A fatigue test device in a high-temperature liquid lead-bismuth environment and a method of use

By designing a fatigue test device in a high-temperature liquid lead-bismuth environment, the shortcomings of the fatigue behavior research of metal materials in a high-temperature liquid lead-bismuth environment in the existing technology are solved, and effective evaluation and research on the fatigue properties of metal materials are achieved, ensuring lead Safety and performance of cold fast reactor equipment materials.

CN113203644BActive Publication Date: 2024-11-22INST OF METAL RESEARCH - CHINESE ACAD OF SCI +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110408480.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-16
Publication Date
2024-11-22
Estimated Expiration
2041-04-16

AI Technical Summary

Technical Problem

The prior art has not yet effectively studied the fatigue behavior and embrittlement damage of metal materials in high-temperature liquid lead-bismuth environments, and the relevant test technology is immature, which limits the service performance and safety of lead-cold fast reactor equipment materials.

Method used

A fatigue testing device in a high-temperature liquid lead-bismuth environment is designed, including a fatigue testing machine, loading shaft, sample rack, fatigue kettle, heater, strain measurement system, conduction tube, etc., through load, temperature control and strain measurement , realize fatigue test of metal materials in liquid lead-bismuth environment.

Benefits of technology

The device can record and collect parameters such as temperature, dissolved oxygen concentration, displacement, load, strain and other real-time, evaluate the fatigue performance of metal materials in high-temperature liquid lead-bismuth environments, and is simple to operate and does not contact lead-bismuth steam. It is suitable for studying metal materials Fatigue life and creep performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003023237150000011
    Figure HDA0003023237150000011
Patent Text Reader

Abstract

The present invention relates to the field of fatigue testing, and specifically to a fatigue testing device and a method for using it in a high-temperature liquid lead-bismuth environment, which is suitable for fatigue performance and creep performance testing of fatigue specimens in a liquid lead-bismuth environment. The device includes a fatigue testing machine, a loading shaft, a specimen rack, a fatigue specimen, a support rod, a fatigue kettle, a heater, a strain measurement system, a dissolved oxygen electrode, a conduction pipe, and a storage kettle. When the fatigue kettle, the storage kettle, and the conduction pipe are greater than 250°C, high-purity argon or high-purity nitrogen is passed through an air inlet pipe of the storage kettle to allow the liquid lead-bismuth alloy in the storage kettle to flow into the fatigue kettle, and high-purity argon or high-purity nitrogen is passed through an air inlet pipe of the fatigue kettle to allow the liquid lead-bismuth alloy in the fatigue kettle to flow into the storage kettle, thereby realizing the mutual transfer of high-temperature liquid lead-bismuth alloy in the fatigue kettle and the storage kettle. The present invention can accurately control the test parameters such as temperature, strain rate, and load of the liquid lead-bismuth alloy, and evaluate the fatigue performance of metal materials in a high-temperature liquid lead-bismuth environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fatigue testing, in particular to a fatigue testing device in a high-temperature liquid lead-bismuth environment and a use method thereof, which is suitable for fatigue performance and creep performance testing of fatigue specimens in a liquid lead-bismuth environment. Background Art

[0002] Due to its high boiling point, no heat release from reaction with water or air, strong transmutation ability and excellent neutron economy, lead or lead-bismuth eutectic is the preferred coolant for special reactor types such as the fourth-generation commercial lead-cooled fast reactor and accelerator-driven advanced nuclear energy system, as well as future space reactors and small reactors. It has broad application prospects and is currently a hot topic in international research. The operating temperature of the lead-bismuth reactor is as high as 450-550℃, and the service performance and safety of its equipment materials are key. The corrosion performance of metal materials in a high-temperature liquid lead-bismuth environment is one of the key issues restricting the development of lead-cooled fast reactors. Structural materials serving in the fourth-generation lead-cooled fast reactor are not only corroded by liquid lead-bismuth, but also bear loads during service. Mechanical and chemical interactions may accelerate material failure. It is necessary to study the mechanical properties of structural materials in a liquid lead-bismuth environment. Under fatigue loads, the fatigue life of metal materials in a liquid lead-bismuth environment may be significantly reduced, and a quasi-cleavage crack morphology appears on the fracture, showing the characteristics of liquid metal embrittlement. However, the relevant experimental technology is not yet mature. Based on this, the present invention has developed a fatigue testing device and a method for use in a high-temperature liquid lead-bismuth environment, which can be used to study the fatigue behavior of metal materials in a liquid lead-bismuth environment. Summary of the invention

[0003] The purpose of the present invention is to provide a fatigue testing device and a method for use in a high-temperature liquid lead-bismuth environment, to realize the fatigue behavior study of metal materials in a high-temperature liquid lead-bismuth environment, and to evaluate the mechanical behavior and embrittlement damage behavior of metal materials in the liquid lead-bismuth environment.

