolved in water. Solid silicate raw materials are immediately added to the resulting solution so that the heat generated when the alkaline salt dissolves contributes to the dissolution of the silicate material. The mixture is stirred for several minutes to form a paste. After stirring, the paste is cured in an oven at a temperature of 70°C to 100°C for several hours to several days to form an expandable precursor material. The precursor is crushed and sieved to the desired particle size.
[0566] The expanded material was produced by expanding a pulverized precursor material. Unless otherwise stated, the pulverized precursor was expanded by heating in an infrared (IR) expansion furnace (type: M3 / 45-SO2, series: AA, CFKN0.44 / 0.64, RPM3000 / 3800) equipped with a stainless steel vibrating table, eight Elstein HTS ceramic infrared panel radiators (having a size of 125x125 mm, a power output of 64 kW / m and a maximum operating temperature of 860°C) and Italvibras G Silingardi vibration elements. The feed into the furnace was regulated using an electromagnetic automatic feeder. The infrared lamps were operated at a temperature of 500°C to 750°C, so that the temperature of the particle precursor reached about 300°C to about 350°C. The pulverized precursor with a particle size of less than 500 μm was expanded by heating in a vertical electric furnace (VEF) or a vertical LPG furnace. Very fine particles with a particle size of less than 100 μm were expanded in a laboratory-scale fluidized bed (FB) reactor.
[0567] Example 1
[0568] Four different expanded materials were formed using borosilicate glass, sodium hydroxide and water as starting materials. Table 2 shows the composition of the four different starting mixtures, the concentration of sodium hydroxide in the initial alkaline solution, the ratio of silicon to sodium in the mixture, the measured "loss on ignition" of the material before expansion, and the measured loose bulk density of the material after expansion at 700°C in a laboratory muffle furnace.
[0569] Table 2.
[0570] mixture A1 A2 A3 A4 Borosilicate glass (weight %) 62.5 59.8 57.8 57.7 NaOH (wt%) 6.3 12.1 17.5 18.6 Water (wt%) 31.2 28.1 24.7 23.7 NaOH concentration (M) 5 10 15 16.1 Si / Na ratio 5.2 2.6 1.7 1.6 LOI unexpanded (wt%) 6.41% 15.09% 19.08% 17.00% <![CDATA[LBD(kg / m 3 )]]> 357 114 58 45
[0571] Example 2
[0572] Six different expandable materials were formed using borosilicate glass, soda-lime glass, sodium hydroxide, and water as starting materials. Table 3 shows the composition of the six different starting mixtures, the ratio of borosilicate glass to soda-lime glass in the mixture ("B / S" ratio), the concentration of sodium hydroxide in the initial alkaline solution, the ratio of silicon to sodium in the mixture, the measured "loss on ignition" of the material before expansion, and the measured loose bulk density of the material after expansion in a laboratory muffle furnace at 600°C, 650°C, or 750°C. Mixtures B4, B5, and B6 did not produce expandable materials.
[0573] Table 3.
[0574] mixture B1 B2 B3 B4 B5 B6 Borosilicate glass (weight %) 66.67 33.33 13.33 6.67 2 0 Soda lime glass (weight %) 0 33.33 53.33 60 64.67 66.67 NaOH (wt%) 5.62 5.62 5.62 5.62 5.62 5.62 Water (wt%) 27.72 27.72 27.72 27.72 27.72 27.72 B / S Ratio ∞ 1 0.25 0.11 0.03 0 NaOH concentration (M) 5 5 5 5 5 5 Si / Na ratio 6.2 5.9 5.8 5.7 5.7 5.7 LOI unexpanded (wt%) 6.46% 8.44% 7.85% 7.55% 7.20% 6.95% E expansion temperature (℃) 600 650 750 - - - <![CDATA[Loose bulk density (kg / m 3 )]]> 162 320 572 - - -
[0575] Example 3
[0576] The expandable material was formed using 13.5 wt% borosilicate glass, 40.5 wt% silica fume, 18 wt% sodium hydroxide and 27.9 wt% water as starting materials. The expandable material was crushed into two different particle size ranges before expansion. The measured loose bulk density, compaction resistance and thermal conductivity of the two different expandable materials are shown in Table 4.
