Indium phosphide substrate, semiconductor epitaxial wafer, and method for manufacturing indium phosphide substrate

By controlling the back shape and contact uniformity of the indium phosphide substrate, the problem of uneven thermal conductivity caused by warping the back surface of the indium phosphide substrate is solved, and the quality of the epitaxial crystal layer and the performance of the semiconductor epitaxial wafer are improved.

CN113207310BActive Publication Date: 2024-11-15JX NIPPON MINING & METALS CORP
View PDF 23 Cites 0 Cited by

Patent Information

Application Number
CN202080006111.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-04-27
Filing Date
2020-06-04
Publication Date
2024-11-15
Estimated Expiration
2040-06-04

AI Technical Summary

Technical Problem

The warping of the back surface of the indium phosphide substrate causes uneven contact between the substrate and the base, which in turn affects the temperature uniformity of heat conduction and epitaxial growth, and reduces the quality of the epitaxial crystal layer and the performance of the semiconductor epitaxial wafer.

Method used

By controlling the back BOW value, SORI value and WARP value of the indium phosphide substrate within a specific range, the flatness and uniformity of the back surface of the substrate are ensured, so that uniform contact between the substrate and the base can be achieved during epitaxial growth. Specific methods include using a wire saw cutting, etching and grinding process, controlling the metal wire supply speed, reciprocating speed and abrasive viscosity, and ensuring the flatness and contact uniformity of the substrate.

Benefits of technology

It effectively suppresses warping on the back of the indium phosphide substrate, ensures uniform contact between the substrate and the base and heat conduction, improves the quality of the epitaxial crystal layer and the performance of the semiconductor epitaxial wafer, and avoids problems such as light emission wavelength shift.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0003059966230000101
    Figure GDA0003059966230000101
Patent Text Reader

Abstract

The present invention provides an indium phosphide substrate, a semiconductor epitaxial wafer and a method for manufacturing an indium phosphide substrate that effectively suppresses warping of the back side of the substrate. The indium phosphide substrate has a main surface for forming an epitaxial crystal layer and a back side opposite to the main surface, and the BOW value of the back side measured with the back side of the indium phosphide substrate facing upward is -2.0 to 2.0 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an indium phosphide substrate, a semiconductor epitaxial wafer and a method for manufacturing the indium phosphide substrate. Background Art

[0002] Indium phosphide (InP) is a III-V compound semiconductor material composed of indium (In) of group III and phosphorus (P) of group V. As a semiconductor material, it has the following characteristics: band gap 1.35eV, electron mobility ~5400cm 2 / V·s, and the electron mobility under high electric field becomes higher than other common semiconductor materials such as silicon and gallium arsenic. In addition, it has the following characteristics: the stable crystal structure at room temperature and pressure is a cubic zinc blende structure, and its lattice constant has a larger lattice constant than compound semiconductors such as gallium arsenide (GaAs) and gallium phosphide (GaP).

[0003] An ingot of indium phosphide, which is a raw material of an indium phosphide substrate, is usually sliced ​​into a predetermined thickness, ground into a desired shape, and mechanically polished as appropriate, and then subjected to etching, precision polishing (polishing), etc., in order to remove grinding debris and damage caused by grinding.

[0004] An epitaxial crystal layer is sometimes formed on the main surface of an indium phosphide substrate by epitaxial growth (Patent Document 1).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2003-218033 Summary of the invention

[0008] Problems to be solved by the invention

[0009] When performing the epitaxial growth, the indium phosphide substrate is usually supported from the back side by a susceptor. At this time, if the back side of the indium phosphide substrate is greatly warped, the contact between the back side of the substrate and the susceptor is uneven.

[0010] If the contact between the back surface of the substrate and the susceptor is uneven, the in-plane distribution of heat conduction to the substrate is also uneven, so the substrate temperature during epitaxial growth is uneven. As a result, the following problems arise: the quality of the generated epitaxial crystal layer is reduced, the emission wavelength is shifted, and the performance of the semiconductor epitaxial wafer is reduced.

