Thermoelectric conversion material, thermoelectric conversion element and thermoelectric conversion module

By forming a concentrated layer of aluminum in the thermoelectric conversion material to inhibit oxidation, the problem of easy oxidation and insufficient thermal conductivity of the thermoelectric conversion material is solved, the oxidation resistance and thermoelectric conversion efficiency are improved, and the manufacturing process is simplified.

CN113272977BActive Publication Date: 2024-10-15MITSUBISHI MATERIALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980084281.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-26
Filing Date
2019-11-12
Publication Date
2024-10-15
Estimated Expiration
2039-11-12

AI Technical Summary

Technical Problem

Existing thermoelectric conversion materials are easily oxidized, resulting in reduced thermoelectric properties and fragile components. The glass coating has problems with thermal expansion differences and high manufacturing costs. The vacuum container increases costs but has insufficient thermal conductivity, which affects thermoelectric conversion efficiency.

Method used

The sintered body uses magnesium silicide as the main component. By forming an aluminum concentrated layer between the magnesium oxide layer and the magnesium silicide phase, the metal aluminum phase composed of aluminum or aluminum alloy is used to suppress oxidation, and the thickness of the aluminum concentrated layer is controlled to be more than 10nm and 100nm. below, maintaining thermal conductivity and stability.

Benefits of technology

A thermoelectric conversion material with excellent oxidation resistance and high thermoelectric conversion efficiency has been realized, which avoids oxidation damage and reduced heat conduction, improves the stability and reliability of components, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113272977B_ABST
    Figure CN113272977B_ABST
Patent Text Reader

Abstract

A thermoelectric conversion material, comprising a sintered body containing magnesium silicide as a main component, characterized in that it comprises a magnesium silicide phase (12) and a magnesium oxide layer (13) formed on the surface of the magnesium silicide phase (12), an aluminum concentrated layer (14) having a higher Al concentration than the interior of the magnesium silicide phase (12) is formed between the magnesium oxide layer (13) and the magnesium silicide phase (12), and the aluminum concentrated layer (14) has a metal aluminum phase (15) composed of aluminum or an aluminum alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermoelectric conversion material, a thermoelectric conversion element and a thermoelectric conversion module composed of a sintered body containing magnesium silicide as a main component.

[0002] This application claims priority based on Japanese Patent Application No. 2018-242588 filed in Japan on December 26, 2018, and the contents are incorporated herein by reference. Background Art

[0003] Thermoelectric conversion elements composed of thermoelectric conversion materials are electronic components that can convert heat and electricity into each other through the so-called Seebeck effect and Peltier effect. The Seebeck effect is an effect that converts thermal energy into electrical energy. It is a phenomenon that an electromotive force is generated when a temperature difference occurs at both ends of a thermoelectric conversion material. This electromotive force is determined by the characteristics of the thermoelectric conversion material. In recent years, the development of thermoelectric power generation using this effect has been booming.

[0004] The thermoelectric conversion element is configured such that electrodes are formed on one end side and the other end side of a thermoelectric conversion material.

[0005] As an index representing the characteristics of such a thermoelectric conversion element (thermoelectric conversion material), for example, a power factor (PF) represented by the following formula (1) or a dimensionless performance index (ZT) represented by the following formula (2) is used. In addition, in a thermoelectric conversion material, since a temperature difference needs to be maintained between one side and the other side, it is preferred that the thermal conductivity is low.

[0006] PF=S 2 σ……(1)

[0007] Where, S: Seebeck coefficient (V / K), σ: electrical conductivity (S / m)

[0008] ZT=S 2 σT / κ……(2)

[0009] Where T = absolute temperature (K), κ = thermal conductivity (W / (m×K))

[0010] As the above-mentioned thermoelectric conversion material, for example, as shown in Patent Document 1, a thermoelectric conversion material obtained by adding various dopants to magnesium silicide has been proposed.

[0011] Here, the thermoelectric conversion material composed of the above-mentioned magnesium silicide tends to be easily oxidized, and the oxidation may cause a decrease in thermoelectric characteristics or embrittlement of the element.

[0012] Therefore, Patent Document 2 mentioned above proposes a technique for preventing oxidation of a thermoelectric conversion material by covering the thermoelectric conversion material with glass.

