Production method of high-viscosity scar patch

By using movable heating and drying equipment and board-frame molds in the production of scar patches, combining high-precision fixed water platform and optimized silicone gel formula, the problem of insufficient adhesion of scar patches is solved, and the scar patches are significantly improved Viscosity and treatment effect, and improve productivity.

CN113304126BActive Publication Date: 2024-11-22HANGZHOU GUILING MEDICAL INSTR CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202110620691.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-03
Publication Date
2024-11-22
Estimated Expiration
2041-06-03

AI Technical Summary

Technical Problem

The existing scar patches are not sticky enough, which makes it easy to fall off when the body is bent or moved, affecting the duration of the work and treatment effect.

Method used

It adopts movable heating and drying equipment and board-frame molds, combined with high-precision fixed water platform, optimizes the silicon gel mixture formula and production process, improves the viscosity and curing molding consistency of silicon gels, and enhances the peel strength of scar patches.

Benefits of technology

It significantly improves the adhesion of scar stickers, reduces the risk of shedding, extends the continuous action time, improves the effect of scar treatment, simplifies the production process and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113304126B_ABST
    Figure CN113304126B_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing a high-viscosity scar patch, and relates to the technical field of medical devices. The method comprises the following steps: S1, preheating; S2, installing a mold; S3, pouring materials; S4, heating materials; S5, laminating, cutting and packaging; in S3, the silicone gel mixture comprises, by mass, 70 to 75 parts of end-side vinyl silicone oil, 13 to 15 parts of end-side hydrogenated silicone oil, 11 to 17 parts of end-side hydrogenated silicone oil, and 0.3 to 0.5 parts of Karstedt platinum catalyst. The present invention optimizes the product formula, so that the peel strength of the scar patch is enhanced by more than two times, the viscosity is greatly improved, the risk of the scar patch falling off during use is reduced, the continuous action time on the scar is increased, and the scar treatment effect is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical devices, and in particular to a production method of a high-viscosity scar patch. Background Art

[0002] Scars are extremely common in daily life, and often occur on exposed parts of the body such as the face, arms, and legs, causing trauma and distress to people physically and psychologically.

[0003] At present, the main active ingredient of scar patches on the market is organic silicone gel. As a type of silicone preparation, it is a first-line product recommended by global medical experts for scar treatment. It is composed of an anti-adhesive film, a silicone gel layer and a release film. After the scar patch is attached to the skin, it can form a local closed environment to reduce the water loss of the skin in the scar area, inhibit the excessive proliferation of fibroblasts, and assist and improve scars through hydration, tension-reducing effect and pressure effect, making the scars soften, flatten and fade.

[0004] The existing scar patch production processes are mainly divided into two types: continuous method and intermittent method. The continuous method production process generally uses automated silicone coating equipment for production, with high production efficiency, low labor costs, and stable product quality. The disadvantage is that the equipment investment is large, often tens to millions. Compared with high-value, durable medical products such as scar patches, the equipment has excess capacity, which may lead to a high equipment idle rate, a large input-output ratio, and poor economic benefits. The intermittent method production process generally uses a specific plate-and-frame mold, pours a fluid rubber into the mold, and then places the whole in a heating device for high-temperature curing and molding. The equipment investment is small and the production is flexible, but the production efficiency is low, the labor cost is high, and it is difficult to ensure stable product quality.

[0005] Moreover, no matter the continuous method or the intermittent method, the scar patch produced has the problem of insufficient viscosity (peel strength is about 0.2N / cm), and it is easy to fall off without the help of auxiliary fixation. Especially when used on bent or moving parts of the body, the probability of falling off is higher, resulting in a short duration of action of the scar patch and a greatly reduced treatment effect. Summary of the invention

[0006] 1. Technical issues to be solved

[0007] In view of the shortcomings of the prior art, the present invention provides a method for producing a high-viscosity scar patch, which solves the problem of insufficient viscosity of the scar patch.

