Oil-water separation filter and method for manufacturing the same
By forming a water- and oil-repellent membrane on the surface of nonwoven fibers, the problems of poor separation of emulsified oil and water-soluble oil and performance degradation in cold environments in existing technologies are solved, achieving efficient and convenient oil-water separation.
Patent Information
- Application Number
- CN202110126339.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-25
- Filing Date
- 2021-01-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-01-29
AI Technical Summary
Existing oil-water separators are ineffective at separating emulsified or water-soluble oils, and their performance deteriorates after thawing in cold environments.
A water- and oil-repellent membrane is formed on the surface of nonwoven fibers, containing fluorinated functional groups and silica sol gel. Heat treatment is used to improve the membrane's strength and permeability, ensuring that it maintains high-efficiency separation performance even after freezing and thawing.
It achieves efficient separation of emulsified oil and water-soluble oil, and maintains good oil-water separation performance during freezing and thawing, simplifying the manufacturing process.
Smart Images

Figure CN113274765B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an oil-water separation filter capable of separating emulsified oil or water-soluble oil obtained by emulsifying oil into water and oil and a method for manufacturing the same. More specifically, the present invention relates to an oil-water separation filter having a water-repellent and oil-repellent film (hereinafter sometimes referred to as water-repellent and oil-repellent) formed on the fiber surface of a nonwoven fabric and a method for manufacturing the same. Background Art
[0002] Generally, a mixed liquid containing water and oil is classified into floating oil in which oil floats on the water surface, dispersed oil in which oil particles float in water, and emulsified oil or water-soluble oil in which oil and water are mixed and emulsified, depending on the mixing state of the oil and water.
[0003] The applicant has proposed an oil-water separation porous body having a porous substrate and an oil-water separation filter having the same, wherein the porous substrate is formed of a nonwoven fabric having a plurality of pores extending between a side into which a mixed liquid containing water and oil flows and another side opposite to the side (see Patent Document 1 (claim 1, claim 7, paragraph
[0020] , paragraph
[0074] )). The opening diameter of the pores of the oil-water separation porous body is greater than or equal to 0.1 μm and less than or equal to 180 μm, and an oil-water separation body is formed on the surface of the pores, and the oil-water separation body has an oil-water separation material containing a fluorine-based compound, and the fluorine-based compound has an oil-repellent imparting group and a hydrophilic imparting group.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-64405
[0007] Patent document 2: Japanese Patent Application Publication No. 2000-202247. Summary of the invention
[0008] Problem that the invention aims to solve
[0009] When the mixed liquid containing water and oil is the above-mentioned floating oil, dispersed oil, i.e., water-insoluble oil, Fig.12 As shown in (a), the surface of the oil particle 1a of the water-insoluble oil 1 is covered with an alkyl group 1b such as CH3. The alkyl group 1b has no affinity with water and is non-hydrophilic. Therefore, if the water-insoluble oil 1 is left, the oil particle 1a has a smaller specific gravity than the water 1c. Therefore, in order to reduce its surface tension, the oil particles 1a float while bonding to each other. Therefore, the oil-water separation filter having an oil-water separation body with hydrophilic and oil-repellent properties shown in Patent Document 1 can separate the mixed liquid into water and oil and filter it when the mixed liquid is a water-insoluble oil.
[0010] On the other hand, in the case where the mixed liquid is an emulsified oil or a water-soluble oil which is emulsified by mixing oil and water, Fig.12 As shown in (b), the surface of the oil particle 2a of the water-soluble oil 2 is covered with a hydroxyl group 2b. The hydroxyl group 2b has a high affinity for water 2c, and even if the water-soluble oil 2 is left standing, the oil particles 2a will be stably dispersed in the water. The oil-water separation filter shown in Patent Document 1 has the following problem: Since the oil-water separator is a fluorine-based compound with hydrophilic and oil-repellent properties, the water-soluble oil in which the oil particles are stably dispersed in water is not chemically blocked by the oil-water separator having a hydrophilicity-imparting group on the oil particles covered with hydroxyl groups, but passes through a porous substrate such as a non-woven fabric, making it impossible to separate the mixed liquid into water and oil. Therefore, it is known that an emulsified oil or aqueous oil is separated into water and oil by using an oil-water separation device using a hollow fiber membrane (for example, refer to Patent Document 2 (claim 6, paragraph
[0028] , Figure 5 )). However, this oil-water separation device has a problem of complex structure.
[0011] In addition, the oil-water separation filter shown in Patent Document 1 has the following problem: even if the heat treatment described later is performed, the oil-water separation membrane is composed of only fluorine-based compounds and does not contain a binder such as silica sol hydrolyzate (referred to as silica sol gel in this specification) that binds to the non-woven fabric. Therefore, when the oil-water separation filter is frozen by cold air and then thawed and used in a cold area, the oil-water separation performance of the oil-water separation filter deteriorates.
[0012] The first object of the present invention is to provide an oil-water separation filter that can separate emulsified oil or water-soluble oil obtained by emulsifying oil into water and oil with a simple structure. The second object of the present invention is to provide an oil-water separation filter whose oil-water separation performance does not deteriorate even if it is thawed and dried after freezing. The third object of the present invention is to provide an oil-water separation filter that has good filtration efficiency for removing oil from a liquid containing water and oil and has a short liquid flow time. The fourth object of the present invention is to provide a method for simply manufacturing such an oil-water separation filter.
[0013] Solutions for solving problems
[0014] The present inventors have performed the following operations: first, by making the oil-water separation membrane formed on the fiber surface of the non-woven fabric of the oil-water separation filter contain a fluorine-containing functional group component having water-repellency and oil-repellency, the fiber surface of the non-woven fabric chemically bounces off the oil particles of the water-soluble oil and solidifies the non-woven fabric; second, by using a silica sol gel having a hydroxyl group as the main component in the water-repellent and oil-repellent membrane, the non-woven fabric maintains water permeability; third, by making the air permeability of the oil-water separation filter a specified value, the pores of the non-woven fabric are reduced and the oil particles of the water-soluble oil are physically prevented from passing through, thereby completing the present invention. In addition, the present inventors have found that if the non-woven fabric formed with the water-repellent and oil-repellent membrane containing the above-mentioned fluorine-containing functional group component is heat-treated at 30°C to 120°C for 1 hour to 24 hours, the silanol groups contained in the silica sol gel are bonded to each other, and the bonding of the silanol groups to the surface of the non-woven fabric is promoted. As a result, the siloxane bond with the surface of the nonwoven fabric becomes strong, so the hardness is further increased, and the oil-water separation performance does not deteriorate even if it is thawed after freezing.
[0015] A first aspect of the present invention is an oil-water separation filter, characterized in that it comprises a nonwoven fabric having a plurality of pores formed between fibers, the plurality of pores extending between a side through which a mixed liquid containing water and oil flows in and another side opposite to the side through which the mixed liquid flows out, a water-repellent and oil-repellent film is formed on the fiber surface of the nonwoven fabric, the water-repellent and oil-repellent film comprises a fluorine-containing functional group component (A) having both water-repellent and oil-repellent functions and a silica sol gel (C), and the air permeability of the oil-water separation filter is 0.05 ml / cm 2 / sec~14ml / cm 2 / sec, the fluorinated functional group component (A) comprises a perfluoroether structure represented by the following general formula (1) or (2).
[0016] [Chemistry 1]
[0017]
[0018] In the above formula (1) and formula (2), p, q and r are the same or different from each other and are integers of 1 to 6, and may be linear or branched. In the above formula (1) and formula (2), X is a hydrocarbon group having 2 to 10 carbon atoms and may contain one or more bonds selected from ether bonds, CO-NH bonds, O-CO-NH bonds and sulfonamide bonds. In the above formula (1) and formula (2), Y is a hydrolyzate of silane or a main component of silica sol-gel.
[0019] The second viewpoint of the present invention is an oil-water separation filter, which is an invention based on the first viewpoint. When a 20 mm square polyethylene terephthalate film contact moves on the aforementioned side with a vertical load of 50 g, a moving speed of 5 mm / second, and a moving distance of 20 mm, the reduction rate of the dynamic friction coefficient after 10 reciprocating movements relative to the initial dynamic friction coefficient is less than 10%.
[0020] The third aspect of the present invention is an oil-water separation filter, which is an invention based on the first aspect, wherein the fiber surface of the nonwoven fabric is provided with a plurality of layers of oil-water separation filter per 1 m 2 The water- and oil-repellent film is formed on the nonwoven fabric in a ratio of 0.1 g to 30 g.
[0021] A fourth aspect of the present invention is an oil-water separation filter, which is an invention based on the first aspect, wherein the fluorine-containing functional group component (A) is contained in a ratio of 0.01% to 10% by mass when the silica sol gel (C) is set to 100% by mass (hereinafter sometimes referred to as "the silica sol gel (C)").
[0022] The fifth aspect of the present invention is an oil-water separation filter, which is an invention based on the first aspect, wherein the water-repellent and oil-repellent membrane comprises metal oxide particles (B) having an average particle size of 2nm~90nm and silica sol gel (C) bonded to the fluorine-based functional group component (A), and when the water-repellent and oil-repellent membrane is set to 100% by mass, the fluorine-based functional group component (A) is contained in a ratio of 0.3% by mass to 5.0% by mass, and when the water-repellent and oil-repellent membrane is set to 100% by mass, the fluorine-based functional group component (A) and the metal oxide particles (B) are contained in a total ratio of 20% by mass to 80% by mass, and the mass ratio (A / B) of the fluorine-based functional group component (A) to the metal oxide particles (B) is in the range of 0.01~0.2.
[0023] The sixth aspect of the present invention is an oil-water separation filter, which is an invention based on the first aspect, wherein the fluorine-based functional group component (A) has a first fluorine-containing functional group component (A1) bonded to metal oxide particles (B) having an average particle size of 2nm to 90nm, and a second fluorine-containing functional group component (A2) contained in the silica sol gel (C), and when the water-repellent and oil-repellent film is set to 100% by mass, the total content ratio of the first fluorine-containing functional group component (A1) and the second fluorine-containing functional group component (A2) is 0.5% by mass to 15% by mass, and the mass ratio (C:B) of the silica sol gel (C) to the metal oxide particles (B) is in the range of 10:90 to 90:10.
[0024] A seventh aspect of the present invention is an oil-water separation filter, which is the invention based on the fifth aspect or the sixth aspect, wherein the metal oxide particles (B) are oxide particles of one or two metals selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr.
[0025] An eighth aspect of the present invention is an oil-water separation filter according to the sixth aspect of the invention, wherein the content of the first fluorine-functional component (A1) is equal to or greater than the content of the second fluorine-functional component (A2) in terms of mass ratio.
[0026] A ninth aspect of the present invention is an oil-water separation filter according to the first aspect of the invention, wherein the silica sol gel further contains 0.5 to 20 mass % of an alkylene component having 2 to 7 carbon atoms, when the silica sol gel is 100 mass %.
[0027] A tenth aspect of the present invention is an oil-water separation filter according to the invention of the first aspect, wherein the nonwoven fabric is composed of a single layer or a laminate of multiple layers.
[0028] The eleventh aspect of the present invention is an oil-water separation filter, which is an invention based on the first aspect, wherein the fibers constituting the non-woven fabric are one or more fibers selected from the group consisting of polyethylene terephthalate (PET), polypropylene (PP), glass, alumina, carbon, cellulose, pulp, nylon and metal.
[0029] A twelfth aspect of the present invention is an oil-water separation filter according to the invention according to the eleventh aspect, wherein the fibers constituting the nonwoven fabric corresponding to the side into which the mixed liquid containing water and oil flows are glass fibers.
[0030] The thirteenth aspect of the present invention is a method for manufacturing an oil-water separation filter, which includes the following steps: a step of adding a catalyst to a mixed solution obtained by mixing a silicon alkoxide, a fluorine-based compound containing the fluorine-containing functional group component (A) of the first aspect, an alcohol and water to prepare a liquid composition for forming a water-repellent and oil-repellent film; a step of mixing the aforementioned liquid composition for forming a water-repellent and oil-repellent film with a solvent to prepare a diluent; a step of immersing a non-woven fabric in the aforementioned diluent; a step of forming a water-repellent and oil-repellent film on the fiber surface of the aforementioned non-woven fabric by dehydrating and drying the aforementioned impregnated non-woven fabric; and a step of heat-treating the non-woven fabric formed with the aforementioned water-repellent and oil-repellent film in the atmosphere at a temperature of 30°C to 120°C for 1 hour to 24 hours.
[0031] The fourteenth aspect of the present invention is a method for manufacturing an oil-water separation filter, which includes the following steps: a step of dispersing the metal oxide particles (B) of the fifth aspect in an organic solvent to prepare a dispersion of the metal oxide particles; a step of mixing a fluorine-containing compound containing the fluorine-containing functional group component (A) described in claim 1, water and a catalyst into the dispersion of the aforementioned metal oxide particles to prepare a dispersion of fluorine-containing metal oxide particles; a step of adding a catalyst to a mixed solution obtained by mixing silicon alkoxide, alcohol and water to prepare a silica sol-gel solution; a step of mixing the aforementioned dispersion of fluorine-containing metal oxide particles with a diluted solution of the aforementioned silica sol-gel solution to prepare a liquid composition for forming a water-repellent and oil-repellent film; a step of immersing a non-woven fabric in the diluted solution of the aforementioned liquid composition for forming a water-repellent and oil-repellent film; and a step of dehydrating and drying the aforementioned immersed non-woven fabric.
[0032] A fifteenth aspect of the present invention is a method for manufacturing an oil-water separation filter, which is the invention based on the fourteenth aspect, wherein the metal oxide particles (B) are oxide particles of one or two metals selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr.
[0033] The sixteenth aspect of the present invention is a method for manufacturing an oil-water separation filter, which includes the following steps: a step of dispersing the metal oxide particles (B) of the sixth aspect in an organic solvent to prepare a dispersion of the metal oxide particles; a step of mixing a fluorine-containing compound containing the first fluorine-containing functional group component (A1) of the sixth aspect, water and a catalyst into the aforementioned dispersion of the metal oxide particles to prepare a dispersion of fluorine-containing metal oxide particles; a step of adding a mixed catalyst to a mixed solution obtained by mixing a fluorine-containing compound containing the second fluorine-containing functional group component (A2) of the sixth aspect, a silicon alkoxide, an alcohol and water to prepare a fluorine-containing silica sol-gel solution; a step of mixing the aforementioned dispersion of fluorine-containing metal oxide particles with the aforementioned fluorine-containing silica sol-gel solution to prepare a liquid composition for forming a water-repellent and oil-repellent film; a step of immersing a non-woven fabric in a diluted solution of the aforementioned liquid composition for forming a water-repellent and oil-repellent film; and a step of dehydrating and drying the aforementioned immersed non-woven fabric.
[0034] The seventeenth aspect of the present invention is a method for manufacturing an oil-water separation filter, which is the invention based on the sixteenth aspect, wherein the metal oxide particles (B) are oxide particles of one or two metals selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr.
[0035] Effects of the Invention
[0036] In the oil-water separation filter of the first aspect of the present invention, the water-repellent and oil-repellent membrane comprises a fluorine-containing functional group component having both water-repellent and oil-repellent functions represented by the aforementioned general formula (1) or formula (2), and at the same time, the air permeability of the oil-water separation filter is set to 0.05 ml / cm 2 / sec~14ml / cm 2 / second to limit the pores of the nonwoven fabric. Therefore, when the mixed liquid is immersed in the oil-water separation filter, if the oil particles in the mixed liquid are larger than the pore size, the oil particles in the mixed liquid are physically blocked from passing through. Moreover, even if the oil particles in the mixed liquid are slightly smaller than the pore size, the fiber surface of the nonwoven fabric will chemically bounce off the oil particles of the water-soluble oil.
[0037] On the other hand, the water-repellent and oil-repellent materials represented by polytetrafluoroethylene and the like are difficult to impart water permeability to nonwoven fabrics due to the absence of hydroxyl groups, but in the present invention, the water-repellent and oil-repellent film is a silica sol gel having a hydroxyl group as a main component, therefore, water permeability can be imparted to the nonwoven fabric. As a result, even if the mixed liquid is an emulsified oil or a water-soluble oil, the oil will be retained in the oil-water separation filter, and the water will pass through the oil-water separation filter, thereby being able to be separated into water and oil. Furthermore, the water-repellent and oil-repellent film of the present invention includes a silica sol gel as a main component, therefore, the water-repellent and oil-repellent film is firmly adhered to the fiber surface of the nonwoven fabric and has durability.
[0038] The oil-water separation filter of the second aspect of the present invention is an oil-water separation filter in which, when a contact of a 20 mm square polyethylene terephthalate film moves on the above-mentioned one side with a vertical load of 50 g, a moving speed of 5 mm / second, and a moving distance of 20 mm, the reduction rate of the dynamic friction coefficient after 10 reciprocating movements relative to the initial dynamic friction coefficient is less than 10%. Therefore, the non-woven fabric having a water-repellent and oil-repellent film formed with a silica sol gel containing the above-mentioned fluorine-containing functional group component has a high hardness, and the oil-water separation performance of the oil-water separation filter does not deteriorate even if it is thawed after being frozen.
[0039] In the oil-water separation filter according to the third aspect of the present invention, the fiber surface of the nonwoven fabric is provided with a thickness of 1 m 2 The nonwoven fabric forms a water- and oil-repellent film in a ratio of 0.1 g to 30 g, and therefore, the water- and oil-repellent effect is higher and the air permeability of the nonwoven fabric can be appropriately maintained.
[0040] In the oil-water separation filter according to the fourth aspect of the present invention, the fluorine-containing functional group component (A) is contained in a ratio of 0.01% to 10% by mass when the silica sol-gel (C) is 100% by mass. Therefore, the water- and oil-repellent effect is higher without impairing the adhesion of the water- and oil-repellent film to the nonwoven fabric.
[0041] The oil-water separation filter of the fifth aspect of the present invention comprises metal oxide particles (B) with an average particle size of 2nm to 90nm bonded with a fluorine-based functional group component (A) and a silica sol gel (C). Therefore, when the oil-water separation filter is frozen by cold air in a cold area and the non-woven fabric is thawed and dried for use, the strength of the water-repellent and oil-repellent membrane is increased due to the presence of the metal oxide particles, and the oil-water separation membrane is difficult to peel off from the fibers of the non-woven fabric. As a result, the expansion of the fibers of the non-woven fabric is suppressed, the air permeability of the oil-water separation filter remains almost unchanged, and the oil-water separation performance does not deteriorate.
[0042] In addition, when the water-repellent and oil-repellent film is set to 100% by mass, the fluorine-based functional group component (A) is included in a ratio of 0.3% by mass to 5.0% by mass, so the oil-repellent effect is higher, and the adhesion of the water-repellent and oil-repellent film to the nonwoven fabric is not damaged. In addition, when the aforementioned water-repellent and oil-repellent film is set to 100% by mass, the fluorine-based functional group component (A) and the aforementioned metal oxide particles (B) are included in a ratio of 20% by mass to 80% by mass, and the mass ratio (A / B) of the aforementioned fluorine-based functional group component (A) relative to the metal oxide particles (B) is in the range of 0.01 to 0.2, so the oil-repellent effect is higher, and the adhesion of the water-repellent and oil-repellent film to the nonwoven fabric is not damaged.
