Silicon oxide-based negative electrode material and method for producing the same
By heating lithium silicate under the coexistence of Si elemental substances to produce uniform SiO and Li gas, the problem of uneven distribution of Li concentration in the silicon oxide-based negative electrode material is solved, and the battery performance is improved and the stability is improved.
Patent Information
- Application Number
- CN202110646277.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-10-19
- Filing Date
- 2017-09-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2037-09-28
AI Technical Summary
Uneven distribution of Li concentration in existing silicon oxide-based negative electrode materials leads to a decrease in battery performance. Especially during the Li doping process, the problem of degradation of battery performance due to uneven doping of Li is difficult to effectively solve.
By heating lithium silicate under the condition of coexistence of Si elemental substances, uniformly mixed SiO gas and Li gas are generated, and cooled and recovered on the same surface to produce uniformly mixed SiO and Li precipitates, and after pulverization, uniform Li is obtained The concentration distribution of silica powder ensures that the Li concentration distribution inside and between the powder particles is evenly distributed.
Effectively avoid the degradation of battery performance due to uneven distribution of Li concentration, improve the initial efficiency and performance stability of the battery, ensure the uniform distribution of Li concentration in powder particles, reduce the generation of Li-rich phases, and improve the battery's Reactivity and service life.
Smart Images

Figure CN113394389B_ABST
Abstract
Description
[0001] This application is a divisional application for an invention patent application with an application date of September 28, 2017, application number 201780036498.9, and invention name “Silicon oxide-based negative electrode material and its manufacturing method”. Technical Field
[0002] The present invention relates to a silicon oxide negative electrode material used in forming a negative electrode of a Li ion secondary battery and a method for producing the same, and more particularly to a silicon oxide negative electrode material doped with Li for irreversible capacity elimination and a method for producing the same. Background Art
[0003] Silicon oxide (SiO x ) is a negative electrode material for Li ion secondary batteries with large capacitance and excellent life characteristics. For the silicon oxide-based negative electrode material, a material obtained by mixing silicon oxide powder, a conductive aid and a binder and slurrying is applied to a collector composed of copper foil or the like as a thin film negative electrode. The silicon oxide powder is obtained, for example, by the following method: that is, after cooling and precipitating silicon monoxide gas generated by heating a mixture of silicon dioxide and silicon, finely crushing is performed. It is known that the silicon oxide powder manufactured by this precipitation method contains a large amount of amorphous parts, and the volume change during charge and discharge is reduced to improve the cycle characteristics.
[0004] A typical problem of such silicon oxide-based negative electrode materials is low initial efficiency. This is a phenomenon in which an irreversible capacity Li compound that does not contribute to charge and discharge is generated during the first charge, significantly reducing the first discharge capacity. As a method for eliminating this phenomenon, Li doping, which is adding Li ions to silicon oxide powder, is known.
[0005] For example, Patent Document 1 proposes a solid phase method, that is, heating and sintering a mixture of silicon oxide powder and metal Li powder or a mixture of silicon oxide powder and Li compound powder in an inert atmosphere or under reduced pressure. In addition, Patent Document 2 proposes a gas phase method, that is, mixing SiO gas and Li gas after generating the two gases, cooling them and recovering them. In either method, it is expected that by generating Li compounds as irreversible capacity that do not contribute to charging and discharging in advance, the generation of Li compounds as irreversible capacity during the first charge and discharge can be suppressed and the initial efficiency can be improved. This is the irreversible capacity elimination process.
[0006] However, in silicon oxide-based negative electrode materials that are subjected to irreversible capacity elimination treatment by Li doping, a phenomenon in which battery performance is degraded due to non-uniform Li doping has become a problem.
[0007] That is, in the solid phase method (calcination method) described in Patent Document 1, Li doping is performed by surface reaction of the powder particles, that is, Li ions are doped on the surface of the silicon oxide powder particles during the calcination process, so the Li concentration distribution inside the powder particles is prone to become uneven, and in particular, the Li concentration on the particle surface is prone to become high. In addition, the deviation of the powder composition also becomes a cause of the uneven distribution of Li concentration inside the powder particles, especially the uneven distribution of Li concentration on the particle surface.