[0008] (II) Technical solution

[0009] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0010] A method for producing a high-viscosity scar patch, the method comprising the following steps:

[0011] S1. Preheating:

[0012] Turn on the heating button of the movable heating and drying device and set a certain temperature to preheat the heating cavity;

[0013] S2. Install the mold:

[0014] The anti-sticking film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the center of the upper surface of the anti-sticking film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0015] S3. Casting materials:

[0016] Pour the prepared silicone gel mixture into the plate-frame mold and let it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0017] S4. Heating materials:

[0018] After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally above the mold so that the heating area completely covers the plate-frame mold, and the material is allowed to stay in this area for a period of time;

[0019] S5, Laminating, Cutting and Packaging:

[0020] After the silicone gel in the mold is cured and formed, the movable heating and drying equipment is moved horizontally to the next station, and another plate of silicone gel mixture is heated and cured according to the same residence time. During this period, the cured material is transferred to a horizontal table, and then the silicone gel surface is covered and attached with a protective film. Finally, the semi-finished scar patch is taken out of the plate frame mold for cutting and packaging;

[0021] S6. Repeated continuous production:

[0022] Perform reciprocating cycle operation according to steps S2 to S5 to achieve continuous production of scar patch;

[0023] In S3, the preparation process of the silicone gel mixture is as follows:

[0024] T1. Weigh 70-75 parts of end-side vinyl silicone oil, 13-15 parts of end-side hydrogen-containing silicone oil, 11-17 parts of end-side hydrogen-containing silicone oil, and 0.3-0.5 parts of Karstedt platinum catalyst in order by mass and add them into a glass beaker;

[0025] Wherein, the vinyl content of the end-side vinyl silicone oil is 7-9% (wt%), and the viscosity is 300-500mPa·s; the hydrogen content of the end-side hydrogen-containing silicone oil is 0.78-0.82% (wt%), and the viscosity is 30-40mPa·s; the hydrogen content of the end-side hydrogen-containing silicone oil is 0.17-0.19% (wt%), and the viscosity is 8-12mPa·s; the Pt content in the Karstedt platinum catalyst is 3000ppm;

[0026] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 1000-2000RPM, and the stirring time is 5-10min;

[0027] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0028] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0029] Preferably, in S1, the set temperature is 110-130°C.

[0030] Preferably, in S2, the low-viscosity silicone oil is dimethyl silicone oil with a viscosity of 50 to 200 mPa·s.

[0031] Preferably, the anti-sticking bottom film is a silicone mesh film with PET as the substrate and PE as the protective film.

[0032] Preferably, the base plate is made of tempered glass.

[0033] Preferably, the pressing frame is made of silicone rubber.

[0034] Preferably, the fixed horizontal platform is formed by splicing a plurality of tempered glass plates and constructing them with a support frame, and each tempered glass plate is independently leveled using a Z-axis micrometer.

[0035] (III) Beneficial effects

[0036] The present invention provides a method for producing a high-viscosity scar patch. Compared with the prior art, the present invention has the following beneficial effects:

[0037] The present invention optimizes the product formula, so that the peeling strength of the scar patch is enhanced by more than two times, the viscosity is greatly improved, the risk of the scar patch falling off during use is reduced, the continuous action time on the scar is increased, and the scar treatment effect is excellent. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 The flowchart of the production method of the high-viscosity scar patch in the embodiment of the present invention is shown in FIG. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The embodiment of the present application solves the problem of insufficient adhesion of scar patches by providing a production method of a high-adhesion scar patch.

[0042] The technical solution in the embodiment of the present application is to solve the above technical problems, and the overall idea is as follows:

[0043] Through product formula optimization, the peel strength of the scar patch has been increased by more than two times, which greatly improves the stickiness, reduces the risk of the scar patch falling off during use, increases the duration of the effect on the scar, and makes the scar treatment effect excellent.

[0044] In addition, the method adopts low-cost movable heating and drying equipment, cooperates with plate-frame molds and high-precision fixed horizontal platforms to achieve continuous production of scar patches. During the production process, the curing and molding process parameters of the scar patch raw materials are simple, stable and reliable, which greatly simplifies the production process and improves production efficiency.