[0004] The technical solution of the present invention is:

[0005] A fatigue test device in a high-temperature liquid lead-bismuth environment, the device comprises: a fatigue testing machine, a loading shaft, a sample rack, a fatigue sample, a support rod, a fatigue kettle, a heater, a strain measurement system, a dissolved oxygen electrode, a conduction pipe, and a storage kettle, and the specific structure is as follows:

[0006] Two upright posts are arranged relatively parallel, a crossbeam is installed on the two upright posts, a fatigue testing machine is fixedly installed on the crossbeam, and the bottom of the crossbeam is connected to the fatigue kettle cover through two vertical support rods; the fatigue kettle is composed of a fatigue kettle cover and a fatigue kettle body arranged up and down, which are connected by bolts; a heater is wrapped around the outer side of the fatigue kettle body, a groove-shaped sample rack is arranged in the inner cavity of the fatigue kettle body, the upper end of the groove-shaped sample rack is installed at the bottom of the fatigue kettle cover, and the fatigue sample is vertically arranged in the sample rack; the lead-bismuth alloy is placed in the fatigue kettle or the storage kettle, the fatigue kettle is connected to the bottom of the inner cavity of the storage kettle through a conducting pipe, and the outer sides of the storage kettle and the conducting pipe are wrapped with a heater;

[0007] The fatigue kettle cover is provided with a loading shaft through hole, a linear differential variable voltage displacement sensor installation port, a dissolved oxygen electrode installation port, a fatigue kettle air inlet pipe, and a fatigue kettle air outlet pipe, wherein: the loading shaft at the output end of the fatigue testing machine passes through a crossbeam, the fatigue kettle cover and is connected with the upper end of the fatigue specimen in the fatigue kettle body; the lower end of the fatigue specimen is connected with the inner bottom of the grooved specimen holder through a connector, and the upper and lower gauge length sections of the fatigue specimen are respectively connected with two linear differential variable voltage displacement sensors of the strain measurement system through a displacement transfer rod; the upper end of the dissolved oxygen electrode extends to the top of the fatigue kettle cover, and the lower end of the dissolved oxygen electrode passes through the fatigue kettle cover and extends to the middle of the inner cavity of the fatigue kettle body.

[0008] In the fatigue test device in a high-temperature liquid lead-bismuth environment, an O-ring is used to seal the loading shaft and the fatigue kettle cover at the loading shaft through hole.

[0009] In the fatigue test device in a high-temperature liquid lead-bismuth environment, a copper gasket is placed between the fatigue kettle body and the fatigue kettle cover, and sealing is achieved through bolt connection.

[0010] The fatigue testing device in the high-temperature liquid lead-bismuth environment, the control cabinet is connected with the fatigue testing machine, the fatigue kettle heater and thermocouple, the storage kettle heater and thermocouple, the conduction tube heater and thermocouple, so as to realize the control of the fatigue testing machine, the temperature control of the fatigue kettle, the storage kettle and the conduction tube heater, and collect test data.

[0011] In the fatigue test device in a high-temperature liquid lead-bismuth environment, two linear differential variable voltage displacement sensors are installed on the fatigue kettle cover, and two displacement transmission rods are respectively assembled at both ends of the fatigue specimen gauge section and inserted into the linear differential variable voltage displacement sensor; the linear differential variable voltage displacement sensor is connected to the control cabinet through a line, and the signal of the linear differential variable voltage displacement sensor is collected through the control cabinet, and the signal difference of the two linear differential variable voltage displacement sensors is the fatigue specimen gauge section strain.

[0012] The fatigue test device in a high-temperature liquid lead-bismuth environment has one end of the fatigue kettle air inlet pipe extending to the outside of the fatigue kettle cover, and the other end of the fatigue kettle air inlet pipe passes through a channel on the fatigue kettle cover and extends to the lower part of the inner cavity of the fatigue kettle body; one end of the fatigue kettle air outlet pipe extends to the outside of the fatigue kettle cover, and the other end of the fatigue kettle air outlet pipe passes through a channel on the fatigue kettle cover and extends to the upper part of the inner cavity of the fatigue kettle body.

[0013] The fatigue testing device in the high-temperature liquid lead-bismuth environment is a U-shaped structure. The fatigue testing machine has a load control mode, a displacement control mode or a strain control mode, and can realize triangular wave, sine wave, trapezoidal wave or combined waveform functions.