[0043] In the oil-water separation filter of the sixth aspect of the present invention, the water-repellent and oil-repellent membrane comprises metal oxide particles (B) with an average particle size of 2nm~90nm bonded to the first fluorine-based functional group component (A1) and a silica sol gel (C) containing a second fluorine-based functional group component (A2), so that the formed membrane has high water repellency and oil repellency. In addition, during film formation, the metal oxide particles (B) with an average particle size of 2nm~90nm are bonded to each other in the membrane through the silica sol gel (C), so that the strength of the membrane and the adhesion of the membrane can be improved. The oil-water separation filter has the advantages of good filtration efficiency for removing oil from a liquid containing water and oil and a short liquid flow time.
[0044] In the oil-water separation filter of the seventh aspect of the present invention, the metal oxide particles contained in the water-repellent and oil-repellent membrane are oxide particles of one or two metals selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr. Therefore, metal oxide particles suitable for the use environment of the oil-water separation filter can be included from the multiple metal oxide particles.
[0045] In the oil-water separation filter of the eighth aspect of the present invention, the mass ratio of the first fluorine-functional group component (A1) to the second fluorine-functional group component (A2) is the same or the mass ratio of the first fluorine-functional group component (A1) is greater than that of the second fluorine-functional group component (A2), so that the water- and oil-repellent film has high adhesion to the fiber surface of the nonwoven fabric.
[0046] In the oil-water separation filter of the ninth aspect of the present invention, when the silica sol gel is set to 100 mass %, the silica sol gel also contains 0.5 mass % to 20 mass % of an alkylene component having 2 to 7 carbon atoms. Therefore, close adhesion with the fiber can be obtained, the thickness of the water-repellent and oil-repellent film becomes uniform, and the water-repellent and oil-repellent film can be given a better oil-water separation performance.
[0047] In the oil-water separation filter of the tenth aspect of the present invention, when the non-woven fabric is composed of a single layer, it becomes an oil-water separation filter with a simple structure. When the non-woven fabric is composed of a multi-layer stack, each layer can be constructed according to the properties such as the oil content ratio of the mixed liquid flowing in, the size of the oil particles, etc.
[0048] In the oil-water separation filter of the eleventh aspect of the present invention, the material of the fibers constituting the non-woven fabric can be selected from fibers of polyethylene terephthalate (PET), polypropylene (PP), glass, alumina, carbon, cellulose, pulp, nylon and metal, depending on the oil content ratio of the mixed liquid flowing in, the size of the oil particles and other properties, or according to the content of the alkylene component with 2 to 7 carbon atoms formed by hydrolysis of the epoxy-containing silane in the liquid composition used to form the water-repellent and oil-repellent film described later.
[0049] In the oil-water separation filter of the twelfth aspect of the present invention, by setting the fibers constituting the non-woven fabric corresponding to the side into which the mixed liquid containing water and oil flows into glass fibers, the water-repellent and oil-repellent film containing silica sol gel as the main component will be more firmly adhered to the glass fibers and will be difficult to peel off from the fibers of the non-woven fabric.
[0050] In the manufacturing method of the thirteenth aspect of the present invention, if a water-repellent and oil-repellent film having a silica sol gel containing the above-mentioned fluorine-containing functional group component is formed on the fiber surface of the non-woven fabric by drying, and then heat treatment is performed, the silanol groups contained in the silica sol gel are bonded to each other, and the bonding of the silanol groups to the surface of the non-woven fabric is promoted. As a result, since the siloxane bond with the surface of the non-woven fabric becomes strong, the hardness of the non-woven fabric is increased, and even if it is thawed after freezing, its oil-water separation performance will not deteriorate.
[0051] In the manufacture method of the 14th viewpoint of the present invention, by mixing the dispersion liquid of fluorinated metal oxide particles with silica sol gel liquid to prepare water-repellent and oil-repellent film-forming liquid composition, nonwoven fabric is impregnated in the diluent of the water-repellent and oil-repellent film-forming liquid composition, nonwoven fabric is deliquated and dried, thus manufacture oil-water separation filter, therefore, the first is to manufacture simply. The second is to be able to uniformly form water-repellent and oil-repellent film on the fiber surface of nonwoven fabric. In addition, the third is that the metal oxide particles that particle surface is water-repellent and oil-repellent are present in silica sol gel, therefore, both maintain water-repellent and oil-repellent and easily reduce the air permeability of nonwoven fabric.
[0052] In the manufacturing method according to the fifteenth aspect of the present invention, the metal oxide particles (B) are oxide particles of one or two metals selected from the group consisting of Si, Al, Mg, Ca, Ti, Zn and Zr. Therefore, an oil-water separation filter can be manufactured that includes metal oxide particles suitable for the use environment of the oil-water separation filter from a plurality of metal oxide particles.
[0053] In the manufacture method of the 16th viewpoint of the present invention, by mixing the dispersion of fluorine-containing metal oxide particles with fluorine-containing silica sol gel liquid and preparing water-repellent and oil-repellent film-forming liquid composition, nonwoven fabric is impregnated in the diluent of the water-repellent and oil-repellent film-forming liquid composition, nonwoven fabric is deliquated and dried, thus manufacture oil-water separation filter, therefore, the first is to manufacture simply. The second is to make water-repellent and oil-repellent film uniformly bonded to the fiber surface of nonwoven fabric, therefore oil-repellent performance can be fully obtained. In addition, the 3rd is that the particle surface is that the metal oxide particles of water-repellent and oil-repellent are present in the fluorine-containing silica sol gel, therefore, while the abrasion strength of film is improved, the air permeability of nonwoven fabric is easily reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 This is a configuration diagram of an oil-water separation device including an oil-water separation filter common to the first to third embodiments of the present invention.
[0055] Figure 2 This is a cross-sectional view of a single-layer nonwoven fabric according to the first embodiment of the present invention.
[0056] Figure 3 This is a cross-sectional view of a two-layer nonwoven fabric according to the first embodiment of the present invention.
[0057] Figure 4 This is a flow chart for manufacturing the oil-water separation filter according to the first embodiment of the present invention.
[0058] Figure 5 This is a cross-sectional view of a single-layer nonwoven fabric according to a second embodiment of the present invention.
[0059] Figure 6 This is a cross-sectional view of a two-layer nonwoven fabric according to a second embodiment of the present invention.
[0060] Figure 7 This is a flow chart for manufacturing the oil-water separation filter according to the second embodiment of the present invention.
[0061] Figure 8 This is a cross-sectional view of a single-layer nonwoven fabric according to a third embodiment of the present invention.
[0062] Fig. 9 This is a cross-sectional view of a two-layer nonwoven fabric according to a third embodiment of the present invention.
[0063] Fig.10 This is a flow chart for manufacturing the oil-water separation filter according to the third embodiment of the present invention.
[0064] Fig.11 It is a diagram showing the configuration of an apparatus used in the filtration test of each oil-water separation filter of the embodiment and the comparative example.
[0065] Fig.12 (a) is a schematic diagram of oil particles when the mixed liquid containing water and oil is a water-insoluble oil. Fig.12 (b) is a schematic diagram of oil particles when the mixed liquid containing water and oil is water-soluble oil. DETAILED DESCRIPTION
[0066] Next, the present specific embodiment will be described with reference to the drawings.
[0067] 〔Oil-water separation device〕
[0068] like Figure 1 As shown in the figure, the oil-water separation device 10 commonly used in the first to third embodiments of the present invention comprises: a cylindrical mixed liquid inflow portion 12 into which a mixed liquid 11 containing water and oil flows; a sheet-like oil-water separation filter 13, 113, 213 for separating the oil in the mixed liquid 11 from the water (see Figure 2 , Figure 5 , Figure 8 ); a funnel-shaped water collecting portion 16 for collecting the water 14 separated by the oil-water separation filter; and a bottomed cylindrical water storage portion 17 for storing the water 14 flowing in from the water collecting portion 16. An inflow pipe 18 for the mixed liquid is provided above the mixed liquid inflow portion 12, and a drain pipe 19 is provided at the bottom of the water storage portion 17.
[0069] When the oil-water separation filter 13, 113, 213 is composed only of non-woven fabric, although not shown in the figure, a metal porous support plate for reinforcing the non-woven fabric is provided on the lower surface of the oil-water separation filter 13, 113, 213 as a whole, so as to enable the filter to withstand the hydraulic pressure of the mixed liquid in the mixed liquid inlet part 12, and the oil-water separation filter 13, 113, 213 and the support plate are clamped by the mixed liquid inlet part 12 and the water collection part 16.
[0070] <First Embodiment>
[0071] 〔Oil-water separation filter〕
[0072] like Figure 2As shown in the figure, the oil-water separation filter 13 of the first embodiment comprises a nonwoven fabric 20 and a water-repellent and oil-repellent film 21 formed on the fiber surface of the nonwoven fabric. The nonwoven fabric 20, which is a main component of the oil-water separation filter 13, has a surface 20a into which a mixed liquid containing water and oil flows, and another surface 20b opposite to the surface 20a and from which the filtrate flows out, and is composed of a single layer. Figure 3 As shown in the figure, the nonwoven fabric can also be made into a two-layer laminate of an upper nonwoven fabric 30 and a lower nonwoven fabric 40 to form an oil-water separation filter 23. In this case, the upper surface of the upper nonwoven fabric 30 becomes a side 30a into which a mixed liquid containing water and oil flows, and the lower surface of the lower nonwoven fabric 40 becomes the other side 40b opposite to the side 30a and from which the filtrate flows out. The lower surface 30b of the nonwoven fabric 30 is in close contact with the upper surface 40a of the nonwoven fabric 40. It should be noted that the laminate is not limited to two layers, and can also be composed of multiple layers such as three layers and four layers.
[0073] like Figure 2 As shown in the enlarged view of FIG. 2 , the nonwoven fabric 20 is formed by entanglement of a plurality of fibers 20c, and pores 20d are formed between the fibers. The pores 20d penetrate between one side 20a and the other side 20b of the nonwoven fabric 20. A water-repellent and oil-repellent film 21 is formed on the surface of the fibers 20c of the nonwoven fabric. 2 The nonwoven fabric is formed into a water-repellent and oil-repellent film 21 at a ratio of 0.1 g to 30 g. The water-repellent and oil-repellent film 21 is formed by a silica sol gel containing a fluorine-containing functional group component having water-repellent and oil-repellent properties represented by the aforementioned general formula (1) or formula (2). When the silica sol gel is set to 100% by mass, the fluorine-containing functional group component is contained at a ratio of 0.01% to 10% by mass. In the state of the oil-water separation filter 13 having the water-repellent and oil-repellent film 21 formed on the fiber surface, the nonwoven fabric 20 has a 0.05 ml / cm 2 / sec~10ml / cm 2 The air permeability was measured using a Frazier tester described in JIS-L1913:2000.
[0074] Water and oil repellent film per 1m 2 When the amount of fluorine-containing functional group in the nonwoven fabric is less than 0.1 g or less than 0.01% by mass, the water-repellent and oil-repellent properties are insufficient, and the oil-water separation performance becomes insufficient. 2 If the non-woven fabric exceeds 30g, the air permeability is less than 0.05ml / cm 2 / sec. If the fluorine-containing functional group component exceeds 10% by mass, the adhesion to the nonwoven fabric will deteriorate. 2In nonwoven fabrics, the content is preferably 0.5 g to 10 g. In addition, when the silica sol gel is set to 100% by mass, the fluorine-containing functional group component is preferably contained in the range of 0.1% to 5% by mass. The air permeability is less than 0.05 ml / cm 2 / second, the water permeability is poor and it is difficult to obtain filtrate. If it exceeds 10ml / cm 2 / second, the size of the pores 20d of the nonwoven fabric is significantly larger than the oil particles 22 in the mixed liquid, and the oil particles 22 and water pass through the pores of the nonwoven fabric and escape from the oil-water separation filter 13, making it impossible to separate water from oil. The air permeability is preferably 0.1ml / cm 2 / sec~5ml / cm 2 / Second.
[0075] The function of the oil-water separation device 10 having the oil-water separation filter 13 will be described. Figure 1 As shown in FIG. 1 , first, the oil-water separation filter 13 is clamped by the mixed liquid inlet 12 and the water collecting part 16. Next, the mixed liquid 11 containing water and oil is supplied from the inlet pipe 18 to the mixed liquid inlet 12. The mixed liquid in this embodiment is a water-soluble oil. The mixed liquid 11 stored in the mixed liquid inlet 12 is in contact with one side 20a ( Figure 2 ). Here, the oil-water separation filter 13 has a predetermined air permeability, and the water-repellent and oil-repellent membrane 21 exhibits water-repellent and oil-repellent properties. Therefore, although water (not shown) of the water-soluble oil is repelled by the water-repellent and oil-repellent membrane 21, it can pass through due to the hydroxyl groups present in the silica sol gel. Figure 2 The water 14 reaches the other side 20b through the pores 20d formed between the fibers 20c and the fibers 20c as shown in the enlarged view of the embodiment, and is dripped from there and collected in the water collecting section 16. The collected water 14 flows from the water collecting section 16 to the water storage section 17 and is stored in the water storage section 17. When a certain amount of water 14 is stored in the water storage section 17, the drain valve (not shown) is opened to obtain the water 14 separated from the oil from the drain pipe 19.
[0076] On the other hand, Figure 2 As shown in the enlarged view of FIG. 1 , due to the oil repellency of the water-repellent and oil-repellent film 21 formed on the fiber surface of the nonwoven fabric 20, and due to the specified air permeability of the oil-water separation filter, it is needless to say that when the particle size is larger than the aperture of the pore 20d, even if the particle size is slightly smaller than the aperture of the pore 20d, the oil particles 22 cannot pass through the oil-water separation filter 13, but are retained between the fibers 20c and 20c of the nonwoven fabric 20. The oil retained in the nonwoven fabric 20 is recovered by periodically removing the oil-water separation filter 13 from the oil-water separation device 10.
[0077] [Method for manufacturing oil-water separation filter]
[0078] The oil-water separation filter is simply manufactured by the following method.
[0079] like Figure 4 As shown, a fluorine-containing silica sol gel (C) liquid is prepared by mixing silicon alkoxide, alcohol, a fluorine-containing functional group component (A), water, and an alkylene component as required, and a catalyst is added to the mixed liquid. A liquid composition for forming a water-repellent and oil-repellent film is prepared by mixing a solvent into the silica sol gel (C) liquid. A liquid obtained by diluting the liquid composition with a solvent is prepared, and the non-woven fabric 20 is immersed in the diluent and pulled from the diluent, and the non-woven fabric is spread on a horizontal metal mesh or the like in the atmosphere and at room temperature, and the liquid is removed until a certain amount of liquid is reached, and dried, so that a water-repellent and oil-repellent film is formed on the fiber surface of the non-woven fabric, and the non-woven fabric is heat-treated at a temperature of 30°C to 120°C in the atmosphere for 1 hour to 24 hours, thereby manufacturing an oil-water separation filter 13.
[0080] 〔Preparation of non-woven fabric〕
[0081] First, prepare a 0.3 ml / cm 2 / sec~10ml / cm 2 Specifically, in a state where an oil-water separation filter having a water-repellent and oil-repellent film described later is formed on the fiber surface of the nonwoven fabric, a nonwoven fabric having an air permeability of 0.05 ml / cm 2 / sec~10ml / cm 2 / sec air permeability of nonwoven fabric. 2 When the nonwoven fabric is slightly larger than the above range and forms a thick water-repellent and oil-repellent film, a nonwoven fabric with high air permeability is selected, and the air permeability is 1m 2 When the nonwoven fabric is slightly less than the above range and forms a thin water-repellent and oil-repellent film, a nonwoven fabric with low air permeability is selected.
[0082] As the nonwoven fabric, there are, for example, a cellulose mixed ester membrane filter, a glass fiber filter paper, and a nonwoven fabric mixed with polyethylene terephthalate fiber and glass fiber (manufactured by Anji Filter Paper Co., Ltd., trade name: 356). As such, the nonwoven fabric is made of one or more fibers selected from the group consisting of polyethylene terephthalate (PET), polypropylene (PP), glass, alumina, carbon, cellulose, pulp, nylon and metal. The fiber can be a fiber mixed with two or more fibers. In order to obtain the above-mentioned air permeability, the thickness of the fiber (fiber diameter) is preferably a thickness of 0.01 μm~10 μm. When the oil-water separation filter is a single layer, the thickness of the nonwoven fabric is 0.1 mm~5 mm, and when it is a multi-layer laminate, the thickness of the laminate is a thickness of 0.3 mm~7 mm. The main component of the water-repellent and oil-repellent film-forming material of the present invention is a silica sol gel, so in order to obtain adhesion with the fiber, it is preferably a material with a hydroxyl group. Among them, glass, alumina, cellulose nanofibers, etc. also have thin fiber diameters and can make the air permeability a low value within the above range.
[0083] As mentioned above, nonwoven fabrics such as Figure 3 In the case of a laminated body having a plurality of nonwoven fabrics 30, 40 as shown, by making the fibers constituting the nonwoven fabric 30 corresponding to the side into which the mixed liquid containing water and oil flows into glass fibers, the water-repellent and oil-repellent film containing silica sol gel as the main component will be more firmly adhered to the glass fibers and will be difficult to peel off from the fibers of the nonwoven fabric.
[0084] [Method for forming a water- and oil-repellent film on the fiber surface of a nonwoven fabric and method for heat treating the nonwoven fabric]
[0085] In order to form a water-repellent and oil-repellent film on the fiber surface of the nonwoven fabric of the first embodiment, a liquid composition for forming a water-repellent and oil-repellent film described later is prepared by diluting the liquid composition with an alcohol having a boiling point of less than 120°C and a carbon number in the range of 1 to 4 in a manner to reach a mass ratio (liquid composition: alcohol) of 1:1 to 50 relative to the liquid composition, and the nonwoven fabric is immersed in the diluent and pulled from the diluent, and the nonwoven fabric is spread on a horizontal metal mesh, etc. in the atmosphere and at room temperature, and the liquid is removed until a certain amount of liquid is reached. As another method, the nonwoven fabric pulled out is passed through a squeeze roll (press) for removal of liquid. The nonwoven fabric after removal of liquid is dried in the atmosphere at a temperature of 25 to 120°C for 0.5 hours to 24 hours.
[0086] Therefore, if Figure 2 As shown in the enlarged view of FIG. 2 , a water-repellent and oil-repellent film 21 is formed on the surface of the fiber 20c constituting the nonwoven fabric 20. 2In the range of 0.1g~30g of non-woven fabric, when the amount of deliquescence is small, the water-repellent and oil-repellent film forms a thick film on the fiber surface of the non-woven fabric, and when the amount of deliquescence is large, the water-repellent and oil-repellent film forms a thin film on the fiber surface of the non-woven fabric. Then, the dried non-woven fabric is heat-treated at a temperature of 30°C~120°C in the atmosphere for 1 hour to 24 hours. The heat treatment temperature is preferably 40°C~100°C, and the heat treatment time is preferably 1 hour to 20 hours. When the heat treatment temperature is less than the above lower limit or the heat treatment time is less than the above lower limit, the hardness of the non-woven fabric will not increase, and when thawing after freezing, the oil-water separation performance of the oil-water separation filter is easily deteriorated. In addition, if the heat treatment temperature exceeds the above upper limit or the heat treatment time exceeds the above upper limit, the water-repellent and oil-repellent film is thermally damaged, and the oil-water separation performance of the oil-water separation filter is easily deteriorated.