[0577] Table 4.
[0578]
[0579] Example 4
[0580] The expandable material was formed using 15 wt% borosilicate glass, 45 wt% perlite tailings, 10 wt% sodium hydroxide and 30 wt% water as starting materials. The expandable material was crushed to a particle size range of 0.5 mm to 1 mm before expansion. The measured loose bulk density and thermal conductivity of the expanded material are shown in Table 5.
[0581] Table 5.
[0582]
[0583] Example 5
[0584] 51 different intumescent materials were formed using different combinations of borosilicate glass, silica fume, perlite tailings, sodium hydroxide, lithium hydroxide, water, and water repellent as starting materials. Tables 6 to 16 show the compositions of 40 starting mixtures, as well as the ratio of the combined total amount of silica fume and perlite tailings to the total amount of borosilicate glass ("(SF+P) / BG" ratio), the ratio of the total amount of silica fume to the total amount of perlite tailings ("SF / P" ratio), and some or all of the following: the ratio of silicon to sodium, the particle size of the unexpanded precursor material, the temperature at which the expansion was performed, the measured loose bulk density of the expanded material, the particle size of the expanded material, the d of the expanded material 50 , water absorption of the expanded material, water repellency of the expanded material, percentage of expanded particles as floaters, compaction resistance of the expanded material at 1" or 2", thermal conductivity of the expanded material, pH of the foamed material and skeletal density of the foamed material. Unless otherwise stated, expansion was performed in an IR oven.
[0585] Table 6.
[0586]
[0587]
[0588] Table 7.
[0589]
[0590] Table 8.
[0591]
[0592] Table 9.
[0593]
[0594]
[0595] Table 10.
[0596]
[0597] Table 11.
[0598]
[0599] Table 12.
[0600]
[0601]
[0602] Table 13.
[0603]
[0604] Table 14.
[0605]
[0606] Table 15.
[0607]
[0608] Table 16.
[0609]
[0610] Example 6
[0611] Different combinations of borosilicate glass, silica fume, perlite tailings, soda lime glass sodium hydroxide, water and water repellent are used as starting materials to form 9 different expansion materials. Tables 17 and 18 show the composition of the 9 starting mixtures, the ratio of the total amount of silica fume and perlite tailings to the total amount of borosilicate glass ("(SF+P) / BG" ratio), the ratio of the total amount of silica fume to the total amount of perlite tailings ("SF / P" ratio), the ratio of borosilicate glass to soda lime glass ("B / S" ratio), the ratio of silicon to sodium, the particle size of the unexpanded precursor material, the temperature at which the expansion is performed, the measured loose bulk density of the expanded material, and the water absorption (i.e., water load) of the expanded material. Unless otherwise stated, the samples were expanded in an IR furnace.
[0612] The water absorption (water load) of each granular material is measured by first measuring 400ml of granular material. The sample is transferred to a 500ml cylinder with a very fine sieve at the bottom, which is enough to retain the granular material in the cylinder, but also allows water to pass through. Then tap 50 times in an automatic tapping device. Measure another 30ml of granular material and add it to the cylinder, and then tap the cylinder 30 times. Finally, according to the sedimentation of the sample, add a few milliliters of material and tap 20 times again to produce a 400 ml sample of tapping in the cylinder, record its weight. The cylinder is then connected to a water pump. Use a water pump to first fill the cylinder with water, and then drain the water out of the cylinder. Measure the new wet mass. The water absorption of the granular material is then calculated as the mass of the water retained by the sample (i.e. the mass of the water absorbed) / mass of the granular material in the cylinder (expressed in g / g).