[0014] The method for using the fatigue test device in a high-temperature liquid lead-bismuth environment comprises the following specific steps:

[0015] (1) placing the lead-bismuth alloy into a storage kettle;

[0016] (2) Use a wiping paper to clean the storage kettle body and the sealing surface of the storage kettle cover, wipe the copper gasket clean and put it into the sealing groove on the top of the storage kettle body, and place the storage kettle cover on the storage kettle body;

[0017] (3) Turn on the fatigue testing machine and adjust it to the displacement control mode;

[0018] (4) Place the fatigue specimen on the specimen rack in the fatigue autoclave, change the fatigue machine control mode to load control, adjust the load to 1-2 kN, and fix the fatigue specimen;

[0019] (5) Use wiping paper to clean the fatigue kettle body and the sealing surface of the fatigue kettle cover, wipe the copper gasket clean and put it into the sealing groove on the top of the fatigue kettle body, and place the fatigue kettle cover on the fatigue kettle body;

[0020] (6) Inert gas is filled into the corresponding kettle body from the air inlet pipe of the storage kettle and the air inlet pipe of the fatigue kettle respectively, and the air in the kettle body is removed, so that the inside of the kettle body is in an inert gas protection state;

[0021] (7) Set the target temperature on the control cabinet. The recommended initial target temperature of the storage kettle and the conduction pipe is 250°C ± 10°C, and the target temperature of the fatigue kettle is 200°C. Start heating and maintain the target temperature for 20 to 40 minutes after reaching the target temperature value to completely melt the lead-bismuth alloy in the storage kettle.

[0022] (8) Connect high-purity argon gas to the storage kettle inlet pipe, open the storage kettle inlet pipe valve, close the storage kettle outlet pipe valve, close the fatigue kettle inlet pipe valve, and open the fatigue kettle outlet pipe valve;

[0023] (9) high-purity argon gas is blown into the storage kettle, and the liquid lead-bismuth alloy is pushed into the fatigue kettle through the conducting pipe by gas pressure;

[0024] (10) After the fatigue specimen is completely immersed in the liquid lead-bismuth alloy in the fatigue reactor, close the inlet valve of the storage reactor while keeping the outlet valve closed, and close the outlet valve of the fatigue reactor while keeping the inlet valve closed;

[0025] (11) Reduce the temperature of the fatigue reactor to 180°C ± 10°C;

[0026] (12) preheating the dissolved oxygen electrode at a temperature of 150 to 200° C. for 20 to 40 minutes, and then completely inserting the dissolved oxygen electrode into the liquid lead-bismuth alloy; connecting the dissolved oxygen electrode to a high-precision voltmeter to measure and collect the dissolved oxygen value in the liquid lead-bismuth alloy in real time;

[0027] (13) Start heating the fatigue kettle to the target value and keep it warm for 30 to 60 minutes;

[0028] (14) Input test parameters into the fatigue testing machine;

[0029] (15) Adjust the load to 0 N on the fatigue testing machine and reset the displacement to zero;

[0030] (16) Click Start to start the fatigue test;

[0031] (17) After the fatigue test is carried out for 100 to 500 cycles, the fatigue test stop condition is set, and the test is stopped when the peak tensile stress drops to 75% of the maximum peak tensile stress;

[0032] (18) After the test, save the fatigue test data;

[0033] (19) Start cooling down. When the temperature drops to 250°C ± 10°C, take out the dissolved oxygen electrode and then quickly tighten the ferrule to keep the kettle sealed.

[0034] (20) Connect high-purity argon gas to the inlet pipe of the fatigue reactor, open the valve of the outlet pipe of the storage reactor, keep the valve of the inlet pipe closed, open the valve of the inlet pipe of the fatigue reactor, and keep the valve of the outlet pipe closed;

[0035] (21) starting to blow high-purity argon gas into the fatigue reactor at a rate controlled at 0.1 to 1 L / min, and using gas pressure to push the liquid lead-bismuth alloy into the storage reactor through the conducting pipe;

[0036] (22) Cool the storage kettle, fatigue kettle and conducting tube to room temperature, open the fatigue kettle, remove the sample and store it properly;

[0037] (23) Close the fatigue kettle cover and the test is finished.

[0038] The method for using the fatigue test device in a high-temperature liquid lead-bismuth environment is as follows: when the temperature of the fatigue kettle, the storage kettle and the conducting pipe is greater than 250°C, high-purity argon or high-purity nitrogen is passed through the air inlet pipe of the storage kettle to allow the liquid lead-bismuth alloy in the storage kettle to flow into the fatigue kettle; and high-purity argon or high-purity nitrogen is passed through the air inlet pipe of the fatigue kettle to allow the liquid lead-bismuth alloy in the fatigue kettle to flow into the storage kettle, thereby realizing the mutual transfer of the high-temperature liquid lead-bismuth alloy in the fatigue kettle and the storage kettle.