[0087] [Method for producing a liquid composition for forming a water- and oil-repellent film]
[0088] The liquid composition for forming a water- and oil-repellent film is produced by the following method.
[0089] 〔Preparation of mixed solution〕
[0090] First, tetramethoxysilane or tetraethoxysilane as silicon alkoxide, silane containing epoxy group as alkylene component, fluorine-containing silane as fluorine-containing functional group component, alcohol and water with boiling point less than 120°C and carbon number in the range of 1 to 4 are mixed to prepare a mixed solution. As the silicon alkoxide, specifically, tetramethoxysilane, its oligomer or tetraethoxysilane, its oligomer can be listed. For example, in order to obtain a durable water-repellent and oil-repellent film, tetramethoxysilane is preferably used. On the other hand, in the case of avoiding methanol generated during hydrolysis, tetraethoxysilane is preferably used. The silane containing epoxy group as the alkylene component can be mixed as needed.
[0091] As the epoxy-containing silane that becomes the above-mentioned alkylene component, specifically, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane or multifunctional epoxysilane can be cited. Relative to the total mass of silicon alkoxide and alkylene components, 1% to 40% by mass, preferably 2.5% to 20% by mass of alkylene components are included. When the alkylene component is less than 1% by mass as the lower limit, in the case of forming a film on the fiber of a non-woven fabric that does not contain hydroxyl groups, the adhesion to the fiber is likely to become insufficient. In addition, if it exceeds 40% by mass as the upper limit, the durability of the formed film is likely to be low. If the silane containing an epoxy group is included in such a manner that the alkylene component reaches the above-mentioned range of 1 to 40 mass %, the epoxy group also undergoes ring opening during the hydrolysis polymerization process and contributes to the polymerization, thereby improving the leveling property during the drying process and making the film thickness uniform. It should be noted that when the fibers of the non-woven fabric contain hydrophilic groups such as glass fibers, the content of the alkylene component can be a very small amount or zero. On the other hand, when the fibers of the non-woven fabric do not contain a hydrophilic group, it is preferred to contain 0.5 to 20 mass % of the alkylene component when the silica sol gel (C) is set to 100 mass %.
[0092] The alcohol having a carbon number in the range of 1 to 4 can include one or more alcohols in the range. As the alcohol, for example, methanol (boiling point is 64.7°C), ethanol (boiling point is about 78.3°C), propanol (n-propanol (boiling point is 97-98°C), isopropanol (boiling point is 82.4°C)) can be listed. Methanol or ethanol is particularly preferred. This is because these alcohols are easily mixed with silicon alkoxides. As the above-mentioned water, in order to prevent the mixing of impurities, it is desirable to use ion exchange water, pure water, etc. A mixed solution is prepared by adding an alcohol having a carbon number in the range of 1 to 4 and water to silicon alkoxides and silanes containing epoxy groups, preferably stirring at a temperature of 10°C to 30°C for 5 minutes to 20 minutes.
[0093] 〔Preparation of silica sol-gel solution〕
[0094] The mixed liquid prepared as above is mixed with a catalyst containing an organic acid, an inorganic acid or a titanium compound. At this time, the liquid temperature is preferably maintained at a temperature of 30°C to 80°C, and is preferably stirred for 1 to 24 hours. Thus, a silica sol-gel liquid containing silicon alkoxide, an epoxy-containing silane which becomes an alkylene component, and a fluorine-containing compound containing a fluorine-containing functional group component is prepared. When the silica sol-gel liquid is set to 100% by mass, the silica sol-gel liquid is composed of silicon alkoxide at a ratio of 2 to 50% by mass, epoxy-containing silane at a maximum ratio of 30% by mass, fluorine-containing compounds containing fluorine-containing functional groups at a ratio of 0.005% to 3% by mass, and alcohols having a carbon number in the range of 1 to 4 at a ratio of 20% by mass. ~ 98% by mass, water 0.1% by mass ~ The ratio of 40 mass %, the organic acid, inorganic acid or titanium compound as the catalyst is mixed in the ratio of 0.01 mass % to 5 mass %, and the hydrolysis reaction of silicon alkoxide, silane containing epoxy group and fluorine-containing functional group component is carried out to obtain. When the fluorine-containing functional group component is less than 0.005 mass % as the lower limit, the formed film is difficult to generate water and oil repellency, and if it exceeds 3 mass % as the upper limit, it is difficult to fit closely to the fiber surface of the nonwoven fabric.
[0095] The ratio of alcohol having a carbon number of 1 to 4 is limited to the above range because: when the ratio of alcohol is less than the lower limit, the silicon alkoxide will not dissolve in the solution but will separate, and the reaction solution will easily gel in the hydrolysis reaction. On the other hand, if it exceeds the upper limit, the amount of water and catalyst required for hydrolysis will be relatively small, so the reactivity of hydrolysis will decrease, polymerization will not proceed, and the adhesion of the film will decrease. The ratio of water is limited to the above range because: when it is less than the lower limit, the hydrolysis rate will slow down, so polymerization will not proceed, and the adhesion of the coating film will become insufficient. On the other hand, if it exceeds the upper limit, the reaction solution will gel in the hydrolysis reaction, and there will be too much water, so the silicon alkoxide compound will not dissolve in the alcohol aqueous solution but will separate.
[0096] When the silica sol-gel is set to 100 mass %, the SiO2 concentration (SiO2 amount) is preferably 1 mass % to 40 mass %. When the SiO2 concentration is less than the lower limit, polymerization is insufficient, and the adhesion of the film is reduced and cracks are easily generated. If it exceeds the upper limit, the proportion of water becomes relatively high, and the silicon alkoxide does not dissolve and the reaction solution gels.
[0097] Organic acid, inorganic acid or titanium compound functions as a catalyst for promoting hydrolysis reaction. As organic acid, formic acid and oxalic acid can be exemplified, as inorganic acid, hydrochloric acid, nitric acid, phosphoric acid can be exemplified, as titanium compound, tetrapropoxy titanium, tetrabutoxy titanium, tetraisopropoxy titanium, titanium lactate, etc. can be exemplified. Catalyst is not limited to the above substances. The ratio of the above catalyst is limited to the above range because: when it is lower than the lower limit, it lacks reactivity, polymerization becomes insufficient, and therefore no film is formed. On the other hand, even if it exceeds the upper limit, it does not affect reactivity, but the residual acid causes fiber corrosion of the nonwoven fabric and other unfavorable conditions.
[0098] The fluorine-based compound containing a fluorine-containing functional group component is represented by the following general formula (3) and formula (4). More specifically, the perfluoroether group in the above formula (3) and formula (4) includes perfluoroether structures represented by the following formulas (5) to (13).
[0099] [Chemistry 2]
[0100]
[0101] [Chemistry 3]
[0102]
[0103] [Chemistry 4]
[0104]
[0105] In addition, as X in the above formula (2) and formula (3), structures represented by the following formulas (14) to (18) can be listed. It should be noted that the following formula (14) shows an example including an ether bond, the following formula (15) shows an example including an ester bond, the following formula (16) shows an example including an amide bond, the following formula (17) shows an example including a carbamate bond, and the following formula (18) shows an example including a sulfonamide bond.
[0106] [Chemistry 5]
[0107]
[0108] Here, in the above formulas (14) to (18), R 2 and R 3 is a hydrocarbon group having 0 to 10 carbon atoms, R 4 is a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. 3 Examples of the hydrocarbon group include alkylene groups such as methylene and ethylene. 4 Examples of the hydrocarbon group include phenyl and the like in addition to alkyl groups such as methyl and ethyl.
[0109] In addition, in the above formula (3) and formula (4), R1 Examples thereof include a methyl group, an ethyl group, and a propyl group.
[0110] In the above formula (3) and formula (4), Z is not particularly limited as long as it is a hydrolyzable group that can be hydrolyzed to form a Si-O-Si bond. Specific examples of such hydrolyzable groups include alkoxy groups such as methoxy, ethoxy, propoxy, and butoxy; aryloxy groups such as phenoxy and naphthoxy; aralkyloxy groups such as benzyloxy and phenethoxy; and acyloxy groups such as acetoxy, propionyloxy, butyryloxy, valeryloxy, pivaloyloxy, and benzoyloxy. Among these, methoxy and ethoxy are preferably used.
[0111] Here, as specific examples of the fluorine-based compounds represented by the above formula (3) and formula (4) and containing a fluorine-containing functional group component having a perfluoroether structure, for example, the structures represented by the following formula (19) to formula (27) can be cited. It should be noted that in the following formulas (19) to (27), R is a methyl group or an ethyl group.
[0112] [Chemistry 6]
[0113]
[0114] [Chemistry 7]
[0115]
[0116] As described above, the fluorine-containing functional group component contained in the liquid composition for forming a water- and oil-repellent film of the first embodiment has a structure having one or more perfluoroether groups and one or more alkoxysilyl groups in the molecule, having a perfluoroether group having a plurality of short-chain perfluoroalkyl groups and perfluoroalkylene groups having a carbon number of 6 or less bonded to an oxygen atom, and a high fluorine content in the molecule, and therefore, can impart excellent water- and oil-repellency to the formed film.
[0117] [Liquid composition for forming water- and oil-repellent film]
[0118] The first embodiment of the liquid composition for forming a water- and oil-repellent film is produced by the above-mentioned production method, and comprises a solvent and a silica sol-gel comprising the above-mentioned fluorine-containing functional group component. The fluorine-containing functional group component has a perfluoroether structure represented by the above-mentioned general formula (1) and formula (2), and contains 0.01% by mass to 10% by mass when the silica sol-gel is set to 100% by mass.
[0119] The solvent is a mixed solvent of water and an alcohol having 1 to 4 carbon atoms, or a mixed solvent of water, an alcohol having 1 to 4 carbon atoms and an organic solvent other than the alcohol. Specific examples of the perfluoroether structure include the structures represented by the above formulas (5) to (27).
[0120] The first embodiment of the liquid composition for forming a water-repellent and oil-repellent film contains silica sol gel as a main component, so the film has excellent adhesion to the fibers of the non-woven fabric, and a water-repellent and oil-repellent film that is difficult to peel off and has high strength can be obtained. In addition, the silica sol gel contains a fluorine-containing functional group component of a perfluoroether structure shown in the above general formula (1) or (2), so it has water-repellent and oil-repellent effects, and the non-woven fabric is cured. When the content ratio of the fluorine-containing functional group component is less than 0.01% by mass, it is impossible to impart water-repellent and oil-repellent properties to the formed film. If it exceeds 10% by mass, the film will bounce off, etc., and the film-forming property will be poor. The content ratio of the fluorine-containing functional group component is preferably 0.1% by mass to 5% by mass.
[0121] <Second Embodiment>
[0122] 〔Oil-water separation filter〕
[0123] like Figure 5 As shown in the figure, the oil-water separation filter 113 of the second embodiment comprises a nonwoven fabric 120 and a water-repellent and oil-repellent film 121 formed on the fiber surface of the nonwoven fabric. The nonwoven fabric 120, which is a main component of the oil-water separation filter 113, has a surface 120a into which a mixed liquid containing water and oil flows, and another surface 120b opposite to the surface 120a and from which the filtrate flows out, and is composed of a single layer. Figure 6 As shown in the figure, the nonwoven fabric can also be made into a two-layer laminate of an upper nonwoven fabric 130 and a lower nonwoven fabric 140 to form an oil-water separation filter 123. In this case, the upper surface of the upper nonwoven fabric 130 becomes a side 130a into which a mixed liquid containing water and oil flows, and the lower surface of the lower nonwoven fabric 140 becomes the other side 140b opposite to the side 130a and from which the filtrate flows out. The lower surface 130b of the nonwoven fabric 130 is closely attached to the upper surface 140a of the nonwoven fabric 140. It should be noted that the laminate is not limited to two layers, and can also be composed of multiple layers such as three layers and four layers.
[0124] like Figure 5 As shown in the enlarged view in the center, the nonwoven fabric 120 is formed by entanglement of a plurality of fibers 120c, and pores 120d are formed between the fibers. The pores 120d penetrate between one side 120a and the other side 120b of the nonwoven fabric 120. A water-repellent and oil-repellent film 121 is formed on the surface of the fibers 120c of the nonwoven fabric. The unit weight of the nonwoven fabric is preferably 100 g / m 2 ~400g / m 2 The range of 200 g / m 2 ~350g / m 2range, but is not limited to this range. The water-repellent and oil-repellent film 121 comprises metal oxide particles (B) having an average particle size of 2 nm to 90 nm and a silica sol gel (C). The metal oxide particles (B) are bonded with a fluorine-based functional group component (A) represented by the aforementioned general formula (1) or formula (2). When the water-repellent and oil-repellent film 121 is set to 100% by mass, the fluorine-based functional group component (A) is contained in a ratio of 0.3% to 5.0% by mass. In addition, when the water-repellent and oil-repellent film 121 is set to 100% by mass, the fluorine-based functional group component (A) and the metal oxide particles (B) are contained in a ratio of 20% to 80% by mass in total. Furthermore, the mass ratio (A / B) of the fluorine-based functional group component (A) to the metal oxide particles (B) is in the range of 0.01 to 0.2.
[0125] like Figure 5 As shown in the further enlarged figure of the upper part, the water-repellent and oil-repellent film 121 is formed by bonding a plurality of metal oxide particles 121a whose particle surfaces are covered with fluorine-based functional group components through a silica sol-gel 121b as a binder. The water-repellent and oil-repellent film 121 includes metal oxide particles 121a, and therefore, a thick film is formed on the surface, which can reduce the pores 120d between the fibers. In addition, the film thickness can be controlled by changing the particle size of the metal oxide particles and the proportion of the metal oxide particles in the film component.
[0126] In the state of the oil-water separation filter 113 with the water-repellent and oil-repellent film 121 formed on the fiber surface, the nonwoven fabric 120 has a 0.05 ml / cm 2 / sec~10ml / cm 2 / sec air permeability. Air permeability is less than 0.05ml / cm 2 / second or the weight per unit area exceeds 400g / m 2 When the water permeability is poor, it is difficult to obtain the filtrate. The air permeability exceeds 10ml / cm 2 / second or the unit area weight of the non-woven fabric is less than 100g / m 2 When the size of the pores 120d of the nonwoven fabric is significantly larger than the oil particles 122 in the mixed liquid, the oil particles 122 and the water pass through the pores of the nonwoven fabric and escape from the oil-water separation filter 113, and the water and oil cannot be separated. The air permeability is preferably 0.1ml / cm 2 / sec~8ml / cm 2 / sec. The air permeability was measured using the above-mentioned Frazier tester.
[0127] When the water-repellent and oil-repellent film 121 is set to 100% by mass, when the content ratio of the fluorine-based functional group component (A) is less than 0.3% by mass, the oil-repellent effect is lacking, and the performance of repelling oil particles becomes insufficient. If the content ratio of the fluorine-based functional group component (A) exceeds 5.0% by mass, the film-forming property is poor, and the adhesion of the water-repellent and oil-repellent film to the non-woven fabric becomes poor. When the water-repellent and oil-repellent film 121 is set to 100% by mass, the content ratio of the fluorine-based functional group component (A) is preferably 0.4% by mass to 4.0% by mass.
[0128] The average particle size of the metal oxide particles (B) contained in the water-repellent and oil-repellent film 121 is in the range of 2nm~90nm, preferably in the range of 2nm~85nm. When the average particle size is less than 2nm, the aggregation of metal oxide particles is likely to occur, and it is difficult to disperse in the medium. If it exceeds 90nm, the metal oxide particles (B) fall off from the water-repellent and oil-repellent film. When the water-repellent and oil-repellent film 121 is set to 100% by mass, the total amount of fluorine-based functional group components (A) and metal oxide particles (B) is 20% by mass to 80% by mass, preferably 7% by mass to 75% by mass, and the mass ratio (A / B) of the fluorine-based functional group component (A) relative to the metal oxide particles (B) is in the range of 0.01~0.2, preferably 0.014~0.18. When the water-repellent and oil-repellent film 121 is set to 100% by mass, when the total amount of component (A) and particles (B) is less than 20% by mass, the oil repellency of the water-repellent and oil-repellent film is reduced. In addition, if the total exceeds 80% by mass, the content of silica sol gel (C) becomes relatively low, and the water-repellent and oil-repellent film is no longer firmly bonded to the surface of the nonwoven fabric. In addition, when the mass ratio (A / B) is less than 0.01, the oil repellency of the water-repellent and oil-repellent film is poor, and if it exceeds 0.2, the adhesion of the water-repellent and oil-repellent film to the fiber surface is reduced. It should be noted that in this specification, the average particle size of the metal oxide particles refers to: among the particle shapes observed using a transmission electron microscope (TEM), the average value of the numerical values obtained by measuring the particle size of 200 points by image analysis.
[0129] In the oil-water separation device 10 equipped with such an oil-water separation filter 113, water in the water-soluble oil plays the same role as described in the first embodiment and is stored until Figure 1 In the water storage portion 17 shown. On the other hand, Figure 5As shown in the enlarged view of the figure, due to the oil repellency of the oil-water separation membrane 121 formed on the fiber surface of the nonwoven fabric 120, in addition, due to the specified air permeability of the oil-water separation filter, it is needless to say that when the particle size is larger than the pore size of the pore 120d, even if the particle size is slightly smaller than the pore size of the pore 120d, the oil particles 122 in the liquid cannot pass through the oil-water separation filter 113, but are retained between the fibers 120c and 120c of the nonwoven fabric 120. Since the water-repellent and oil-repellent film 121 contains metal oxide particles 121a, the film presents concavoconvexity, and the degree of attachment of the oil particles 122 to the film is low. Thus, the oil particles 122 are captured by the nonwoven fabric. The oil retained in the nonwoven fabric 120 is recycled by regularly unloading the oil-water separation filter 113 from the oil-water separation device 10.
[0130] [Method for manufacturing oil-water separation filter]
[0131] The oil-water separation filter is simply manufactured by the following method.
[0132] like Figure 7 As shown in the figure, metal oxide particles are mixed with an organic solvent to prepare a dispersion of metal oxide particles. A fluorine compound containing a fluorine functional group component (A) is mixed into the dispersion, and water and a catalyst are further mixed to prepare a dispersion of fluorine-containing metal oxide particles. On the other hand, a silica sol-gel solution is prepared by mixing silicon alkoxide, alcohol, water and an alkylene component as required, and adding a catalyst to the mixed solution.
[0133] A liquid composition for forming a water-repellent and oil-repellent film is prepared by mixing a solvent into the silica sol-gel solution and mixing the mixed solution with the dispersion of the fluorinated metal oxide particles. A liquid is prepared by diluting the liquid composition for forming a water-repellent and oil-repellent film with a solvent containing an alcohol having a boiling point of less than 120° C. and a carbon number in the range of 1 to 4 in a mass ratio (liquid composition: alcohol) of 1:1 to 50 relative to the liquid composition, immersing the nonwoven fabric 120 in the diluent and pulling it from the diluent, spreading the nonwoven fabric on a horizontal metal mesh or the like in the atmosphere and at room temperature, deliquating until a certain amount of liquid is reached, and drying, thereby manufacturing an oil-water separation filter 113.
[0134] 〔Preparation of non-woven fabric〕
[0135] First, prepare a 0.05 ml / cm 2 / sec~15ml / cm 2 Specifically, a nonwoven fabric having an air permeability of 0.05 ml / cm 2 / sec~14ml / cm 2 When the water-repellent and oil-repellent film is formed as a thick film, a nonwoven fabric with high air permeability is selected, and when the water-repellent and oil-repellent film is formed as a thin film, a nonwoven fabric with low air permeability is selected.