[0013] Patent Document 1: Japanese Patent Application Publication No. 2013-179322 (A)

[0014] Patent Document 2: Japanese Patent Application Publication No. 2017-050325 (A)

[0015] As shown in Patent Document 2, when the thermoelectric conversion material is coated with glass, there is a concern that the glass may peel off and oxidation of the thermoelectric conversion material may not be suppressed due to the difference in thermal expansion coefficients between the thermoelectric conversion material and the glass. In addition, the glass must be coated on the entire surface of the thermoelectric conversion material constituting each thermoelectric conversion element, resulting in a problem of increased manufacturing costs.

[0016] Here, in order to suppress oxidation of the thermoelectric conversion material, it is conceivable to house the module incorporating the thermoelectric conversion material in a container filled with a vacuum or an inert gas.

[0017] However, in this case, in order to ensure the strength of the container, the manufacturing cost may increase.

[0018] In addition, when the container is made of stainless steel, the thermal conductivity of stainless steel is lower than that of copper, aluminum, etc., so the heat transfer to the element becomes poor, resulting in heat loss. Moreover, even if the container is formed thicker to ensure the strength of the container, the thermal conductivity becomes insufficient. Therefore, the thermoelectric conversion efficiency of the thermoelectric conversion module may be reduced. Summary of the invention

[0019] The present invention has been completed in view of the above situation, and its purpose is to provide a thermoelectric conversion material composed of a sintered body containing magnesium silicide as a main component and capable of constituting a thermoelectric conversion module having excellent oxidation resistance and excellent thermoelectric conversion efficiency, as well as a thermoelectric conversion element and a thermoelectric conversion module using the thermoelectric conversion material.

[0020] In order to solve the above-mentioned problems, the thermoelectric conversion material of the present invention is composed of a sintered body containing magnesium silicide as a main component, characterized in that it has a magnesium silicide phase and a magnesium oxide layer formed on the surface of the magnesium silicide phase, an aluminum concentrated layer having a higher Al concentration than that inside the magnesium silicide phase is formed between the magnesium oxide layer and the magnesium silicide phase, and the aluminum concentrated layer has a metallic aluminum phase composed of aluminum or an aluminum alloy.

[0021] According to the thermoelectric conversion material of this structure, an aluminum concentration layer having a higher Al concentration than that inside the magnesium silicide phase is formed between the magnesium oxide layer and the magnesium silicide phase, and the aluminum concentration layer has a metallic aluminum phase composed of aluminum or an aluminum alloy. Therefore, through the aluminum concentration layer, it is possible to suppress the intrusion of oxygen into the magnesium silicide phase and suppress the oxidation of the magnesium silicide phase.

[0022] Therefore, a thermoelectric conversion material having excellent oxidation resistance and stable characteristics can be provided. In addition, due to the excellent oxidation resistance, it is not necessary to accommodate the thermoelectric conversion module in which the thermoelectric conversion element is assembled in a container, and a thermoelectric conversion module having excellent thermoelectric conversion efficiency and ensuring thermal conductivity can be constructed.

[0023] In addition, the metal aluminum phase is composed of aluminum or an aluminum alloy (containing Al and one or two of Mg and Si).

[0024] Here, in the thermoelectric conversion material of the present invention, the thickness of the aluminum concentrated layer is preferably in the range of 10 nm to 100 nm.

[0025] In this case, since the thickness of the aluminum concentration layer is set to be 10 nm or more, the aluminum concentration layer can reliably suppress the intrusion of oxygen into the magnesium silicide phase. On the other hand, since the thickness of the aluminum concentration layer is set to be 100 nm or less, the aluminum concentration layer does not increase the thermal conductivity of the entire thermoelectric element, and the thermal conductivity of the main constituent elements can be maintained. Therefore, it is possible to prevent the dimensionless figure of merit ZT from being reduced.

[0026] Furthermore, in the thermoelectric conversion material of the present invention, the magnesium silicide phase may be composed of undoped magnesium silicide.

[0027] In this case, the magnesium silicide phase is composed of undoped magnesium silicide containing no dopant, but since the Mg2Si phase is stabilized by a trace amount of Al diffused into the Mg2Si phase and becomes an n-type with a high ZT, there is no need to use various dopant elements that are complicated to process, thereby improving manufacturing efficiency.

[0028] Here, undoped magnesium silicide containing no dopant means that the content of impurities, i.e., dopant elements (e.g., Li, Na, K, B, Ga, In, N, P, As, Sb, Bi, Ag, Cu, Y) added to make thermoelectric materials is 1.0×10 18 Atom / cm 3 the following.

[0029] Alternatively, in the thermoelectric conversion material of the present invention, the magnesium silicide phase may contain one or more selected from Li, Na, K, B, Ga, In, N, P, As, Sb, Bi, Ag, Cu, and Y as dopants.