[0011] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide an indium phosphide substrate, a semiconductor epitaxial wafer, and a method for manufacturing an indium phosphide substrate in which warping of the back surface of the substrate is well suppressed.

[0012] Solutions for solving problems

[0013] In one embodiment, the present invention is an indium phosphide substrate, characterized in that the indium phosphide substrate has a main surface for forming an epitaxial crystal layer and a back surface opposite to the main surface, and the BOW value of the back surface measured with the back surface of the indium phosphide substrate facing upward is -2.0 to 2.0 μm.

[0014] In another embodiment of the indium phosphide substrate of the present invention, a BOW value of the back surface measured in a state where the back surface of the indium phosphide substrate faces upward is -1.5 to 1.0 μm.

[0015] In another embodiment of the indium phosphide substrate of the present invention, a BOW value of the back surface measured in a state where the back surface of the indium phosphide substrate faces upward is -0.3 to 0.9 μm.

[0016] In another embodiment of the indium phosphide substrate of the present invention, the BOW value of the back surface measured with the back surface of the indium phosphide substrate facing upward is -0.3 to 0.9 μm, and the diameter of the substrate is 100 mm or less.

[0017] In another embodiment of the indium phosphide substrate of the present invention, the BOW value of the back surface measured with the back surface of the indium phosphide substrate facing upward is -0.3 to 0.5 μm, and the diameter of the substrate is 76.2 mm or less.

[0018] In another embodiment of the indium phosphide substrate of the present invention, the BOW value of the back surface measured with the back surface of the indium phosphide substrate facing upward is 0.0 to 0.7 μm, and the diameter of the substrate is 50.8 mm or less.

[0019] In still another embodiment, the present invention provides an indium phosphide substrate, wherein a SORI value of the back surface of the indium phosphide substrate measured with the back surface facing upward is 2.5 μm or less.

[0020] In another embodiment of the indium phosphide substrate of the present invention, a SORI value of the back surface of the indium phosphide substrate measured with the back surface facing upward is 1.6 to 2.5 μm.

[0021] In still another embodiment, the present invention provides an indium phosphide substrate, wherein a WARP value of the back surface of the indium phosphide substrate measured with the back surface facing upward is 3.5 μm or less.

[0022] In another embodiment of the indium phosphide substrate of the present invention, a WARP value of the back surface measured with the back surface of the indium phosphide substrate facing upward is 1.8 to 3.5 μm.

[0023] In another embodiment of the indium phosphide substrate of the present invention, a WARP value of the back surface measured with the back surface of the indium phosphide substrate facing upward is 1.8 to 3.4 μm.

[0024] In still another embodiment, the present invention is a semiconductor epitaxial wafer including an epitaxial crystal layer on the main surface of the indium phosphide substrate according to the embodiment of the present invention.

[0025] In another embodiment, the present invention is a method for manufacturing an indium phosphide substrate of the present invention, which includes: a step of cutting a wafer from an ingot of indium phosphide using a wire saw; a step of etching the cut wafer; a step of chamfering the outer peripheral portion of the etched wafer; a step of grinding at least one surface of the chamfered wafer; and a step of etching the ground wafer, wherein the step of cutting a wafer from an ingot of indium phosphide using a wire saw includes: continuously feeding a new wire while reciprocating a metal wire in a horizontal direction, and causing the ingot carrying the indium phosphide to be cut. A process in which a stage moves vertically toward the metal wire, a new wire supply speed of the metal wire is 10 to 60 m / min, a reciprocating speed of the metal wire is 300 to 350 m / min, a vertical movement speed of the stage carrying the ingot of indium phosphide is 200 to 400 μm / min, a viscosity of the abrasive of the wire saw is 300 to 400 mPa·s, and in a process of etching the cut wafer, only 5 to 15 μm is etched from both sides in total, and in a process of etching the ground wafer, only 8 to 15 μm is etched from both sides in total.