[0136] The material of the nonwoven fabric is the same as that of the nonwoven fabric of the first embodiment. In order to obtain the above-mentioned air permeability, the thickness (fiber diameter) of the fibers constituting the nonwoven fabric is preferably 0.01 μm to 10 μm, but is not limited to this range. When the oil-water separation filter is a single layer, the thickness of the nonwoven fabric is 0.2 mm to 0.8 mm, and when it is a multi-layer laminate, the thickness of the laminate is preferably 0.2 mm to 1.6 mm. When the main component of the water-repellent and oil-repellent film-forming material of the present invention is silica sol gel, in order to obtain adhesion with the fiber, it is preferably a material in which the fiber has hydroxyl groups. Among them, glass, alumina, cellulose nanofibers, etc. also have materials with thin fiber diameters, which can make the air permeability a low value within the above range.
[0137] As mentioned above, nonwoven fabrics such as Figure 6 In the case of a laminated body having a plurality of nonwoven fabrics 130, 140 as shown, by making the fibers constituting the nonwoven fabric 130 on one side into which the liquid containing water and oil flows into glass fibers, the water- and oil-repellent film containing silica sol gel as the main component will be more firmly adhered to the glass fibers and will be difficult to peel off from the fibers of the nonwoven fabric.
[0138] [Method for producing a liquid composition for forming a water- and oil-repellent film]
[0139] [Preparation of metal oxide particle dispersion]
[0140] First, the metal oxide particles are dispersed in an organic solvent to prepare a dispersion of the metal oxide particles. Examples of organic solvents include methanol, ethanol, isopropanol (hereinafter sometimes referred to as IPA), tetrahydrofuran, hexane, chloroform, toluene, ethyl acetate, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), acetone, and fluorine-based solvents. Among these, alcohols such as methanol, ethanol, and isopropanol having a boiling point of less than 120°C and a carbon number in the range of 1 to 4 are preferred. Examples of metal oxide particles include particles of SiO2, Al2O3, MgO, CaO, TiO2, ZnO, and ZrO2, mixed particles thereof, and composite oxide particles.
[0141] [Preparation of Fluorine-Containing Metal Oxide Particle Dispersion]
[0142] Next, a fluorine compound containing a fluorine-containing functional group component represented by the above formula (1) or (2) is added to the prepared dispersion of the metal oxide particles to synthesize a composite material obtained by nanocompositing the metal oxide particles and the fluorine-containing functional group component. Furthermore, water and a catalyst are added to promote the reaction. Thus, a dispersion of fluorine-containing metal oxide particles is prepared.
[0143] As the above-mentioned catalyst, organic acid, inorganic acid or titanium compound can be listed, formic acid and oxalic acid can be exemplified as organic acid, hydrochloric acid, nitric acid and phosphoric acid can be exemplified as inorganic acid, and tetrapropoxytitanium, tetrabutoxytitanium, tetraisopropoxytitanium, titanium lactate and the like can be exemplified as titanium compound. The catalyst is not limited to the above-mentioned substances. As the above-mentioned water, in order to prevent the mixing of impurities, it is desirable to use ion exchange water, pure water and the like.
[0144] The fluorine-based compound containing a fluorine-based functional group component is represented by the above-mentioned general formula (3) or formula (4). As the perfluoroether group in these formulas (3) or (4), more specifically, the perfluoroether structures represented by the above-mentioned formulas (5) to (13) can be listed. As specific examples of the fluorine-based compound containing a fluorine-based functional group component having a perfluoroether structure represented by the above-mentioned formula (3) or formula (4), for example, the structures represented by the above-mentioned formulas (19) to (27) can be listed.
[0145] As described above, the fluorine-based compound contained in the liquid composition for forming a water- and oil-repellent film of the second embodiment is the same as the fluorine-based compound described in the first embodiment, and has a perfluoroether group obtained by bonding a plurality of short-chain perfluoroalkyl and perfluoroalkylene groups with a carbon number of 6 or less to an oxygen atom in the molecule, and the fluorine content in the molecule is high, so that the formed film can be given excellent water- and oil-repellent properties.
[0146] 〔Preparation of silica sol-gel solution〕
[0147] First, tetramethoxysilane or tetraethoxysilane as silicon alkoxide, alcohol having a boiling point of less than 120°C and a carbon number in the range of 1 to 4, and water are mixed to prepare a mixed solution. At this time, a silane containing an epoxy group that becomes an alkylene component can also be mixed together. As the silicon alkoxide, specifically, tetramethoxysilane, its oligomer or tetraethoxysilane, its oligomer can be listed. For example, for the purpose of obtaining a durable water-repellent and oil-repellent film, tetramethoxysilane is preferably used. On the other hand, when avoiding methanol generated during hydrolysis, tetraethoxysilane is preferably used.
[0148] Specific examples of the epoxy group-containing silane serving as the alkylene component and the content ratio thereof are the same as the specific examples of the alkylene component and the content ratio thereof described in the first embodiment.
[0149] The alcohol having a boiling point of less than 120° C. and a carbon number of 1 to 4 is the same as the alcohol described in the first embodiment. As described in the first embodiment, an alcohol having a carbon number of 1 to 4 and water are added to silicon alkoxide or silicon alkoxide and epoxy-containing silane, and stirred at a temperature of preferably 10° C. to 30° C. for 5 to 20 minutes to prepare a mixed solution.
[0150] The same catalyst as that described in the first embodiment is added and mixed to the mixed solution prepared above by the method described in the first embodiment. Thus, a silica sol-gel solution is prepared. For the next step, a mixed alcohol is added to the silica sol-gel solution.
[0151] When the silica sol-gel solution mixed with the alcohol is added, it is preferred that 2% to 50% by mass of silicon alkoxide, 20% to 98% by mass of alcohol having a carbon number of 1 to 4, 0.1% to 40% by mass of water are contained, and 0.01% to 5% by mass of the catalyst are contained. When the silane containing an epoxy group as an alkylene component is mixed, it is preferred that up to 30% by mass of the silane containing an epoxy group is contained.
[0152] The reason why the ratio of the alcohol having a carbon number of 1 to 4 and the ratio of water are limited to the above ranges is the same as that described in the first embodiment.
[0153] When the silica sol-gel is assumed to be 100 mass %, the range of SiO 2 concentration (SiO 2 amount) and the reason thereof are the same as those described in the first embodiment.
[0154] Specific examples of the above-mentioned catalyst and the content ratio thereof are the same as the specific examples and the content ratio thereof described in the first embodiment.
[0155] [Liquid composition for forming water- and oil-repellent film]
[0156] The second embodiment of the water-repellent and oil-repellent film-forming liquid composition is manufactured by the above-mentioned manufacturing method, comprising metal oxide particles, silica sol gel and solvent bonded with the above-mentioned fluorine-based functional group component. The fluorine-based functional group component has a perfluoroether structure shown in the above-mentioned general formula (1) or formula (2), and when the water-repellent and oil-repellent film-forming liquid composition excluding the solvent is set to 100% by mass, it contains 0.3% to 5.0% by mass. It should be noted that the proportion of the fluorine-based functional group component when the water-repellent and oil-repellent film-forming liquid composition excluding the solvent is set to 100% by mass is the same as the proportion of the fluorine-based functional group component when the water-repellent and oil-repellent film is set to 100% by mass. Other components are also the same.
[0157] The solvent is a mixed solvent of water and an alcohol having 1 to 4 carbon atoms, or a mixed solvent of water, an alcohol having 1 to 4 carbon atoms and an organic solvent other than the alcohol. Specific examples of the perfluoroether structure include the structures represented by the above formulae (19) to (27).
[0158] The liquid composition for forming a water-repellent and oil-repellent film of the second embodiment contains a silica sol-gel liquid as a main component and also contains metal oxide particles, so that the strength of the water-repellent and oil-repellent film is improved, the adhesion to the fibers of the non-woven fabric is excellent, and a water-repellent and oil-repellent film that is difficult to peel off and has high strength can be obtained. In addition, the liquid composition for forming a water-repellent and oil-repellent film contains a fluorine-based functional group component of a perfluoroether structure represented by the above general formula (1) or formula (2), and therefore has an oil-repellent effect.
[0159] [Method for forming a water- and oil-repellent film on the fiber surface of a nonwoven fabric]
[0160] The method for forming the water-repellent and oil-repellent film on the fiber surface of the nonwoven fabric of the second embodiment is the same as the method described in the first embodiment. Figure 5 As shown in the enlarged view in the center, a water-repellent and oil-repellent film 121 is formed on the surface of the fiber 120c constituting the nonwoven fabric 120. When the amount of liquid removal is small, the water-repellent and oil-repellent film is formed on the fiber surface of the nonwoven fabric in the form of a thick film, and when the amount of liquid removal is large, the water-repellent and oil-repellent film is formed on the fiber surface of the nonwoven fabric in the form of a thin film.
[0161] <Third Embodiment>
[0162] 〔Oil-water separation filter〕
[0163] like Figure 8 As shown in the figure, the oil-water separation filter 213 of the third embodiment comprises a nonwoven fabric 220 and a water-repellent and oil-repellent film 221 formed on the fiber surface of the nonwoven fabric. The nonwoven fabric 220, which is a main component of the oil-water separation filter 213, has a surface 220a into which a liquid containing water and oil flows, and another surface 220b opposite to the surface 220a and from which the filtrate flows out, and is composed of a single layer. Fig. 9 As shown in the figure, the nonwoven fabric can also be made into a two-layer laminate of an upper nonwoven fabric 230 and a lower nonwoven fabric 240 to form an oil-water separation filter 223. In this case, the upper surface of the upper nonwoven fabric 230 becomes a side 230a into which the liquid containing water and oil flows, and the lower surface of the lower nonwoven fabric 240 becomes the other side 240b opposite to the side 230a and from which the filtrate flows out. The lower surface 230b of the nonwoven fabric 230 is closely attached to the upper surface 240a of the nonwoven fabric 240. It should be noted that the laminate is not limited to two layers, and can also be composed of multiple layers such as three layers and four layers.
[0164] like Figure 8As shown in the enlarged view in the center, the nonwoven fabric 220 is formed by entanglement of a plurality of fibers 220c, and pores 220d are formed between the fibers. The pores 220d penetrate between one side 220a and the other side 220b of the nonwoven fabric 220. A water-repellent and oil-repellent film 221 is formed on the surface of the fibers 220c of the nonwoven fabric. The unit weight of the nonwoven fabric is preferably 10 g / m 2 ~400g / m 2 The range is preferably 100 g / m 2 ~350g / m 2 range, but is not limited to this range. The water-repellent and oil-repellent film 221 comprises metal oxide particles (B) having an average particle size of 2 nm to 90 nm and a silica sol gel (C). The metal oxide particles (B) are bonded with a first fluorine-based functional group component (A1) represented by the aforementioned general formula (1) or (2). In addition, the silica sol gel (C) comprises a second fluorine-based functional group component (A2) represented by the aforementioned general formula (1) or (2). When the water-repellent and oil-repellent film 221 is set to 100 mass %, the first fluorine-based functional group component (A1) and the second fluorine-based functional group component (A2) are contained in a total ratio of 0.5 mass % to 15 mass %. In addition, the mass ratio (C:B) of the silica sol gel (C) to the metal oxide particles (B) is in the range of 10:90 to 90:10.
[0165] like Figure 8 As shown in the further enlarged figure of the upper part, the water-repellent and oil-repellent film 221 is formed by bonding a plurality of metal oxide particles 221a whose particle surfaces are covered with fluorine-based functional group components through a fluorine-containing silica sol gel 221b as a binder. The water-repellent and oil-repellent film 221 includes metal oxide particles 221a, and therefore, a thick film is formed on the surface, and the pores 220d between the fibers can be reduced. In addition, the film thickness can be controlled by changing the particle size of the metal oxide particles and the proportion of the metal oxide particles in the film component.
[0166] In the state of the oil-water separation filter 213 with the water-repellent and oil-repellent film 221 formed on the fiber surface, the nonwoven fabric 220 has a 0.05 ml / cm 2 / sec~14ml / cm 2 / sec air permeability. Air permeability is less than 0.05ml / cm 2 / second, the liquid permeability is poor, it is difficult to obtain the filtrate, and the practicality is poor. If the air permeability exceeds 14ml / cm 2 / second, a water-repellent and oil-repellent film 221 is fully formed on the fiber surface, but the size of the pores 220d of the non-woven fabric is obviously larger than the oil particles 222 in the mixed liquid. The oil particles 222 pass through the pores of the non-woven fabric together with the water and escape from the oil-water separation filter 213, and the water and oil cannot be separated. The air permeability is preferably 0.1ml / cm2 / sec~10ml / cm 2 / sec. The air permeability was measured using the above-mentioned Frazier tester.
[0167] When the total content ratio of the first fluorine-based functional group component (A1) and the second fluorine-based functional group component (A2) is less than 0.5% by mass when the water-repellent and oil-repellent film 221 is set to 100% by mass, the formed film cannot be given oil repellency, and the performance of repelling oil particles becomes insufficient. In addition, if the total content ratio exceeds 15% by mass, the adhesion of the water-repellent and oil-repellent film to the non-woven fabric deteriorates, and when the oil-water separation filter is made, the liquid containing water and oil will not pass through. When the water-repellent and oil-repellent film 221 is set to 100% by mass, the total content ratio of the first fluorine-based functional group component (A1) and the second fluorine-based functional group component (A2) is preferably 0.8% by mass to 12% by mass.
[0168] The average particle size of the metal oxide particles (B) contained in the water-repellent and oil-repellent film 221 is in the range of 2nm to 90nm. Preferably, it is in the range of 2nm to 85nm. When the average particle size is less than 2nm, the metal oxide particles are easily aggregated and difficult to disperse in the medium. If it exceeds 90nm, the metal oxide particles (B) are difficult to adhere to the fiber surface of the non-woven fabric and are easily removed from the water-repellent and oil-repellent film. The mass ratio (C:B) of the silica sol gel (C) and the metal oxide particles (B) is in the range of 10:90 to 90:10. That is, when the total amount of the silica sol gel (C) and the metal oxide particles (B) is set to 100% by mass, when the silica sol gel (C) is less than 10% by mass and the metal oxide particles (B) exceed 90% by mass, the binder component in the water-repellent and oil-repellent film becomes too small, and the water-repellent and oil-repellent film is easily peeled off from the fiber surface of the non-woven fabric. On the other hand, when the metal oxide particles (B) are less than 10% by mass and the silica sol-gel (C) exceeds 90% by mass, the metal oxide particles are too few, the strength of the water-repellent and oil-repellent film is insufficient, or it is difficult to maintain the size of the nonwoven fabric against environmental changes. The preferred mass ratio (C:B) is 20:80 to 80:20.
[0169] In the oil-water separation device 10 equipped with such an oil-water separation filter 213, water in the water-soluble oil plays the same role as that described in the first embodiment and is stored until Figure 1 In the water storage portion 17 shown. On the other hand, Figure 8As shown in the enlarged view, due to the oil repellency of the oil-water separation membrane 221 formed on the fiber surface of the nonwoven fabric 220, in addition, due to the specified air permeability of the oil-water separation filter, therefore, in the case where the particle size is greater than the aperture of the pore 220d, it goes without saying that even if the particle size is slightly smaller than the aperture of the pore 220d, the oil particles 222 in the liquid cannot pass through the oil-water separation filter 213, but are retained between the fibers 220c and 220c of the nonwoven fabric 220. Since the water-repellent and oil-repellent film 221 contains metal oxide particles 221a, the film presents concavoconvexity, and the degree of attachment of the oil particles 222 to the film is low. Thus, the oil particles 222 are captured by the nonwoven fabric. The oil retained in the nonwoven fabric 220 is recycled by regularly unloading the oil-water separation filter 13 from the oil-water separation device 10.
[0170] [Method for manufacturing oil-water separation filter]
[0171] The oil-water separation filter is simply manufactured by the following method.
[0172] like Fig.10 As shown in the figure, metal oxide particles are mixed with a solvent to prepare a metal oxide particle dispersion. A fluorine compound containing a first fluorine functional group component (A1) is mixed into the dispersion, and water and a catalyst are further mixed to prepare a dispersion of fluorine-containing metal oxide particles. On the other hand, a fluorine-containing silica sol-gel solution is prepared by mixing silicon alkoxide, alcohol, a fluorine compound containing a second fluorine functional group component (A2), water, and an alkylene component as required, and adding a catalyst to the mixed solution.
[0173] A liquid composition for forming a water-repellent and oil-repellent film is prepared by mixing a solvent in the silica sol-gel solution and mixing the mixed solution with the dispersion of the fluorinated metal oxide particles. A liquid obtained by diluting the liquid composition for forming a water-repellent and oil-repellent film with a solvent is prepared, a nonwoven fabric 220 is immersed in the diluent and pulled from the diluent, the nonwoven fabric is spread on a horizontal metal mesh or the like in the atmosphere and at room temperature, the liquid is removed until a certain amount of liquid is reached, and the oil-water separation filter 213 is manufactured.
[0174] 〔Preparation of non-woven fabric〕
[0175] First, prepare a 0.05 ml / cm 2 / sec~18ml / cm 2 Specifically, a nonwoven fabric having an air permeability of 0.05 ml / cm 2 / sec~14ml / cm 2When the water-repellent and oil-repellent film is formed as a thick film, a nonwoven fabric with high air permeability is selected, and when the water-repellent and oil-repellent film is formed as a thin film, a nonwoven fabric with low air permeability is selected.
[0176] The material of the nonwoven fabric is the same as that of the nonwoven fabric of the first embodiment. In order to obtain the above-mentioned air permeability, the thickness (fiber diameter) of the fibers constituting the nonwoven fabric is preferably 0.01 μm to 10 μm, but is not limited to this range. When the oil-water separation filter is a single layer, the thickness of the nonwoven fabric is 0.2 mm to 0.8 mm, and when it is a multi-layer laminate, the thickness of the laminate is preferably 0.2 mm to 1.6 mm. When the main component of the water-repellent and oil-repellent film-forming material of the present invention is silica sol gel, in order to obtain adhesion with the fiber, it is preferably a material in which the fiber has hydroxyl groups. Among them, glass, alumina, cellulose nanofibers, etc. also have materials with thin fiber diameters, which can make the air permeability a low value within the above range.
[0177] As mentioned above, nonwoven fabrics such as Fig. 9 In the case of a stacked body having a plurality of nonwoven fabrics 230, 240 as shown, by making the fibers constituting the nonwoven fabric 230 on one side into which the liquid containing water and oil flows into glass fibers, the water- and oil-repellent film containing silica sol gel as the main component will be more firmly adhered to the glass fibers and will be difficult to peel off from the fibers of the nonwoven fabric.
[0178] [Method for producing a liquid composition for forming a water- and oil-repellent film]
[0179] [Preparation of metal oxide particle dispersion]
[0180] First, the metal oxide particles are dispersed in a solvent to prepare a dispersion of the metal oxide particles. Examples of the solvent include methanol, ethanol, isopropanol (hereinafter sometimes referred to as IPA), tetrahydrofuran, hexane, chloroform, toluene, ethyl acetate, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), acetone, and fluorine-based solvents. Among these, alcohols such as methanol, ethanol, and isopropanol having a boiling point of less than 120°C and a carbon number in the range of 1 to 4 are preferred. Examples of metal oxide particles include particles of SiO2, Al2O3, MgO, CaO, TiO2, ZnO, and ZrO2, their mixed particles, and composite oxide particles.