[0613] Table 17.
[0614]
[0615] Table 18.
[0616]
[0617] Example 7
[0618] Five different expandable materials (E1 to E5) were formed using different mixtures of borosilicate glass, silica fume, perlite tailings, sodium hydroxide, lithium hydroxide and water as starting materials. The compositions of the five starting mixtures are listed in Table 19.
[0619] The expandable materials were tested for their suitability as non-intumescent foaming flame retardant additives for polymer compositions. Intumescents are substances that expand due to heat exposure, thus increasing in volume and decreasing in density. Intumescent additives are often used for passive fire protection.
[0620] The functionality of these novel flame retardant formulations is based on the ability to: (i) release up to 30 wt. % of bound water by absorbing heat; (ii) expand and create a thermal barrier that hinders heat transfer and destabilization of the surrounding polymer matrix (i.e., avoids burning droplets); and (iii) melt at temperatures above 700° C. while retaining at least part of the original shape without collapsing.
[0621] Discover all preparations:
[0622] 1. Release chemically bound water in the range of 200-500℃.
[0623] 2. Expands into expandable foam in the range of 400-600℃.
[0624] 3. Starts to melt at a temperature ≥700℃.
[0625] Tested according to DIN EN 45545 (fire test).
[0626] For each different polymer loaded with flame retardant additive, the softening point, melting point and flow point were successfully adjusted to meet a specific target narrow temperature range. As shown in Table 19, the adjustment was achieved by changing the starting mixture.
[0627] Two different polymers were loaded with flame retardant additives with the highest melting points: (1) PVC with 10 wt% D2; (2) PVC with 10 wt% D4; (3) polypropylene with 5 wt% and 10 wt% D2 (i.e., two different loading levels); and (4) polypropylene with 5 wt% and 10 wt% D4 (i.e., two different loading levels). The polyurethane (PU) foam was also loaded with 8 wt% of each flame retardant additive. Prior to loading, the softening point, melting point, and flow point of the flame retardant additive were successfully adjusted (relative to the baseline material as material D5) to maximize fire resistance. As shown in Table 19, the adjustments were achieved by changing the starting mixture.
[0628] Table 19.
[0629] Material E1 E2 E3 E4 E5 Borosilicate glass (weight %) 14.63 15 14.2 15 57.72 Silica fume (weight %) 14.63 10.38 9.83 0 0 Perlite tailings (wt%) 29.25 34.62 32.78 45 0 NaOH (wt%) 16.37 12.83 13.09 10.04 18.55 Water (wt%) 25.12 27.17 24.58 29.96 23.74 <![CDATA[LiOH.H2O (wt%)]]> 0 0 5.51 0 0 Water repellent(%) 0 0 0 0 0 (SF+P) / BG ratio 3 3 3 3 0 SF / P Ratio 0.5 0.3 0.3 ∞ ∞ Si / Na ratio 1.72 2.1 2 2.35 1.46 <![CDATA[H2O 950℃]]> 20,90 19,30 24,00 12,00 30,00 <![CDATA[H2O 105℃]]> 12,88 13,19 12,74 1,66 12,41 Softening point DIN 51730 617 634 562 686 627 Melting point DIN 51730 868 913 775 900 790 Flow point DIN 51730 991 1068 875 996 835
[0630] According to the particle size distribution, different particle size determinations listed in Table 20 have been examined in various polymers:
[0631] Table 20.
[0632] Particle size application 0mm-20mm Fireproof rings, fireproof pillows, fireproof building bricks. 0.15mm–1mm PU foam, plastic. <0.15mm PU foam, plastics, elastomers, cable insulation.