[0030] In this case, the thermoelectric conversion material can be made into a specific semiconductor type, that is, an n-type thermoelectric conversion material or a p-type thermoelectric conversion material.

[0031] The thermoelectric conversion element of the present invention is characterized by comprising the above-mentioned thermoelectric conversion material and electrodes respectively bonded to one surface and the other surface of the thermoelectric conversion material.

[0032] According to the thermoelectric conversion element of this structure, since it includes the thermoelectric conversion material having excellent oxidation resistance, various characteristics are stabilized. Therefore, the thermoelectric conversion performance is stable and the reliability is excellent.

[0033] The thermoelectric conversion module of the present invention is characterized by comprising the above-mentioned thermoelectric conversion element and terminals respectively connected to the electrodes of the thermoelectric conversion element.

[0034] According to the thermoelectric conversion module of this structure, since the thermoelectric conversion element is provided, the thermoelectric conversion material has excellent oxidation resistance and various characteristics are stabilized. Therefore, the thermoelectric conversion performance is stable and the reliability is excellent.

[0035] According to the present invention, a thermoelectric conversion material composed of a sintered body containing magnesium silicide as a main component and capable of constituting a thermoelectric conversion module having excellent oxidation resistance and excellent thermoelectric conversion efficiency, and a thermoelectric conversion element and a thermoelectric conversion module using the thermoelectric conversion material can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a cross-sectional view of a thermoelectric conversion material, a thermoelectric conversion element, and a thermoelectric conversion module according to an embodiment of the present invention.

[0037] Figure 2 It is an explanatory diagram of a thermoelectric conversion material according to an embodiment of the present invention.

[0038] Figure 3 This is a diagram showing an example of XPS analysis results of the thermoelectric conversion material according to the embodiment of the present invention.

[0039] Figure 4 This is a flowchart of a method for producing a thermoelectric conversion material according to an embodiment of the present invention.

[0040] Figure 5 This is a cross-sectional view showing an example of a sintering device used in the method for producing a thermoelectric conversion material according to an embodiment of the present invention. DETAILED DESCRIPTION

[0041] Hereinafter, with reference to the accompanying drawings, a thermoelectric conversion material, a thermoelectric conversion element, and a thermoelectric conversion module according to an embodiment of the present invention will be described. In addition, the embodiments shown below are specifically described for the purpose of better understanding the gist of the invention, and unless otherwise specified, the present invention is not limited thereto. Furthermore, in order to facilitate understanding of the features of the present invention and for convenience, the drawings used in the following description sometimes enlarge the main parts, and the dimensional ratios of the various components are not necessarily the same as the actual ones.

[0042] Figure 1Detailed Description of the Invention A thermoelectric conversion material 11 according to an embodiment of the present invention, and a thermoelectric conversion element 10 and a thermoelectric conversion module 1 using the thermoelectric conversion material 11 are shown.

[0043] The thermoelectric conversion element 10 includes a thermoelectric conversion material 11 of the present embodiment, and electrodes 18 a and 18 b formed on one surface 11 a and the other surface 11 b of the thermoelectric conversion material 11 .

[0044] Furthermore, the thermoelectric conversion module 1 includes terminals 19 a and 19 b respectively connected to the electrodes 18 a and 18 b of the thermoelectric conversion element 10 .

[0045] The electrodes 18a and 18b are made of nickel, silver, cobalt, tungsten, molybdenum, etc. The electrodes 18a and 18b can be formed by electric sintering, electroplating, electrodeposition, etc.

[0046] Terminals 19a and 19b are formed of a metal material with excellent electrical conductivity, such as a plate material such as copper or aluminum. In this embodiment, a rolled plate of aluminum is used. In addition, the thermoelectric conversion material 11 (electrodes 18a and 18b) and the terminals 19a and 19b can be joined by Ag wax or Ag plating.

[0047] Furthermore, the thermoelectric conversion material 11 of the present embodiment is a sintered body containing magnesium silicide as a main component.

[0048] Here, the thermoelectric conversion material 11 can be composed of undoped magnesium silicide that does not contain a dopant, or it can be composed of magnesium silicide that contains one or more selected from Li, Na, K, B, Ga, In, N, P, As, Sb, Bi, Ag, Cu, and Y as a dopant.

[0049] Here, it means that the content of magnesium silicide in the sintered body containing magnesium silicide as a main component is 90 mass % or more.