[0008] On the other hand, in the gas phase method (precipitation method) described in Patent Document 2, since the uniform mixing of SiO gas and Li gas, the control of temperature and partial pressure are very difficult, it is impossible to avoid the uneven distribution of Li concentration in the mixed gas and even the uneven distribution of Li concentration in the precipitate. In addition, since the precipitate is crushed to become the negative electrode material powder, the uneven Li concentration in the precipitate becomes the cause of the uneven distribution of Li concentration between the powder particles of the negative electrode material powder.
[0009] When the Li concentration distribution is uneven, whether inside the powder particles or between the particles, a highly reactive Li-rich phase such as LiSi alloy is formed in the portion with high Li concentration. Since the Li-rich phase reacts with the binder or solvent during the aforementioned electrode manufacturing process, the Li-rich phase becomes the cause of the deterioration of battery performance.
[0010] Patent Document 1: Japanese Patent No. 4702510
[0011] Patent Document 2: Japanese Patent No. 3852579 Summary of the invention
[0012] An object of the present invention is to provide a silicon oxide-based negative electrode material and a method for producing the same which can avoid as much as possible the degradation of battery performance caused by non-uniform Li concentration distribution.
[0013] As mentioned above, the biggest problem of Li-doped silicon oxide-based negative electrode materials is the uneven distribution of Li concentration in silicon oxide powder. In addition, the uneven distribution of Li concentration in silicon oxide powder also includes uneven distribution of Li concentration in powder particles and uneven distribution of Li concentration between powder particles, as mentioned above.
[0014] The present inventors believed that in order to avoid the degradation of battery performance caused by uneven Li concentration distribution, it is necessary to eliminate two types of uneven Li concentration distribution in silicon oxide powder, namely, uneven Li concentration distribution in powder particles and uneven Li concentration distribution between powder particles, and thus focused on a method for producing Li-doped silicon oxide powder. In particular, the inventors focused on a gas phase method (precipitation method) as described in Patent Document 2.
[0015] In the gas phase method (precipitation method), a mixture of SiO and Li is produced from SiO gas and Li gas. As the simplest method, a method of simply mixing SiO gas generating raw materials and Li gas generating raw materials and heating them can be considered. However, this method does not produce SiO gas and Li gas at the same time. It only preferentially produces Li gas with high vapor pressure. Therefore, it is impossible to obtain a material formed by uniformly mixing SiO and Li.
[0016] As another gas phase method (precipitation method), it is conceivable to generate SiO gas and Li gas simultaneously by heating a composite compound of Li and Si represented by lithium silicate such as Li2Si2O5 under reduced pressure. However, if it is lithium silicate alone, it will not generate gas by heating under reduced pressure. However, such lithium silicate, in the case of the coexistence of Si, especially Si simple substance, generates SiO gas and Li gas simultaneously by heating under reduced pressure, and as a result, the generated gas is a gas formed by uniformly mixing SiO and Li. By cooling the generated gas and causing it to precipitate, a material formed by uniformly mixing SiO and Li is obtained.
[0017] If SiO and Li are uniformly mixed by pulverizing, the Li-containing SiO powder becomes a negative electrode material that eliminates both the uneven distribution of Li concentration between powder particles and the uneven distribution of Li concentration in each powder particle. The reason why SiO gas and Li gas are simultaneously generated from lithium silicate in the presence of Si single substance is presumed to be that lithium silicate is reduced by Si single substance.
[0018] The silicon oxide-based negative electrode material of the present invention is developed based on such a finding, and is characterized in that the silicon oxide-based negative electrode material is SiLi x O y A powder representing an average composition satisfies 0.05<x<y<1.2 and an average particle size of 1 μm or more, and when 10 particles of the powder are randomly selected and the Li concentration L1 at a depth of 50 nm from the outermost surface and the Li concentration L2 at a depth of 400 nm from the outermost surface are measured in each particle, L1 / L2 satisfies 0.8<L1 / L2<1.2 in any particle, and the standard deviation of L2 is less than 0.1.