[0026] Effects of the Invention

[0027] According to the embodiments of the present invention, it is possible to provide an indium phosphide substrate, a semiconductor epitaxial wafer, and a method for manufacturing an indium phosphide substrate in which warping of the back surface of the substrate is well suppressed. DETAILED DESCRIPTION

[0028] 〔Indium Phosphide Substrate〕

[0029] Hereinafter, the configuration of the indium phosphide substrate according to the present embodiment will be described.

[0030] The indium phosphide (InP) substrate of the present embodiment has a main surface for forming an epitaxial crystal layer and a back surface opposite to the main surface.

[0031] The principal surface for forming an epitaxial crystal layer is a surface on which epitaxial growth is actually performed when an indium phosphide substrate is used as a substrate for epitaxial growth in order to form a semiconductor device structure.

[0032] The maximum diameter of the main surface of the indium phosphide substrate is not particularly limited, and may be 50 to 151 mm, or 50 to 101 mm. The planar shape of the indium phosphide substrate may be circular, or may be a quadrilateral such as a rectangle.

[0033] The thickness of the indium phosphide substrate is not particularly limited, for example, preferably 300 to 900 μm, more preferably 300 to 700 μm. In particular, in the case of a large aperture, the following problems may occur: if the thickness of the indium phosphide substrate is less than 300 μm, it may break, and if the thickness of the indium phosphide substrate exceeds 900 μm, the base material crystal is wasted.

[0034] In the case of an indium phosphide substrate, a dopant (impurity) can be used to increase the carrier concentration to 1×10 16 cm -3 Above and 1×10 19 cm -3 The following method contains Zn (zinc) and can also be used to make the carrier concentration 1×10 16 cm -3 Above and 1×10 19 cm -3 The following method contains S (sulfur) and can also be used to increase the carrier concentration to 1×10 16 cm -3 Above and 1×10 19 cm -3 The following method includes Sn (tin) and can also be used to increase the carrier concentration to 1×10 6 cm -3 Above 1×10 9 cm -3 The following aspects contain Fe (iron).

[0035] (BOW value)

[0036] In one embodiment of the indium phosphide substrate of the present invention, the BOW value of the back side measured with the back side facing upward is controlled to -2.0 to 2.0 μm. According to such a configuration, an indium phosphide substrate in which warping of the back side of the substrate is well suppressed can be obtained. More specifically, when epitaxial growth is performed, even if the indium phosphide substrate is supported from the back side by a susceptor, the contact between the back side of the substrate and the susceptor is uniform. Therefore, heat conduction is evenly distributed in the plane of the indium phosphide substrate, and the substrate temperature during epitaxial growth is uniform. As a result, the quality of the generated epitaxial crystal layer is improved, and the performance degradation of the semiconductor epitaxial wafer such as the emission wavelength shift can be well suppressed.

[0037] Here, the "BOW value" is explained. When the measurement is carried out in a manner that supports the indium phosphide substrate and does not change the original shape, a triangle with three points as vertices is drawn on the measurement surface of the indium phosphide substrate in a manner that surrounds the center point of the substrate, and the plane containing the triangle is set as a three-point reference plane. The three points are (0.97R, 90°), (0.97R, 210°), and (0.97R, 330°) when the radius of the substrate is set to R with the center of the substrate as the origin and the polar coordinates of the OF center being 270°. In the direction perpendicular to the three-point reference plane, the value representing the distance between the center point of the substrate and the three-point reference plane in a manner that the upper direction is set to a positive value and the lower direction is set to a negative value is the BOW value. The BOW value can be measured, for example, using Ultrasort manufactured by Corning Tropel, and the back of the indium phosphide substrate can be placed in a PP box facing the upper side and automatically transported, thereby measuring. At this time, in order to prevent the warping of the substrate from changing, the substrate is measured in a non-adsorbed state.