[0050] The content of magnesium silicide can be directly obtained by analyzing the sintered body by existing analytical methods (e.g., electron probe microanalyzer (EPMA) method, powder X-ray diffraction method, etc.), and can also be indirectly derived from the mass % of Mg2Si relative to elements (e.g., Mg2Si, Sb, Al) other than elements lost from the sintered body under sintering conditions, in the compounds (or elements) contained in the raw material powder for producing the sintered body.

[0051] In the present embodiment, the thermoelectric conversion material 11 is obtained by adding antimony (Sb) as a dopant to magnesium silicide (Mg2Si). For example, the thermoelectric conversion material 11 of the present embodiment has a composition containing antimony in the range of 0.1 atomic % or more and 2.0 atomic % or less in Mg2Si. In addition, in the thermoelectric conversion material 11 of the present embodiment, by adding antimony as a pentavalent donor, it becomes an n-type thermoelectric conversion material with a high carrier density.

[0052] Here, as a donor for making the thermoelectric conversion material 11 as an n-type thermoelectric conversion element, bismuth, phosphorus, arsenic, etc. can be used in addition to antimony.

[0053] Furthermore, the thermoelectric conversion material 11 can be used as a p-type thermoelectric conversion element, which can be obtained by adding a dopant such as lithium or silver as an acceptor.

[0054] Furthermore, in the thermoelectric conversion material 11 of the present embodiment, Figure 2 As shown, it comprises a magnesium silicide phase 12 composed of the above-mentioned magnesium silicide (Mg2Si doped with Sb), a magnesium oxide layer 13 formed on the surface of the magnesium silicide phase 12, and an aluminum concentrated layer 14 formed between the magnesium silicide phase 12 and the magnesium oxide layer 13 and having an Al concentration higher than that inside the magnesium silicide phase 12.

[0055] Furthermore, the aluminum-concentrated layer 14 has a metal aluminum phase 15 composed of aluminum or an aluminum alloy.

[0056] Furthermore, the aluminum concentrated layer 14 may include an aluminum oxide phase composed of aluminum oxide and an aluminum alloy oxide phase composed of aluminum alloy oxide in addition to the metal aluminum phase 15 composed of aluminum or an aluminum alloy.

[0057] Figure 3 2 shows the XPS analysis results of the thermoelectric conversion material 11 of the present embodiment. Figure 3 The horizontal axis of represents the sputtering depth, which corresponds to the depth from the surface layer (the outermost surface of the magnesium oxide layer 13), and the vertical axis represents the atomic concentration.

[0058] Immediately after the start of sputtering (ie, the outermost layer), a region (magnesium oxide layer 13) having high concentrations of magnesium and oxygen is formed.

[0059] According to XPS analysis, the oxygen concentration in the magnesium oxide layer 13 is 45 atomic % or more, the magnesium concentration is 40 atomic % or more, the Al concentration is 1.5 atomic % or less, and the silicon concentration is 1.0 atomic % or less.

[0060] Then, as the sputtering time progresses, there is a region where the oxygen concentration decreases unidirectionally and the silicon concentration increases unidirectionally. In this region, the aluminum concentration increases (1.5 times or more of the Al concentration at a depth of 500 nm from the surface (corresponding to the inside of the magnesium silicide phase)), which corresponds to the aluminum concentrated layer 14 described above.

[0061] According to XPS analysis, the oxygen concentration in the aluminum concentrated layer 14 decreases unidirectionally from 48 atomic % to 3.0 atomic % from the surface toward the inside, the magnesium concentration is maintained in the range of 36 atomic % to 45 atomic %, and the silicon concentration increases unidirectionally from 2 atomic % to 48 atomic % from the surface toward the inside.

[0062] As the sputtering time progresses, a region appears where the aluminum concentration decreases to less than 1.5 times the Al concentration at a depth of 500 nm from the surface layer while the oxygen concentration remains below 5 atomic % and the silicon concentration and magnesium concentration remain above 45 atomic %. This region becomes the magnesium silicide phase 12.

[0063] Furthermore, in the present embodiment, the thickness of the aluminum concentration layer 14 is preferably within a range of 10 nm to 100 nm.

[0064] The thickness of the aluminum concentration layer 14 is more preferably 20 nm or more, and more preferably 30 nm or more. On the other hand, the thickness of the aluminum concentration layer 14 is more preferably 90 nm or less, and more preferably 80 nm or less.

[0065] Below, reference Figure 4 and Figure 5 A method for producing the thermoelectric conversion material 11 according to the present embodiment will be described.