[0019] In the silicon oxide-based negative electrode material of the present invention, the Li concentration L1 at a depth of 50 nm from the outermost surface of each particle refers to the Li concentration on the particle surface, and the Li concentration L2 at a depth of 400 nm from the outermost surface refers to the Li concentration inside the particle. The condition of 0.8<L1 / L2<1.2 in 10 randomly selected particles means that the Li concentration from the particle surface to the inside is uniform, that is, the uneven distribution of Li concentration in the particles is eliminated. In addition, the standard deviation of L2 between 10 particles is less than 0.1, which means that the uneven distribution of Li concentration between 10 particles is eliminated. Therefore, the degradation of battery performance caused by uneven distribution of Li concentration can be effectively avoided.
[0020] If any one of the 10 randomly selected particles does not satisfy 0.8<L1 / L2<1.2, a Li-rich phase may appear due to uneven distribution of Li concentration in the particles, and a powder with high battery performance may not be obtained due to reduced reactivity. If the standard deviation of L2 is greater than 0.1, a Li-rich phase may appear in the particles due to uneven distribution of Li concentration between particles, and a powder with high battery performance may not be obtained due to reduced reactivity.
[0021] The Li concentrations L1 and L2 can be relatively determined by the ratio of the Li spectrum intensity to the Si spectrum intensity, wherein the ratio of the Li spectrum intensity to the Si spectrum intensity is obtained by performing cross-sectional TEM observation of the powder particles and performing EELS measurement at respective specific depth positions, for example, in a range of 20 nm in length and 400 nm in width.
[0022] For SiLi as the average composition of the powder x O y In general, if x is too small, the effect of Li addition cannot be fully obtained. When x is greater than y, a LiSi alloy is generated, and the reactivity of the powder increases. When y is too large, the charge and discharge capacity of the powder decreases. Therefore, it is set to 0.05<x<y<1.2. The ratio of each element can be measured by ICP emission spectroscopy and infrared absorption method.
[0023] For the average particle size of the powder particles, the Li concentration L2 inside the particles is defined as the Li concentration at a depth of 400 nm from the outermost surface. Therefore, if the average particle size is less than 1 μm, it is possible that L2 cannot represent the Li concentration inside the particles, and the reliability of L1 / L2 decreases, so the average particle size is set to be greater than 1 μm. Although the upper limit of the average particle size is not particularly specified, it is difficult to coat the electrode when the average particle size is large, and it is easy to cause cracks and performance degradation caused by expansion and contraction during charge and discharge, so the average particle size is preferably less than 20 μm.
[0024] The method for producing a silicon oxide-based negative electrode material of the present invention is a method of heating a raw material containing Si, O, and Li to simultaneously generate SiO gas and Li gas from the raw material, and cooling and recovering these gases on the same surface.
[0025] In the method for producing a silicon oxide-based negative electrode material of the present invention, SiO gas and Li gas are simultaneously generated from a raw material, and the simultaneously generated SiO gas and Li gas are cooled and recovered on the same surface, thereby obtaining a precipitate in which SiO and Li are uniformly mixed. If the precipitate is crushed into a powder, a powder can be obtained in which not only the uneven distribution of Li concentration between powder particles but also the uneven distribution of Li concentration in each particle is eliminated.
[0026] The raw material containing Si, O and Li is specifically a raw material containing Si and lithium silicate in which part of Si exists as Si simple substance and Li exists as lithium silicate. When this raw material is used, SiO gas and Li gas are simultaneously generated from the lithium silicate by heating the lithium silicate in the presence of Si simple substance.
[0027] The raw material containing Si and lithium silicate is typically a mixture of Si elemental substance and lithium silicate or a mixture of Si elemental substance, lithium silicate and Si oxide. Si oxide is contained for the purpose of adjusting the amount of O, such as SiO, SiO2, etc. x (0<X≤2). If lithium silicate is represented by a general formula, it is xLi2O·ySiO2, and specific examples include Li2Si2O5 (x=1, y=2), Li2SiO3 (x=1, y=1), Li4SiO4 (x=2, y=1), Li6Si2O7 (x=3, y=2), etc.