[0038] For the indium phosphide substrate of the embodiment of the present invention, the BOW value of the back side measured with the back side of the indium phosphide substrate facing upward is preferably -1.5 to 1.0 μm, more preferably -0.3 to 0.9 μm. Furthermore, it may be -0.3 to 0.9 μm when the diameter of the substrate is 100 mm or less, -0.3 to 0.5 μm when the diameter of the substrate is 76.2 mm or less, and 0.0 to 0.7 μm when the diameter of the substrate is 50.8 mm or less.

[0039] (SORI value)

[0040] With respect to the indium phosphide substrate of the embodiment of the present invention, the SORI value of the back side measured except for the peripheral portion with a width of 3 mm when the back side is facing upward is preferably controlled to be less than 2.5 μm. According to such a configuration, an indium phosphide substrate that suppresses the warping of the back side of the substrate more effectively can be obtained. More specifically, when epitaxial growth is performed, even if the indium phosphide substrate is supported from the back side by a susceptor, the contact between the back side of the substrate and the susceptor is more uniform. Therefore, the in-plane distribution of heat conduction to the indium phosphide substrate is more uniform, and the substrate temperature during epitaxial growth is more uniform. As a result, the quality of the generated epitaxial crystal layer is improved, and the performance degradation of the semiconductor epitaxial wafer such as the emission wavelength shift can be more effectively suppressed.

[0041] Here, "SORI value" means the sum of the maximum absolute values ​​of the positive direction (upward direction) and the negative direction (downward direction) from the least-squares plane calculated according to the shape of the measured surface of the indium phosphide substrate when the indium phosphide substrate is supported and measured without changing its original shape. The SORI value can be measured, for example, using Ultrasort manufactured by Corning Tropel, where the indium phosphide substrate can be stored in a box with the back side facing upward and automatically transported, thereby measuring. At this time, in order to prevent the warping of the substrate from changing, the substrate is measured in a non-adsorbed state.

[0042] In the indium phosphide substrate of the embodiment of the present invention, the SORI value of the back surface measured with the back surface of the indium phosphide substrate facing upward may be 1.6 to 2.5 μm. Furthermore, it may be 1.6 to 2.5 μm when the diameter of the substrate is 100 mm or less, 1.6 to 1.8 μm when the diameter of the substrate is 76.2 mm or less, and 1.7 μm or less when the diameter of the substrate is 50.8 mm or less.

[0043] (WARP value)

[0044] In the case of the indium phosphide substrate of the embodiment of the present invention, the WARP value of the back side measured except for the peripheral portion with a width of 3 mm when the back side is facing upward is preferably controlled to be less than 3.5 μm. According to such a structure, an indium phosphide substrate in which the warping of the back side of the substrate is better suppressed can be obtained. More specifically, when epitaxial growth is performed, even if the indium phosphide substrate is supported from the back side by a susceptor, the contact between the back side of the substrate and the susceptor is more uniform. Therefore, the in-plane distribution of heat conduction to the indium phosphide substrate is more uniform, and the substrate temperature during epitaxial growth is more uniform. As a result, the quality of the generated epitaxial crystal layer is improved, and the performance degradation of the semiconductor epitaxial wafer such as the emission wavelength shift can be better suppressed.

[0045] Here, the "WARP value" is explained. When the measurement is performed in a manner that the indium phosphide substrate is supported and the original shape is not changed, a triangle with three points as vertices is drawn on the measurement surface of the indium phosphide substrate in a manner that surrounds the center point of the substrate, and the plane containing the triangle is set as a three-point reference plane. The three points are (0.97R, 90°), (0.97R, 210°), and (0.97R, 330°) when the polar coordinates of the OF center are taken as 270° with the center of the substrate as the origin and the radius of the substrate is set as R. In the direction perpendicular to the three-point reference plane, the sum of the distance between the highest position of the measurement surface of the substrate observed from the three-point reference plane and the three-point reference plane and the distance between the lowest position of the measurement surface of the substrate observed from the three-point reference plane and the three-point reference plane is the WARP value. The WARP value can be measured, for example, using Ultrasort manufactured by Corning Tropel, and the back of the indium phosphide substrate can be placed in a PP box facing upward and automatically transported to perform the measurement. At this time, the substrate was measured in a non-adsorption state in order to prevent the warpage of the substrate from changing.