[0039] The advantages and beneficial effects of the present invention are:

[0040] 1. The present invention provides a fatigue testing device in a high-temperature liquid lead-bismuth environment and a method for using the same. The testing device includes a fatigue testing machine, a fatigue kettle, a sample rack, a fatigue sample, a strain measurement system, a support rod, a storage kettle, a conducting tube, a control cabinet, a heater, a lead-bismuth alloy, etc. The fatigue testing device can be carried out on the fatigue sample in a high-temperature liquid lead-bismuth environment, and the test parameters such as temperature, dissolved oxygen concentration, displacement, load, strain, etc. can be recorded and collected in real time, and can be used to evaluate the fatigue performance of metal materials in a high-temperature liquid lead-bismuth environment.

[0041] 2. The device of the present invention connects the fatigue reactor and the storage reactor through a conducting pipe to realize the transfer of high-temperature liquid lead and bismuth between the fatigue reactor and the storage reactor, which is convenient for loading and unloading fatigue specimens in normal temperature air. The operation is simple and convenient and does not contact lead and bismuth vapor. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 The structure diagram of the device of the present invention is shown in the figure: 1, fatigue testing machine; 2, loading shaft; 3, sample rack; 4, fatigue sample; 5, support rod; 6, fatigue kettle; 7, fatigue kettle cover; 8, fatigue kettle body; 9, heater; 10, strain measurement system; 11, dissolved oxygen electrode; 12, O-ring; 13, fatigue kettle air inlet pipe; 14, fatigue kettle air outlet pipe; 15, conduction pipe; 16, storage kettle; 17, storage kettle air inlet pipe; 18, storage kettle air outlet pipe; 19, control cabinet; 20, crossbeam; 21, column. DETAILED DESCRIPTION

[0043] like Figure 1 As shown, the fatigue test device in a high-temperature liquid lead-bismuth environment of the present invention comprises: a fatigue testing machine 1, a loading shaft 2, a sample rack 3, a fatigue sample 4, a support rod 5, a fatigue kettle 6, a fatigue kettle cover 7, a fatigue kettle body 8, a heater 9, a strain measurement system 10, a dissolved oxygen electrode 11, an O-ring 12, a fatigue kettle air inlet pipe 13, a fatigue kettle air outlet pipe 14, a conducting pipe 15, a storage kettle 16, a storage kettle air inlet pipe 17, a storage kettle air outlet pipe 18, a control cabinet 19, a lead-bismuth alloy, etc. The specific structure is as follows:

[0044] Two upright posts 21 are arranged relatively parallel, and a crossbeam 20 is mounted on the two upright posts 21. The fatigue testing machine 1 is fixedly mounted on the crossbeam 20, and the bottom of the crossbeam 20 is connected to the fatigue kettle cover 7 through two vertical support rods 5; the fatigue kettle 6 is composed of a fatigue kettle cover 7 and a fatigue kettle body 8 arranged up and down, which are connected by bolts, and a copper gasket is placed between the fatigue kettle body 8 and the fatigue kettle cover 7, and the sealing is achieved by tightening the bolts; a heater 9 is wrapped around the outer side of the fatigue kettle body 8, and a groove-shaped sample rack 3 is arranged in the inner cavity of the fatigue kettle body 8, and the upper end of the groove-shaped sample rack 3 is mounted on the bottom of the fatigue kettle cover 7, and the fatigue sample 4 is vertically arranged in the sample rack 3; the control cabinet 19 is connected to the heater 9 (matching thermocouple) through a line, and the control cabinet 19 is used for power supply and temperature control to achieve temperature control of the lead-bismuth alloy in the fatigue kettle body 8;

[0045] The fatigue kettle cover 7 is provided with a loading shaft through hole, a linear differential variable voltage displacement sensor installation port, a dissolved oxygen electrode installation port, a fatigue kettle air inlet pipe 13, and a fatigue kettle air outlet pipe 14, wherein: the loading shaft 2 at the output end of the fatigue testing machine 1 passes through the crossbeam 20, the fatigue kettle cover 7 is connected to the upper end of the fatigue specimen 4 in the fatigue kettle body 8, and at the loading shaft through hole, the loading shaft 2 and the fatigue kettle cover 7 are sealed by an O-ring 12; the lower end of the fatigue specimen 4 is connected to the inner bottom of the groove-shaped specimen holder 3 through a connector, and the upper and lower gauge length sections of the fatigue specimen 4 are respectively connected by displacement The transfer rod is connected to two linear differential variable voltage displacement sensors (LVDT) of the strain measurement system 10, and the strain measurement system 10 can measure the strain of the gauge section of the fatigue specimen 4 in the liquid lead-bismuth environment in situ; two linear differential variable voltage displacement sensors (LVDT) are installed on the fatigue kettle cover 7 (outside), and two displacement transfer rods are respectively assembled at both ends of the fatigue specimen gauge section and inserted into the linear differential variable voltage displacement sensor (LVDT); the LVDT signal is collected by the control cabinet, and the difference between the two LVDTs is the strain of the fatigue specimen gauge section. The upper end of the dissolved oxygen electrode 11 extends to the top of the fatigue kettle cover 7, and the lower end of the dissolved oxygen electrode 11 passes through the fatigue kettle cover 7 and extends to the middle of the inner cavity of the fatigue kettle body 8. One end of the fatigue kettle air inlet pipe 13 extends to the outside of the fatigue kettle cover 7, and the other end of the fatigue kettle air inlet pipe 13 passes through the channel on the fatigue kettle cover 7 and extends to the lower part of the inner cavity of the fatigue kettle body 8; one end of the fatigue kettle air outlet pipe 14 extends to the outside of the fatigue kettle cover 7, and the other end of the fatigue kettle air outlet pipe 14 passes through the channel on the fatigue kettle cover 7 and extends to the upper part of the inner cavity of the fatigue kettle body 8.