[0028] In the raw material containing Si, O and Li, instead of using lithium silicate, a material that generates lithium silicate by heating can also be used. Specifically, the material is a material containing one or two of LiOH and Li2CO3 and Si simple substance, and the material is heated and sintered as a primary raw material. Lithium silicate is generated by heating and sintering LiOH or Li2CO3 in the state where Si simple substance coexists, and the excess elements are removed as gas components, thereby obtaining a raw material containing Si simple substance and lithium silicate, and if the raw material containing Si and lithium silicate is heated as a secondary raw material, SiO gas and Li gas are generated at the same time. In addition, as a primary material, a material containing Li2O and Si simple substance and Si oxide (SiO x; 0<X≤2) or a material using an organic lithium compound instead of Li2CO3, but from the perspective of raw material cost or ease of handling, a material containing one or both of LiOH and Li2CO3 and Si is particularly preferred. Similar to the secondary raw material, i.e., the raw material containing Si and lithium silicate, the primary raw material may also contain Si oxide (SiO x ; 0<X≤2).
[0029] The lithium silicate generation reaction can be carried out before the reaction that simultaneously produces SiO gas and Li gas is about to be carried out. That is, after the primary raw material is heated and fired in the same reaction vessel to become a secondary raw material, the secondary raw material can be heated. In addition, the primary raw material can also be heated and fired in advance to become a secondary raw material. By heating and firing the primary raw material under reduced pressure, it is easier to separate the impurity elements. In the case of heating and firing the primary raw material in advance, in order to prevent oxidation, it is preferably heated and fired in an inert atmosphere under reduced pressure.
[0030] The average composition of the raw material containing Si, O and Li can be expressed as SiLi x O y To represent the average composition, preferably 0.05<x<y<1.2, particularly preferably x is 0.05<x<0.7, and y is 0.9<y<1.1, and the Li, Si and O in the raw material are adjusted so as to have the target element ratio within this range.
[0031] If x is too small, the effect of Li addition cannot be fully obtained. On the other hand, when x is large, the amount of Li gas generated is large, and a highly reactive Li-rich phase may be formed. If the y value is too small or too large, in addition to the possibility of increasing the residual of the raw material, a large amount of Li gas is generated due to the change in the Li composition ratio, and a Li-rich phase may be generated.
[0032] The material (precipitate) recovered by cooling on the same plane is adjusted and crushed into a predetermined particle size to become a powder for negative electrode material. The crushing method is not particularly limited, but it is best to consider that no metal impurities are mixed in. Specifically, it is preferred to use non-metallic materials such as ceramics in the powder contact portion.
[0033] The negative electrode material powder may also be coated with a conductive carbon film on part or all of the surface of the powder particles. By coating with the conductive carbon film, the surface resistance is reduced and the battery characteristics are improved. The conductive carbon film here is obtained, for example, by a thermal CVD reaction using a hydrocarbon gas, but the method is not particularly limited.
[0034] The silicon oxide-based negative electrode material of the present invention can effectively avoid the degradation of battery performance caused by uneven Li concentration distribution by eliminating the two uneven Li concentration distributions in the negative electrode material powder particles and the uneven Li concentration distribution between the powder particles, and has a greater effect on improving battery performance.
[0035] In addition, the method for manufacturing the silicon oxide-based negative electrode material of the present invention can produce negative electrode material powder that eliminates the two uneven distributions of Li concentration in the powder particles and the uneven distribution of Li concentration between the powder particles. Therefore, it can effectively avoid the degradation of battery performance caused by the uneven distribution of Li concentration and has a greater effect on improving battery performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a particle image of the powder of the silicon oxide-based negative electrode material of the present invention observed by cross-sectional TEM. DETAILED DESCRIPTION
[0037] Embodiments of the present invention will be described below. The silicon oxide-based negative electrode material of the present invention is typically produced by the following method.
[0038] First, as a raw material containing Si, O and Li, Si powder and lithium silicate powder such as Li2Si2O5 powder are mixed. If necessary, SiO2 powder is mixed to adjust the amount of O. x O y The mixing ratio of each powder is adjusted so that the element ratio of Li, Si and O (Li:Si:O) satisfies the range of 0.05<x<y<1.2 and reaches a target value (for example, 1:0.4:1).