[0045] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0046] Example:

[0047] like Figure 1 As shown, the present invention provides a method for producing a high-viscosity scar patch, the method comprising the following steps:

[0048] S1. Preheating:

[0049] Turn on the heating button of the movable heating and drying device and set a certain temperature to preheat the heating cavity;

[0050] S2. Install the mold:

[0051] The anti-sticking film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the center of the upper surface of the anti-sticking film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0052] S3. Casting materials:

[0053] Pour the prepared silicone gel mixture into the plate-frame mold and let it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0054] S4. Heating materials:

[0055] After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally above the mold so that the heating area completely covers the plate-frame mold, and the material is allowed to stay in this area for a period of time;

[0056] S5, Laminating, Cutting and Packaging:

[0057] After the silicone gel in the mold is cured and formed, the movable heating and drying equipment is moved horizontally to the next station, and another plate of silicone gel mixture is heated and cured according to the same residence time. During this period, the cured material is transferred to a horizontal table, and then the silicone gel surface is covered and attached with a protective film. Finally, the semi-finished scar patch is taken out of the plate frame mold for cutting and packaging;

[0058] S6. Repeated continuous production:

[0059] The steps S2 to S5 are repeated in a reciprocating cycle to achieve continuous production of scar patches.

[0060] In S3, the preparation process of the silicone gel mixture is as follows:

[0061] T1. Weigh 70-75 parts of end-side vinyl silicone oil, 13-15 parts of end-side hydrogen-containing silicone oil, 11-17 parts of end-side hydrogen-containing silicone oil, and 0.3-0.5 parts of Karstedt platinum catalyst in order by mass and add them into a glass beaker;

[0062] Wherein, the vinyl content of the end-side vinyl silicone oil is 7-9% (wt%), and the viscosity is 300-500mPa·s; the hydrogen content of the end-side hydrogen-containing silicone oil is 0.78-0.82% (wt%), and the viscosity is 30-40mPa·s; the hydrogen content of the end-side hydrogen-containing silicone oil is 0.17-0.19% (wt%), and the viscosity is 8-12mPa·s; the Pt content in the Karstedt platinum catalyst is 3000ppm;

[0063] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 1000-2000RPM, and the stirring time is 5-10min;

[0064] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0065] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0066] In S1, the set temperature is 110-130°C.

[0067] In S2, the low-viscosity silicone oil is dimethyl silicone oil with a viscosity of 50 to 200 mPa·s, and its function is to adsorb the anti-sticking base film flatly on the base plate to prevent the base film from deforming, bending, and bulging during heating, thereby resulting in poor thickness uniformity of the finished product.

[0068] The anti-sticking bottom film is a silicone mesh film with PET as a substrate and PE as a protective film.

[0069] The bottom plate is made of tempered glass and has high levelness.

[0070] The pressing frame is made of silicone rubber, which is resistant to high temperatures and has good flexibility, and can be closely attached to the surface of the anti-sticking base film, thereby preventing the silicone gel mixture from seeping out of the mold during the self-leveling process.

[0071] The fixed horizontal platform is formed by splicing a plurality of tempered glass plates and building them with a support frame. Each tempered glass plate is independently leveled using a Z-axis micrometer to ensure an extremely high levelness of the horizontal platform.

[0072] Embodiment 1:

[0073] The present invention provides a method for producing a high-viscosity scar patch, the method comprising the following steps:

[0074] S1. Turn on the heating button of the movable heating and drying device and set the temperature to 110°C to preheat the heating cavity;

[0075] S2, the anti-sticking bottom film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the central position of the upper surface of the anti-sticking bottom film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0076] S3, pouring the prepared silicone gel mixture into the plate frame mold, and letting it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0077] S4. After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally above the mold so that the heating area completely covers the plate-frame mold, and the material is allowed to stay in this area for 20 minutes;

[0078] S5. After the silicone gel in the mold is cured and formed, transfer the cured material to a horizontal table, then cover and adhere the silicone gel surface with a protective film, and finally take the semi-finished scar patch out of the plate frame mold for cutting and packaging.