[0181] [Preparation of Fluorine-Containing Metal Oxide Particle Dispersion]
[0182] Next, a fluorine compound containing the first fluorine-containing functional group component (A1) represented by the above formula (1) or (2) is added to the prepared dispersion of the metal oxide particles to synthesize a composite material obtained by nanocompositing the metal oxide particles and the fluorine-containing functional group component. Furthermore, water and a catalyst are added to promote the reaction. Thus, a dispersion of fluorine-containing metal oxide particles is prepared.
[0183] As the above-mentioned catalyst, organic acid, inorganic acid, alkali or titanium compound can be listed, formic acid and oxalic acid can be exemplified as organic acid, hydrochloric acid, nitric acid and phosphoric acid can be exemplified as inorganic acid, sodium hydroxide, lithium hydroxide, magnesium hydroxide, potassium hydroxide, calcium hydroxide and ammonia can be exemplified as alkali, tetrapropoxy titanium, tetrabutoxy titanium, tetraisopropoxy titanium and titanium lactate can be exemplified as titanium compound. Catalyst is not limited to the above-mentioned substances. As the above-mentioned water, in order to prevent the mixing of impurities, it is desirable to use ion exchange water, pure water and the like.
[0184] The fluorine-based compound containing the first fluorine-based functional group component (A1) is represented by the above general formula (3) or formula (4). As the perfluoroether group in these formulas (3) or (4), more specifically, the perfluoroether structures represented by the above formulas (5) to (13) can be listed. As specific examples of the fluorine-based compound containing a fluorine-based functional group component having a perfluoroether structure represented by the above formulas (3) or (4), for example, the structures represented by the above formulas (19) to (27) can be listed.
[0185] As described above, the fluorine-based compound contained in the liquid composition for forming a water- and oil-repellent film of the third embodiment is the same as the fluorine-based compound described in the first embodiment, and has a perfluoroether group obtained by bonding a plurality of short-chain perfluoroalkyl and perfluoroalkylene groups with a carbon number of 6 or less to an oxygen atom in the molecule, and the fluorine content in the molecule is high, so that the formed film can be given excellent water- and oil-repellent properties.
[0186] [Preparation of fluorine-containing silica sol-gel solution]
[0187] First, tetramethoxysilane or tetraethoxysilane as a silicon alkoxide, an alcohol having a boiling point of less than 120°C and a carbon number in the range of 1 to 4, a fluorine compound containing a second fluorine functional group component (A2) represented by the above formula (1) or (2), and water are mixed to prepare a mixed solution. At this time, an alkylene component having a carbon number of 2 to 7 may also be mixed together. As the alkylene component, silane containing an epoxy group can be listed. As the silicon alkoxide, specifically, tetramethoxysilane (TMOS), its oligomers or tetraethoxysilane (TEOS), its oligomers can be listed. For example, for the purpose of obtaining a highly durable water- and oil-repellent film, tetramethoxysilane is preferably used. On the other hand, when avoiding the methanol produced during hydrolysis, tetraethoxysilane is preferably used.
[0188] The second fluorine-based functional group component (A2) contained in the fluorine-based compound is represented by the above formula (1) or formula (2), and the specific fluorine-based compound containing the first fluorine-based functional group component (A1) and the specific fluorine-based compound containing the second fluorine-based functional group component (A2) may be the same as or different from each other.
[0189] Specific examples of the epoxy group-containing silane serving as the alkylene component and the content ratio thereof are the same as the specific examples of the alkylene component and the content ratio thereof described in the first embodiment.
[0190] The alcohol having a boiling point of less than 120° C. and a carbon number of 1 to 4 is the same as the alcohol described in the first embodiment. As described in the first embodiment, an alcohol having a carbon number of 1 to 4 and water are added to silicon alkoxide or silicon alkoxide and epoxy-containing silane, and stirred at a temperature of preferably 10° C. to 30° C. for 5 to 20 minutes to prepare a mixed solution.
[0191] The same catalyst as that described in the first embodiment is added to the mixed solution prepared above by the method described in the first embodiment. Thus, a fluorine-containing silica sol-gel solution is prepared. It should be noted that a mixed alcohol may be added to the fluorine-containing silica sol-gel solution for the next step.
[0192] When the alcohol is added and mixed, the fluorine-containing silica sol-gel solution preferably contains silicon alkoxide at a ratio of 2% to 50% by mass, an alcohol having a carbon number of 1 to 4 at a ratio of 20% to 98% by mass, water at a ratio of 0.1% to 40% by mass, and a catalyst at a ratio of 0.01% to 5% by mass. When an epoxy-containing silane serving as an alkylene component is mixed, it is preferred that the epoxy-containing silane be contained at a ratio of up to 30% by mass.
[0193] The reason why the ratio of the alcohol having a carbon number of 1 to 4 and the ratio of water are limited to the above ranges is the same as that described in the first embodiment.
[0194] When the silica sol-gel is assumed to be 100 mass %, the range of SiO 2 concentration (SiO 2 amount) and the reason thereof are the same as those described in the first embodiment.
[0195] Specific examples of the above-mentioned catalyst and the content ratio thereof are the same as the specific examples and the content ratio thereof described in the first embodiment.
[0196] [Water- and oil-repellent film-forming liquid composition]
[0197] The liquid composition for forming a water-repellent and oil-repellent film of the third embodiment is manufactured by the above-mentioned manufacturing method, and includes metal oxide particles (B) bonded with the above-mentioned first fluorine-based functional group component (A1), a silica sol gel (C) containing the above-mentioned second fluorine-based functional group component (A2), and a solvent. Examples of the solvent include water, methanol, ethanol, isopropyl alcohol (hereinafter sometimes referred to as IPA), tetrahydrofuran, hexane, chloroform, toluene, ethyl acetate, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), acetone, fluorine-based solvents, etc. These fluorine-based functional group components (A1) and (A2) have a perfluoroether structure represented by the above-mentioned general formula (1) or formula (2), and when the total amount of components excluding the solvent (D) is set to 100% by mass, the total amount is 0.5% to 15% by mass in the liquid composition. The preferred total content ratio of the fluorine-based functional group components (A1+A2) is 0.8% to 12% by mass. The reason for setting the total content ratio to the above-mentioned numerical range is as described above.
[0198] The first fluorine-functional component (A1) and the second fluorine-functional component (A2) are preferably contained in the same mass ratio or in a larger amount than the second fluorine-functional component (A2) because the adhesion of the water- and oil-repellent film to the fiber surface of the nonwoven fabric is improved.
[0199] As described above, the fluorine compound contained in the liquid composition for forming a water-repellent and oil-repellent film of the third embodiment has a perfluoroether group obtained by bonding a plurality of short-chain perfluoroalkyl groups and perfluoroalkylene groups having a carbon number of 6 or less to an oxygen atom in the molecule, and the fluorine content in the molecule is high, so that the formed film can be given excellent water-repellent and oil-repellent properties. As specific examples of perfluoroether structures, the structures shown in the above formulas (19) to (27) can be cited.
[0200] Furthermore, in the liquid composition for forming a water-repellent and oil-repellent film of the third embodiment, the mass ratio (C:B) of the silica sol gel (C) and the metal oxide particles (B) is preferably in the range of 10:90 to 90:10. That is, when the total amount of the silica sol gel (C) and the metal oxide particles (B) is set to 100% by mass, when the silica sol gel (C) is less than 10% by mass and the metal oxide particles (B) exceed 90% by mass, the binder component in the liquid composition becomes too small, and the formed film is easily peeled off from the fiber surface of the non-woven fabric. On the contrary, when the metal oxide particles (B) are less than 10% by mass and the silica sol gel (C) exceeds 90% by mass, the metal oxide particles are too small, the strength of the water-repellent and oil-repellent film is insufficient, or it is difficult to maintain the size of the non-woven fabric relative to environmental changes. The more preferred mass ratio (C:B) is 20:80 to 80:20.
[0201] The liquid composition for forming a water- and oil-repellent film of the third embodiment contains a dispersion of fluorine-containing metal oxide particles and a fluorine-containing silica sol-gel liquid. Therefore, when a film is formed on the fiber surface of a non-woven fabric, it can impart better oil-repellent properties than conventional liquid compositions, and the water- and oil-repellent film has excellent adhesion to the fiber surface of the non-woven fabric, so that a water- and oil-repellent film that is difficult to peel off and has high strength can be obtained.
[0202] [Method for forming a water- and oil-repellent film on the fiber surface of a nonwoven fabric]
[0203] The method for forming a water-repellent and oil-repellent film on the fiber surface of the nonwoven fabric of the third embodiment is the same as the method described in the first embodiment. Figure 8 As shown in the enlarged view in the center, a water-repellent and oil-repellent film 221 is formed on the surface of the fiber 220c constituting the nonwoven fabric 220. When the amount of liquid removal is small, the water-repellent and oil-repellent film is formed on the fiber surface of the nonwoven fabric in the form of a thick film, and when the amount of liquid removal is large, the water-repellent and oil-repellent film is formed on the fiber surface of the nonwoven fabric in the form of a thin film. Example
[0204] Next, examples of the present invention will be described in detail together with comparative examples.
[0205] First, examples 1 to 6 and comparative examples 1 to 6 related to an oil-water separation filter composed of a non-woven fabric that is not frozen and thawed after forming a water-repellent and oil-repellent film corresponding to the first embodiment are described. Next, test examples 1 to 3 and comparative test examples 1 to 4 related to an oil-water separation filter composed of a non-woven fabric that is frozen and thawed after forming a water-repellent and oil-repellent film are described.
[0206] Next, Synthesis Examples 1 to 9 and Comparative Synthesis Examples 1 to 3 for preparing dispersions of metal oxide particles corresponding to the second embodiment are described, and then Examples 7 to 15 and Comparative Examples 7 to 11 related to the preparation of liquid compositions for forming water- and oil-repellent films and the manufacture of oil-water separation filters using these Synthesis Examples and Comparative Synthesis Examples are described.
[0207] Furthermore, Synthesis Examples 10 to 18 and Comparative Synthesis Examples 4 to 5 for preparing a dispersion of metal oxide particles corresponding to the third embodiment are described, followed by Synthesis Examples 19 to 22 and Comparative Synthesis Example 6 for preparing a fluorine-containing silica sol-gel solution, and then Examples 16 to 24 and Comparative Examples 12 to 20 related to the manufacture of a liquid composition for forming a water- and oil-repellent film and the manufacture of an oil-water separation filter using these Synthesis Examples and Comparative Synthesis Examples are described.
[0208] <Examples and Comparative Examples Corresponding to the First Embodiment>
[0209] <Example 1>
[0210] 8.52 g of tetramethoxysilane (TMOS) trimer to pentamer (Mitsubishi Chemical Corporation, trade name: MKC SILICATE MS51) as silicon alkoxide, 0.48 g of 3-glycidoxypropyltrimethoxysilane (GPTMS: Shin-Etsu Chemical Co., Ltd., trade name: KBM-403) as an epoxy-containing silane as an alkylene component, 0.24 g of fluorine-containing silane (R: ethyl) represented by formula (19) as a fluorine-containing functional group component, and 17.34 g of ethanol (EtOH) (boiling point: 78.3° C.) as an organic solvent were mixed, and 3.37 g of ion-exchanged water was further added, and the mixture was stirred at a temperature of 25° C. for 5 minutes in a separable flask to prepare a mixed solution. In addition, 0.05 g of hydrochloric acid at a concentration of 35% by mass was added to the mixed solution as a catalyst, and the mixture was stirred at 40° C. for 2 hours. Thus, a liquid composition for forming a water-repellent and oil-repellent film containing a silica sol gel was prepared. The preparation contents are shown in Table 1.
[0211]
[0212] In the silica sol gel of the obtained liquid composition for forming a water-repellent and oil-repellent film, when the silica sol gel is set to 100 mass%, it contains 4.5 mass% of fluorine-containing functional group components and 7.8 mass% of alkylene components with a carbon number of 7. Next, 29.0 g of industrial alcohol (AP-7 manufactured by Nippon Alcohol Industry Co., Ltd.) as a solvent was added and mixed to 1.0 g of the liquid composition for forming a water-repellent and oil-repellent film to prepare a dilution of the liquid composition. A 2.5 ml / cm 2 / second of air permeability was immersed in the dilute solution for 30 seconds. The two-layer nonwoven fabric is a laminate of an upper nonwoven fabric made of glass fiber and a lower nonwoven fabric made of PET fiber. The two-layer nonwoven fabric was pulled out of the dilute solution, spread on a horizontal metal net, and left at room temperature for 30 minutes to deliquate. Thereafter, the two-layer nonwoven fabric was placed in a dryer maintained at 100°C for 30 minutes to dry, thereby obtaining an oil-water separation filter. The air permeability of the oil-water separation filter is 1.2 ml / cm 2 / second. The difference between the mass of the two layers of nonwoven fabric before immersion and the mass after drying was converted into the mass of the water-repellent and oil-repellent film formed on the fiber surface of the nonwoven fabric. As a result, the water-repellent and oil-repellent film was calculated per 1m 2 The above results are shown in Table 2.
[0213]
[0214] <Examples 2 to 6, Comparative Examples 2 to 4>
[0215] For Examples 2 to 6 and Comparative Examples 2 to 4, as shown in Table 2, the type of non-woven fabric and the type of fluorine-based compound of the oil-water separation filter are selected, and the amount of TMOS, GPTMS and fluorine-containing silane added shown in Example 1 are changed respectively. In addition, the same operation as in Example 1 is performed to obtain liquid compositions for forming water-repellent and oil-repellent films of Examples 2 to 6 and Comparative Examples 2 to 4. The same industrial alcohol as in Example 1 is added to these liquid compositions, and the same operation as in Example 1 is performed to prepare a diluent for impregnating the non-woven fabric. The non-woven fabric shown in Table 2 is immersed in these diluents in the same manner as in Example 1, and dried to obtain an oil-water separation filter having the characteristics shown in Table 2. It should be noted that in Table 2, as fluorine-based compounds, R in the formula of the fluorine-containing silane shown in Formula (19) to Formula (23) is ethyl.
[0216] It should be noted that the nonwoven fabrics used in Examples 5, 6 and Comparative Example 4 are different from the nonwoven fabric in Example 1 and are made of mixed fibers of PET fiber and glass fiber (PET: glass = 80:20 in mass ratio). Their air permeabilities (before dilution immersion) are 12.0 ml / cm 2 / sec, 12.0ml / cm 2 / sec and 24.0ml / cm 2 / sec. In addition, the air permeability of the oil-water separation filter after being immersed in the diluent was 9.6 ml / cm 2 / sec, 7.7ml / cm 2 / sec and 12.0ml / cm 2 / sec. In addition, the nonwoven fabrics used in Comparative Examples 1 to 3 were composed of two layers of glass fiber nonwoven fabric and PET fiber nonwoven fabric having the same structure as in Example 1, and their air permeabilities (before immersion in the diluent) were 2.5 ml / cm 2 / sec, 2.5ml / cm 2 / sec and 1.1ml / cm 2 / sec. In addition, the air permeability of the oil-water separation filter after immersion in the diluent was 2.3 ml / cm 2 / sec, 0.02ml / cm 2 / sec and 0.03ml / cm 2 / Second.
[0217] <Comparative Example 1>
[0218] In Comparative Example 1, the same nonwoven fabric as in Example 1 was used, but the silica sol-gel did not contain fluorine-containing silane as a fluorine-containing functional group component.
[0219] <Comparative Example 5>
[0220] In Comparative Example 5, a commercially available polytetrafluoroethylene (PTFE) membrane filter with a mesh size of 1 μm was used as the base material of the oil-water separation filter without being treated. The base material was not immersed in a diluted solution of the water- and oil-repellent film-forming liquid composition as in Example 1.
[0221] <Comparative Example 6>
[0222] As a fluorine-based compound, a fluorine-based compound represented by the following formula (28) shown in Synthesis Example 1 of Patent Document 1 having an oil repellency imparting group and a hydrophilicity imparting group (oil repellency and hydrophilicity) was prepared. 0.5 g of the fluorine-based compound was dissolved in 99.5 g of the same industrial alcohol as in Example 1 to prepare a dilution (concentration of 0.5 mass %).
[0223] [Chemistry 8]
[0224]
[0225] Will have 1.1ml / cm 2 A two-layer nonwoven fabric having an air permeability of 1.1 ml / cm2 and the same structure as in Example 1 was immersed in the dilution for 30 seconds. Except for this, the same operation as in Example 1 was performed to obtain an oil-water separation filter. The air permeability of the oil-water separation filter was 1.1 ml / cm2. 2 / second, calculate the water-repellent and oil-repellent film per 1m 2 The amount for nonwoven fabric is 1.0 g.
[0226] <Comparative Test 1 and Evaluation>
[0227] The 12 oil-water separation filters consisting only of nonwoven fabrics obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were installed in Fig.11 The oil-water separation test device 300 shown in FIG. Figure 1300 is added to each symbol of the corresponding element of the oil-water separation device 10 shown, indicating each symbol of the test device 300. In the oil-water separation test device 300, as emulsified oil, HISCREW OIL NEXT 0.25 g of screw compressor oil manufactured by Hitachi Industrial Machinery Co., Ltd. was mixed with 5 liters of ion exchange water at 9000 rpm for 3 minutes, and an emulsified oil (mixed liquid containing water and oil) with a turbid oil concentration of 50 ppm was used. The emulsified oil was supplied to the mixed liquid inflow part 312 and filtered by the oil-water separation filter 313. The filtrate 314 that passed through the oil-water separation filter 313 and was stored in the water storage part (branch flask) 317 was taken, and the turbidity and oil concentration of the filtrate were evaluated by the following method. The results are shown in Table 3. It should be noted that the oil-water separation filter 313 is supported by a metal porous plate 320. In addition, when filtering the emulsified oil, the 12 oil-water separation filters obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were adjusted to a predetermined vacuum degree (-10 kPa) by a suction pump not shown connected to the branch pipe 321 of the flask 317, and the inside of the flask was depressurized to perform suction filtration on the oil-water separation filter 313. Reference numeral 322 is a vacuum gauge.
[0228] (a) Turbidity of the filtrate
[0229] The turbidity of the filtrate was measured using a Lacom Tester turbidity meter TN-100 (manufactured by AS-ONE Co., Ltd.) When the turbidity is small, the oil-water separation is good, and 1.5 or less is a pass level.
[0230] (b) Oil concentration of filtrate
[0231] The oil concentration of the filtrate was determined by measuring the residual oil in the filtrate using an oil content meter (OCMA-555, manufactured by Horiba, Ltd.). The detection limit of the oil content meter varies depending on the type of oil, and the detection limit of the emulsified oil used was 1 ppm.
[0232]
[0233] As is clear from Table 3, in Comparative Example 1, when the silica sol gel is set to 100 mass %, since no fluorine-containing silane as a fluorine-containing functional group component is contained, the turbidity of the filtrate passing through the oil-water separation filter is 3.0, and 15.0 ppm of oil is mixed in the filtrate.
[0234] In Comparative Example 2, when the silica sol-gel was set to 100 mass %, the content of the fluorine-containing functional group component was 11.6 mass %, which was too much. Therefore, the mixed liquid did not pass through the oil-water separation filter and could not be filtered.