[0039] Next, by charging the mixed powder as the raw material into a reaction container and heating it under reduced pressure, gas is generated from the mixed raw material, especially from lithium silicate. The gas generation reaction here is a reaction that simultaneously generates SiO gas and Li gas. If explained in terms of chemical formulas, the general formula can be inferred to be formula (1), and in the case where the lithium silicate is Li2Si2O5, it can be inferred to be formula (2). As mentioned above, lithium silicate is represented as xLi2O·ySiO2 in the general formula.
[0040] (x+y)Si+(xLi2O·ySiO2)→(x+2y)SiO↑+2xLi↑ (1)
[0041] 3Si+Li2Si2O5→5SiO↑+2Li↑ (2)
[0042] As can be seen from equations (1) and (2), SiO gas and Li gas are simultaneously generated from lithium silicate by heating in the presence of Si alone. The reaction here is considered to be a reduction reaction based on Si.
[0043] In addition, while the gas is generated from the raw material in the reaction container, the generated gas is cooled and precipitated on the surface of the vapor deposition table arranged at the upper part of the reaction container. After the reaction is completed, the precipitate is recovered from the surface of the vapor deposition table. The recovered precipitate is a Li-containing silicon oxide material, and the Li-containing silicon oxide material is crushed to obtain a powder for a negative electrode material of a predetermined particle size.
[0044] Since SiO gas and Li gas are simultaneously generated from the raw materials in the reaction container, the concentration distribution of the mixed gas of the two is uniform, and the concentration distribution of the precipitate obtained by cooling the mixed gas on the same surface of the vapor deposition stage is also uniform. Therefore, in the powder obtained by pulverizing the precipitate, the Li concentration distribution between the powder particles and the Li concentration distribution in each powder particle are also uniform. When the powder is used as a powder for negative electrode materials, the generation of a Li-rich phase is suppressed, thereby reducing reactivity and improving battery performance.
[0045] As another embodiment, Si powder and LiOH powder are mixed. SiO2 powder is mixed as needed to adjust the amount of O. The mixed powder is loaded into a reaction vessel as a primary raw material, and heated and sintered in an Ar atmosphere. If the reaction when LiOH is heated in the presence of Si single substance is expressed by a chemical formula, it can be inferred to be the first half of formula (3).
[0046] 4Si+4LiOH→3Si+Li4SiO4+2H2↑
[0047] 3Si+Li4SiO4→4SiO↑+4Li↑ (3)
[0048] 4Si+2Li2CO3→3Si+Li4SiO4+2CO↑
[0049] 3Si+Li4SiO4→4SiO↑+4Li↑ (4)
[0050] As can be seen from the first half of formula (3), by heating and firing LiOH in the presence of Si, lithium silicate (Li4SiO4) is generated, and H, an excess element, is removed as a gas component. As a result, the fired product becomes a mixture of lithium silicate (Li4SiO4) and residual Si. This mixture corresponds to the raw material containing Si, O, and Li used in the previous embodiment.
[0051] And, the sintered product is continuously heated under reduced pressure as a secondary raw material. Thus, as shown in the second half of formula (3), lithium silicate (Li4SiO4) is heated in a state where Si single substance coexists in the secondary raw material, thereby simultaneously generating Si gas and Li gas from the lithium silicate (Li4SiO4). The generated gas here is cooled and recovered on the same surface, thereby obtaining a powder for negative electrode material with uniform Li concentration distribution, which is also the same as the case of the previous embodiment. Instead of continuing to heat the secondary raw material, the secondary raw material can also be reheated.
[0052] In this way, by heating and calcining the primary raw material containing Si simple substance and LiOH, a raw material containing Si simple substance and lithium silicate (raw material containing Si and lithium silicate) is obtained, and by heating this raw material as a secondary raw material, SiO gas and Li gas can be generated simultaneously.
[0053] Li2CO3 can also be used instead of LiOH. That is, Si powder and Li2CO3 powder are mixed. SiO2 powder is mixed as needed to adjust the amount of O. The mixed powder is loaded into a reaction container as a primary raw material, and heated and sintered in an Ar atmosphere. If the reaction when Li2CO3 is heated in the presence of Si single substance is expressed by a chemical formula, it can be inferred to be the first half of formula (4).