[0079] In S3, the preparation process of the silicone gel mixture is as follows:

[0080] T1, weigh 154g of end-side vinyl silicone oil, 28.6g of end-side hydrogen silicone oil, 36.3g of end-side hydrogen silicone oil, and 1.1g of Karstedt platinum catalyst and add them into a glass beaker;

[0081] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 1000RPM, and the stirring time is 10min;

[0082] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0083] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0084] Embodiment 2:

[0085] S1. Turn on the heating button of the movable heating and drying device and set the temperature to 115°C to preheat the heating chamber;

[0086] S2, the anti-sticking bottom film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the central position of the upper surface of the anti-sticking bottom film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0087] S3, pouring the prepared silicone gel mixture into the plate frame mold, and letting it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0088] S4. After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally above the mold so that the heating area completely covers the plate-frame mold, and the material is allowed to stay in this area for 20 minutes;

[0089] S5. After the silicone gel in the mold is cured and formed, transfer the cured material to a horizontal table, then cover and adhere the silicone gel surface with a protective film, and finally take the semi-finished scar patch out of the plate frame mold for cutting and packaging.

[0090] In S3, the preparation process of the silicone gel mixture is as follows:

[0091] T1, weigh 156.2g of end-side vinyl silicone oil, 29.3g of end-side hydrogen silicone oil, 33.4g of end-side hydrogen silicone oil, and 1.1g of Karstedt platinum catalyst and add them into a glass beaker;

[0092] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 1500RPM, and the stirring time is 10min;

[0093] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0094] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0095] Embodiment 3:

[0096] S1. Turn on the heating button of the movable heating and drying device and set the temperature to 120°C to preheat the heating cavity;

[0097] S2, the anti-sticking bottom film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the central position of the upper surface of the anti-sticking bottom film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0098] S3, pouring the prepared silicone gel mixture into the plate frame mold, and letting it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0099] S4. After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally above the mold so that the heating area completely covers the plate-frame mold, and the material is allowed to stay in this area for 15 minutes;

[0100] S5. After the silicone gel in the mold is cured and formed, transfer the cured material to a horizontal table, then cover and adhere the silicone gel surface with a protective film, and finally take the semi-finished scar patch out of the plate frame mold for cutting and packaging.

[0101] In S3, the preparation process of the silicone gel mixture is as follows:

[0102] T1, weigh 158.4g of end-side vinyl silicone oil, 30.8g of end-side hydrogen silicone oil, 29.9g of end-side hydrogen silicone oil, and 0.88g of Karstedt platinum catalyst and add them into a glass beaker;

[0103] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 1500RPM, and the stirring time is 10min;

[0104] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0105] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0106] Embodiment 4:

[0107] S1. Turn on the heating button of the movable heating and drying device and set the temperature to 125°C to preheat the heating cavity;

[0108] S2, the anti-sticking bottom film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the central position of the upper surface of the anti-sticking bottom film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0109] S3, pouring the prepared silicone gel mixture into the plate frame mold, and letting it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0110] S4. After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally above the mold so that the heating area completely covers the plate-frame mold, and the material is allowed to stay in this area for 15 minutes;

[0111] S5. After the silicone gel in the mold is cured and formed, transfer the cured material to a horizontal table, then cover and adhere the silicone gel surface with a protective film, and finally take the semi-finished scar patch out of the plate frame mold for cutting and packaging.

[0112] In S3, the preparation process of the silicone gel mixture is as follows:

[0113] T1, weigh 161.5g of end-side vinyl silicone oil, 31.5g of end-side hydrogen silicone oil, 26.2g of end-side hydrogen silicone oil, and 0.88g of Karstedt platinum catalyst and add them into a glass beaker;

[0114] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 2000RPM, and the stirring time is 5min;

[0115] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0116] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0117] Embodiment 5:

[0118] S1. Turn on the heating button of the movable heating and drying device and set the temperature to 130°C to preheat the heating cavity;

[0119] S2, the anti-sticking bottom film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the central position of the upper surface of the anti-sticking bottom film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0120] S3, pouring the prepared silicone gel mixture into the plate frame mold, and letting it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0121] S4. After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally to the top of the mold so that the heating area completely covers the plate frame mold, and the material is allowed to stay in this area for 10 minutes;

[0122] S5. After the silicone gel in the mold is cured and formed, transfer the cured material to a horizontal table, then cover and adhere the silicone gel surface with a protective film, and finally take the semi-finished scar patch out of the plate frame mold for cutting and packaging.