[0046] The lead-bismuth alloy is placed in the fatigue kettle 6 or the storage kettle 16. The fatigue kettle 6 and the bottom of the inner cavity of the storage kettle 16 are connected by a conducting tube 15. The outer side of the storage kettle 16 is wrapped with a heater 9 (with a matching thermocouple). The control cabinet 19 is connected to the heater 9 through a line, and the control cabinet 19 is used to supply power and control the temperature to achieve temperature control of the lead-bismuth alloy in the storage kettle 16. In addition, the outer side of the conducting tube 15 can also be wrapped with a heater (with a matching thermocouple). The control cabinet 19 is connected to the heater through a line, and the control cabinet 19 is used to supply power and control the temperature.

[0047] The fatigue specimen 4 is mounted on the specimen rack 3, the lead-bismuth alloy is placed in the fatigue kettle 6 or the storage kettle 16, and the temperature is raised to the target value by the control cabinet 19 and the heater, and the fatigue behavior of the metal material in the high-temperature liquid lead-bismuth environment can be studied. When the temperature of the fatigue kettle 6, the storage kettle 16, and the conducting pipe 15 is greater than 250°C, the liquid lead-bismuth alloy in the storage kettle 16 can flow into the fatigue kettle 6 by passing high-purity argon or high-purity nitrogen (99.999% by volume purity) through the storage kettle inlet pipe 17, and the liquid lead-bismuth alloy in the fatigue kettle 6 can flow into the storage kettle 16 by passing high-purity argon or high-purity nitrogen (99.999% by volume purity) through the fatigue kettle inlet pipe 13, so that the high-temperature liquid lead-bismuth alloy can be transferred between the fatigue kettle 6 and the storage kettle 16, and the fatigue specimen 4 can be loaded and unloaded under normal temperature air conditions. The control cabinet 19 is connected to the fatigue testing machine 1, the fatigue kettle heater and thermocouple, the storage kettle heater and thermocouple, and the conduction tube heater and thermocouple to control the fatigue testing machine 1, the fatigue kettle, the storage kettle, and the conduction tube heater temperature control, and collect test data. Thus, the test temperature in the liquid lead-bismuth environment can be accurately controlled, the test device remains sealed to prevent lead-bismuth vapor leakage during the test, and fatigue tests of fatigue specimens in the liquid lead-bismuth environment can be carried out.

[0048] The fatigue testing machine 1 is a U-shaped structure (the actuator is placed on the top and the bottom is a steel plate). The fatigue testing machine has load control, displacement control and strain control modes, and can realize functions such as triangular wave, sine wave, trapezoidal wave, and combined waveform.

[0049] Below, the present invention is further described in detail by examples.

[0050] Example

[0051] In this embodiment, the fatigue specimen is 316L stainless steel, and the fatigue test is carried out in a 350°C liquid lead-bismuth environment under saturated dissolved oxygen concentration conditions, with a strain rate of 4×10 -4 s -1 , rod-shaped fatigue specimen, the gauge section diameter is 8mm and the length is 16mm.

[0052] like Figure 1As shown, the device of the present invention can carry out slow fatigue and creep test research of metal materials in a liquid lead-bismuth environment, and can control / collect test temperature, dissolved oxygen concentration in liquid lead-bismuth alloy, displacement, load, strain and other parameters in real time. The use steps are as follows:

[0053] (1) Place an appropriate amount of lead-bismuth alloy into a storage kettle.

[0054] (2) Use a cleaning paper to clean the storage kettle body and the sealing surface of the storage kettle cover. After cleaning, put the copper gasket into the sealing groove on the top of the storage kettle body. Place the storage kettle cover on the storage kettle body. Use a torque wrench to tighten the main sealing bolt (tighten gradually along the diagonal line, increasing by 50 N·m each time). The recommended maximum torque is 100-150 N·m.