[0046] In the indium phosphide substrate of the embodiment of the present invention, the WARP value of the back surface measured with the back surface of the indium phosphide substrate facing upward may be 1.8 to 3.5 μm, or 1.8 to 3.4 μm. Furthermore, when the diameter of the substrate is 100 mm or less, the WARP value of the back surface may be 1.8 to 3.4 μm, when the diameter of the substrate is 76.2 mm or less, the WARP value of the back surface may be 1.8 to 2.2 μm, and when the diameter of the substrate is 50.8 mm or less, the WARP value of the back surface may be 2.2 μm or less.

[0047] [Method for producing indium phosphide substrate]

[0048] Next, a method for producing an indium phosphide substrate according to an embodiment of the present invention will be described.

[0049] As a method for producing an indium phosphide substrate, first, an ingot of indium phosphide is prepared by a known method.

[0050] Next, the ingot of indium phosphide was ground into a cylindrical shape.

[0051] Next, a wafer having a main surface and a back surface is cut out from the ground ingot of indium phosphide. At this time, a wire saw is used to cut off both ends of the crystal of the ingot of indium phosphide along a specified crystal plane, and a plurality of wafers are cut out with a specified thickness. In the process of cutting out the wafer, a new wire is continuously fed while the metal wire is reciprocated in the horizontal direction, and a stage carrying the ingot of indium phosphide is moved in the vertical direction toward the metal wire.

[0052] The conditions for cutting the ingot using a wire saw are as follows.

[0053] · New wire supply speed of metal wire: 10~60m / min

[0054] ·Reciprocating speed of metal wire: 300~350m / min

[0055] ·Vertical moving speed of the stage carrying the indium phosphide ingot: 200 to 400 μm / min

[0056] ·Management of abrasives for wire saws

[0057] The abrasive used was GC#1200, and the cutting oil was PS-LP-500D, and the abrasive was managed so that the viscosity became 300 to 400 mPa·s when the rotation speed of the rotor shaft of the viscometer was 60 rpm. The viscosity can be measured using a TVB-10 viscometer manufactured by Toki Sangyo.

[0058] Next, in order to remove the process-degraded layer generated in the cutting process using the wire saw, the cut wafer was etched by 5 to 15 μm in total from both sides using a mixed solution of 85% by mass phosphoric acid aqueous solution and 30% by mass hydrogen peroxide. The wafer was etched by immersing the entire wafer in the etching solution.

[0059] Next, the outer peripheral portion of the wafer is chamfered, and at least one surface of the chamfered wafer, preferably both surfaces, is ground. This grinding process is also called a lapping process, and grinding is performed using a predetermined abrasive to remove the unevenness of the wafer surface while maintaining the flatness of the wafer.

[0060] Next, the polished wafer was etched by 8 to 15 μm in total from both sides using a mixed solution of 85% by mass phosphoric acid aqueous solution, 30% by mass hydrogen peroxide, and ultrapure water. The wafer was etched by immersing the entire wafer in the etching solution.

[0061] Next, the main surface of the wafer is polished with a mirror polishing material to be finished into a mirror surface.

[0062] Next, cleaning is performed to manufacture the indium phosphide wafer according to the embodiment of the present invention.