Claims
1. A method for producing an expanded granular material, the method comprising: forming a mixture comprising: Silicate glass; Basic compounds; and water; wherein the ratio of the total weight % of silicon in the mixture to the total weight % of sodium in the mixture is no greater than 4, wherein the weight % of silicon in the mixture is expressed as an equivalent content of SiO2, and the weight % of sodium in the mixture is expressed as an equivalent content of Na2O; curing the mixture to form a solid precursor; comminuting and / or grinding the solid precursor to form an expandable particulate material; as well as The expandable particulate material is heated to form an expanded particulate material.
2. The method according to claim 1, wherein the mixture comprises glass network forming elements, glass network intermediate elements and / or glass network modifying elements other than silicon, and optionally wherein: The glass network forming elements other than silicon are selected from the group consisting of boron, germanium and phosphorus; The glass network intermediate element is selected from the group consisting of: titanium, aluminum, zirconium, beryllium, magnesium and zinc; and / or The glass network modifying element is selected from the group consisting of: calcium, lead, lithium, sodium and potassium.
3. The method of claim 1 or claim 2, wherein the mixture further comprises reactive silica.
4. The method according to claim 3, wherein the reactive silica is selected from silica fume and / or fumed silica.
5. The method according to claim 1 or 2, wherein the mixture comprises two different silicate materials, The mixture comprises: silicate glass; and silicate minerals. 6 . The method of claim 5 , wherein the mixture comprises: a first silicate glass that is a first aluminosilicate glass; and a second silicate glass that is a second aluminosilicate glass.
7. The method according to claim 5, wherein: One of the two different silicate materials is selected from: volcanic glass; phyllosilicate minerals; diatomaceous earth; or a combination thereof; and / or One of the two different silicate materials is a silicate glass selected from the group consisting of fused silica glass, soda lime glass, borosilicate glass, lead oxide glass, aluminosilicate glass, silicon germanium glass, optionally wherein the silicate glass is recycled glass.
8. The method of claim 7, wherein the volcanic glass is a perlite material.
9. The method of claim 8, wherein the perlite material is an unexpanded natural perlite ore having a water content greater than 2% by weight.
10. The method of claim 7, wherein the phyllosilicate mineral is bentonite, kaolin or calcined kaolin.
11. The method according to claim 1 or 2, wherein the mixture comprises: 10 to 80 wt% silicate material; 5 to 25 wt % of a basic compound; and 15 to 50% by weight of water, Optionally, wherein the mixture comprises 5 wt % to 75 wt % reactive silica.
12. The method of claim 11, wherein the silicate material comprises: 50 to 95 wt. % SiO2; 1 to 30 wt % Na2O; 0 to 15 wt% K2O; 0 to 20 wt% CaO; 0 to 20 wt% Al2O3; Not more than 20% by weight of B2O3; Not more than 20 wt. % PbO; not more than 10 wt. % MgO; and Not more than 10 wt. % BaO.
13. The method of claim 1 or 2, wherein the mixture comprises boron in an amount such that the expanded particulate material comprises less than 5.0 wt. % B2O3.
14. The method according to claim 1 or 2, wherein: The step of curing the mixture to form a solid precursor comprises curing the mixture at a temperature not greater than 250°C; and / or The step of heating the particulate material to form an expanded particulate material comprises heating the particulate material to a temperature of no greater than 1100°C.
15. An expanded granular material having: 15kg / m2 measured according to PI 200-77 3 Up to 450kg / m 3 The loose bulk density; Compaction resistance of 3 PSI to 350 PSI at 2” as measured in accordance with PI 306-80; and / or Thermal conductivity of 0.0300 W / mK to 0.0700 W / mK measured according to EN 12667.
16. The expanded particulate material of claim 15, wherein the expanded particulate material comprises: 8 to 30 wt% of X2O, X being an alkali metal selected from Na or Li; 0 wt % to 15 wt % Al2O3; and 50 wt % to 80 wt % SiO2; and optionally 0 to 10 wt% H2O; And optionally wherein the expanded particulate material contains less than B2O3.