[0055] (3) Turn on the fatigue testing machine, adjust the fatigue testing machine to the displacement control mode, and adjust the loading axis to the appropriate position.

[0056] (4) Place the fatigue specimen on the specimen rack in the fatigue autoclave, adjust the loading axis to an appropriate position, change the fatigue machine control mode to load control, adjust the load size to 1-2 kN, and fix the fatigue specimen.

[0057] (5) Use a wiping paper to clean the fatigue kettle body and the sealing surface of the fatigue kettle cover. After wiping the copper gasket clean, put it into the sealing groove on the top of the fatigue kettle body. Place the fatigue kettle cover on the fatigue kettle body and tighten the main sealing bolt with a torque wrench (it is recommended to tighten it gradually along the diagonal line, increasing by 50N·m each time). The recommended maximum torque is 100~150N·m.

[0058] (6) Inert gas (high-purity argon or high-purity nitrogen) is filled into the corresponding kettle body from the storage kettle air inlet pipe and the fatigue kettle air inlet pipe respectively, and the air in the kettle body is removed, so that the inside of the kettle body is in an inert gas protection state.

[0059] (7) Set the target temperature on the control cabinet. The recommended initial target temperature of the storage kettle and the conduction tube is about 250°C (higher than the eutectic melting point of the lead-bismuth alloy, so that the lead-bismuth alloy is converted from solid to liquid). The target temperature of the fatigue kettle is 200°C. Start heating and maintain the target temperature for about 30 minutes after reaching the target temperature value to completely melt the lead-bismuth alloy in the storage kettle.

[0060] (8) Connect high-purity argon gas to the air inlet pipe of the storage kettle, open the air inlet pipe valve of the storage kettle, close the air outlet pipe valve of the storage kettle, close the air inlet pipe valve of the fatigue kettle, and open the air outlet pipe valve of the fatigue kettle.

[0061] (9) High-purity argon gas is blown into the storage kettle, and the liquid lead-bismuth alloy is pushed into the fatigue kettle through the conducting tube by gas pressure. At the same time, the thermocouple in the fatigue kettle is observed. When the temperature suddenly changes, it indicates that the liquid level of the liquid lead-bismuth alloy has reached the position where the thermocouple is installed.

[0062] (10) After the fatigue specimen is completely immersed in the liquid lead-bismuth alloy in the fatigue kettle, close the inlet pipe valve of the storage kettle (while keeping the outlet pipe valve closed), and close the outlet pipe valve of the fatigue kettle (while keeping the inlet pipe valve closed).

[0063] (11) Reduce the fatigue kettle temperature to about 180°C.

[0064] (12) After preheating the dissolved oxygen electrode at 180°C for 30 minutes, the dissolved oxygen electrode is completely inserted into the liquid lead-bismuth alloy and the ferrule is tightened to seal. The dissolved oxygen electrode is connected to a high-precision voltmeter (with an accuracy of 0.01 mV) to measure and collect the dissolved oxygen value in the liquid lead-bismuth alloy in real time.

[0065] (13) Start heating the kettle to the target temperature and keep it at that temperature for 60 minutes.

[0066] (14) Input the test parameters (displacement amplitude, frequency, waveform) into the fatigue testing machine.

[0067] (15) Adjust the load to 0 N on the fatigue testing machine and reset the displacement to zero.

[0068] (16) Click Start to start the fatigue test.

[0069] (17) After the fatigue test is carried out for 300 cycles, the fatigue test stop condition is set, which is generally set to stop the test when the peak tensile stress drops to 75% of the maximum peak tensile stress.

[0070] (18) After the test, save the fatigue test data (displacement, load, time, etc.).

[0071] (19) Start cooling down. When the temperature drops to about 250°C (it is forbidden to cool down to the solidification point of the lead-bismuth alloy eutectic to prevent damage to the dissolved oxygen electrode), take out the dissolved oxygen electrode and then quickly tighten the ferrule to keep the kettle sealed.

[0072] (20) Connect high-purity argon gas to the inlet pipe of the fatigue reactor, open the valve of the outlet pipe of the storage reactor (keep the valve of the inlet pipe closed), and open the valve of the inlet pipe of the fatigue reactor (keep the valve of the outlet pipe closed).

[0073] (21) High-purity argon gas is blown into the fatigue kettle at a rate of 0.1 to 1 L / min. The liquid lead-bismuth alloy is forced into the storage kettle through the conducting tube by gas pressure. At the same time, the thermocouple in the storage kettle is observed. When the temperature suddenly changes, it indicates that the liquid level of the liquid lead-bismuth alloy has reached the position where the thermocouple is installed, and the liquid lead-bismuth alloy in the storage kettle is completely discharged.

