Organic light emitting display device and method for manufacturing the same
Through the combination of peeling layer and photoresist, combined with the vapor deposition process, the shadowing effect and defect problems caused by fine metal masks are solved, and high-quality manufacturing of high-resolution organic luminescent display equipment is achieved.
Patent Information
- Application Number
- CN201980083789.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-17
- Filing Date
- 2019-05-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-05-23
AI Technical Summary
When manufacturing high-resolution organic luminescent display devices, the shadowing effect of fine metal masks leads to an increase in defects, requiring an alternative deposition technique to reduce the number of defects.
Using a combination of a stripping layer and a photoresist, the top surface and openings of the exposed pixel electrode are patterned and the intermediate layer and counter electrode are sequentially formed thereon, followed by covering the passivation layer to completely cover the pair. The top surface and ends of the electrode, and finally the remaining release layer and photoresist are removed, and a passivation layer is formed using a physical vapor deposition or a chemical vapor deposition process to optimize coverage.
The quality of the organic light emitting display device is improved by avoiding the misalignment problem of fine metal masks, reducing manufacturing costs, and reducing defects of the light emitting elements through dry etching and peeling processes.
Smart Images

Figure CN113196516B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an organic light emitting display device and a method of manufacturing the same, and more particularly, to an organic light emitting display device and a method of manufacturing the same through a simplified process to have a reduced number of defects. Background Art
[0002] An organic light emitting display device includes an organic light emitting element including a hole injection electrode, an electron injection electrode, and an organic emission layer therebetween. The organic light emitting display device is a self-luminous display device in which light is emitted when excitons fall from an excited state to a ground state, the excitons being generated when holes injected from the hole injection electrode and electrons injected from the electron injection electrode are combined with each other in the organic emission layer.
[0003] Although a fine metal mask (FMM) may be used as a technique for depositing an organic emission layer on a substrate, there are limitations in manufacturing a high-resolution organic light-emitting display device due to a shadow effect of the metal mask. Therefore, an alternative deposition technique is needed. Summary of the invention
[0004] Technical issues
[0005] An organic light emitting display device and a method of manufacturing the organic light emitting display device through a simplified process to have a reduced number of defects are provided. However, such technical problems are examples and the disclosure is not limited thereto.
[0006] Technical Solution
[0007] According to aspects of the present disclosure, a method for manufacturing an organic light-emitting display device includes the following steps: forming a pixel electrode and a pixel defining layer on a substrate, the pixel defining layer covering the edge of the pixel electrode; sequentially forming a stripping layer and a photoresist on the pixel electrode and the pixel defining layer; patterning the stripping layer and the photoresist to form an opening exposing a top surface of the pixel electrode and a portion of the pixel defining layer; sequentially forming an intermediate layer and a counter electrode in the opening and on the photoresist, the intermediate layer including an emission layer; forming a passivation layer to completely cover the top surface and end of the counter electrode; and removing the stripping layer and the photoresist remaining outside the opening.
[0008] The photoresist may be patterned by a photolithography process.
[0009] The release layer may include a fluoropolymer.
[0010] The opening may be formed by etching the lift-off layer using a first solvent including fluorine.
[0011] The intermediate layer may be formed by a first deposition process, the counter electrode may be formed by a second deposition process, and the passivation layer may be formed by a third deposition process that may make the step coverage greater than that for the intermediate layer and the counter electrode.
[0012] The first deposition process may use a physical vapor deposition process.
[0013] The second deposition process may use a physical vapor deposition process.
[0014] The third deposition process may use a chemical vapor deposition process or an atomic layer deposition process.
[0015] The first to third deposition processes may be performed in the same chamber.
[0016] After the third deposition process, dry etching may be performed in the same chamber as the chamber in which the third deposition process is performed.
[0017] The top surface of the pixel defining layer may be exposed by dry etching.
[0018] The method may further include forming an auxiliary electrode on the pixel defining layer, wherein the counter electrode may be formed to contact the auxiliary electrode.
[0019] After the step of forming the passivation layer, dry etching may be performed in the same chamber as the chamber in which the passivation layer is formed, and the top surface of the auxiliary electrode may be exposed by the dry etching.
[0020] The remaining release layer may be removed by using a second solvent including fluorine.
[0021] The step of removing the release layer may be performed in the atmosphere.
[0022] According to aspects of the present disclosure, a method for manufacturing an organic light-emitting display device includes the following steps: after forming a first pixel electrode and a second pixel electrode on a substrate and forming a pixel defining layer covering ends of the first pixel electrode and the second pixel electrode, performing a first unit operation including the following operations (a1) to (a5): (a1) sequentially forming a first peeling layer and a first photoresist on the first pixel electrode, the second pixel electrode and the pixel defining layer; (a2) patterning the first peeling layer and the first photoresist to form a first opening exposing a top surface of the first pixel electrode and a portion of the pixel defining layer; (a3) sequentially forming a first intermediate layer and a first pair of electrodes in the first opening and on the first photoresist, the first intermediate layer including a first emission layer; (a4) forming a first passivation layer to cover the top surface and ends of the first pair of electrodes; part; and (a5) removing the first stripping layer and the first photoresist remaining outside the first opening; and after the first unit operation, performing a second unit operation including the following operations (b1) to (b5): (b1) sequentially forming a second stripping layer and a second photoresist on the first passivation layer, the second pixel electrode and the pixel defining layer; (b2) patterning the second stripping layer and the second photoresist to form a second opening exposing the top surface of the second pixel electrode and a portion of the pixel defining layer; (b3) sequentially forming a second intermediate layer and a second pair of electrodes in the second opening and on the second photoresist, the second intermediate layer including a second emission layer; (b4) forming a second passivation layer to completely cover the top surface and end portions of the second pair of electrodes; and (b5) removing the second stripping layer and the second photoresist remaining outside the second opening.
[0023] The color emitted from the first emission layer may be different from the color emitted from the second emission layer.
[0024] A first intermediate layer, a first counter electrode, and a first passivation layer may be formed in the first chamber.
[0025] The method may include the step of performing dry etching in the first chamber after the step of forming the first passivation layer.
[0026] The method may include the step of forming a second intermediate layer, a second counter electrode, and a second passivation layer in a second chamber different from the first chamber.
[0027] The method may include the step of performing dry etching in the second chamber after forming the second passivation layer.
[0028] The intermediate layer may further include at least one of a hole injection layer, a hole transport layer, an electron transport layer, and an electron injection layer.
[0029] The method may further include forming an encapsulation member that is sequentially disposed on the first passivation layer and the second passivation layer and includes at least one organic layer and at least one inorganic layer.
[0030] According to aspects of the present disclosure, an organic light-emitting display device includes: a first pixel electrode and a second pixel electrode, which are separated from each other on a substrate; a pixel defining layer, which covers ends of the first pixel electrode and the second pixel electrode; a first intermediate layer and a second intermediate layer, which respectively include a first emission layer and a second emission layer arranged as islands on the first pixel electrode and the second pixel electrode; a first pair of electrodes and a second pair of electrodes, which are respectively arranged in an island pattern on the first intermediate layer and the second intermediate layer; a first passivation layer and a second passivation layer, which are respectively arranged in an island pattern on the first pair of electrodes and the second pair of electrodes and completely cover the first pair of electrodes and the second pair of electrodes; and an encapsulation member, which covers the first passivation layer and the second passivation layer.