[0063] 〔Semiconductor epitaxial wafer〕

[0064] On the main surface of the indium phosphide substrate of the embodiment of the present invention, a semiconductor thin film is epitaxially grown by a known method to form an epitaxial crystal layer, thereby making it possible to manufacture a semiconductor epitaxial wafer. As an example of this epitaxial growth, a HEMT structure can be formed by epitaxially growing an InAlAs buffer layer, an InGaAs channel layer, an InAlAs spacer layer, and an InP electron supply layer on the main surface of the indium phosphide substrate. In the case of manufacturing a semiconductor epitaxial wafer having such a HEMT structure, generally, the mirror-finished indium phosphide substrate is subjected to an etching treatment using an etching solution such as sulfuric acid / hydrogen peroxide to remove impurities such as silicon (Si) attached to the surface of the substrate. In a state where the back side of the indium phosphide substrate after the etching treatment is in contact with a base and supported by the base, an epitaxial film is formed on the main surface of the indium phosphide substrate by a molecular beam epitaxy method (MBE: Molecular Beam Epitaxy) or an organic metal vapor deposition method (MOCVD: Metal Organic Chemical Vapor Deposition).

[0065] At this time, the warping of the back side of the indium phosphide substrate of the embodiment of the present invention is reduced as described above, so the contact between the back side of the substrate and the susceptor becomes uniform. Therefore, heat conduction is evenly distributed in the surface of the indium phosphide substrate, and epitaxial growth can be performed while the substrate temperature is uniform.

[0066] [Example]

[0067] Hereinafter, examples are provided for better understanding of the present invention and its advantages, but the present invention is not limited to these examples.

[0068] Examples 1 to 6 and Comparative Examples 1 to 5 were prepared as follows.

[0069] First, an ingot of a single crystal of indium phosphide grown to a predetermined diameter is prepared.

[0070] Next, the outer circumference of the ingot of the single crystal of indium phosphide was ground into a cylindrical shape.

[0071] Next, a wafer having a main surface and a back surface is cut out from the ground ingot of indium phosphide. At this time, a wire saw is used to cut off both ends of the crystal of the ingot of indium phosphide along a specified crystal plane, and a plurality of wafers are cut out with a specified thickness. In the process of cutting out the wafer, a new wire is continuously fed while the metal wire is reciprocated in the horizontal direction, and a stage carrying the ingot of indium phosphide is moved in the vertical direction toward the metal wire.

[0072] The conditions for cutting the ingot using a wire saw are as follows.

[0073] · New wire supply speed of metal wire: 10~60m / min

[0074] ·Reciprocating speed of metal wire: recorded in Table 1

[0075] ·Vertical moving speed of the stage carrying the ingot of indium phosphide: as shown in Table 1

[0076] ·Management of abrasives for wire saws

[0077] The abrasive used was GC#1200, and the cutting oil was PS-LP-500D. The abrasive was managed so that the viscosity of the viscometer rotor shaft at a rotation speed of 60 rpm would be the viscosity shown in Table 1. The viscosity was measured using a TVB-10 viscometer manufactured by Toki Sangyo.

[0078] Next, in order to remove the process-degraded layer generated in the cutting process using the wire saw, the cut wafer was etched from both sides by a mixed solution of 85 mass % phosphoric acid aqueous solution and 30 mass % hydrogen peroxide by the amount listed in Table 1 (etching after cutting). The wafer was etched by immersing the entire wafer in the etching solution.

[0079] Next, the outer peripheral portion of the wafer is chamfered, and both sides of the chamfered wafer are ground (lapped). At this time, grinding is performed using a predetermined grinding material, thereby removing the unevenness of the wafer surface while maintaining the flatness of the wafer.

[0080] Next, the polished wafer was etched from both sides by a mixed solution of 85 mass % phosphoric acid aqueous solution, 30 mass % hydrogen peroxide, and ultrapure water by a total etching amount (etching thickness from the surface) listed in Table 1 (etching after polishing). The wafer was etched by immersing the entire wafer in the etching solution.