[0074] (22) Cool the storage kettle, fatigue kettle and conducting tube to room temperature, open the fatigue kettle, remove the sample and store it properly.

[0075] (23) Close the fatigue kettle cover and the test is finished.

[0076] The results of the embodiments show that the present invention can accurately control the test parameters such as the temperature, strain rate, and load of the liquid lead-bismuth alloy, and evaluate the fatigue performance of the metal material in a high-temperature liquid lead-bismuth environment.

Claims

1. A method for using a fatigue test device in a high-temperature liquid lead-bismuth environment, characterized in that: The device includes: fatigue testing machine, loading shaft, sample rack, fatigue sample, support rod, fatigue kettle, heater, strain measurement system, dissolved oxygen electrode, conduction pipe, storage kettle, and the specific structure is as follows: Two upright posts are arranged relatively parallel, a crossbeam is installed on the two upright posts, a fatigue testing machine is fixedly installed on the crossbeam, and the bottom of the crossbeam is connected to the fatigue kettle cover through two vertical support rods; the fatigue kettle is composed of a fatigue kettle cover and a fatigue kettle body arranged up and down, which are connected by bolts; a heater is wrapped around the outer side of the fatigue kettle body, a groove-shaped sample rack is arranged in the inner cavity of the fatigue kettle body, the upper end of the groove-shaped sample rack is installed at the bottom of the fatigue kettle cover, and the fatigue sample is vertically arranged in the sample rack; the lead-bismuth alloy is placed in the fatigue kettle or the storage kettle, the fatigue kettle is connected to the bottom of the inner cavity of the storage kettle through a conducting pipe, and the outer sides of the storage kettle and the conducting pipe are wrapped with a heater; The fatigue kettle cover is provided with a loading shaft through hole, a linear differential variable voltage displacement sensor installation port, a dissolved oxygen electrode installation port, a fatigue kettle air inlet pipe, and a fatigue kettle air outlet pipe, wherein: the loading shaft at the output end of the fatigue testing machine passes through the crossbeam, the fatigue kettle cover and is connected with the upper end of the fatigue specimen in the fatigue kettle body; the lower end of the fatigue specimen is connected to the inner bottom of the groove-shaped specimen rack through a connecting piece, and the upper and lower gauge length sections of the fatigue specimen are respectively connected to two linear differential variable voltage displacement sensors of the strain measurement system through a displacement transmission rod; the upper end of the dissolved oxygen electrode extends to the top of the fatigue kettle cover, and the lower end of the dissolved oxygen electrode passes through the fatigue kettle cover and extends to the middle of the inner cavity of the fatigue kettle body; The method for using the fatigue test device in a high-temperature liquid lead-bismuth environment comprises the following specific steps: (1) placing the lead-bismuth alloy into a storage kettle; (2) Use wiping paper to clean the storage kettle body and the sealing surface of the storage kettle cover, wipe the copper gasket clean and put it into the sealing groove on the top of the storage kettle body, and place the storage kettle cover on the storage kettle body; (3) Turn on the fatigue testing machine and adjust it to the displacement control mode; (4) Place the fatigue specimen on the specimen rack in the fatigue autoclave, change the fatigue machine control mode to load control, adjust the load size to 1~2kN, and fix the fatigue specimen; (5) Use wiping paper to clean the fatigue kettle body and the sealing surface of the fatigue kettle cover, wipe the copper gasket clean and put it into the sealing groove on the top of the fatigue kettle body, and place the fatigue kettle cover on the fatigue kettle body; (6) Inert gas is filled into the corresponding kettle body from the air inlet pipe of the storage kettle and the air inlet pipe of the fatigue kettle respectively, and the air in the kettle body is removed, so that the inside of the kettle body is in an inert gas protection state; (7) Set the target temperature on the control cabinet. The recommended initial target temperature for the storage kettle and the conduction pipe is 250°C ± 10°C, and the target temperature for the fatigue kettle is 200°C. Start heating and maintain the target temperature for 20 to 40 minutes after reaching the target temperature to completely melt the lead-bismuth alloy in the storage kettle. (8) Connect high-purity argon gas to the storage kettle inlet pipe, open the storage kettle inlet pipe valve, close the storage kettle outlet pipe valve, close the fatigue kettle inlet pipe valve, and open the fatigue kettle outlet pipe valve; (9) High-purity argon gas is blown into the storage kettle, and the liquid lead-bismuth alloy is pushed into the fatigue kettle through the conducting pipe by gas pressure; (10) After the fatigue specimen is completely immersed in the liquid lead-bismuth alloy in the fatigue reactor, close the inlet valve of the storage reactor while keeping the outlet valve closed, and close the outlet valve of the fatigue reactor while keeping the inlet valve closed; (11) Reduce the temperature of the fatigue reactor to 180℃±10℃; (12) After preheating the dissolved oxygen electrode at a temperature of 150 to 200° C. for 20 to 40 minutes, the dissolved oxygen electrode is completely inserted into the liquid lead-bismuth alloy; the dissolved oxygen electrode is connected to a high-precision voltmeter to measure and collect the dissolved oxygen value in the liquid lead-bismuth alloy in real time; (13) Start heating the fatigue kettle to the target value and keep it warm for 30 to 60 minutes; (14) Input the test parameters on the fatigue testing machine; (15) Adjust the load to 0 N on the fatigue testing machine and reset the displacement to zero; (16) Click Start to start the fatigue test; (17) After the fatigue test is carried out for 100 to 500 cycles, the fatigue test stop condition is set, and the test is stopped when the peak tensile stress drops to 75% of the maximum peak tensile stress; (18) After the test, save the fatigue test data; (19) Start cooling down. When the temperature drops to 250℃±10℃, take out the dissolved oxygen electrode and then quickly tighten the ferrule to keep the kettle sealed. (20) Connect high-purity argon gas to the inlet pipe of the fatigue reactor, open the valve of the outlet pipe of the storage reactor, keep the valve of the inlet pipe closed, open the valve of the inlet pipe of the fatigue reactor, and keep the valve of the outlet pipe closed; (21) High-purity argon gas is blown into the fatigue reactor at a rate of 0.1-1 L / min, and the liquid lead-bismuth alloy is pushed into the storage reactor through the conducting pipe by gas pressure; (22) Cool the storage kettle, fatigue kettle and conducting tube to room temperature, open the fatigue kettle, remove the sample and store it properly; (23) Close the fatigue kettle cover and the test is finished.