[0031] The first passivation layer and the second passivation layer may each include a nitride-based material.
[0032] Beneficial Effects
[0033] According to the embodiment, since the intermediate layer including the emission layer is formed through a lift-off process instead of using a fine metal mask, a misalignment problem of the fine metal mask may be prevented and manufacturing costs may be reduced.
[0034] In addition, according to the embodiment, the passivation layer is formed by a vapor deposition method with excellent step coverage, thereby completely covering the counter electrode. Therefore, defects of the light emitting element can be reduced.
[0035] In addition, according to the embodiment, a portion of the passivation layer is dry-etched in the deposition chamber, thereby preventing the counter electrode from being exposed to the atmosphere. Therefore, defects of the light emitting element can be reduced.
[0036] The scope of the present disclosure is not limited by the above-mentioned effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a cross-sectional view of an organic light emitting display device 1 according to an embodiment.
[0038] Figure 2 yes Figure 1 Part of the floor plan.
[0039] Figure 3 1 is a process diagram illustrating a method of manufacturing the organic light emitting display device 1 according to an embodiment.
[0040] Figure 4 is a cross-sectional view illustrating an operation of forming first to third pixel electrodes 101 , 102 , and 103 and a pixel defining layer 110 on a substrate 100 of an organic light emitting display device 1 according to an embodiment.
[0041] Figure 5a to Figure 5f is a cross-sectional view illustrating a first unit process for the organic light emitting display device 1 according to an embodiment.
[0042] Figures 6a to 6f is a cross-sectional view illustrating a second unit process for the organic light emitting display device 1 according to an embodiment.
[0043] Figures 7a to 7f is a cross-sectional view illustrating a third unit process for the organic light emitting display device 1 according to an embodiment.
[0044] Figure 8 yes Figure 5d An enlarged cross-sectional view of region VIII of FIG.
[0045] Fig. 9 yes Figure 5e An enlarged cross-sectional view of region IX.
[0046] Fig.10 is a cross-sectional view of an organic light emitting display device according to another embodiment.
[0047] Fig.11 is a cross-sectional view illustrating an operation of forming first to third pixel electrodes 101 , 102 , and 103 , an auxiliary electrode 120 , and a pixel defining layer 110 on a substrate 100 of an organic light emitting display device 2 according to another embodiment.
[0048] Figures 12a to 12f is a cross-sectional view illustrating a first unit process for an organic light emitting display device 2 according to another embodiment. DETAILED DESCRIPTION
[0049] A method for manufacturing an organic light-emitting display device is provided, the method comprising the following steps: forming a pixel electrode and a pixel defining layer on a substrate, the pixel defining layer covering an edge of the pixel electrode; sequentially forming a stripping layer and a photoresist on the pixel electrode and the pixel defining layer; forming an opening exposing a top surface of the pixel electrode and a portion of the pixel defining layer by patterning the stripping layer and the photoresist; sequentially forming an intermediate layer and a counter electrode in the opening and on the photoresist, the intermediate layer including an emission layer; forming a passivation layer to completely cover the top surface and end of the counter electrode; and removing the stripping layer and the photoresist remaining outside the opening.
[0050] Public Mode
[0051] Since the present disclosure allows various changes and numerous embodiments, specific embodiments will be shown in the drawings and described in the written description. The disclosed effects and features and methods for achieving them will be explained with reference to the embodiments described in detail below with reference to the drawings. However, the disclosure is not limited to the following embodiments and can be implemented in various forms.
[0052] Hereinafter, embodiments will be described with reference to the accompanying drawings, wherein like reference numerals refer to like elements throughout and repeated descriptions thereof will be omitted.
[0053] Although terms such as "first" and "second" may be used to describe various components, such components are not necessarily limited to the above terms. The above terms are used to distinguish one component from another.
[0054] As used herein, the singular forms "a", "an" and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise.
[0055] It will be understood that the terms “comprises,” “comprising,” and / or variations thereof as used herein specify the presence of stated features or components, but do not preclude the addition of one or more other features or components.
[0056] It will also be understood that when a layer, region or component is referred to as being “on” another layer, region or component, it can be directly or indirectly on the other layer, region or component. That is, for example, intervening layers, regions or components may be present.
[0057] For the convenience of explanation, the size of the elements in the drawings may be exaggerated or reduced. For example, since the size and thickness of the elements in the drawings are arbitrarily shown for the convenience of explanation, the disclosure is not limited thereto.
[0058] When the embodiments can be implemented differently, the specific process order can be performed differently from the described order. For example, two consecutively described processes can be performed substantially simultaneously or in the reverse order of the described order.
[0059] It will be understood that when a layer, region, or component is referred to as being "connected" to another layer, region, or component, the layer, region, or component may be "directly connected" to the other layer, region, or component, or may be "indirectly connected" to the other layer, region, or component with other layers, regions, or components interposed therebetween. For example, it will be understood that when a layer, region, or component is referred to as being "electrically connected" to another layer, region, or component, the layer, region, or component may be "directly electrically connected" to the other layer, region, or component, or may be "indirectly electrically connected" to the other layer, region, or component with other layers, regions, or components interposed therebetween.
[0060] Figure 1 is a cross-sectional view of an organic light emitting display device 1 according to an embodiment, Figure 2 yes Figure 1 Part of the floor plan.
[0061] Reference Figure 1 and Figure 2 In the organic light emitting display device 1 according to the present embodiment, a plurality of pixel electrodes are separated from each other on a substrate 100 , and the plurality of pixel electrodes include a first pixel electrode 101 , a second pixel electrode 102 , and a third pixel electrode 103 .
[0062] The pixel defining layer 110 covers ends of the plurality of first to third pixel electrodes 101 , 102 , and 103 , defines an emission region, and prevents an electric field from being concentrated to an end of each pixel electrode.
[0063] The first to third intermediate layers 301, 302, and 303 are respectively arranged on the first to third pixel electrodes 101, 102, and 103, and the first to third intermediate layers 301, 302, and 303 respectively include first to third emission layers (not shown). The first to third counter electrodes 401, 402, and 403 are respectively arranged on the first to third intermediate layers 301, 302, and 303.
[0064] The first to third pixel electrodes 101, 102, and 103, the first to third intermediate layers 301, 302, and 303, and the first to third counter electrodes 401, 402, and 403 all have an island pattern. The island pattern may be a pattern in which a predetermined region is patterned in an island shape to be distinguished from another region near the predetermined region.
[0065] The first to third pixel electrodes 101 , 102 , and 103 and the first to third intermediate layers 301 , 302 , and 303 may each be deposited by physical vapor deposition (PVD).
[0066] The first to third passivation layers 501 , 502 , and 503 , each having an island type pattern, are disposed on the first to third counter electrodes 401 , 402 , and 403 , respectively.