[0066] (Magnesium silicide powder preparation step S01)

[0067] First, a powder of magnesium silicide (Mg 2 Si) which is to be a parent phase of a sintered body of the thermoelectric conversion material 11 is produced.

[0068] In the present embodiment, the magnesium silicide powder preparation step S01 includes a bulk magnesium silicide formation step S11 of obtaining bulk magnesium silicide and a pulverization step S12 of pulverizing the bulk magnesium silicide (Mg2Si) into powder.

[0069] In the bulk magnesium silicide forming step S11, silicon powder, magnesium powder and a dopant added as needed are measured and mixed. For example, when forming an n-type thermoelectric conversion material, a pentavalent material such as antimony and bismuth is mixed as a dopant, and when forming a p-type thermoelectric conversion material, a material such as lithium or silver is mixed as a dopant. In addition, no dopant may be added to form undoped magnesium silicide.

[0070] In the present embodiment, antimony is used as a dopant in order to obtain an n-type thermoelectric conversion material, and the amount of dopant added is set within a range of 0.1 atomic % to 2.0 atomic %.

[0071] Then, for example, the mixed powder is introduced into an alumina crucible, heated to a temperature in the range of 800° C. to 1150° C., and cooled to solidify, thereby obtaining bulk magnesium silicide.

[0072] In addition, since a small amount of magnesium sublimes during heating, when measuring the raw materials, magnesium is preferably added in an amount of, for example, about 3 atomic % to 5 atomic % relative to the stoichiometric composition of Mg:Si=2:1.

[0073] In the pulverizing step S12, the obtained bulk magnesium silicide is pulverized by a pulverizer to form magnesium silicide powder.

[0074] Here, it is preferable that the average particle size of the magnesium silicide powder be within a range of 1 μm to 100 μm.

[0075] In addition, regarding the magnesium silicide powder to which the dopant is added, the dopant is uniformly present in the magnesium silicide powder.

[0076] In addition, when a commercially available magnesium silicide powder or a magnesium silicide powder to which a dopant is added is used, the bulk magnesium silicide forming step S11 and the pulverizing step S12 can also be omitted.

[0077] (Sintering Raw Material Powder Forming Step S02)

[0078] Next, the obtained magnesium silicide powder is mixed with metal aluminum powder to obtain a sintering raw material powder.

[0079] Here, the content of the metal aluminum powder in the sintering raw material powder is preferably within a range of 0.01 mass % to 1.00 mass %.

[0080] Furthermore, as the metal aluminum powder, it is preferable to use aluminum powder having an aluminum purity of 99.0 mass % or more.

[0081] Furthermore, the average particle size of the metal aluminum powder is preferably within a range of 0.5 μm to 50 μm.

[0082] (Sintering process S03)

[0083] Next, the sintering raw material powder obtained as described above is heated while being pressurized to obtain a sintered body. In the sintering step S03, since the sintering raw material powder is a mixed powder of magnesium silicide powder and metal aluminum powder, metal aluminum exists between the magnesium silicide powders, and an aluminum concentration layer 14 having a metal aluminum phase 15 is formed on the surface layer of the magnesium silicide phase 12. In addition, Al in the metal aluminum powder reacts with Mg and Si in the magnesium silicide powder to form an aluminum alloy containing Al and one or both of Mg and Si. In addition, the magnesium oxide layer 13 is formed by oxidation of the surface of the magnesium silicide powder.

[0084] Here, in this embodiment, in the sintering step S03, Figure 5 The sintering device shown (electric sintering device 100).

[0085] Figure 5 The sintering device (electric sintering device 100) shown in the figure is provided with, for example, a pressure-resistant frame 101, a vacuum pump 102 for decompressing the interior of the pressure-resistant frame 101, a hollow cylindrical carbonaceous model 103 distributed in the pressure-resistant frame 101, a pair of electrode parts 105a, 105b for pressurizing the sintering raw material powder Q filled in the carbonaceous model 103 and applying current, and a power supply device 106 for applying voltage between the pair of electrode parts 105a, 105b. In addition, a carbon plate 107 and a carbon sheet 108 are respectively arranged between the electrode parts 105a, 105b and the sintering raw material powder Q. In addition, a thermometer, a displacement meter, etc. not shown in the figure are also provided. In addition, in the present embodiment, a heater 109 is arranged on the outer peripheral side of the carbonaceous model 103. The heater 109 is arranged on the four side surfaces in a manner covering the entire surface of the outer peripheral side of the carbonaceous model 103. As the heater 109 , a carbon heater, a nichrome wire heater, a molybdenum heater, a Kanthal wire heater, a high-frequency heater, or the like can be used.