[0081] Next, the main surface of the wafer was polished with a mirror polishing material to a mirror finish, and then cleaned, thereby producing an indium phosphide substrate having a wafer outer diameter shown in Table 1.

[0082] (evaluate)

[0083] ·Back evaluation

[0084] The samples of Examples 1 to 6 and Comparative Examples 1 to 5 were placed in a PP box with the back side facing upward using Ultrasort manufactured by Corning Tropel, and the SORI value and WARP value were measured by automatic conveyance except for the outer peripheral portion with a width of 3 mm, and the BOW value was also measured. This measurement was performed in a non-adsorption manner.

[0085] Surface evaluation

[0086] The samples of Examples 1 to 6 and Comparative Examples 1 to 5 were placed in a PP box with the surface facing upward using Ultrasort manufactured by Corning Tropel, and the WARP value and TTV value excluding the outer peripheral portion with a width of 3 mm were measured by automatic conveyance. The measurement was performed without adsorption.

[0087] It should be noted that the "TTV value" is explained. As for TTV (Total Thickness Variation), the indium phosphide substrate is supported, the surface opposite to the measurement surface is adsorbed, and the adsorbed surface is set as the reference surface. In the direction perpendicular to the reference surface, the difference between the highest position and the lowest position of the measurement surface of the substrate observed from the reference surface is the TTV value. The TTV value can be measured using, for example, Ultrasort manufactured by Corning Tropel, and the indium phosphide substrate surface can be placed in a PP box facing upward and automatically transported, thereby measuring.

[0088] Table 1 shows the above-mentioned production conditions and evaluation results.

[0089] [Table 1]

[0090]

[0091] (Evaluation results)

[0092] In Examples 1 to 6, each of the indium phosphide substrates having an absolute value of BOW of 2.0 μm or less when placed on a flat surface with the back surface facing upward and having uniform contact between the back surface of the substrate and the susceptor was obtained.

[0093] In Comparative Examples 1 to 3, the parameters in the cutting step using the wire saw were inappropriate, resulting in indium phosphide substrates with large back surface warpage.

[0094] In Comparative Example 4, in the etching step after cutting, the etching amount was inappropriate, and processing damage during cutting could not be removed, resulting in an indium phosphide substrate with large back surface warpage.

[0095] In Comparative Example 5, in the etching step after polishing, the etching amount was inappropriate, and processing damage during polishing could not be removed, resulting in an indium phosphide substrate with large back surface warpage.

Claims

1. An indium phosphide substrate, characterized in that: The indium phosphide substrate has a main surface for forming an epitaxial crystal layer and a back surface opposite to the main surface. The BOW value of the back surface of the indium phosphide substrate measured with the back surface facing upward is -2.0 to 2.0 μm, wherein the BOW value is measured as follows: When the measurement is performed in a manner that the indium phosphide substrate is supported and the original shape is not changed, a triangle with three points as vertices is drawn on the measurement surface of the indium phosphide substrate in a manner that surrounds the center point of the substrate, and the plane containing the triangle is set as a three-point reference plane. The three points are (0.97R, 90°), (0.97R, 210°), and (0.97R, 330°) when the polar coordinates of the center of the OF are taken as 270° with the center of the substrate as the origin and the radius of the substrate is set as R. In the direction perpendicular to the three-point reference plane, the distance between the center point of the substrate and the three-point reference plane is expressed as a BOW value by setting the upward direction as a positive value and the downward direction as a negative value. The indium phosphide substrate is obtained by the following manufacturing method: While the metal wire is reciprocated at a reciprocating speed of 300 to 350 m / min in the horizontal direction, a new wire is continuously fed, and a stage carrying an ingot of indium phosphide is moved toward the metal wire at a moving speed of 200 to 400 μm / min in the vertical direction. A wafer is cut from the ingot of indium phosphide using a wire saw with an abrasive viscosity of 300 to 400 mPa·s, and the cut wafer is ground by etching only 5 to 15 μm in total from both sides, and the ground wafer is etched only 8 to 15 μm in total from both sides.