[0067] The first to third passivation layers 501, 502, and 503 may include a material that may be deposited by chemical vapor deposition (CVD) or atomic layer deposition (ALD), which has a step coverage superior to that by physical vapor deposition. In an embodiment, the first to third passivation layers 501, 502, and 503 may include a nitride-based material.
[0068] The first to third passivation layers 501, 502, and 503 may each prevent the first to third intermediate layers 301, 302, and 303 and the first to third counter electrodes 401, 402, and 403 from being degraded during a process by completely covering the first to third intermediate layers 301, 302, and 303 and the first to third counter electrodes 401, 402, and 403. As an example, the first to third passivation layers 501, 502, and 503 may have an area larger than that of the first to third intermediate layers 301, 302, and 303 and the first to third counter electrodes 401, 402, and 403.
[0069] The encapsulation member 700 may be disposed on the first to third passivation layers 501, 502, and 503. The encapsulation member 700 may include at least one organic layer and at least one inorganic layer. Figure 1 A structure is shown in which a first inorganic layer 701 , an organic layer 702 , and a second inorganic layer 703 are sequentially stacked.
[0070] The organic layer 702 may include a polymer-based material such as polymethyl methacrylate (PMMA), polycarbonate (PC), polystyrene (PS), acrylic resin, epoxy resin, polyimide, and polyethylene.
[0071] The first inorganic layer 701 and the second inorganic layer 703 may include aluminum nitride (AlN), aluminum oxide (Al 2 O 3 ), titanium nitride (TiN), titanium oxide (TiO 2 ), silicon oxynitride (SiON), silicon nitride (SiN x ) or silicon oxide (SiO x ).
[0072] The encapsulation member 700 prevents moisture from penetrating, and thus may prevent damage to the organic light emitting element that is susceptible to moisture in cooperation with the first to third passivation layers 501 , 502 , and 503 .
[0073] The first emission layer to the third emission layer (not shown) of the first to third intermediate layers 301, 302, and 303 arranged in the first to third sub-pixels P1, P2, and P3 can emit light having different colors. The first sub-pixel P1 can emit red light, the second sub-pixel P2 can emit green light, and the third sub-pixel P3 can emit blue light. Although the present embodiment shows a case where three sub-pixels are arranged, the embodiment is not limited thereto.
[0074] In the following, reference is made to Figures 3 to 9 A method of manufacturing the organic light emitting display device 1 according to the present embodiment and the organic light emitting display device 1 manufactured by the manufacturing method are described in detail.
[0075] Figure 3 is a process diagram showing a method of manufacturing an organic light emitting display device 1 according to an embodiment, Figure 4 is a cross-sectional view illustrating an operation of forming first to third pixel electrodes 101, 102, and 103 and a pixel defining layer 110 on a substrate 100 of an organic light-emitting display device 1 according to an embodiment,
[0076] Figure 5a to Figure 5f is a cross-sectional view of a first unit process of an organic light emitting display device 1 according to an embodiment, Figures 6a to 6f is a cross-sectional view of a second unit process of the organic light emitting display device 1 according to the embodiment, Figures 7a to 7f is a cross-sectional view of a third unit process of the organic light emitting display device 1 according to the embodiment, Figure 8 yes Figure 5d An enlarged cross-sectional view of region VIII of Fig. 9 yes Figure 5e An enlarged cross-sectional view of region IX.
[0077] Reference Figure 3 According to an embodiment, the method for manufacturing an organic light-emitting display device 1 includes the following steps: forming a pixel electrode and a pixel defining layer on a substrate, the pixel defining layer covering an end portion of the pixel electrode (S10); sequentially forming a lift-off layer and a photoresist on the pixel electrode and the pixel defining layer (S20); forming an opening exposing a top surface of the pixel electrode and a portion of the pixel defining layer by patterning the lift-off layer and the photoresist (S30); sequentially forming an intermediate layer and a counter electrode in the opening and on the photoresist, the intermediate layer including an emission layer (S40); forming a passivation layer to completely cover the top surface and the end portion of the counter electrode (S50); and removing the lift-off layer and the photoresist remaining outside the opening (S60). Here, referring to Figures 4 to 9 Describe the manufacturing method.
[0078] Reference Figure 4 , a plurality of pixel electrodes are formed on a substrate 100 , and the plurality of pixel electrodes include a first pixel electrode 101 , a second pixel electrode 102 , and a third pixel electrode 103 .
[0079] The substrate 100 may be formed by using various materials. As an example, the substrate 100 may include glass or plastic. The plastic may include a material having excellent heat resistance and durability such as polyimide, polyethylene naphthalate, polyethylene terephthalate, polyarylate, polycarbonate, polyetherimide, or polyethersulfone.
[0080] Although Figure 4Although not shown in the figure, a flat surface may be formed on the substrate 100, and a buffer layer (not shown) for blocking penetration of impurity elements may also be formed. As an example, the buffer layer (not shown) may include silicon nitride and / or silicon oxide, and include a single layer or a plurality of layers.
[0081] The first to third pixel electrodes 101 , 102 , and 103 may be formed by forming a conductive material layer (not shown) and then patterning it in an island type.
[0082] The conductive material layer may include a reflective layer and a transparent conductive oxide layer (TCO) located on or below the reflective layer, and the reflective layer includes Mg, Al, Pt, Pd, Au, Ni, Nd, Ir, Cr or a mixture thereof. Optionally, the conductive material layer may include a thin layer including Ag or Al alloy, or include a transparent conductive oxide layer formed on the thin layer. Depending on the conductive material layer, the first pixel electrode to the third pixel electrode 101, 102, 103 may be a reflective electrode or a light-transmitting electrode.
[0083] The pixel defining layer 110 is formed by forming an insulating layer (not shown) on the substrate 100 on which the first to third pixel electrodes 101, 102, and 103 have been formed and patterning the insulating layer. The pixel defining layer 110 covers ends of the first to third pixel electrodes 101, 102, and 103. The pixel defining layer 110 may include an organic insulating material or an inorganic insulating material.
[0084] In an embodiment, the pixel defining layer 110 may include an organic insulating layer including a general polymer such as polymethyl methacrylate (PMMA) or polystyrene (PS), an acrylic polymer, an imide polymer, an aromatic ether polymer, an amide polymer, a fluorine polymer, a paraxylene polymer, a vinyl alcohol polymer, or a blend thereof.
[0085] Although in Figure 4 Although not shown, the first to third pixel electrodes 101, 102, and 103 may be electrically connected to first to third thin film transistors (not shown) disposed between the substrate 100 and the first to third pixel electrodes 101, 102, and 103, respectively.
[0086] Reference Figure 5a ,exist Figure 4 A first lift-off layer LOL1 and a first photoresist PR1 are sequentially formed on the structure.
[0087] The first peeling layer LOL1 may include a non-photosensitive organic material. The first peeling layer LOL1 may include a fluorine-containing polymer. The fluorine-containing polymer included in the first peeling layer LOL1 may be formed by using a polymer including a fluorine content of about 20wt% to about 60wt%. As an example, the fluorine-containing polymer may include at least one of polytetrafluoroethylene, polychlorotrifluoroethylene, polydichlorodifluoroethylene, a copolymer of chlorotrifluoroethylene and dichlorodifluoroethylene, a copolymer of tetrafluoroethylene and perfluoroalkyl vinyl ether, and a copolymer of chlorotrifluoroethylene and perfluoroalkyl vinyl ether. The first peeling layer LOL1 may be formed by methods such as coating, printing, and deposition.