[0235] In Comparative Example 3, since every 1m 2The mass of the water-repellent and oil-repellent film of the nonwoven fabric was 33.0 mass %, which was too much. Therefore, the air permeability of the oil-water separation filter was 0.03 ml / cm 2 / second, is too low, therefore, the mixed liquid will not pass through the oil-water separation filter and cannot be filtered.
[0236] In Comparative Example 4, a gas permeability of 12.0 ml / cm 2 / second oil-water separation filter, but every 1m 2 The mass of the water- and oil-repellent film of the nonwoven fabric was 0.05 g, which was too small. Therefore, the oil-repellent effect of the oil-water separation filter was insufficient, the turbidity of the filtrate was 2.0, and 8.0 ppm of oil was mixed in the filtrate, and the oil removal was insufficient.
[0237] In Comparative Example 5, a PTFE membrane filter was used as the oil-water separation filter, but the mixed liquid did not pass through the filter and could not be filtered.
[0238] In Comparative Example 6, since the water-repellent and oil-repellent membrane of the oil-water separation filter was imparted with hydrophilic and oil-repellent properties and the mixed liquid was emulsified oil, the turbidity of the filtrate was 3.0, and 13.0 ppm of oil was mixed in the filtrate, indicating insufficient oil removal.
[0239] In contrast, in the oil-water separation filters of Examples 1 to 6, 2 The nonwoven fabric has a water-repellent and oil-repellent film formed in a ratio of 0.15g to 28g. When the silica sol gel is set to 100% by mass, the fluorine-containing functional group component having both water-repellent and oil-repellent functions is contained in a ratio of 0.02% to 9.8% by mass. The air permeability of the oil-water separation filter is 0.08ml / cm 2 / sec~9.6ml / cm 2 / sec. Therefore, when the evaluation test is performed, when the turbidity of the filtrate is small, the oil-water separation performance is good, and when it is below 1.5, it is qualified and "good". When it exceeds this, it is "bad". The oil concentration of the filtrate meets the 5ppm allowable amount of n-hexane extract (mineral oil content), which confirms that the oil-water separation filters of Examples 1 to 6 have oil-water separation performance.
[0240] Next, Test Examples 1 to 3 and Comparative Test Examples 1 to 4 for measuring the oil-water separation performance of an oil-water separation filter in which the oil-water separation filter is frozen and then thawed will be described.
[0241] <Test Example 1>
[0242] In Test Example 1, the nonwoven fabric of the oil-water separation filter obtained in Example 1 was heat-treated at a temperature of 100° C. for 12 hours in the atmosphere. The initial dynamic friction coefficient based on the following contact and the dynamic friction coefficient after the contact was reciprocated 10 times were measured on one side of the heat-treated nonwoven fabric (the side into which the mixed liquid of water and oil flowed) under the following conditions, and the reduction rate of the dynamic friction coefficient after 10 reciprocating movements when the initial dynamic friction coefficient was set to 100% (hereinafter referred to as "reduction rate of dynamic friction coefficient") was calculated.
[0243] (1) Measuring instrument: Static and dynamic friction measuring machine TL201Tt (Trinita Lab Co., Ltd.)
[0244] (2) Measurement conditions:
[0245] ・Moving distance: 20mm
[0246] ・Vertical load: 50g
[0247] ・Moving speed: 5mm / sec
[0248] ・Contact: 20mm square polyethylene terephthalate film
[0249] The nonwoven fabric for which the dynamic friction coefficient was measured was immersed in water in a container and kept at -22°C for 20 hours to freeze the nonwoven fabric. Then, warm water at 40°C was poured into the container to thaw the nonwoven fabric, and then the nonwoven fabric was dehydrated and kept at a humidity condition with a dew point temperature of -50°C for 24 hours to dry the nonwoven fabric. The heat treatment conditions of the nonwoven fabric of Example 1 and the reduction rate of the dynamic friction coefficient are shown in Table 4.
[0250]
[0251] <Comparative Test Example 1>
[0252] In Comparative Test Example 1, the nonwoven fabric of the oil-water separation filter obtained in Example 1 was not heat-treated, and the dynamic friction coefficient of the nonwoven fabric was measured under the same conditions as in Test Example 1, and the reduction rate was calculated. Next, the nonwoven fabric was immersed in water contained in a container. Hereinafter, the nonwoven fabric was frozen under the same conditions as in Test Example 1, and the nonwoven fabric was thawed and dried under the same conditions as in Test Example 1.
[0253] <Test Examples 2~3, Comparative Test Examples 2~3>
[0254] In Test Examples 2 to 3 and Comparative Test Examples 2 to 3, the nonwoven fabric of the oil-water separation filter obtained in Example 1 was heat treated under the conditions shown in Table 4, and the dynamic friction coefficient of the nonwoven fabric was measured under the same conditions as in Test Example 1, and the reduction rate was calculated. Next, the nonwoven fabric was frozen under the same conditions as in Test Example 1, and the nonwoven fabric was thawed and dried under the same conditions as in Test Example 1.
[0255] <Comparative Test Example 4>
[0256] In Comparative Test Example 4, the nonwoven fabric of the oil-water separation filter obtained in Comparative Example 6 was heat treated under the conditions shown in Table 4, and the dynamic friction coefficient of the nonwoven fabric was measured under the same conditions as in Test Example 1, and the reduction rate was calculated. Next, the nonwoven fabric was frozen under the same conditions as in Test Example 1, and the nonwoven fabric was thawed and dried under the same conditions as in Test Example 1.
[0257] <Comparative Test 2 and Evaluation>
[0258] For the seven oil-water separation filters obtained in Test Examples 1 to 3 and Comparative Test Examples 1 to 4, Comparative Test 2 was conducted in the same manner as Comparative Test 1. Fig.11 In the oil-water separation test device 300 shown, the oil-water separation filter 313 is supported by a metal porous plate 320. And, the same mixed liquid containing water and oil as in the first comparative test and in the same amount as in the first comparative test was filtered by suction at a vacuum degree of -10 kPa using a suction pump. The turbidity of the filtrate and the oil concentration of the filtrate were measured in the same manner as in the first comparative test. In addition, the time for the mixed liquid to pass through the oil-water separation filter was also measured in the same manner as in the first comparative test. The results are shown in Table 5.
[0259]
[0260] It is clear from Table 5 that in Comparative Test Example 1, since the nonwoven fabric was not heat-treated, the reduction rate of the dynamic friction coefficient on one side of the nonwoven fabric increased to 8%, but in the oil-water separation test device, when the vacuum was filtered at -10kPa, the oil concentration of the filtrate was as low as 1ppm, and the turbidity of the filtrate was also as low as 0.5. However, the passage time of the filtrate was as long as 1500 seconds (25 minutes). Therefore, in Comparative Test Example 1, the oil-water separation performance was slightly deteriorated.
[0261] In Comparative Test Example 2, since the heat treatment temperature was 150°C, which was too high, the reduction rate of the dynamic friction coefficient on one side of the nonwoven fabric was as high as 15%. In addition, in the oil-water separation test device, when the vacuum was filtered at -10kPa, the oil concentration of the filtrate was as high as 38ppm, and the turbidity of the filtrate was as high as 25. Furthermore, the passage time of the filtrate was as short as 55 seconds. Therefore, oil leakage was observed in Comparative Test Example 1, and it can be considered that the nonwoven fabric was damaged.
[0262] In Comparative Test Example 3, since the heat treatment time was 36 hours, which was too long, the reduction rate of the dynamic friction coefficient on one side of the nonwoven fabric was as high as 17%. In addition, in the oil-water separation test device, when the filtration was performed at a vacuum degree of -10kPa, the oil concentration of the filtrate was as high as 45ppm, and the turbidity of the filtrate was as high as 51. Furthermore, even after 3600 seconds (60 minutes), the filtrate did not completely pass through the oil-water separation filter, and the filtration test was terminated in the process. Oil leakage was observed in Comparative Test Example 3, and the oil-water separation performance deteriorated.
[0263] In the oil-water separation filter of Patent Document 1 of Comparative Test Example 4, the fluorine-based compound constituting the water-repellent and oil-repellent membrane does not contain silica sol gel, so although heat treatment was performed at 120°C and 3 hours, the reduction rate of the dynamic friction coefficient on one side of the non-woven fabric was as high as 35%. In addition, in the oil-water separation test device, when the vacuum filtration was performed at a vacuum degree of -10kPa, the oil concentration of the filtrate was as high as 41ppm, and the turbidity of the filtrate was as high as 48. Furthermore, even after 3600 seconds (60 minutes), the filtrate did not completely pass through the oil-water separation filter, and the filtration test was terminated in the process. Therefore, in Comparative Test Example 4, the oil-water separation performance deteriorated.
[0264] In contrast, the oil-water separation filters of Test Examples 1 to 3 use the non-woven fabric of Example 1 and meet the heat treatment conditions of Aspect 13. Therefore, during the evaluation test, the turbidity of the filtrate is below 0.6, which is qualified. The oil concentration of the filtrate meets the allowable amount of n-hexane extract (mineral oil content) of 5ppm, and the processing time for oil-water separation is also below 150 seconds, which can confirm that it has oil-water separation performance.
[0265] <Examples and Comparative Examples Corresponding to the Second Embodiment>
[0266] [Synthesis Examples 1 to 9 for Preparing Metal Oxide Particle Dispersion Liquids, Comparative Synthesis Examples 1 to 3]
[0267] <Synthesis example 1>
[0268] To a beaker containing 50.0 g of an IPA dispersion of silicon dioxide having an average particle size of 12 nm (IPA-ST, manufactured by Nissan Chemical Co., Ltd., with a SiO2 concentration of 30%), 0.23 g of the fluorine compound represented by the above formula (19) was added and mixed. Next, 0.08 g of water was added and mixed. Furthermore, 0.001 g of nitric acid was added and mixed at 40° C. for 2 hours to obtain a dispersion of silicon dioxide (silica) particles in which the fluorine compound was bonded to the silicon dioxide particles. The mass ratio (A / B) of the fluorine functional group component (A) to the silicon dioxide as the metal oxide particles (B) was 0.014.
[0269] <Synthesis example 2>
[0270] 0.45 g of the fluorine compound represented by the above formula (20) was added to a beaker containing 50.0 g of an IPA dispersion of silicon dioxide having an average particle size of 45 nm (IPA-ST-L, manufactured by Nissan Chemical Co., Ltd., with a SiO2 concentration of 30%), and mixed. Next, 0.16 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 1 was performed to obtain a dispersion of silicon dioxide (silica) particles. The mass ratio (A / B) was 0.027.
[0271] <Synthesis example 3>
[0272] 0.75 g of the fluorine compound represented by the above formula (21) was added to a beaker containing 50.0 g of an IPA dispersion of silicon dioxide having an average particle size of 80 nm (IPA-ST-ZL, manufactured by Nissan Chemical Co., Ltd., with a SiO2 concentration of 30%), and mixed. Next, 0.27 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 1 was performed to obtain a dispersion of silicon dioxide (silica) particles. The mass ratio (A / B) was 0.046.
[0273] <Synthesis example 4>
[0274] 3.15 g of the fluorine compound represented by the above formula (22) was added to a beaker containing 50.0 g of the IPA dispersion of silica as in Synthesis Example 1, and mixed. Next, 1.13 g of water was added and mixed. Furthermore, 0.010 g of nitric acid was added, and the same operation as in Synthesis Example 1 was performed to obtain a dispersion of silica (silica) particles. The mass ratio (A / B) was 0.196.
[0275] <Synthesis example 5>
[0276] In a beaker containing 50.0 g of an IPA dispersion of silica as in Synthesis Example 1, the same operation as in Synthesis Example 2 was performed except that the fluorine compound used in Synthesis Example 2 was replaced with the fluorine compound represented by the above formula (27) and the nitric acid was changed to 0.010 g to obtain a dispersion of silica (silica) particles. The mass ratio (A / B) was 0.028.
[0277] <Synthesis example 6>
[0278] 0.45 g of the fluorine compound represented by the above formula (27) was added to a beaker containing 50.0 g of a methanol dispersion of zirconium dioxide having an average particle size of 3 nm (SZR-M, manufactured by Sakai Chemical Co., Ltd., with a ZrO2 concentration of 30%), and mixed. Next, 0.16 g of water was added and mixed. Furthermore, 0.001 g of nitric acid was added, and the same operation as in Synthesis Example 1 was performed to obtain a dispersion of zirconium dioxide particles. The mass ratio (A / B) of the fluorine-based functional group component (A) to the zirconium dioxide as the metal oxide particles (B) was 0.028.
[0279] <Synthesis Example 7>
[0280] 0.27 g of the fluorine compound represented by the above formula (27) was added to a beaker containing 50.0 g of an IPA dispersion of titanium dioxide having an average particle size of 6 nm (TKD-701, manufactured by TEICA Co., Ltd., TiO2 concentration of 18%), and mixed. Next, 0.10 g of water was added and mixed. Furthermore, 0.010 g of nitric acid was added, and the same operation as in Synthesis Example 1 was performed to obtain a dispersion of titanium dioxide particles. The mass ratio (A / B) of the fluorine-based functional group component (A) to the titanium dioxide as the metal oxide particles (B) was 0.028.
[0281] <Synthesis example 8>
[0282] 0.15 g of the fluorine compound represented by the above formula (27) was added to a beaker containing 50.0 g of an IPA dispersion of aluminum oxide and silicon dioxide having an average particle size of 60 nm (Bial AS-L10, manufactured by Taki Chemical Co., Ltd., 3Al2O3・2SiO2 concentration of 10%), and mixed. Next, 0.05 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 1 was performed to obtain a dispersion of aluminum oxide and silicon dioxide particles. The mass ratio (A / B) of the fluorine-based functional group component (A) to the aluminum oxide and silicon dioxide as the metal oxide particles (B) was 0.028.
[0283] <Synthesis Example 9>
[0284] To a beaker containing 50.0 g of an IPA dispersion of zinc oxide having an average particle size of 25 nm (MZ-500, manufactured by Teika Co., Ltd., with a ZnO concentration of 30%), 0.45 g of the fluorine compound represented by the above formula (27) was added and mixed. Next, 0.16 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 1 was performed to obtain a dispersion of zinc oxide particles. The mass ratio (A / B) of the fluorine-based functional group component (A) to the zinc oxide as the metal oxide particles (B) was 0.028.
[0285] <Comparative Synthesis Example 1>
[0286] 0.45 g of the fluorine compound represented by the above formula (27) was added to a beaker containing 50.0 g of an IPA dispersion of titanium dioxide having an average particle size of 230 nm (R32, manufactured by Sakai Chemical Co., Ltd., TiO2 concentration of 30%), and mixed. Next, 0.16 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 1 was performed to obtain a dispersion of titanium dioxide particles. The mass ratio (A / B) of the fluorine-based functional group component (A) to the titanium dioxide as the metal oxide particles (B) was 0.028.
[0287] <Comparative Synthesis Example 2>
[0288] 0.08 g of the fluorine compound represented by the above formula (27) was added to a beaker containing 50.0 g of the IPA dispersion of the same silicon dioxide as in Synthesis Example 1, and mixed. Next, 0.03 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 1 was performed to obtain a dispersion of silicon dioxide (silica) particles. The mass ratio (A / B) was 0.005.
[0289] <Comparative Synthesis Example 3>
[0290] 3.45 g of the fluorine compound represented by the above formula (27) was added to a beaker containing 50.0 g of the IPA dispersion of the same silicon dioxide as in Synthesis Example 1, and mixed. Next, 1.24 g of water was added and mixed. Furthermore, 0.011 g of nitric acid was added, and the same operation as in Synthesis Example 1 was performed to obtain a dispersion of silicon dioxide (silica) particles. The mass ratio (A / B) was 0.218.
[0291] The following Table 6 shows the contents of the dispersions of the fluorine-containing metal oxide particles of Synthesis Examples 1 to 9 and Comparative Synthesis Examples 1 to 3. In Table 6, R in the formula of the fluorine-containing silane represented by Formula (19) to Formula (22) and Formula (27) as the fluorine-based compounds is ethyl.
[0292]
[0293] [Examples 7 to 15 and Comparative Examples 7 to 11 for preparing a liquid composition for forming a water- and oil-repellent film and manufacturing an oil-water separation filter]
[0294] <Example 7>
[0295] After mixing 30 g of ethyl orthosilicate, 60 g of ethanol and 10 g of water, 1 g of nitric acid was added, and the mixture was mixed at 30° C. for 3 hours to obtain a silica sol-gel solution. After adding 104.63 g of industrial alcohol (AP-7, manufactured by Nippon Alcohol Industry Co., Ltd.) to 3.00 g of the obtained silica sol-gel solution and mixing, 0.37 g of the dispersion of the metal oxide particles of Synthesis Example 1 was added and mixed to obtain a liquid composition for forming a water-repellent and oil-repellent film.
[0296] As the base material of the oil-water separation filter, a laminate of a nonwoven fabric formed of glass fibers on the upper layer and a nonwoven fabric formed of PET fibers on the lower layer (a two-layer nonwoven fabric) was used. The air permeability of the laminate was 2.1 ml / m 2 The two layers of nonwoven fabric were immersed in the above-mentioned liquid composition for forming a water-repellent and oil-repellent film, the excess liquid was shaken off, and the nonwoven fabric was dried at room temperature for 24 hours to produce a nonwoven fabric with an air permeability of 2.1 ml / cm 2 / sec oil-water separation filter.
[0297] The contents are shown in the following Tables 7 and 8. In Table 7, "(A) mass %" in "the content ratio of the liquid composition excluding the solvent" means "(A) / [(A)+(B)+(C)]×100 mass %", and similarly, "[(A)+(B)] mass %" means "[(A)+(B)] / [(A)+(B)+(C)]×100 mass %", and similarly, "(C) mass %" means "(C) / [(A)+(B)+(C)]×100 mass %".
[0298]
[0299]
[0300] <Examples 8 to 15 and Comparative Examples 7 to 10>
[0301] For Examples 8 to 15 and Comparative Examples 7 to 10, the type and weight of the dispersion of fluorine-containing metal oxide particles, the weight of the silica sol-gel solution, and the weight of the same industrial alcohol as in Example 7 were selected or determined as shown in Table 7.
[0302] Regarding the silica sol-gel solution, in Examples 8 to 15 and Comparative Examples 7 to 10, 28.50 g of a trimer to a pentamer of tetramethoxysilane (TMOS) (manufactured by Mitsubishi Chemical Corporation, trade name: MKC SILICATE MS51) and 1.50 g of 3-glycidoxypropyltrimethoxysilane (GPTMS: manufactured by Shin-Etsu Chemical Co., Ltd., trade name: KBM-403) as a silane containing an epoxy group serving as an alkylene component were used instead of the ethyl orthosilicate used in Example 7. Other than this, the same operation as in Example 7 was performed.
[0303] Furthermore, as shown in Table 8, the air permeability of the nonwoven fabric before immersion, the type of the base material of the oil-water separation filter, and the air permeability of the oil-water separation filter (after immersion) were selected.
[0304] Furthermore, in the same manner as in Example 7, water- and oil-repellent film-forming liquid compositions of Examples 8 to 15 and Comparative Examples 7 to 10 were obtained.
[0305] Furthermore, in the same manner as in Example 7, the nonwoven fabric was immersed in the diluted liquid of the water- and oil-repellent film-forming liquid composition, deliquored and dried to obtain oil-water separation filters of Examples 8 to 15 and Comparative Examples 7 to 10 having air permeabilities shown in Table 8.