[0123] In S3, the preparation process of the silicone gel mixture is as follows:

[0124] T1, weigh 165g of end-side vinyl silicone oil, 32.3g of end-side hydrogen silicone oil, 24.2g of end-side hydrogen silicone oil, and 0.67g of Karstedt platinum catalyst and add them into a glass beaker;

[0125] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 2000RPM, and the stirring time is 5min;

[0126] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0127] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0128] Comparative Example 1:

[0129] S1. Turn on the heating button of the movable heating and drying device and set the temperature to 110°C to preheat the heating cavity;

[0130] S2, the anti-sticking bottom film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the central position of the upper surface of the anti-sticking bottom film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0131] S3, pouring the prepared silicone gel mixture into the plate frame mold, and letting it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0132] S4. After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally above the mold so that the heating area completely covers the plate-frame mold, and the material is allowed to stay in this area for 20 minutes;

[0133] S5. After the silicone gel in the mold is cured and formed, transfer the cured material to a horizontal table, then cover and adhere the silicone gel surface with a protective film, and finally take the semi-finished scar patch out of the plate frame mold for cutting and packaging.

[0134] In S3, the preparation process of the silicone gel mixture is as follows:

[0135] T1. Weigh 154 g vinyl silicone oil, 64.9 g hydrogen silicone oil and 1.1 g platinum complex in turn and add them into a glass beaker;

[0136] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 1000RPM, and the stirring time is 10min;

[0137] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0138] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0139] Comparative Example 2:

[0140] S1. Turn on the heating button of the movable heating and drying device and set the temperature to 115°C to preheat the heating chamber;

[0141] S2, the anti-sticking bottom film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the central position of the upper surface of the anti-sticking bottom film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0142] S3, pouring the prepared silicone gel mixture into the plate frame mold, and letting it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0143] S4. After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally above the mold so that the heating area completely covers the plate-frame mold, and the material is allowed to stay in this area for 20 minutes;

[0144] S5. After the silicone gel in the mold is cured and formed, transfer the cured material to a horizontal table, then cover and adhere the silicone gel surface with a protective film, and finally take the semi-finished scar patch out of the plate frame mold for cutting and packaging.

[0145] In S3, the preparation process of the silicone gel mixture is as follows:

[0146] T1. Weigh 156.2 g of vinyl silicone oil, 62.7 g of hydrogenated silicone oil, and 1.1 g of platinum complex in a glass beaker;

[0147] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 1500RPM, and the stirring time is 10min;

[0148] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0149] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0150] Comparative Example 3:

[0151] S1. Turn on the heating button of the movable heating and drying device and set the temperature to 120°C to preheat the heating cavity;

[0152] S2, the anti-sticking bottom film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the central position of the upper surface of the anti-sticking bottom film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0153] S3, pouring the prepared silicone gel mixture into the plate frame mold, and letting it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0154] S4. After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally above the mold so that the heating area completely covers the plate-frame mold, and the material is allowed to stay in this area for 15 minutes;

[0155] S5. After the silicone gel in the mold is cured and formed, transfer the cured material to a horizontal table, then cover and adhere the silicone gel surface with a protective film, and finally take the semi-finished scar patch out of the plate frame mold for cutting and packaging.

[0156] In S3, the preparation process of the silicone gel mixture is as follows:

[0157] T1. Weigh 158.4 g vinyl silicone oil, 60.7 g hydrogen silicone oil and 0.88 g platinum complex in turn and add them into a glass beaker;

[0158] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 1500RPM, and the stirring time is 10min;

[0159] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0160] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0161] Comparative Example 4:

[0162] S1. Turn on the heating button of the movable heating and drying device and set the temperature to 125°C to preheat the heating cavity;

[0163] S2, the anti-sticking bottom film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the central position of the upper surface of the anti-sticking bottom film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0164] S3, pouring the prepared silicone gel mixture into the plate frame mold, and letting it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0165] S4. After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally above the mold so that the heating area completely covers the plate-frame mold, and the material is allowed to stay in this area for 15 minutes;

[0166] S5. After the silicone gel in the mold is cured and formed, transfer the cured material to a horizontal table, then cover and adhere the silicone gel surface with a protective film, and finally take the semi-finished scar patch out of the plate frame mold for cutting and packaging.