[0088] A first photoresist PR1 is formed on the first lift-off layer LOL1, and a portion of the first photoresist PR1 corresponding to the first pixel electrode 101 is exposed through a first photomask M1 including a light-transmitting portion M11 and a light-blocking portion M12.
[0089] Reference Figure 5b , and develop the first photoresist PR1. The first photoresist PR1 may be one of a positive photoresist and a negative photoresist. In the present embodiment, the first photoresist PR1 as a positive photoresist is described as an example. The developed first photoresist PR1 includes a first opening C1 corresponding to the first pixel electrode 101.
[0090] Reference Figure 5c , by using Figure 5b The patterned first photoresist PR1 is used as an etching mask to etch the first lift-off layer LOL1.
[0091] In the case where the first peeling layer LOL1 includes a fluoropolymer, a solvent that can etch the fluoropolymer is used as an etching solution. The first solvent may include a hydrofluoroether. The hydrofluoroether is an electrochemically stable material due to its low interaction with other materials and an environmentally stable material due to its low global warming coefficient and low toxicity.
[0092] While the first lift-off layer LOL1 is etched during the etching process, a first undercut profile UC1 is formed under the first opening C1 of the first photoresist PR1, and a second opening C2 exposing a top surface of the first pixel electrode 101 and a portion of the pixel defining layer 110 is formed by a first solvent including fluorine. The first undercut profile UC1 is formed, and therefore, a wider deposition space can be secured on the first pixel electrode 101.
[0093] Reference Figure 5d ,exist Figure 5c A first intermediate layer 301, a first counter electrode 401 and a first passivation layer 501 are formed on the structure, and the first intermediate layer 301 includes a first emission layer (not shown).
[0094] The first intermediate layer 301, the first counter electrode 401 and the first passivation layer 501 are formed by vacuum deposition. A deposition source (not shown) is arranged in the first chamber CH1, and deposition is performed by adjusting a deposition incident angle so that a material emitted from the deposition source (not shown) is incident toward the substrate 100.
[0095] The first intermediate layer 301 may further include at least one of a hole injection layer, a hole transport layer, an electron transport layer, and an electron injection layer in addition to the first emission layer (not shown).
[0096] The first pair of electrodes 401 may be a light-transmitting electrode or a reflective electrode. In an embodiment, the first pair of electrodes 401 may be a metal film or a metal thick layer including at least one of Ag, Mg, Al, Yb, Ca, Li, and Au. The first pair of electrodes 401 covers the first intermediate layer 301 and thus may be used as a protective layer to protect the first intermediate layer 301 that is susceptible to moisture and oxygen.
[0097] The first intermediate layer 301 and the first counter electrode 401 are deposited on a top surface of the first pixel electrode 101 disposed in the second opening C2 and a portion of an end of the pixel defining layer 110 , and are also stacked on the first photoresist PR1 .
[0098] The first intermediate layer 301 and the first counter electrode 401 may be deposited by physical vapor deposition (PVD). In an embodiment, the first intermediate layer 301 may be deposited in the first chamber CH1 by one of sputtering, thermal evaporation, electron beam evaporation, laser molecular beam epitaxy, and pulsed laser deposition. The first counter electrode 401 is formed to cover the first intermediate layer 301 by adjusting a deposition incident angle, chamber pressure, temperature, reaction gas, etc. in the first chamber CH1.
[0099] The first passivation layer 501 is formed to completely cover the top surface and the end of the first pair of electrodes 401. The first passivation layer 501 may be deposited by a chemical vapor deposition (CVD) process or an atomic layer deposition (ALD) process, which has a step coverage superior to that of physical vapor deposition. In an embodiment, the first passivation layer 501 may be deposited by one of thermal CVD, plasma CVD, metal-organic chemical vapor deposition (MOCVD), and hydride vapor phase epitaxy (HVPE).
[0100] As a result of CVD or ALD, the first passivation layer 501 is also stacked on the first photoresist PR1. In addition, in the region where the first undercut profile UC1 is formed, the first passivation layer 501 is also deposited on the bottom surface of the first photoresist PR1, the top surface of the pixel defining layer 110, and the side surface of the first lift-off layer LOL1.
[0101] Reference as Figure 5d Magnified view of region VIII Figure 8 , around the area in which the first undercut profile UC1 has been formed, the thickness D2 of the first passivation layer 501 deposited on the bottom surface of the first photoresist PR1, the top surface of the pixel defining layer 110, and the side surface of the first peeling layer LOL1 is thinner than the thickness D1 of the first passivation layer 501 deposited on the top surface of the first pair of electrodes 401 and the thickness D3 of the first passivation layer 501 deposited on the top surface of the first peeling layer LOL1.
[0102] Reference Figure 5e ,right Figure 5d As a result of the dry etching process, the first passivation layer 501 is etched and removed around the region in which the first undercut profile UC1 has been formed.
[0103] Reference as Figure 5e Magnified view of area IX Fig. 9 , showing that the thickness of the first passivation layer 501 is reduced. Figure 8 The thickness D1' of the first passivation layer 501 deposited on the top surface of the first pair of electrodes 401 and the thickness D3' of the first passivation layer 501 deposited on the top surface of the first peeling layer LOL1 are reduced when compared. Around the area where the first undercut profile UC1 has been formed, the thickness D2' of the first passivation layer 501 deposited on the bottom surface of the first photoresist PR1, the top surface of the pixel defining layer 110, and the side surface of the first peeling layer LOL1 is reduced and completely removed when compared to the thickness before the dry etching process is performed.
[0104] Reference Figure 5f ,right Figure 5e The lift-off process is performed outside the first chamber CH1. In an embodiment, the lift-off process may be performed in the atmosphere at room temperature.
[0105] In the case where the first peeling layer LOL1 includes a fluorine-containing polymer, the first peeling layer LOL1 can be removed by using a second solvent including fluorine. Since the peeling process is performed after forming the first intermediate layer 301 including the first emission layer (not shown), it is preferred to use a material having low reactivity with the first intermediate layer 301 as the second solvent. Similar to the first solvent, the second solvent may include hydrofluoroether.
[0106] As a result of the lift-off, the first intermediate layer 301 , the first counter electrode 401 , and the first passivation layer 501 disposed on the first pixel electrode 101 remain as a pattern.
[0107] In the present embodiment, since the first passivation layer 501 is formed by a deposition method with large step coverage, the first passivation layer 501 completely covers the first counter electrode 401 and thus protects the first counter electrode 401 and the first intermediate layer 301 which may be damaged during the stripping process which is a wet process.
[0108] As a result of performing a deposition process with large step coverage, the first passivation layer 501 deposited around an area where a first undercut profile UC1 has been formed (e.g., area A1 where the bottom surface of the first peeling layer LOL1 intersects the top surface of the pixel defining layer 110) may be an obstacle to the peeling process.