[0306] <Comparative Example 11>
[0307] In Comparative Example 11, a liquid composition for forming a water- and oil-repellent film was obtained in the same manner as in Example 7 described in Patent Document 1. Specifically, 8.52 g of a trimer to a pentamer of tetramethoxysilane (TMOS) as a silicon alkoxide (manufactured by Mitsubishi Chemical Corporation, trade name: MKC SILICATE MS51), 0.48 g of 3-glycidoxypropyltrimethoxysilane (GPTMS: manufactured by Shin-Etsu Chemical Co., Ltd., trade name: KBM-403) as a silane containing an epoxy group, 0.24 g of a fluorine-containing silane (R: ethyl) represented by the following formula (29) as a fluorine-based compound, and 17.58 g of ethanol (EtOH) (boiling point: 78.3° C.) as an organic solvent were mixed, and further, 3.37 g of ion-exchanged water was added, and the mixture was stirred at 25° C. for 5 minutes in a separable flask to prepare a mixed solution. Furthermore, 0.05 g of hydrochloric acid at a concentration of 35% by mass was added to the mixed solution as a catalyst, and the mixture was stirred at 40° C. for 2 hours. Thus, a liquid composition for forming an oil-water separation membrane containing a silica sol hydrolyzate was prepared. In the same manner as in Example 7, the same nonwoven fabric as in Example 1 was immersed in the diluted liquid of the water-repellent and oil-repellent film-forming liquid composition, and deliquored and dried to obtain an oil-water separation filter having the characteristics shown in Table 8.
[0308] [Chemistry 9]
[0309]
[0310] It should be noted that the nonwoven fabric used in Example 15 is different from the nonwoven fabric in Example 7. It is a layer of nonwoven fabric formed by mixed fibers of PET fibers and glass fibers (PET: glass = 80:20 in terms of mass ratio), and the air permeability before impregnation is 9.5 ml / cm 2 / Second.
[0311] <Comparative test and evaluation>
[0312] The 14 oil-water separation filters obtained in Examples 7 to 15 and Comparative Examples 7 to 11 were installed in Fig.11 The oil-water separation test apparatus 300 shown above was used. Using the test apparatus 300 and the above method, (a) the oil concentration of the filtrate, (b) the turbidity of the filtrate, and (c) the passage time of the filtrate were evaluated. The results are shown in Table 8 above.
[0313] (a) Oil concentration of filtrate
[0314] The oil concentration of the filtrate was determined using the above-mentioned oil content meter (manufactured by Horiba, Ltd., OCMA-555). In the “oil concentration of the filtrate” in Table 8 and Table 9 described below, “<1” means that it is below the detection limit of the oil content meter.
[0315] (b) Turbidity of the filtrate
[0316] The turbidity of the filtrate was measured using the above-mentioned Lacom Tester turbidity meter TN-100 (manufactured by AS-ONE Co., Ltd.).
[0317] (c) Filtrate passage time
[0318] In the measurement of the passage time of the filtrate, the time from when the suction pump starts to operate until the total amount of the emulsified oil passes through the oil-water separation filter 313 and reaches the water storage part (branch flask) 317 is measured.
[0319] It is clear from Table 8 that the oil-water separation filter of Comparative Example 7 is prepared by preparing a liquid composition for forming a water-repellent and oil-repellent film from Comparative Synthesis Example 1 containing metal oxide (titanium dioxide) particles with an average particle size of 230 nm, immersing a non-woven fabric in the liquid composition, deliquoring and drying, and therefore, the average particle size of the metal oxide particles is too large, and it is difficult to bond the metal oxide particles to the fiber surface of the non-woven fabric through the silica sol as a binder component. As a result, the oil concentration of the filtrate is less than the detection limit of less than 1 ppm, but the turbidity of the filtrate is as high as 3.5, and the passage time of the filtrate is 100 seconds, which is relatively long.
[0320] In the oil-water separation filter of Comparative Example 8, the fluorine-based functional group component (A) was 0.07% by mass when the water-repellent and oil-repellent membrane was set to 100% by mass. This was too small, so the oil repellency was poor and the passage time of the filtrate was as short as 65 seconds. However, the oil concentration of the filtrate was as high as 7.0 ppm and the turbidity of the filtrate was as high as 2.3.
[0321] The air permeability of the oil-water separation filter of Comparative Example 9 is 14.7 ml / cm 2 / second, which is too large, so the passage time of the filtrate is as short as 35 seconds, but the fluorine-based functional group component (A) when the water-repellent and oil-repellent film is set to 100 mass % is 5.6 mass %, which is too much, so the adhesion of the water-repellent and oil-repellent film to the non-woven fabric is deteriorated, the oil concentration of the filtrate is 45.0ppm, which is very high, and the turbidity of the filtrate is also 4.5, which is very high.
[0322] In the oil-water separation filter of Comparative Example 10, the air permeability is 0.03 ml / cm 2 / second, which is too small, so the passage time of the filtrate is as long as more than 3000 seconds (15 minutes). In addition, when the water-repellent and oil-repellent film is set to 100% by mass, the total ratio of the fluorine-based functional group component (A) and the metal oxide particles (B) is 82% by mass, which is too much. Therefore, the content of the silica sol gel (C) becomes relatively low, and the adhesion of the water-repellent and oil-repellent film to the non-woven fabric becomes poor. As a result, the oil concentration of the filtrate is less than the detection limit of less than 1ppm, but the turbidity of the filtrate is as high as 2.1.
[0323] The air permeability of the oil-water separation filter of Comparative Example 11 is 2.1 ml / cm 2 / second and appropriate, the oil concentration of the filtrate is less than the detection limit of 1 ppm, and the turbidity of the filtrate is 0.5. On the other hand, since the fluorine-based compound having the perfluoroamine structure of formula (29) is used, the structure of the fluorine-based compound in the oil-water separation filter of Comparative Example 11 is rigid and easily exhibits strong water repellency. Therefore, compared with the oil-water separation filters of Examples 7 to 15 containing the fluorine-based compound having the perfluoroether structure, the passage time of the filtrate is 120 seconds, which is longer.
[0324] In contrast, the oil-water separation filters of Examples 7 to 15 satisfy the necessary conditions of the fifth aspect of the present invention, and therefore, the oil concentration of the filtrate is less than the detection limit of 1 ppm or 3.0 ppm (Example 15), the turbidity of the filtrate is less than 0.5 or 1.5 (Example 15), and the passage time of the filtrate is 30 seconds to 68 seconds or 180 seconds (Example 14). In Example 15, the oil concentration of the filtrate is 3.0 ppm and the turbidity of the filtrate is 1.5 because the air permeability of the oil-water separation filter is 9.3 ml / cm 2 / sec, which is relatively large. In addition, the time for the filtrate to pass through the oil-water separation filter of Example 14 is 180 seconds because the air permeability of the oil-water separation filter is 0.098 ml / cm 2 / second, smaller.
[0325] <Comparative test and evaluation>
[0326] The two oil-water separation filters of Example 8 and Comparative Example 11 were immersed in water contained in a container respectively, and kept at a temperature of -22°C for 20 hours to freeze the oil-water separation filters. Then, warm water at 40°C was flowed into the container to thaw the oil-water separation filters, and then dehydrated and kept at a humidity condition of a dew point temperature of -50°C for 24 hours to dry the oil-water separation filters. Using the oil-water separation test device 300 used in Comparative Test 3, the oil concentration of the filtrate and the passage time of the filtrate of the dried oil-water separation filters were measured in the same manner as in Comparative Test 3. The results are shown in Table 9 below.
[0327]
[0328] It can be clearly seen from Table 9 that in the oil-water separation filter of Comparative Example 11, the oil concentration of the filtrate is less than the detection limit of 1 ppm, but the water-repellent and oil-repellent membrane is only a silica sol hydrolyzate containing fluorine-containing silane, so the water-repellent and oil-repellent membrane of the oil-water separation filter that is thawed and dried after freezing is peeled off from the fibers of the non-woven fabric. Therefore, the passage time of the filtrate is as long as 1500 seconds (25 minutes). In contrast, in the oil-water separation filter of Example 8, the water-repellent and oil-repellent membrane includes metal oxide particles (B) bonded with a fluorine-based functional group component (A) and silica sol gel (C), so the oil-water separation membrane of the oil-water separation filter that is thawed and dried after freezing will not be peeled off from the fibers of the non-woven fabric. Therefore, the expansion of the fibers of the non-woven fabric is suppressed, the oil concentration of the filtrate is less than the detection limit of 1 ppm, and the passage time of the filtrate is 48 seconds, which has the same degree of oil-water separation performance as the oil-water separation filter that has not been subjected to the freezing test.
[0329] <Examples and Comparative Examples Corresponding to the Third Embodiment>
[0330] [Synthesis Examples 10 to 18 for Preparing Metal Oxide Particle Dispersion Liquids, Comparative Synthesis Examples 4 to 5]
[0331] <Synthesis example 10>
[0332] 0.50 g of the fluorine compound represented by the above formula (19) was added to a beaker containing 50.0 g of an IPA dispersion of silicon dioxide having an average particle size of 12 nm (IPA-ST, manufactured by Nissan Chemical Co., Ltd., with a SiO2 concentration of 30%), and mixed. Next, 0.10 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and mixed at 40° C. for 2 hours to obtain a dispersion of silicon dioxide (silica) particles in which the fluorine compound was bonded to the silicon dioxide particles.
[0333] <Synthesis Example 11>
[0334] 0.50 g of the fluorine compound represented by the above formula (20) was added to a beaker containing 50.0 g of an IPA dispersion of silicon dioxide having an average particle size of 45 nm (IPA-ST-L, manufactured by Nissan Chemical Co., Ltd., with a SiO2 concentration of 30%), and mixed. Next, 0.10 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 10 was performed to obtain a dispersion of silicon dioxide (silica) particles.
[0335] <Synthesis Example 12>
[0336] 0.50 g of the fluorine compound represented by the above formula (21) was added to a beaker containing 50.0 g of an IPA dispersion of silicon dioxide having an average particle size of 80 nm (IPA-ST-ZL, manufactured by Nissan Chemical Co., Ltd., with a SiO2 concentration of 30%), and mixed. Next, 0.10 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 10 was performed to obtain a dispersion of silicon dioxide (silica) particles.
[0337] <Synthesis Example 13>
[0338] 0.25 g of the fluorine compound represented by the above formula (22) was added to a beaker containing 50.0 g of the IPA dispersion of the same silicon dioxide as in Synthesis Example 12, and mixed. Next, 0.05 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 10 was performed to obtain a dispersion of silicon dioxide (silica) particles.
[0339] <Synthesis Example 14>
[0340] 0.75 g of the fluorine compound represented by the above formula (23) was added to a beaker containing 50.0 g of the IPA dispersion of the same silicon dioxide as in Synthesis Example 12, and mixed. Next, 0.15 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 10 was performed to obtain a dispersion of silicon dioxide (silica) particles.
[0341] <Synthesis Example 15>
[0342] 1.50 g of the fluorine compound represented by the above formula (27) was added to a beaker containing 50.0 g of a methanol dispersion of zirconium dioxide having an average particle size of 3 nm (SZR-M, manufactured by Sakai Chemical Co., Ltd., ZrO2 concentration of 30%), and mixed. Next, 4.05 g of water was added and mixed. Furthermore, 0.035 g of nitric acid was added, and the same operation as in Synthesis Example 10 was performed to obtain a dispersion of zirconium dioxide particles.
[0343] <Synthesis Example 16>
[0344] 1.00 g of the fluorine compound represented by the above formula (27) was added to a beaker containing 50.0 g of an IPA dispersion of titanium dioxide having an average particle size of 6 nm (TKD-701, manufactured by Teika Co., Ltd., TiO2 concentration of 18%), and mixed. Next, 0.97 g of water was added and mixed. Furthermore, 0.010 g of nitric acid was added, and the same operation as in Synthesis Example 10 was performed to obtain a dispersion of titanium dioxide particles.
[0345] <Synthesis Example 17>
[0346] 0.01 g of the fluorine compound represented by the above formula (27) was added to a beaker containing 50.0 g of an IPA dispersion of aluminum oxide and silicon dioxide having an average particle size of 60 nm (Bail AS-L10, manufactured by Taki Chemical Co., Ltd., 3Al2O3・2SiO2 concentration of 10%), and mixed. Next, 0.02 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 10 was performed to obtain a dispersion of aluminum oxide and silicon dioxide particles.
[0347] <Synthesis Example 18>
[0348] 0.15 g of the fluorine compound represented by the above formula (27) was added to a beaker containing 50.0 g of an IPA dispersion of zinc oxide having an average particle size of 25 nm (MZ-500, manufactured by Teika Co., Ltd., with a ZnO concentration of 30%), and mixed. Next, 0.11 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 10 was performed to obtain a dispersion of zinc oxide particles.
[0349] <Comparative Synthesis Example 4>
[0350] 0.75 g of the fluorine compound represented by the above formula (27) was added to a beaker containing 50.0 g of an IPA dispersion of titanium dioxide having an average particle size of 230 nm (R32, manufactured by Sakai Chemical Co., Ltd., TiO2 concentration of 30%), and mixed. Next, 0.27 g of water was added and mixed. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 10 was performed to obtain a dispersion of titanium dioxide particles.
[0351] <Comparative Synthesis Example 5>
[0352] In a beaker containing 50.0 g of the same IPA dispersion as in Synthesis Example 10, 0.10 g of water was added and mixed without adding any fluorine-based compound. Furthermore, 0.005 g of nitric acid was added, and the same operation as in Synthesis Example 10 was repeated to obtain a dispersion of silica particles.
[0353] Table 10 below shows the contents of the dispersions of fluorine-containing metal oxide particles of Synthesis Examples 10 to 18 and Comparative Synthesis Example 4, and the dispersion of fluorine-free metal oxide particles of Comparative Synthesis Example 5. It should be noted that in Table 10, as fluorine-based compounds, R in the formula of the fluorine-containing silane represented by Formula (19) to Formula (23) and Formula (27) is ethyl.
[0354]
[0355] [Synthesis Examples 19 to 22 for preparing fluorine-containing silica sol-gel solutions, Comparative Synthesis Example 6]
[0356] <Synthesis Example 19>
[0357] 0.06 g (0.2 mass %) of the fluorine compound represented by the above formula (27) was added to a beaker containing 28.5 g of a trimer to a pentamer of tetramethoxysilane (TMOS) (manufactured by Mitsubishi Chemical Corporation, trade name: MKCSILICATE MS51) and 59.8 g of ethanol, and mixed. Next, 1.5 g of an epoxy-containing silane as an alkylene component, namely 3-glycidoxypropyltrimethoxysilane (GPTMS: manufactured by Shin-Etsu Chemical Co., Ltd., trade name: KBM-403) and 10 g of water were added and mixed. Furthermore, 0.1 g of nitric acid was added, and the mixture was mixed at 30° C. for 3 hours to obtain a fluorine-containing silica sol-gel solution.
[0358] <Synthesis example 20>
[0359] To a beaker containing 24.0 g of the same TMOS trimer to pentamer as in Synthesis Example 19 and 59.8 g of ethanol, 0.03 g (0.1 mass %) of the fluorine-based compound represented by the above formula (27) was added and mixed. Next, 6.0 g of the same GPTMS as in Synthesis Example 19 and 10 g of water were added as an alkylene component and mixed. Furthermore, 0.1 g of nitric acid was added, and the mixture was mixed at 30° C. for 3 hours to obtain a fluorine-containing silica sol-gel solution.
[0360] <Synthesis Example 21>
[0361] To a beaker containing 29.8 g of the same TMOS trimer to pentamer as in Synthesis Example 19 and 59.9 g of ethanol, 3.00 g (4.2% by mass) of the fluorine-based compound represented by the above formula (27) was added and mixed. Next, 0.2 g of the same GPTMS as in Synthesis Example 19 and 10 g of water were added as an alkylene component and mixed. Furthermore, 0.1 g of nitric acid was added, and the mixture was mixed at 30° C. for 3 hours to obtain a fluorine-containing silica sol-gel solution.
[0362] <Synthesis example 22>
[0363] 0.30 g (0.3% by mass) of the fluorine compound represented by the above formula (27) was added to a beaker containing 30.0 g of tetraethoxysilane (TEOS, manufactured by Tokyo Chemical Industry Co., Ltd.) and 56.9 g of ethanol, and mixed. Next, 10 g of water was added without adding an alkylene component, and mixed. Furthermore, 0.1 g of nitric acid was added, and mixed at 30° C. for 3 hours to obtain a fluorine-containing silica sol-gel solution.
[0364] <Comparative Synthesis Example 6>
[0365] In a beaker containing 28.5 g of the same TMOS trimer to pentamer as in Synthesis Example 19 and 59.6 g of ethanol, 1.5 g of the same GPTMS as in Synthesis Example 19 and 10 g of water were added as an alkylene component without adding any fluorine-based compound, and mixed. Furthermore, 0.1 g of nitric acid was added, and the mixture was mixed at 30° C. for 3 hours to obtain a fluorine-free silica sol-gel solution.
[0366] The contents of the fluorine-containing silica sol-gel solutions of Synthesis Examples 19 to 22 and the fluorine-free silica sol-gel solution of Comparative Synthesis Example 6 are shown in Table 11 below.
[0367]
[0368] [Examples 16 to 24 and Comparative Examples 12 to 20 for preparing a liquid composition for forming a water- and oil-repellent film and manufacturing an oil-water separation filter]
[0369] <Example 16>
[0370] To 6.4 g of the fluorine-containing silica sol-gel solution obtained by Synthesis Example 19, 126.0 g of industrial alcohol (AP-7, manufactured by Nippon Alcohol Industry Co., Ltd.) as a solvent was added and mixed. Thereafter, 5.1 g of the dispersion of the metal oxide particles of Synthesis Example 10 was added and mixed to prepare a liquid composition for forming a water-repellent and oil-repellent film. 50 g of the obtained liquid composition for forming a water-repellent and oil-repellent film was diluted with 10 g of a mixed solvent of water and industrial alcohol (water: industrial alcohol = 1:1 by mass ratio) to prepare a diluted solution. As the substrate of the oil-water separation filter, a laminate (two-layer non-woven fabric) of an upper layer of non-woven fabric formed of glass fibers and a lower layer of non-woven fabric formed of PET fibers was used. The air permeability of the laminate is 2.1 ml / m 2 / sec. The two layers of nonwoven fabric were immersed in the above dilution, excess liquid was shaken off, and dried at room temperature for 24 hours to produce an air permeability of 2.0 ml / cm 2 / sec oil-water separation filter.
[0371] The contents are shown in Tables 12 and 13 below.
[0372]
[0373]
[0374] <Examples 17 to 24 and Comparative Examples 12 to 20>
[0375] For Examples 17 to 24 and Comparative Examples 12 to 20, as shown in Table 12, the type and weight of the dispersion of fluorinated metal oxide particles, the type and weight of the fluorinated silica sol-gel liquid, and the weight of the same solvent as in Example 16 were determined respectively to prepare the liquid compositions for forming water- and oil-repellent films of Examples 17 to 24 and Comparative Examples 12 to 20.