[0167] In S3, the preparation process of the silicone gel mixture is as follows:

[0168] T1. Weigh 161.5 g vinyl silicone oil, 57.7 g hydrogen silicone oil, and 0.88 g platinum complex in turn and add them into a glass beaker;

[0169] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 2000RPM, and the stirring time is 5min;

[0170] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0171] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0172] Comparative Example 5:

[0173] S1. Turn on the heating button of the movable heating and drying device and set the temperature to 130°C to preheat the heating cavity;

[0174] S2, the anti-sticking bottom film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the central position of the upper surface of the anti-sticking bottom film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform;

[0175] S3, pouring the prepared silicone gel mixture into the plate frame mold, and letting it stand to allow the material to fully self-level on the surface of the anti-sticking base film;

[0176] S4. After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally to the top of the mold so that the heating area completely covers the plate frame mold, and the material is allowed to stay in this area for 10 minutes;

[0177] S5. After the silicone gel in the mold is cured and formed, transfer the cured material to a horizontal table, then cover and adhere the silicone gel surface with a protective film, and finally take the semi-finished scar patch out of the plate frame mold for cutting and packaging.

[0178] In S3, the preparation process of the silicone gel mixture is as follows:

[0179] T1. Weigh 165 g vinyl silicone oil, 56.5 g hydrogen silicone oil and 0.67 g platinum complex in turn and add them into a glass beaker;

[0180] T2, then use an electric stirring device to stir the mixture thoroughly, the stirring speed is 2000RPM, and the stirring time is 5min;

[0181] T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa;

[0182] T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

[0183] The products produced in Examples 1 to 5 and Comparative Examples 1 to 5 were tested for thickness, tensile strength, elongation at break and peel strength, and the results are shown in Table 1:

[0184] Table 1

[0185]

[0186] Note: The peel strength test substrate is a clean stainless steel plate with a surface roughness of 0.2-0.4 μm.

[0187] According to the test results in Table 1, by using the same production process, the peel strength of the scar patches produced by the formulas of Examples 1 to 5 is more than twice that of the scar patches produced by the conventional formulas of Comparative Examples 1 to 5, which greatly improves the viscosity, reduces the risk of the scar patches falling off during use, increases the duration of the effect on the scar, and achieves excellent scar treatment effects.

[0188] On the other hand, the method uses low-cost movable heating and drying equipment, in conjunction with a plate-frame mold and a high-precision fixed level to achieve continuous production of scar patches. During the production process, the curing and molding process parameters of the scar patch raw materials are simple, stable, and reliable, which greatly simplifies the production process and improves production efficiency. During the production process, a Z-axis micrometer is used to level and calibrate the fixed horizontal platform to ensure that the platform reaches a very high level, so that the silicone gel can fully self-level in the mold frame before losing its fluidity due to heat, thereby ensuring that the thickness of the finished product is uniform. The fixed horizontal platform can be designed with a suitable length according to the number of stations required. The tabletop passes through the heating cavity of the movable heating and drying equipment. The equipment can heat and cure the silicone gel mixture in the mold of each station on the horizontal platform one by one by translation, thereby achieving continuous production of scar patches and greatly improving production efficiency.

[0189] In summary, compared with the prior art, the present invention has the following beneficial effects:

[0190] 1. In the embodiment of the present invention, the peel strength of the scar patch is enhanced by more than two times through product formula optimization, which greatly improves the viscosity, reduces the risk of the scar patch falling off during use, increases the sustained action time on the scar, and achieves excellent scar treatment effect.

[0191] 2. In the embodiment of the present invention, a low-cost movable heating and drying device is used, which is matched with a plate-frame mold and a high-precision fixed level to realize the continuous production of scar patches. During the production process, the curing and molding process parameters of the scar patch raw materials are simple, stable and reliable, which greatly simplifies the production process and improves production efficiency.

[0192] 3. In the embodiment of the present invention, a Z-axis micrometer is used to level and calibrate the fixed horizontal platform during the production process to ensure that the platform reaches a very high level, so that the silicone gel can fully self-level in the mold frame before losing its fluidity due to heat, thereby ensuring the uniform thickness of the finished product. The fixed horizontal platform can be designed with a suitable length according to the number of required stations. The tabletop passes through the heating cavity of the movable heating and drying equipment. The equipment can heat and cure the silicone gel mixture in the mold of each station on the horizontal platform one by one by translation, thereby realizing the continuous production of scar stickers and greatly improving production efficiency.