[0109] However, in the present embodiment, dry etching as an isotropic etching method may be performed to remove the first passivation layer 501 in the relevant region A1, and then a lift-off process may be performed.
[0110] In addition, in the case where the dry etching process is performed in the first chamber CH1 where deposition has been performed, damage to the organic light emitting display device 1 due to the atmosphere and moisture outside the first chamber CH1 can be prevented. Figure 5d , Figure 5e , Figure 8 and Fig. 9 A case where deposition and dry etching are performed in the same first chamber CH1 is shown, but the embodiment is not limited thereto. Dry etching may be performed in a subsequent chamber (not shown) different from the first chamber CH1.
[0111] Hereinafter, the second unit process is described, and the same description as that of the first unit process may be omitted.
[0112] Reference Figure 6a ,exist Figure 5f A second lift-off layer LOL2 and a second photoresist PR2 are sequentially formed on the structure.
[0113] The second peeling layer LOL2 may include the same material as that of the first peeling layer LOL1. The second peeling layer LOL2 may be formed by a method such as coating, printing, deposition, or the like.
[0114] A second photoresist PR2 is formed on the second lift-off layer LOL2, and a portion of the second photoresist PR2 corresponding to the second pixel electrode 102 is exposed through a second photomask M2 including a light-transmitting portion M21 and a light-blocking portion M22.
[0115] Reference Figure 6b , and the second photoresist PR2 is developed. The developed second photoresist PR2 includes a third opening C3 corresponding to the second pixel electrode 102 .
[0116] Reference Figure 6c , by using Figure 6b The patterned second photoresist PR2 is used as an etching mask to etch the second lift-off layer LOL2.
[0117] In the case where the second peeling layer LOL2 includes a fluorine-containing polymer, a solvent that can etch the fluorine-containing polymer is used as the etching liquid. The first solvent may include hydrofluoroether.
[0118] While etching the second lift-off layer LOL2 during the etching process, a second undercut profile UC2 is formed under the third opening C3 of the second photoresist PR2, and a fourth opening C4 exposing a top surface of the second pixel electrode 102 and a portion of the pixel defining layer 110 is formed by a first solvent including fluorine. The second undercut profile UC2 is formed, and therefore, a wider deposition space can be secured on the second pixel electrode 102.
[0119] Reference Figure 6d ,exist Figure 6c A second intermediate layer 302, a second counter electrode 402 and a second passivation layer 502 are formed on the structure, and the second intermediate layer 302 includes a second emission layer (not shown).
[0120] The second intermediate layer 302, the second counter electrode 402 and the second passivation layer 502 are formed by vacuum deposition. A deposition source (not shown) is arranged in the second chamber CH2, and deposition is performed by adjusting a deposition incident angle so that a material emitted from the deposition source (not shown) is incident toward the substrate 100.
[0121] The second intermediate layer 302 may further include at least one of a hole injection layer, a hole transport layer, an electron transport layer, and an electron injection layer in addition to the second emission layer (not shown).
[0122] The second counter electrode 402 may be a light-transmitting electrode or a reflective electrode. The second counter electrode 402 covers the second intermediate layer 302 and thus may serve as a protective layer for protecting the second intermediate layer 302 that is susceptible to moisture and oxygen.
[0123] The second passivation layer 502 is formed to completely cover the top surface and end portions of the second counter electrode 402 .
[0124] Similar to the first unit process, the second intermediate layer 302 and the second counter electrode 402 may be deposited by a PVD process, and the second passivation layer 502 may be deposited by a CVD process or an ALD process having excellent step coverage compared to the PVD process.
[0125] As a result of the deposition, the second intermediate layer 302 , the second counter electrode 402 , and the second passivation layer 502 are deposited on a top surface of the second pixel electrode 102 disposed in the fourth opening C4 and a portion of an end of the pixel defining layer 110 , and are also stacked on the second photoresist PR2 .
[0126] In the region where the second undercut profile UC2 has been formed, a second passivation layer 502 is deposited on the bottom surface of the second photoresist PR2, the top surface of the pixel defining layer 110, and the side surface of the second lift-off layer LOL2.
[0127] Reference Figure 6e ,right Figure 6d As a result of the dry etching process, the second passivation layer 502 is etched and removed around the region in which the second undercut profile UC2 has been formed.
[0128] Reference Figure 6f ,right Figure 6e The stripping process is performed outside the second chamber CH2. In an embodiment, the stripping process may be performed in the atmosphere at room temperature.
[0129] In the case where the second peeling layer LOL2 includes a fluorine-containing polymer, the second peeling layer LOL2 can be removed by using a second solvent including fluorine. Since the peeling process is performed after forming the second intermediate layer 302 including the second emission layer (not shown), it is preferred to use a material having low reactivity with the second intermediate layer 302 as the second solvent. Similar to the first solvent, the second solvent may include a hydrofluoroether.
[0130] As a result of the lift-off, the second intermediate layer 302 , the second counter electrode 402 , and the second passivation layer 502 disposed on the second pixel electrode 102 remain as a pattern.
[0131] Although Figure 6d and Figure 6e A case where deposition and dry etching are performed in the same second chamber CH2 is shown, but the embodiment is not limited thereto. Dry etching may be performed in a subsequent chamber (not shown) different from the second chamber CH2.
[0132] Hereinafter, the third unit process is described. The same description as that of the first unit process and the second unit process may be omitted.
[0133] Reference Figure 7a ,exist Figure 6f A third lift-off layer LOL3 and a third photoresist PR3 are sequentially formed on the structure.
[0134] The third peeling layer LOL3 may include the same material as the first peeling layer LOL1 and the second peeling layer LOL2. The third peeling layer LOL3 may be formed by a method such as coating, printing, deposition, or the like.
[0135] A third photoresist PR3 is formed on the third peeling layer LOL3, and a portion of the third photoresist PR3 corresponding to the third pixel electrode 103 is exposed through a third photomask M3 including a light-transmitting portion M31 and a light-blocking portion M32.
[0136] Reference Figure 7b , and the third photoresist PR3 is developed. The developed third photoresist PR3 includes a fifth opening C5 corresponding to the third pixel electrode 103 .
[0137] Reference Figure 7c , by using Figure 7b The patterned third photoresist PR3 is used as an etching mask to etch the third lift-off layer LOL3.
[0138] In the case where the third peeling layer LOL3 includes a fluorine-containing polymer, a solvent that can etch the fluorine-containing polymer is used as an etching solution. The first solvent may include hydrofluoroether.
[0139] While the third lift-off layer LOL3 is etched during the etching process, a third undercut profile UC3 is formed under the fifth opening C5 of the third photoresist PR3, and a sixth opening C6 exposing a top surface of the third pixel electrode 103 and a portion of the pixel defining layer 110 is formed by a first solvent including fluorine. The third undercut profile UC3 is formed, and therefore, a wider deposition space can be ensured on the third pixel electrode 103.
[0140] Reference Figure 7d ,exist Figure 7c A third intermediate layer 303, a third counter electrode 403 and a third passivation layer 503 are formed on the structure, and the third intermediate layer 303 includes a third emission layer (not shown).