2. The indium phosphide substrate according to claim 1, wherein The BOW value of the back surface of the indium phosphide substrate measured in a state where the back surface is facing upward is −1.5 to 1.0 μm.

3. The indium phosphide substrate according to claim 2, wherein: The BOW value of the back surface of the indium phosphide substrate measured in a state where the back surface is facing upward is −0.3 to 0.9 μm.

4. The indium phosphide substrate according to claim 3, wherein: The BOW value of the back surface of the indium phosphide substrate measured in a state where the back surface is facing upward is −0.3 to 0.9 μm, and the diameter of the substrate is 100 mm or less.

5. The indium phosphide substrate according to claim 3, wherein The BOW value of the back surface of the indium phosphide substrate measured in a state where the back surface was facing upward was −0.3 to 0.5 μm, and the diameter of the substrate was 76.2 mm or less.

6. The indium phosphide substrate according to claim 3, wherein: The BOW value of the back surface of the indium phosphide substrate measured in a state where the back surface is facing upward is 0.0 to 0.7 μm, and the diameter of the substrate is 50.8 mm or less.

7. The indium phosphide substrate according to any one of claims 1 to 6, wherein The SORI value of the back surface of the indium phosphide substrate measured in a state where the back surface is facing upward is 2.5 μm or less.

8. The indium phosphide substrate according to claim 7, wherein: The SORI value of the back surface of the indium phosphide substrate measured in a state where the back surface is facing upward is 1.6 to 2.5 μm.

9. The indium phosphide substrate according to any one of claims 1 to 6, characterized in that The WARP value of the back surface of the indium phosphide substrate measured in a state where the back surface is facing upward is 3.5 μm or less.

10. The indium phosphide substrate according to claim 9, wherein The WARP value of the back surface of the indium phosphide substrate measured in a state where the back surface is facing upward is 1.8 to 3.5 μm.

11. The indium phosphide substrate according to claim 10, wherein: The WARP value of the back surface of the indium phosphide substrate measured in a state where the back surface is facing upward is 1.8 to 3.4 μm. 12 . A semiconductor epitaxial wafer comprising an epitaxial crystal layer on the main surface of the indium phosphide substrate according to claim 1 .

13. A method for manufacturing an indium phosphide substrate according to any one of claims 1 to 11, comprising: The process of cutting wafers from an ingot of indium phosphide using a wire saw; A step of etching the cut wafer; A step of chamfering the outer peripheral portion of the etched wafer; A step of grinding at least one surface of the chamfered wafer; as well as The step of etching the polished wafer, The step of cutting the wafer from the ingot of indium phosphide by using a wire saw includes: moving a metal wire back and forth in a horizontal direction while continuously feeding a new wire, and moving a stage carrying the ingot of indium phosphide in a vertical direction toward the metal wire, The new wire feeding speed of the metal wire is 10-60 m / min, the reciprocating speed of the metal wire is 300-350 m / min, the vertical moving speed of the stage carrying the ingot of indium phosphide is 200-400 μm / min, the viscosity of the abrasive of the wire saw is 300-400 mPa·s, In the step of etching the cut wafer, only 5 to 15 μm in total is etched from both sides. In the step of etching the polished wafer, only 8 to 15 μm in total are etched from both sides.

Citation Information

Patent Citations

  • Method for epitaxial growth

    JP2003218033A

  • Multiple lapping cut-off method for solid substances

    CH629997A5

  • Method for producing an epitaxially coated semiconductor wafer

    CN101575701A

  • Method for machining nitride semiconductor wafer, nitride semiconductor wafer, process for producing nitride semiconductor device, and nitride semiconductor device

    CN101884094A

  • Indium phosphide substrate manufacturing method, epitaxial wafer manufacturing method, indium phosphide substrate, and epitaxial wafer

    CN102187020A