[0376] Table 12 also shows the “total content ratio of the first fluorinated functional group component (A1) and the second fluorinated functional group component (A2) in the liquid composition excluding the solvent”, “the mass ratio of the silica sol gel (C) to the metal oxide particles (B) ((C):(B))” and “the mass ratio of the first fluorinated functional group component (A1) to the second fluorinated functional group component (A2) ((A1):(A2))”. It should be noted that the total content ratio (mass %) of the first fluorinated functional group component (A1) and the second fluorinated functional group component (A2) in the liquid composition excluding the solvent is the same as the total content ratio (mass %) of the first fluorinated functional group component (A1) and the second fluorinated functional group component (A2) in the water- and oil-repellent film.
[0377] Select the type of nonwoven fabric and the substrate of the oil-water separation filter having the same or different air permeability as Example 16 shown in Table 13, and operate in the same manner as Example 16, immerse the diluted liquid of each water-repellent and oil-repellent film-forming liquid composition prepared by Examples 17 to 24 and Comparative Examples 12 to 20 in the selected substrate formed by the nonwoven fabric, deliquore and dry, to obtain an oil-water separation filter having the characteristics shown in Table 13.
[0378] It should be noted that the nonwoven fabrics used in Example 24, Comparative Example 16 and Comparative Example 19 are different from the nonwoven fabrics in Example 16, and include a layer of nonwoven fabric formed of mixed fibers of PET fibers and glass fibers (PET: glass = 80:20 in terms of mass ratio). The air permeabilities of the oil-water separation filters obtained from the nonwoven fabrics used in Example 24, Comparative Example 16 and Comparative Example 19 are 8.1 ml / cm 2 / sec, 8.3ml / cm 2 / sec and 14.3ml / cm 2 / Second.
[0379] <Comparative Test V and Evaluation>
[0380] The 18 oil-water separation filters obtained in Examples 16 to 24 and Comparative Examples 12 to 20 were installed in Fig.11 The oil-water separation test device 300 shown above was used. Using the test device 300, (a) the oil concentration of the filtrate, (b) the turbidity of the filtrate, and (c) the passage time of the filtrate were evaluated by the above method. It should be noted that (a) the oil concentration of the filtrate and (b) the turbidity of the filtrate were performed before and after the membrane strength test and before and after the membrane freezing test. The results are shown in Table 14 below.
[0381]
[0382] (a) Oil concentration of filtrate
[0383] The oil concentration of the liquid that passed through the 18 oil-water separation filters, i.e., the filtrate, was determined using the above-mentioned oil content meter (OCMA-555 manufactured by Horiba, Ltd.). It should be noted that in the "oil concentration of the filtrate" in Table 8 and Table 14 described later, "<1" means that it is below the detection limit of the oil content meter, and if it is "below 1.0 ppm", it is "good".
[0384] (b) Turbidity of the filtrate
[0385] Before the following membrane strength test and membrane freezing test were performed, the turbidity of the liquid passed through the 18 types of oil-water separation filters, that is, the filtrate was measured using the above-mentioned Lacom Tester turbidity meter TN-100 (manufactured by AS-ONE Co., Ltd.).
[0386] Next, on the fiber surface of the nonwoven fabric of another 18 types of oil-water separation filters, the following contact was moved back and forth 10 times under the following conditions while applying a specified load, thereby conducting a strength test of the membrane formed on the fiber surface. Thereafter, the turbidity of the filtrate was measured in the same manner as above. The turbidity of the filtrate after the membrane strength test was compared with the turbidity of the filtrate before the membrane strength test, and the same situation was recorded as "good", and the situation of increase was recorded as "bad".
[0387] (i) Measuring instrument: Static and dynamic friction measuring machine TL201Tt (Trinita Lab Co., Ltd.)
[0388] (ii) Measurement conditions:
[0389] ・Moving distance: 30mm
[0390] ・Vertical load: 500g
[0391] ・Moving speed: 50 mm / sec
[0392] ・Contact: 50mm×50mm square neoprene
[0393] Furthermore, another 18 types of oil-water separation filters were immersed in water contained in a container and kept at a temperature of -22°C for 20 hours to freeze the oil-water separation filters. Next, warm water at 40°C was flowed into the container to thaw the oil-water separation filters, and then dehydrated. The oil-water separation filters were kept at a humidity condition with a dew point temperature of -50°C for 24 hours to dry them, thereby conducting a freezing test of the membrane formed on the fiber surface of the non-woven fabric of the oil-water separation filter. Thereafter, the turbidity of the filtrate was measured in the same manner as above. The turbidity of the filtrate after the freezing test of the membrane was compared with the turbidity of the filtrate before the freezing test of the membrane, and the same situation was recorded as "good", and the increased situation was recorded as "bad".
[0394] (c) Filtrate passage time
[0395] Before the following membrane strength test and membrane freezing test, the time for the total amount of the emulsified oil to pass through the oil-water separation filter 313 and reach the water storage part (branch flask) 317 was measured in the measurement of the passage time of the filtrate through 18 types of oil-water separation filters. The time from when the suction pump started to work to when the total amount of the emulsified oil passed through the oil-water separation filter 313 and reached the water storage part (branch flask) 317 was measured. 240 seconds or less was recorded as "good".
[0396] Next, the passage time of the filtrate after the above-mentioned membrane strength test and the membrane freezing test through the 18 oil-water separation filters was measured respectively. The passage time of the filtrate after the membrane strength test was compared with the passage time of the filtrate before the membrane strength test, and it was recorded as "good" when the difference was within ±10 seconds, and it was recorded as "slightly good" when the filtration time of the filtrate was less than 240 seconds although the difference exceeded 10 seconds, and it was recorded as "poor" when the filtration time of the filtrate exceeded 240 seconds. In addition, the passage time of the filtrate after the membrane freezing test was also compared with the passage time of the filtrate before the membrane freezing test, and it was recorded as "good" when the difference was within ±10 seconds, and it was recorded as "slightly good" when the filtration time of the filtrate was less than 240 seconds although the difference exceeded 10 seconds, and it was recorded as "poor" when the filtration time of the filtrate exceeded 240 seconds.
[0397] It is clear from Table 14 that in the oil-water separation filter of Comparative Example 12, a liquid composition for water-repellent and oil-repellent film formation is prepared by the comparative synthesis example 4 containing metal oxide (titanium dioxide) particles having an average particle size of 230nm. The oil-water separation filter of Comparative Example 12 is made by impregnating a nonwoven fabric in the liquid composition, deliquating and drying, and therefore, the average particle size of the metal oxide particles is too large, and it is difficult to bond the metal oxide particles to the fiber surface of the nonwoven fabric by the silica sol gel as a binder component. As a result, the oil concentration of the filtrate is less than the detection limit of 1ppm, but the turbidity of the filtrate before various tests of the membrane is as high as 3.5, and the passing time of the filtrate before various tests of the membrane is 100 seconds, which is relatively long, poor filtration efficiency, and poor oil repellency. In addition, in the strength test of the membrane, the metal oxide particles fall off, and therefore, the strength test of the membrane and the freezing test of the membrane are not carried out.
[0398] In the oil-water separation filter of Comparative Example 13, a liquid composition for forming a water-repellent and oil-repellent film is prepared from Comparative Synthesis Example 6 in which the silica sol gel does not contain a fluorine-based functional group component (A2). The oil-water separation filter of Comparative Example 13 is made by immersing a nonwoven fabric in the liquid composition, deliquoring and drying. Therefore, the oil concentration of the filtrate is less than the detection limit of 1 ppm, and the concentration of the filtrate before various tests of the membrane is less than 0.5, which are "good", respectively. However, the silica sol gel does not contain a fluorine-based functional group component, so it can be considered that the metal oxide particles are easily fixed to the surface of the membrane component and easily peeled off from the fiber surface of the nonwoven fabric. The turbidity of the filtrate after the strength test of the membrane increased by 2.3, which is "bad". In addition, the passage time of the filtrate before various tests of the membrane is 46 seconds, which is "good", but for the same reason, the passage time of the filtrate after the strength test of the membrane is extended to 242 seconds, which is "bad". On the other hand, after the freezing test of the membrane, due to the size maintenance effect of the metal oxide particles, the turbidity and passage time of the filtrate did not change from those before the test, and both were "good".
[0399] In the oil-water separation filter of Comparative Example 14, the mass ratio of silica sol gel (C) to metal oxide particles (B) is 5:95, and the proportion of silica sol gel is reduced to prepare a liquid composition for forming a water-repellent and oil-repellent film. In the oil-water separation filter of Comparative Example 14, the metal oxide particles realized by the silica sol gel as a binder component have weak adhesion to the fiber surface of the non-woven fabric. As a result, the oil concentration of the filtrate is less than the detection limit of less than 1ppm, but the turbidity of the filtrate before various membrane tests is as high as 3.0. In addition, the air permeability of the substrate is as small as 0.84ml / cm 2 / sec, therefore, the filtrate passage time before various tests of the membrane was 465 seconds, which was very long, and the filtration efficiency was poor, and the oil repellency was poor. Therefore, the strength test and freezing test of the membrane were not carried out.
[0400] In the oil-water separation filter of Comparative Example 15, the mass ratio of silica sol gel (C) to metal oxide particles (B) is 95:5, and the proportion of metal oxide particles is slightly reduced to prepare a liquid composition for forming a water-repellent and oil-repellent film. In the oil-water separation filter of Comparative Example 15, there are few metal oxide particles in the membrane, so the oil concentration of the filtrate is less than the detection limit of 1ppm, the concentration of the filtrate before various tests of the membrane is less than 0.5, which are "good", and the passage time of the filtrate before various tests of the membrane is 44 seconds, which is "good". However, the proportion of metal oxide particles is small, so after the strength test of the membrane or the freezing test of the membrane, there is no strength improvement or size maintenance effect brought by the metal oxide particles. Therefore, after the strength test of the membrane or the freezing test of the membrane, the turbidity and passage time of the filtrate are worse than before the test, and are both "poor".
[0401] In the oil-water separation filter of Comparative Example 16, the air permeability of the substrate is as high as 8.3 ml / cm 2 / second, therefore, the passage time of the filtrate before various tests of the membrane was 45 seconds, which was "good". However, since the value of A1+A2 was 0.4, which was too small, the performance of repelling oil particles became insufficient, the oil concentration of the filtrate before various tests of the membrane was 2.6ppm, and the turbidity of the filtrate before various tests of the membrane was as high as 2.0, indicating poor oil repellency. Therefore, the strength test and freezing test of the membrane were not performed.
[0402] In the oil-water separation filter of Comparative Example 17, the value of A1+A2 was 16.1, which was too large, so liquid did not pass through. Therefore, neither the membrane strength test nor the membrane freezing test was conducted.
[0403] In the oil-water separation filter of Comparative Example 18, a liquid composition for forming a water- and oil-repellent film was prepared from Comparative Synthesis Example 2 in which metal oxide particles were not bonded with a fluorine-based functional group component (A1). In the oil-water separation filter of Comparative Example 18, metal oxide particles that were not subjected to water- and oil-repellent treatment were used. Therefore, the oil concentration of the filtrate was as high as 1.8 ppm, and the turbidity of the filtrate was also as high as 1.6. Furthermore, the passing time of the filtrate before various tests on the membrane was 365 seconds, which was very long, the filtration efficiency was poor, and the oil repellency was poor. Therefore, neither the membrane strength test nor the membrane freezing test was conducted.
[0404] In the oil-water separation filter of Comparative Example 19, the air permeability of the substrate was 14.3 ml / cm 2 / sec, which was too large. Therefore, both the oil concentration and turbidity of the filtrate showed high values. Therefore, neither the membrane strength test nor the membrane freezing test was conducted.
[0405] In the oil-water separation filter of Comparative Example 20, the air permeability of the substrate was 0.03 ml / cm 2 / sec, which was too small. Therefore, the liquid did not pass through. Therefore, neither the membrane strength test nor the membrane freezing test was conducted.
[0406] In contrast, the oil-water separation filters of Examples 16 to 24 satisfied the necessary conditions of the sixth aspect of the present invention. Therefore, including after the membrane strength test and after the freezing test, the oil concentration of the filtrate was below the detection limit of less than 1 ppm or was 1.0 ppm (Example 24), the turbidity of the filtrate was less than 0.5 or at most 0.7 (Example 24), and the passing time of the filtrate was 28 seconds to 210 seconds, and the filtration efficiency was "good" or "slightly good". In Example 23, the passing time of the filtrate was 183 seconds before various tests on the membrane, 210 seconds after the membrane strength test, and 191 seconds after the membrane freezing test. The reason for the relatively long times was that the air permeability of the oil-water separation filter was as small as 0.1 ml / cm 2 / sec. In addition, in Example 24, the oil concentration of the filtrate was 1.0 ppm, the turbidity of the filtrate was 0.6 before various tests on the membrane, 0.7 after the membrane strength test, and 0.6 after the membrane freezing test because the air permeability of the oil-water separation filter was 8.1 ml / cm 2 / sec, which was relatively large.
[0407] Furthermore, in the oil-water separation filters of Examples 20, 22 to 24, A1 < A2 and the necessary conditions of the eighth aspect of the present invention were not satisfied. Therefore, compared with before the membrane strength test, after the membrane strength test, the filtration time of the filtrate was less than 240 seconds and was extended by more than 10 seconds, so it was "slightly good". It can be considered that the adhesion of the water- and oil-repellent film to the fiber surface of the non-woven fabric was not sufficiently high.
[0408] Industrial Applicability
[0409] The oil-water separation filter of the present invention is used in the field where it is necessary to separate oil from emulsified oil or water-soluble oil obtained by emulsifying oil and recover water.
Claims
1. An oil-water separation filter, comprising a nonwoven fabric having a plurality of pores formed between fibers, wherein the plurality of pores penetrate between a side through which a mixed liquid containing water and oil flows in and another side opposite to the side through which the mixed liquid flows out, characterized in that: forming a water- and oil-repellent film on the fiber surface of the nonwoven fabric, The water- and oil-repellent film comprises a fluorine-containing functional group component (A) having both water- and oil-repellent properties and a silica sol gel (C). The air permeability of the oil-water separation filter is 0.05 ml / cm 2 / sec~14ml / cm 2 / Second, The fluorine-containing functional group component (A) comprises a perfluoroether structure represented by the following general formula (1) or formula (2): C p F 2p+1 -O-C q F 2q -O-C r F 2r -X-Y (1) C p F 2p+1 -O-C q F 2q -X-Y (2) In the formula (1) and (2), p, q and r are the same or different from each other and are integers of 1 to 6, and are linear or branched. In addition, in the formula (1) and (2), X is a hydrocarbon group having 2 to 10 carbon atoms, and contains one or more bonds selected from ether bonds, CO-NH bonds, O-CO-NH bonds and sulfonamide bonds. Furthermore, in the formula (1) and (2), Y is a hydrolyzate of silane or a main component of a silica sol-gel. When a 20 mm square polyethylene terephthalate film contact moves on the one surface at a vertical load of 50 g, a moving speed of 5 mm / sec, and a moving distance of 20 mm, the reduction rate of the dynamic friction coefficient after 10 reciprocating movements relative to the initial dynamic friction coefficient is less than 6%.
2. The oil-water separation filter according to claim 1, wherein: On the fiber surface of the non-woven fabric, 2 The water- and oil-repellent film is formed in a ratio of 0.1 g to 30 g of the nonwoven fabric.
3. The oil-water separation filter according to claim 1, wherein: The fluorine-containing functional group component (A) is contained in a ratio of 0.01% by mass to 10% by mass, based on 100% by mass of the silica sol-gel (C).
4. An oil-water separation filter, comprising a nonwoven fabric having a plurality of pores formed between fibers, wherein the plurality of pores penetrate between a side through which a mixed liquid containing water and oil flows in and another side opposite to the side through which the mixed liquid flows out, characterized in that: forming a water- and oil-repellent film on the fiber surface of the nonwoven fabric, The water-repellent and oil-repellent film comprises SiO2, ZnO, ZrO2, TiO2 or Al2O3·SiO2 particles (B) with an average particle size of 2nm to 90nm bonded with a fluorine-containing functional group component (A) having both water-repellent and oil-repellent properties, and silica sol gel (C), The air permeability of the oil-water separation filter is 0.05 ml / cm 2 / sec~14ml / cm 2 / Second, The fluorinated functional group component (A) comprises a perfluoroether structure represented by the following general formula (1) or formula (2), and when the water- and oil-repellent film is taken as 100 mass %, the fluorinated functional group component (A) is contained in a ratio of 0.3 mass % to 5.0 mass %, The fluorine-containing functional group component (A) and the particles (B) are contained in a total amount of 20 to 80% by mass, based on 100% by mass of the water- and oil-repellent film. The mass ratio (A / B) of the fluorine-containing functional group component (A) to the particles (B) is in the range of 0.01 to 0.046, C p F 2p+1 -O-C q F 2q -O-C r F 2r -X-Y (1) C p F 2p+1 -O-C q F 2q -X-Y (2) In the formula (1) and (2), p, q and r are the same or different from each other and are integers of 1 to 6, and are linear or branched. In addition, in the formula (1) and (2), X is a hydrocarbon group having 2 to 10 carbon atoms, comprising one or more bonds selected from an ether bond, a CO-NH bond, an O-CO-NH bond and a sulfonamide bond. Furthermore, in the formula (1) and (2), Y is a hydrolyzate of silane or a main component of a silica sol-gel.
5. The oil-water separation filter according to claim 1 or 4, wherein: The silica sol gel further contains 0.5 to 20 mass % of an alkylene component having 2 to 7 carbon atoms, based on 100 mass % of the silica sol gel (C).
6. The oil-water separation filter according to claim 1 or 4, wherein: The nonwoven fabric is composed of a single layer or a laminate of multiple layers.
7. The oil-water separation filter according to claim 1 or 4, wherein: The fibers constituting the nonwoven fabric are one or more fibers selected from the group consisting of polyethylene terephthalate, polypropylene, glass, alumina, carbon, cellulose, pulp, nylon, and metal.
8. The oil-water separation filter according to claim 1 or 4, wherein: The fibers constituting the nonwoven fabric corresponding to the side into which the mixed liquid containing water and oil flows are glass fibers.
9. The method for manufacturing the oil-water separation filter according to claim 1, comprising the following steps: A step of adding a catalyst to a mixed solution obtained by mixing silicon alkoxide, a fluorine-based compound containing a fluorine-containing functional group component (A), alcohol and water to prepare a liquid composition for forming a water- and oil-repellent film; A step of mixing the water- and oil-repellent film-forming liquid composition with a solvent to prepare a diluted solution; The step of immersing the nonwoven fabric in the diluent; The step of removing liquid from the impregnated nonwoven fabric and drying it to form a water- and oil-repellent film on the fiber surface of the nonwoven fabric; as well as A step of heat-treating the nonwoven fabric having the water- and oil-repellent film formed thereon at a temperature of 30° C. to 120° C. in the air for 1 to 24 hours.
10. The method for manufacturing the oil-water separation filter according to claim 4, comprising the following steps: A step of dispersing the particles (B) according to claim 4 in an organic solvent to prepare a dispersion of the particles; A step of mixing a fluorine-containing compound containing a fluorine-containing functional group component (A), water and a catalyst into the particle dispersion to prepare a fluorine-containing particle dispersion; A step of adding a catalyst to a mixed solution of silicon alkoxide, alcohol and water to prepare a silica sol-gel solution; A step of mixing the dispersion of the fluorine-containing particles with the diluted silica sol-gel solution to prepare a liquid composition for forming a water- and oil-repellent film; a step of immersing a nonwoven fabric in a diluted solution of the water- and oil-repellent film-forming liquid composition; and The impregnated nonwoven fabric is dehydrated and dried.