[0141] The third intermediate layer 303, the third counter electrode 403 and the third passivation layer 503 are formed by vacuum deposition. A deposition source (not shown) is arranged in the third chamber CH3, and deposition is performed by adjusting a deposition incident angle so that a material emitted from the deposition source (not shown) is incident toward the substrate 100.
[0142] The third intermediate layer 303 may further include at least one of a hole injection layer, a hole transport layer, an electron transport layer, and an electron injection layer in addition to the third emission layer (not shown).
[0143] The third counter electrode 403 may be a light-transmitting electrode or a reflective electrode. The third counter electrode 403 covers the third intermediate layer 303 and thus may function as a protective layer for protecting the third intermediate layer 303 that is susceptible to moisture and oxygen.
[0144] The third passivation layer 503 is formed to completely cover the top surface and end portions of the third counter electrode 403 .
[0145] Similar to the first and second unit processes, the third intermediate layer 303 and the third counter electrode 403 may be deposited by a PVD process, and the third passivation layer 503 may be deposited by a CVD process or an ALD process having excellent step coverage compared to the PVD process.
[0146] As a result of the deposition, the third intermediate layer 303 , the third counter electrode 403 , and the third passivation layer 503 are deposited on a top surface of the third pixel electrode 103 disposed in the sixth opening C6 and a portion of an end of the pixel defining layer 110 , and also on the third photoresist PR3 .
[0147] In the region where the third undercut profile UC3 has been formed, a third passivation layer 503 is deposited on the bottom surface of the third photoresist PR3, the top surface of the pixel defining layer 110, and the side surface of the third lift-off layer LOL3.
[0148] Reference Figure 7e ,right Figure 7d As a result of the dry etching process, the third passivation layer 503 is etched and removed around the region in which the third undercut profile UC3 has been formed.
[0149] Reference Figure 7f ,right Figure 7e The stripping process is performed outside the third chamber CH3. In an embodiment, the stripping process may be performed in the atmosphere at room temperature.
[0150] In the case where the third peeling layer LOL3 includes a fluorine-containing polymer, the third peeling layer LOL3 can be removed by using a third solvent including fluorine. Since the peeling process is performed after forming the third intermediate layer 303 including the third emission layer (not shown), it is preferred that a material having low reactivity with the third intermediate layer 303 is used as the third solvent. Similar to the first solvent, the third solvent may include hydrofluoroether.
[0151] As a result of the lift-off, the third intermediate layer 303 , the third counter electrode 403 , and the third passivation layer 503 disposed on the third pixel electrode 103 remain as a pattern.
[0152] Although Figure 7d and Figure 7eA case where deposition and dry etching are performed in the same third chamber CH3 is shown, but the embodiment is not limited thereto. Dry etching may be performed in a subsequent chamber (not shown) different from the third chamber CH3.
[0153] The encapsulation member 700 may be disposed on the first to third passivation layers 501, 502, and 503. The encapsulation member 700 may include at least one organic layer and at least one inorganic layer. Figure 1 A structure is shown in which a first inorganic layer 701 , an organic layer 702 , and a second inorganic layer 703 are sequentially stacked.
[0154] After performing the first to third unit processes, an encapsulation member 700 (see FIG. 1 ) covering all of the top surfaces of the first to third passivation layers 501, 502, and 503 is disposed. Figure 1 ).
[0155] The encapsulation member 700 prevents moisture from penetrating, and thus may prevent damage to the organic light emitting element that is susceptible to moisture in cooperation with the first to third passivation layers 501 , 502 , and 503 .
[0156] As described above, in the present embodiment, since the first to third passivation layers 501, 502, and 503 are formed by a deposition method with large step coverage, the first to third passivation layers 501, 502, and 503 completely cover the first to third pairs of electrodes 401, 402, and 403, thereby protecting the first to third pairs of electrodes 401, 402, and 403 and the first to third intermediate layers 301, 302, and 303 which may be damaged during the stripping process which is a wet process.
[0157] In the following, reference is made to Figure 10 to Figure 12f An organic light emitting display device 2 and a method of manufacturing the same according to another embodiment are described.
[0158] Fig.10 is a cross-sectional view of an organic light emitting display device 2 according to another embodiment, Fig.11 is a cross-sectional view showing an operation of forming first to third pixel electrodes 101, 102, and 103, an auxiliary electrode 120, and a pixel defining layer 110 on a substrate 100 of an organic light-emitting display device 2 according to another embodiment, Figures 12a to 12f is a cross-sectional view of a first unit process of an organic light emitting display device 2 according to another embodiment.
[0159] Reference Fig.10In an organic light-emitting display device 2 according to another embodiment, a plurality of pixel electrodes are separated from each other on a substrate 100, and the plurality of pixel electrodes include a first pixel electrode 101, a second pixel electrode 102, and a third pixel electrode 103. A pixel defining layer 110 covers ends of the plurality of first to third pixel electrodes 101, 102, and 103, prevents an electric field from being concentrated at an end of each pixel electrode, and defines an emission region.
[0160] Different from the previous embodiment, in the present embodiment, the auxiliary electrode 120 is disposed on the pixel defining layer 110 , and the auxiliary electrode 120 is separated from the first to third pixel electrodes 101 , 102 , and 103 .
[0161] The first to third intermediate layers 301, 302, and 303 including the first to third emission layers (not shown) are respectively arranged on the first to third pixel electrodes 101, 102, and 103. The first to third counter electrodes 401, 402, and 403 are respectively arranged on the first to third intermediate layers 301, 302, and 303.
[0162] The first to third pixel electrodes 101 , 102 , and 103 , the first to third intermediate layers 301 , 302 , and 303 , and the first to third counter electrodes 401 , 402 , and 403 may all have an island type pattern.
[0163] In the present embodiment, the first to third pair of electrodes 401 , 402 , and 403 may extend on the pixel defining layer 110 to contact the auxiliary electrode 120 , respectively.
[0164] Although not shown in the drawings, the auxiliary electrode 120 is electrically connected to a common power voltage, and the common power voltage is applied to the first to third pairs of electrodes 401, 402, and 403, all of which contact the auxiliary electrode 120. When a driving current is transmitted from a driving thin film transistor (not shown) to the first to third pixel electrodes 101, 102, and 103 and the common power voltage is applied to the first to third pairs of electrodes 401, 402, and 403 through the auxiliary electrode 120, the first to third emission layers (not shown) emit light.
[0165] The first to third passivation layers 501 , 502 , and 503 are disposed on the first to third counter electrodes 401 , 402 , and 403 .
[0166] The first passivation layer 501 completely covers the first counter electrode 401 and extends on the auxiliary electrode 120, so that an end of the first passivation layer 501 contacts the top surface of the auxiliary electrode 120. The second passivation layer 502 completely covers the second counter electrode 402 and extends on the auxiliary electrode 120, so that an end of the second passivation layer 502 contacts the top surface of the auxiliary electrode 120. The third passivation layer 503 completely covers the third counter electrode 403 and extends on the auxiliary electrode 120, so that an end of the third passivation layer 503 contacts the top surface of the auxiliary electrode 120.