[0086] In the sintering step S03, first, Figure 5 The carbonaceous mold 103 of the electric sintering device 100 shown is filled with sintering raw material powder Q. The interior of the carbonaceous mold 103 is covered with, for example, a graphite sheet or a carbon sheet. In addition, a power supply device 106 is used to flow a direct current between a pair of electrode parts 105a and 105b, so that the current flows through the sintering raw material powder Q, thereby raising the temperature by self-heating. In addition, the electrode part 105a on the movable side of the pair of electrode parts 105a and 105b is moved toward the sintering raw material powder Q, and the sintering raw material powder Q is pressurized at a predetermined pressure between the electrode part 105b on the fixed side. In addition, the heater 109 is heated.

[0087] Thus, the sintering raw material powder Q is sintered by the self-heat of the sintering raw material powder Q and the heat and pressure from the heater 109 .

[0088] In this embodiment, regarding the sintering conditions in the sintering step S03, the sintering temperature of the raw material powder Q is set within a range of 800°C to 1020°C, the holding time at the sintering temperature is set to 5 minutes or less, and the press load is set within a range of 20 MPa to 50 MPa.

[0089] Furthermore, the atmosphere in the pressure-resistant housing 101 may be an inert atmosphere such as an argon atmosphere or a vacuum atmosphere. In the case of a vacuum atmosphere, the pressure may be 5 Pa or less.

[0090] Here, when the sintering temperature of the raw material powder Q is lower than 800°C, the oxide film formed on the surface of each powder of the sintered raw material powder Q cannot be fully removed, resulting in the surface oxide film of the raw material powder itself remaining at the grain boundary, and the raw material powders are not sufficiently bonded to each other and the density of the sintered body is reduced. Therefore, the resistance of the obtained thermoelectric conversion material may become high.

[0091] On the other hand, when the sintering temperature of the raw material powder Q exceeds 1020° C., the decomposition of magnesium silicide proceeds in a short time, causing composition deviation, increasing resistance, and decreasing the Seebeck coefficient.

[0092] Therefore, in the present embodiment, the sintering temperature in the sintering step S03 is set within a range of 800° C. or higher and 1020° C. or lower.

[0093] The sintering temperature in the sintering step S03 is preferably 800° C. or higher, and more preferably 900° C. or higher. On the other hand, the sintering temperature in the sintering step S03 is preferably 1020° C. or lower, and more preferably 1000° C. or lower.

[0094] Furthermore, when the holding time at the sintering temperature exceeds 5 minutes, magnesium silicide decomposes, causing composition deviation, increasing resistance, and decreasing Seebeck coefficient. In addition, particles may coarsen and thermal conductivity may increase.

[0095] Therefore, in the present embodiment, the holding time at the sintering temperature in the sintering step S03 is set to 5 minutes or less.

[0096] In addition, the holding time at the sintering temperature in the sintering step S03 is preferably set to 3 minutes or less, and more preferably 2 minutes or less.

[0097] In addition, when the pressurizing load in the sintering step S03 is less than 20 MPa, the density does not increase and there is a possibility that the resistance of the thermoelectric conversion material may increase.

[0098] On the other hand, when the pressurizing load in the sintering step S03 exceeds 50 MPa, the force applied to the carbon jig is large and may cause the jig to break.

[0099] Therefore, in the present embodiment, the pressurizing load in the sintering step S03 is set within the range of 20 MPa to 50 MPa.

[0100] The pressurizing load in the sintering step S03 is preferably 23 MPa or more, more preferably 25 MPa or more. On the other hand, the pressurizing load in the sintering step S03 is preferably 50 MPa or less, more preferably 45 MPa or less.

[0101] (Heat treatment step S04)

[0102] Next, after the sintering step S03 , heat treatment is performed to form the aluminum concentration layer 14 .

[0103] Here, the conditions of the heat treatment step S04 are preferably to set the atmosphere to air or steam atmosphere, the heat treatment temperature to be in the range of 500° C. to 600° C., and the holding time at the heat treatment temperature to be in the range of 5 minutes to 15 minutes.

[0104] The thermoelectric conversion material 11 of the present embodiment is manufactured through the above-described steps.