[0193] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0194] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for producing a high-viscosity scar patch, characterized in that: The method comprises the following steps: S1. Preheating: Turn on the heating button of the movable heating and drying device and set a certain temperature to preheat the heating cavity; S2. Install the mold: The anti-sticking film is spread flat and attached to the bottom plate with the help of low-viscosity silicone oil, and then the pressing frame is placed flat on the center of the upper surface of the anti-sticking film, and then the whole set of plate-frame molds is placed flat in a specific station on a fixed horizontal platform; S3. Casting materials: Pour the prepared silicone gel mixture into the plate-frame mold and let it stand to allow the material to fully self-level on the surface of the anti-sticking base film; S4. Heating materials: After the actual temperature in the heating chamber reaches the preset temperature, the movable heating and drying equipment is moved horizontally above the mold so that the heating area completely covers the plate-frame mold, and the material is allowed to stay in this area for a period of time; S5, Laminating, Cutting and Packaging: After the silicone gel in the mold is cured and formed, the movable heating and drying equipment is moved horizontally to the next station, and another plate of silicone gel mixture is heated and cured according to the same residence time. During this period, the cured material is transferred to a horizontal table, and then the silicone gel surface is covered and attached with a protective film. Finally, the semi-finished scar patch is taken out of the plate frame mold for cutting and packaging; In S3, the preparation process of the silicone gel mixture is as follows: T1. Weigh 70-75 parts of end-side vinyl silicone oil, 13-15 parts of end-side hydrogen-containing silicone oil, 11-17 parts of end-hydrogen-containing silicone oil, and 0.3-0.5 parts of Karstedt platinum catalyst in order by mass and add them into a glass beaker; The vinyl content of the end-side vinyl silicone oil is 7-9wt%, and the viscosity is 300-500mPa·s; the hydrogen content of the end-side hydrogen-containing silicone oil is 0.78-0.82wt%, and the viscosity is 30-40 mPa·s; the hydrogen content of the end-side hydrogen-containing silicone oil is 0.17-0.19wt%, and the viscosity is 8-12 mPa·s; the Pt content in the Karstedt platinum catalyst is 3000ppm; T2. Then use an electric stirring device to stir the mixture thoroughly at a stirring speed of 1000-2000 RPM for 5-10 minutes; T3. Place the uniformly stirred silicone gel mixture into a vacuum drying oven for degassing, set the temperature to room temperature, and the vacuum degree to -0.1MPa; T4. After all the bubbles in the mixture are removed, turn off the vacuum pump, vent it and take out the material.

2. The method for producing the high-viscosity scar patch according to claim 1, characterized in that: In S1, the set temperature is 110-130°C.

3. The method for producing the high-viscosity scar patch according to claim 1, characterized in that: In S2, the low-viscosity silicone oil is dimethyl silicone oil with a viscosity of 50 to 200 mPa·s.

4. The method for producing the high-viscosity scar patch according to claim 1, characterized in that: The anti-sticking bottom film is a silicone mesh film with PET as a substrate and PE as a protective film.

5. The method for producing the high-viscosity scar patch according to claim 1, characterized in that: The base plate is made of tempered glass.

6. The method for producing the high-viscosity scar patch according to claim 1, characterized in that: The pressing frame is made of silicone rubber.

7. The method for producing the high-viscosity scar patch according to claim 1, characterized in that: The fixed horizontal platform is formed by splicing a plurality of tempered glass plates and building them with a support frame, and each tempered glass plate is independently leveled using a Z-axis micrometer.

Citation Information

Patent Citations

  • Silica gel scar treatment strip and preparation method thereof

    CN105287441A

  • Medical silica gel scar treatment strip with package and production technology thereof

    CN106361765A

  • Organosilicon release agent with ultra-light release force and preparation method thereof

    CN110819261A

  • Polysiloxane prepolymer, demolding agent containing polysiloxane prepolymer, and preparation method of demolding agent

    CN111303432A

  • Self-adhesive silicone gel composition

    CN111732930A