17. An expanded particulate material according to claim 15 or claim 16, wherein the expanded particulate material is formed by expanding a precursor obtained by curing a mixture comprising: Silicate materials; basic compounds; and water; Optionally among them: (a) the mixture contains glass network forming elements, glass network intermediate elements and / or glass network modifying elements other than silicon; (b) the mixture further comprises reactive silica; and / or (c) the mixture comprises two different silicate materials; Further optionally wherein: (i) one of the two different silicate materials is selected from: volcanic glass; phyllosilicate minerals; diatomaceous earth; or any combination thereof; and / or (ii) One of the two different silicate materials is a silicate glass selected from the group consisting of fused silica glass, soda-lime glass, borosilicate glass, lead oxide glass, aluminosilicate glass, and silicon-germanium glass.
18. The expanded particulate material of claim 17, wherein the volcanic glass is a perlite material.
19. The expanded particulate material of claim 18, wherein the perlite material is an unexpanded natural perlite ore having a water content greater than 2% by weight.
20. The expanded particulate material of claim 17, wherein the phyllosilicate mineral is bentonite, kaolin, or calcined kaolin.
21. An expandable material comprising: 0.1 to 25 wt% of X2O, wherein X is an alkali metal selected from Na or Li; 0.1 to 30 wt% Al2O3; 30 wt % to 80 wt % SiO2; and 10 to 30 wt% H2O; Wherein the expandable material optionally comprises less than 5 wt % B2O3.
22. An expandable material according to claim 21, wherein the expandable material is substantially amorphous and / or wherein the expandable material is granular and optionally has a particle size of 10 μm to 2 cm.
23. A method of making an expandable material, the method comprising: (a) forming a mixture comprising: Silicate glass; Basic compounds; and water; wherein the ratio of the total weight % of silicon in the mixture to the total weight % of sodium in the mixture is not greater than 4, wherein the weight % of silicon in the mixture is expressed as an equivalent content of SiO2, and the weight % of sodium in the mixture is expressed as an equivalent content of Na2O, and optionally wherein: (i) the mixture contains glass network forming elements, glass network intermediate elements and / or glass network modifying elements other than silicon; (ii) the mixture further comprises reactive silica; and / or (iii) the mixture comprises two different silicate materials; and (b) curing the mixture to form the expandable material; and Optionally: (c) comminuting the expandable material.
24. An insulation product selected from: bulk material for insulating cavity walls, filler for insulation panels, insulation panels, filler for ceiling tiles selected from acoustic ceiling tiles, ceiling tiles selected from acoustic ceiling tiles, granular material for insulating refrigerated or cryogenic containers, or an insulated refrigerated or cryogenic container, comprising an expanded granular material according to any one of claims 15 to 20, or an expanded granular material formed by expanding an expandable material according to claim 21 or claim 22, or by expanding an expandable material manufactured by the method according to claim 23.
25. A building material selected from: a sheet selected from fiber cement sheets, a mortar or plaster selected from cementitious, gypsum-based and / or acrylic-based mortars or plasters, or concrete, comprising an expanded granular material according to any one of claims 15 to 20, or an expanded granular material formed by expanding an expandable material according to claim 21 or claim 22 or by expanding an expandable material manufactured by the method according to claim 23.
26. A horticultural or agricultural substrate or substrate component comprising an expanded particulate material according to any one of claims 15 to 20, or an expanded particulate material formed by expanding an expandable material according to claim 21 or claim 22, or by expanding an expandable material made by the method of claim 23.
27. A flame retardant functional material, comprising the expandable material according to claim 21 or claim 22 or the expandable particulate material manufactured by the method according to claim 23.
Citation Information
Patent Citations
Method for production of foam glass pellets and pellets produced by this method
EP2647605A1
Inorganic expandable refractory composition
EP3135652A1
Method for manufacture of foam glass
US3951632A
Lightweight porous aggregate comprising alkali metal borosilicoaluminate and process for the preparation thereof
US4308065A