[0105] According to the thermoelectric conversion material 11 of the present embodiment having the above structure, an aluminum concentrated layer 14 having a higher Al concentration than the inside of the magnesium silicide phase 12 is formed between the magnesium silicide phase 12 composed of magnesium silicide and the magnesium oxide layer 13. The aluminum concentrated layer 14 has a metal aluminum phase 15 composed of aluminum or an aluminum alloy. Therefore, the aluminum concentrated layer 14 can suppress the intrusion of oxygen into the magnesium silicide phase 12 and suppress the oxidation of the magnesium silicide phase 12. Therefore, it is possible to provide a thermoelectric conversion material 11 having excellent oxidation resistance and stable characteristics.

[0106] In addition, in the present embodiment, when the thickness of the aluminum concentration layer 14 is set to 10 nm or more, the aluminum concentration layer 14 can reliably suppress the intrusion of oxygen into the magnesium silicide phase 12 .

[0107] On the other hand, when the thickness of the aluminum concentration layer 14 is set to 100 nm or less, the aluminum concentration layer 14 does not increase the thermal conductivity of the entire element and can maintain a thermal conductivity not higher than that of the main component. Therefore, the heat exchange efficiency of the thermoelectric conversion module 1 can be improved.

[0108] Furthermore, in the thermoelectric conversion element 10 and the thermoelectric conversion module 1 of the present embodiment, since the thermoelectric conversion material 11 having excellent oxidation resistance is provided, various characteristics are stabilized. Therefore, the thermoelectric conversion performance is stable and the reliability is excellent.

[0109] As mentioned above, although embodiment of this invention was described, this invention is not limited to this, It can change suitably within the range which does not deviate from the technical idea of ​​this invention.

[0110] For example, in this embodiment, as a configuration such as Figure 1 Although the form of the thermoelectric conversion module of the structure shown is described, it is not limited to this. If the thermoelectric conversion material of the present invention is used, the structure and arrangement of electrodes and terminals are not particularly limited.

[0111] Furthermore, in this embodiment, as the use Figure 5 Although the sintering is performed by the sintering apparatus (electrical sintering apparatus 100 ) shown in the figure, the present invention is not limited thereto, and a method for indirectly sintering by heating and pressurizing the sintering raw material, such as hot pressing, HIP, etc., may be used.

[0112] Furthermore, in the present embodiment, the form of the sintering raw material is described as a magnesium silicide powder to which antimony (Sb) is added as a dopant, but the present invention is not limited to this. For example, one or more selected from Li, Na, K, B, Ga, In, N, P, As, Sb, Bi, Ag, Cu, and Y may be included as a dopant, and these elements may also be included in addition to Sb.

[0113] Furthermore, a sintered body of undoped magnesium silicide containing no dopant may be used.

[0114] Example

[0115] Hereinafter, the results of experiments performed to confirm the effects of the present invention will be described.

[0116] Prepare Mg with a purity of 99.9% by mass (particle size 180 μm: Kojundo Chemical Lab. Co., Ltd.), Si with a purity of 99.99% by mass (particle size 300 μm: Kojundo Chemical Lab. Co., Ltd.), and Sb with a purity of 99.9% by mass (particle size 300 μm: Kojundo Chemical Lab. Co., Ltd.), and weigh them, mix them thoroughly in a mortar, put them in an alumina crucible, and heat them at 850°C for 2 hours in Ar-3 vol% H2. Considering the deviation from the stoichiometric composition of Mg:Si=2:1 caused by the sublimation of Mg, 5 atomic% of Mg is added. Thus, a bulk magnesium silicide (Mg2Si) with the composition shown in Table 1 is obtained.

[0117] Next, the bulk magnesium silicide (Mg2Si) was finely crushed in a mortar and classified to obtain magnesium silicide powder (Mg2Si powder) having an average particle size of 30 μm.

[0118] Furthermore, metal aluminum powder (purity 99.9 mass %, particle size 10 μm) was prepared, and predetermined amounts of magnesium silicide powder and metal aluminum powder were weighed and mixed to obtain a sintering raw material powder.

[0119] The obtained sintering raw material powder is filled into a carbonaceous mold covered with a carbon sheet. Figure 5 The sintering apparatus shown (electrical sintering apparatus 100 ) performed electric sintering under the conditions shown in Table 1.

[0120] Then, a measurement sample was collected from the obtained thermoelectric conversion material, and the aluminum content in the thermoelectric conversion material was measured by fluorescent X-ray analysis (scanning fluorescent X-ray analyzer ZSX PrimusII manufactured by Rigaku Corporation).

[0121] The obtained thermoelectric conversion material was observed as follows to evaluate the presence or absence of a metal aluminum phase in the aluminum concentration layer, the Al concentration ratio to the magnesium silicide phase, the thickness of the aluminum concentration layer, and the oxide film thickness.