[0167] The first to third passivation layers 501 , 502 , and 503 respectively and completely cover the first to third intermediate layers 301 , 302 , and 303 and the first to third counter electrodes 401 , 402 , and 403 , thereby preventing damage to the organic light emitting element during a patterning process.
[0168] Similar to the previous embodiment, in the present embodiment, the first to third pixel electrodes 101, 102, and 103 are separated from each other in an island shape. The first to third intermediate layers 301, 302, and 303 may be arranged in an island shape on the first to third pixel electrodes 101, 102, and 103. In addition, similar to the previous embodiment, the first to third passivation layers 501, 502, and 503 covering the first to third counter electrodes 401, 402, and 403 may be arranged in an island shape.
[0169] The encapsulation member 700 covering all of the top surfaces of the first to third passivation layers 501 , 502 , and 503 and the auxiliary electrode 120 is disposed.
[0170] The encapsulation member 700 may include at least one organic layer and at least one inorganic layer. Fig.10 A structure is shown in which a first inorganic layer 701 , an organic layer 702 , and a second inorganic layer 703 are sequentially stacked.
[0171] The differences between the process of this embodiment and the process of the previous embodiment are mainly described.
[0172] Reference Fig.11 , a plurality of pixel electrodes including a first pixel electrode 101, a second pixel electrode 102, and a third pixel electrode 103 are formed, a pixel defining layer 110 covering ends of the first to third pixel electrodes 101, 102, and 103 is formed, and an auxiliary electrode 120 is formed on the pixel defining layer 110. Patterning of the first to third pixel electrodes 101, 102, and 103, the pixel defining layer 110, and the auxiliary electrode 120 may be performed by a photolithography process.
[0173] Reference Fig.12a ,exist Fig.11A first lift-off layer LOL1 and a first photoresist PR1 are sequentially formed on the structure.
[0174] The first peeling layer LOL1 may be formed by a method such as coating, printing, and deposition.
[0175] A first photoresist PR1 is formed on the first lift-off layer LOL1, and a portion of the first photoresist PR1 corresponding to the first pixel electrode 101 is exposed through a first photomask M1 including a light-transmitting portion M11 and a light-blocking portion M12.
[0176] Reference Figure 12b , and the first photoresist PR1 is developed. The developed first photoresist PR1 includes a first opening C1 corresponding to the first pixel electrode 101 .
[0177] Reference Fig.12c , by using Figure 12b The patterned first photoresist PR1 is used as an etching mask to etch the first lift-off layer LOL1.
[0178] In the case where the first peeling layer LOL1 includes a fluorine-containing polymer, a solvent that can etch the fluorine-containing polymer is used as an etching solution. The first solvent may include hydrofluoroether.
[0179] While the first lift-off layer LOL1 is etched during the etching process, a first undercut profile UC1 is formed under the first opening C1 of the first photoresist PR1, and a second opening C2 exposing the top surface of the first pixel electrode 101, a portion of the auxiliary electrode 120, and a portion of the pixel defining layer 110 is formed by a first solvent including fluorine. The first undercut profile UC1 is formed, and therefore, a wider deposition space can be secured on the first pixel electrode 101.
[0180] Reference Fig.12d ,exist Fig.12c The first intermediate layer 301, the first counter electrode 401 and the first passivation layer 501 are formed on the structure, and the first intermediate layer 301 includes a first emission layer (not shown). The first intermediate layer 301 may also include at least one of a hole injection layer, a hole transport layer, an electron transport layer and an electron injection layer.
[0181] The first intermediate layer 301, the first counter electrode 401 and the first passivation layer 501 are formed by vacuum deposition. A deposition source (not shown) is arranged in the first chamber CH1, and deposition is performed by adjusting a deposition incident angle so that a deposition material emitted from the deposition source (not shown) is incident toward the substrate 100.
[0182] The first intermediate layer 301 is stacked on a top surface of the first pixel electrode 101 and a portion of the pixel defining layer 110 .
[0183] The first counter electrode 401 is stacked to contact top surfaces of the first intermediate layer 301 , the pixel defining layer 110 , and the auxiliary electrode 120 .
[0184] The first passivation layer 501 is stacked to contact top surfaces of the first counter electrode 401 and the auxiliary electrode 120 .
[0185] Similar to the previous embodiment, the first intermediate layer 301 and the first counter electrode 401 may be deposited by a PVD process, and the first passivation layer 501 may be deposited by a CVD process or an ALD process having excellent step coverage compared to a PVD process.
[0186] As a result of the deposition, the first intermediate layer 301 , the first counter electrode 401 , and the first passivation layer 501 are deposited on the top surface of the first pixel electrode 101 disposed in the second opening C2 , and are also stacked on the first photoresist PR1 .
[0187] In the region where the first undercut profile UC1 has been formed, a first passivation layer 501 is deposited on the bottom surface of the first photoresist PR1, the top surface of the auxiliary electrode 120, and the side surface of the first lift-off layer LOL1.
[0188] Reference Fig.12e ,right Fig.12d As a result of the dry etching process, the first passivation layer 501 is etched and removed around the region in which the first undercut profile UC1 has been formed.
[0189] Reference Fig.12f ,right Fig.12e The lift-off process is performed outside the first chamber CH1. In an embodiment, the lift-off process may be performed in the atmosphere at room temperature.
[0190] As a result of the lift-off, the first intermediate layer 301 is disposed on the first pixel electrode 101. The first counter electrode 401 covering the first intermediate layer contacts the auxiliary electrode 120 disposed on the pixel defining layer 110. The first passivation layer 501 covering a portion of the first counter electrode 401 and the auxiliary electrode 120 remains.
[0191] Although Fig.12d and Fig.12e A case where deposition and dry etching are performed in the same first chamber CH1 is shown, but the embodiment is not limited thereto. Dry etching may be performed in a subsequent chamber (not shown) different from the first chamber CH1.
[0192] Compared with the previous embodiment, the first pair of electrodes 401 are connected to the auxiliary electrode 120, and thus the resistance of the common electrode is reduced.
[0193] In this embodiment, similar to the previous embodiment, a full-color organic light-emitting display device can be manufactured by forming an intermediate layer, a counter electrode, and a passivation layer on the second pixel electrode 102 and the third pixel electrode 103 through the second unit process and the third unit process. Since the process similar to the previous embodiment is repeated, its description is omitted.
[0194] As described above, in the organic light-emitting display device 2 according to the present embodiment, since the passivation layer is formed by a deposition method with large step coverage, the passivation layer completely covers the counter electrode, and thus protects the intermediate layer and the counter electrode during the stripping process. Dry etching is performed in the same chamber, and thus damage due to the atmosphere and moisture outside the chamber can be prevented. In addition, an auxiliary electrode is formed, and thus a voltage drop of the common electrode can be prevented.
[0195] Although the present disclosure has been described with reference to the embodiments shown in the drawings, this is provided for descriptive purposes only, and persons skilled in the art will appreciate that various changes in form and details may be made therefrom. Therefore, the scope of the present disclosure should be determined by the claims.