2. The method for using the fatigue testing device in a high temperature liquid lead-bismuth environment according to claim 1, characterized in that: At the through hole of the loading shaft, the loading shaft and the fatigue reactor cover are sealed by an O-ring.

3. The method for using the fatigue testing device in a high temperature liquid lead-bismuth environment according to claim 1, characterized in that: A copper gasket is placed between the fatigue kettle body and the fatigue kettle cover, and sealing is achieved through bolt connection.

4. The method for using the fatigue testing device in a high temperature liquid lead-bismuth environment according to claim 1, characterized in that: The control cabinet is connected to the fatigue testing machine, fatigue kettle heater and thermocouple, storage kettle heater and thermocouple, and conduction tube heater and thermocouple to realize the control of the fatigue testing machine, the temperature control of the fatigue kettle, storage kettle, and the conduction tube heater, and to collect test data.

5. The method for using the fatigue testing device in a high temperature liquid lead-bismuth environment according to claim 1, characterized in that: Two linear differential variable voltage displacement sensors are installed on the cover of the fatigue autoclave, and two displacement transmission rods are respectively assembled at both ends of the fatigue specimen gauge section and inserted into the linear differential variable voltage displacement sensor; the linear differential variable voltage displacement sensor is connected to the control cabinet through the line, and the signal of the linear differential variable voltage displacement sensor is collected through the control cabinet. The signal difference of the two linear differential variable voltage displacement sensors is the strain of the fatigue specimen gauge section.

6. The method for using the fatigue testing device in a high temperature liquid lead-bismuth environment according to claim 1, characterized in that: One end of the fatigue kettle air inlet pipe extends to the outside of the fatigue kettle cover, and the other end of the fatigue kettle air inlet pipe passes through the channel on the fatigue kettle cover and extends to the lower part of the inner cavity of the fatigue kettle body; one end of the fatigue kettle air outlet pipe extends to the outside of the fatigue kettle cover, and the other end of the fatigue kettle air outlet pipe passes through the channel on the fatigue kettle cover and extends to the upper part of the inner cavity of the fatigue kettle body.

7. The method for using the fatigue testing device in a high temperature liquid lead-bismuth environment according to claim 1, characterized in that: The fatigue testing machine has a U-shaped structure. It has load control mode, displacement control mode or strain control mode, and can realize triangular wave, sine wave, trapezoidal wave or combined waveform functions.

8. The method for using the fatigue testing device in a high temperature liquid lead-bismuth environment according to claim 1, characterized in that: When the temperature of the fatigue kettle, the storage kettle and the conducting pipe is greater than 250°C, high-purity argon or high-purity nitrogen is passed through the air inlet pipe of the storage kettle to make the liquid lead-bismuth alloy in the storage kettle flow into the fatigue kettle, and high-purity argon or high-purity nitrogen is passed through the air inlet pipe of the fatigue kettle to make the liquid lead-bismuth alloy in the fatigue kettle flow into the storage kettle, thereby realizing the mutual transfer of high-temperature liquid lead-bismuth alloy in the fatigue kettle and the storage kettle.