[0122] The obtained thermoelectric conversion material was placed in a photoelectron spectrometer (ULVAC-PHI PHI5000VersaProbe2), and the binding energy of Mg2p, Si2p, Al2p, and O1s was analyzed. Regarding the analysis conditions, a 50W Monochromated AlK alpha ray was used as an X-ray source. The measurement area is 200μm×200μm. Then, Ar ion etching was performed for 1 minute, and the binding energy of Mg, Si, Al, and O was analyzed again. This operation was repeated to evaluate the atomic binding state by the concentration change of each element in the depth direction and the change in binding energy. The Ar ion etching conditions are that the acceleration voltage of the ions is set to 2.0kV and the grating width is set to 2.4mm×2.4mm. The depth generated by etching is calculated as follows. A silicon oxide film of a specified film thickness is formed on a Si wafer. First, the sputtering rate of the silicon oxide film is calculated. The etching depth is calculated by setting the etching rate of MgO to half of that of the silicon oxide film.

[0123] Regarding the presence or absence of a metallic aluminum phase in the aluminum concentrated layer, the case where an Al concentration of 1.5 times or more of the Al concentration at a depth of 500 nm was detected was determined as “presence”.

[0124] Regarding the thickness of the aluminum concentrated layer, the aluminum concentrated layer was defined as a range of Al concentration that was 1.5 times or more of the Al concentration at a depth of 500 nm.

[0125] The Al concentration ratio to the magnesium silicide phase is defined as (the peak Al concentration of the aluminum concentrated layer) / (Al concentration at a depth of 500 nm).

[0126] The oxide film thickness is set to a depth where the oxygen concentration becomes 90 atomic % or less of the concentration at the outermost surface.

[0127] [Table 1]

[0128]

[0129] [Table 2]

[0130]

[0131] ※Relative evaluation when Comparative Example 1 is set to 1

[0132] In Comparative Example 1 which does not contain aluminum and is composed of Sb-doped magnesium silicide, no aluminum concentration layer is formed, and the oxide film becomes thicker, 209 nm.

[0133] In Comparative Example 2 which does not contain aluminum and is composed of undoped magnesium silicide, no aluminum concentration layer is formed, and the oxide film thickness becomes thicker, namely 215 nm.

[0134] On the other hand, in Example 1-6 of the present invention in which aluminum was contained and an aluminum concentration layer was formed and a metal aluminum phase was confirmed in the aluminum concentration layer, the oxide film thickness was suppressed to 55 nm or less.

[0135] From the above, it was confirmed that according to the present example, a thermoelectric conversion material composed of a sintered body containing magnesium silicide as a main component and having excellent oxidation resistance can be provided.

[0136] Industrial Applicability

[0137] A thermoelectric conversion module composed of a sintered body containing magnesium silicide as a main component and having excellent oxidation resistance and excellent thermoelectric conversion efficiency can be provided.

[0138] Explanation of symbols

[0139] 1-thermoelectric conversion module, 10-thermoelectric conversion element, 11-thermoelectric conversion material, 12-magnesium silicide phase, 13-magnesium oxide layer, 14-aluminum concentration layer, 15-metal aluminum phase, 18a, 18b-electrodes, 19a, 19b-terminals.

Claims

1. A thermoelectric conversion material, comprising a sintered body containing magnesium silicide as a main component, characterized in that: A magnesium silicide phase and a magnesium oxide layer formed on the surface of the magnesium silicide phase. An aluminum-concentrated layer having a higher Al concentration than the interior of the magnesium silicide phase is formed between the magnesium oxide layer and the magnesium silicide phase, and the aluminum-concentrated layer has a metal aluminum phase composed of aluminum or an aluminum alloy. The thickness of the aluminum concentrated layer is within a range of 10 nm to 100 nm.

2. The thermoelectric conversion material according to claim 1, characterized in that The magnesium silicide phase is composed of undoped magnesium silicide.

3. The thermoelectric conversion material according to claim 1, characterized in that The magnesium silicide phase is composed of magnesium silicide containing a dopant, and the dopant is one or more selected from Li, Na, K, B, Ga, In, N, P, As, Sb, Bi, Ag, Cu, and Y.

4. A thermoelectric conversion element, characterized in that: A thermoelectric conversion material according to any one of claims 1 to 3, and electrodes respectively bonded to one surface and the other surface of the thermoelectric conversion material.

5. A thermoelectric conversion module, characterized in that: A thermoelectric conversion element according to claim 4 and terminals respectively connected to the electrodes of the thermoelectric conversion element.