Claims
1. A method for manufacturing an organic light emitting display device, the method The following steps are involved: forming a pixel electrode and a pixel defining layer on a substrate, wherein the pixel defining layer covers an edge of the pixel electrode; sequentially forming a lift-off layer and a photoresist on the pixel electrode and the pixel defining layer; patterning the lift-off layer and the photoresist to form an opening exposing a top surface of the pixel electrode and a portion of the pixel defining layer; sequentially forming an intermediate layer and a counter electrode in the opening and on the photoresist, the intermediate layer including an emission layer; forming a passivation layer on the top surface and the end of the counter electrode, on the top surface of the pixel defining layer, on the side surface of the lift-off layer, and on the bottom surface of the photoresist to completely cover the top surface and the end of the counter electrode; as well as removing the lift-off layer and the photoresist remaining outside the opening, The step of forming the intermediate layer includes a first deposition process including a physical vapor deposition process, The step of forming the counter electrode includes a second deposition process including a physical vapor deposition process, and The step of forming the passivation layer includes a third deposition process including a chemical vapor deposition process or an atomic layer deposition process so that a step coverage for the passivation layer is greater than a step coverage for the intermediate layer and the counter electrode.
2. The method according to claim 1, in, The step of patterning the photoresist includes a photolithography process.
3. The method according to claim 1, in, The release layer includes a fluoropolymer.
4. The method according to claim 3, in, The opening is formed by etching the lift-off layer using a first solvent including fluorine.
5. The method according to claim 1, in, The first to third deposition processes are performed in the same chamber.
6. The method according to claim 1, in, After the third deposition process, dry etching is performed in the same chamber as the chamber in which the third deposition process is performed or in a chamber different from the chamber in which the third deposition process is performed.
7. The method according to claim 6, in, A top surface of the pixel defining layer is exposed by the dry etching.
8. The method according to claim 1, further comprising: The following steps are involved: forming an auxiliary electrode on the pixel defining layer, Wherein, the counter electrode is formed to contact the auxiliary electrode.
9. The method according to claim 8, in, After the step of forming the passivation layer, dry etching is performed in the same chamber as the chamber in which the passivation layer is formed or in a chamber different from the chamber in which the passivation layer is formed, and A top surface of the auxiliary electrode is exposed by the dry etching.
10. The method according to claim 1, in, The remaining release layer is removed by using a second solvent including fluorine.
11. The method according to claim 1, in, vacuum depositing the intermediate layer, the counter electrode and the passivation layer in a chamber, and The step of removing the release layer is performed outside the chamber in the atmosphere.
12. The method according to claim 11, in, The passivation layer is exposed in the wet process of removing the lift-off layer, and the passivation layer completely covers the top surface and end portions of the counter electrode.
13. A method for manufacturing an organic light emitting display device, the method The following steps are involved: After forming a first pixel electrode and a second pixel electrode on a substrate and forming a pixel defining layer covering ends of the first pixel electrode and the second pixel electrode, performing a first unit operation including the following operations (a1) to (a5): (a1) sequentially forming a first lift-off layer and a first photoresist on the first pixel electrode, the second pixel electrode and the pixel defining layer; (a2) patterning the first stripping layer and the first photoresist to form a first opening exposing a top surface of the first pixel electrode and a portion of the pixel defining layer; (a3) sequentially forming a first intermediate layer and a first pair of electrodes in the first opening and on the first photoresist, the first intermediate layer including a first emission layer; (a4) forming a first passivation layer on a top surface and ends of the first pair of electrodes, on a top surface of the pixel defining layer, on a side surface of the first stripping layer, and on a bottom surface of the first photoresist to cover the top surface and ends of the first pair of electrodes; and (a5) removing the first lift-off layer and the first photoresist remaining outside the first opening, wherein the step of forming the first intermediate layer and the first pair of electrodes comprises a physical vapor deposition process, and the step of forming the first passivation layer comprises a chemical vapor deposition process or an atomic layer deposition process, so that the step coverage for the first passivation layer is greater than the step coverage for the first intermediate layer and the first pair of electrodes; and After the first unit operation, a second unit operation including the following operations (b1) to (b5) is performed: (b1) a second lift-off layer and a second photoresist are sequentially formed on the first passivation layer, the second pixel electrode and the pixel defining layer; (b2) the second lift-off layer and the second photoresist are patterned to form a second opening exposing a top surface of the second pixel electrode and a portion of the pixel defining layer; (b3) a second intermediate layer and a second pair of electrodes are sequentially formed in the second opening and on the second photoresist, the second intermediate layer including a second emission layer; (b4) a second stripping layer is formed on the top surface of the second pair of electrodes; and ends, on the top surface of the pixel defining layer, on the side surfaces of the second peeling layer and on the bottom surface of the second photoresist to completely cover the top surface and ends of the second pair of electrodes; and (b5) removing the second peeling layer and the second photoresist remaining outside the second opening, wherein the step of forming the second intermediate layer and the second pair of electrodes includes a physical vapor deposition process, and the step of forming the second passivation layer includes a chemical vapor deposition process or an atomic layer deposition process, so that the step coverage for the second passivation layer is larger than the step coverage for the second intermediate layer and the second pair of electrodes.
14. The method according to claim 13, in, A color emitted from the first emission layer is different from a color emitted from the second emission layer.
15. The method according to claim 13, in, The first intermediate layer, the first counter electrode, and the first passivation layer are formed in a first chamber.
16. The method according to claim 15, further comprising: The following steps are involved: After the step of forming the first passivation layer, dry etching is performed in the first chamber.
17. The method according to claim 15, further comprising: The following steps are involved: After the step of forming the first passivation layer, dry etching is performed in a subsequent chamber different from the first chamber.
18. The method according to claim 13, in, The first intermediate layer and the second intermediate layer further include at least one of a hole injection layer, a hole transport layer, an electron transport layer, and an electron injection layer.
19. The method according to claim 13, further comprising: The following steps are involved: An encapsulation member sequentially disposed on the first passivation layer and the second passivation layer and including at least one organic layer and at least one inorganic layer is formed.
20. An organic light-emitting display device manufactured by the method according to any one of claims 13 to 19, the organic light-emitting display device include: The first pixel electrode and the second pixel electrode are separated from each other on the substrate; The pixel defining layer covers the ends of the first pixel electrode and the second pixel electrode; The first intermediate layer and the second intermediate layer respectively include the first emission layer and the second emission layer arranged as islands on the first pixel electrode and the second pixel electrode; The first pair of electrodes and the second pair of electrodes are arranged in an island pattern on the first intermediate layer and the second intermediate layer, respectively; The first passivation layer and the second passivation layer are respectively arranged on the first pair of electrodes and the second pair of electrodes in an island pattern and completely cover the first pair of electrodes and the second pair of electrodes; as well as A packaging component covers the first passivation layer and the second passivation layer.
21. The device according to claim 20, in, The first passivation layer and the second passivation layer each include a nitride-based material.
Citation Information
Patent Citations
Organic light-emitting display device and method of manufacturing the same
CN107516665A
Organic Light-Emitting Display Apparatus And Method Of Manufacturing The Same
CN107680985A
Organic light-emitting display device and manufacturing method thereof
CN108074953A
Method for covering step part of semiconductor device and semiconductor device using it
JP2001284734A
Display device and organic light emitting display device
US20140145152A1