[0054] As can be seen from the first part of formula (4), by heating and firing Li2CO3 in the presence of Si, lithium silicate (Li4SiO4) is generated, while the excess element C is removed as a gas component. As a result, the fired product becomes a mixture of lithium silicate (Li4SiO4) and residual Si. This mixture corresponds to the raw material containing Si, O and Li used in the previous embodiment.
[0055] Furthermore, if the sintered product is continuously heated under reduced pressure as a secondary raw material, as shown in the second half of formula (4), lithium silicate (Li4SiO4) is heated in the presence of Si single substance in the secondary raw material, and Si gas and Li gas are simultaneously generated from the lithium silicate (Li4SiO4). The generated gas here is cooled and recovered on the same surface, thereby obtaining a powder for negative electrode material with a uniform Li concentration distribution, which is the same as the case of the previous embodiment. Instead of continuing to heat the secondary raw material, the secondary raw material can also be reheated.
[0056] In this way, by heating and calcining the primary raw material containing Si simple substance and Li2CO3, a raw material containing Si simple substance and lithium silicate (raw material containing Si and lithium silicate) can be obtained, and SiO gas and Li gas can be generated simultaneously by heating the raw material as a secondary raw material. Instead of using LiOH or Li2CO3, LiOH and Li2CO3 can also be used.
[0057] In addition, although the chemical reactions in the implementation method are represented by chemical formulas (1) to (4), these chemical reactions are inferred reactions of model cases that simplify the phenomena. In actual reactions, there are cases where SiO2 is added to adjust the amount of O, etc., and it can be expected that it will become a complicated reaction.
[0058] Example
[0059] (Example 1)
[0060] Si powder, SiO2 powder and Li2Si2O5 powder were mixed in a molar ratio of 21:15:2. The element ratio of the mixed powder was Si:Li:O=1:0.1:1. The powder was charged into a reaction vessel as a raw material and heated to 1400°C under reduced pressure. The generated gas was cooled and recovered on a vapor deposition table arranged at the upper part of the reaction vessel. In addition, copper was ground into powder using a ball mill using a zirconia container and balls. The average particle size of the powder was investigated by laser diffraction particle size distribution measurement, and the average particle size of the powder was 5.2μm.
[0061] Ten particles were randomly selected from the obtained powder, and each particle was observed by cross-section TEM. The Si spectrum intensity and the Li spectrum intensity were obtained by performing EELS measurement on a range of 20 nm in length and 400 nm in width at a depth of 50 nm from the outermost surface of the particle, and the ratio of the Li spectrum intensity to the Si spectrum intensity was set as the Li concentration L1 on the particle surface. The ratio of the Li spectrum intensity to the Si spectrum intensity was also obtained by the same method at a depth of 400 nm from the outermost surface of the particle, and the ratio was set as the Li concentration L2 inside the particle. In addition, while obtaining L1 / L2 for 10 particles, the standard deviation of L2 was obtained.
[0062] That is, for particle measurement, particle cross-sections were cut out by FIB processing in an inert atmosphere using FB-2000A (Hitachi), and TEM observation was performed using an atomic resolution energy analysis electron microscope JEM-ARM200F (JEOL), and EELS measurement was performed using a GATANGIF Quantum energy filter. TEM measurement was performed under the conditions of an accelerating voltage of 200 kV, an electron beam diameter of 0.2 nmφ, and an energy resolution of 0.5 eV FWHM.
[0063] In addition, the Li amount (Li / Si) and the O amount (O / Si) of the obtained powder were measured by ICP emission spectrometry and infrared absorption.
[0064] (Example 2)
[0065] Si powder and Li2Si2O5 were mixed at a molar ratio of 3:1. The element ratio of the mixed powder was Si:Li:O=1:0.4:1. A powder having an average particle size of 5.4 μm was prepared in the same manner as in Example 1. The L1 / L2 and standard deviation of L2 of the prepared powder, as well as the amount of Li and the amount of O were determined. A cross-sectional TEM observation image of the powder particles used to measure L1 and L2 of the powder is shown in FIG. Figure 1 .
[0066] (Example 3)
[0067] Si powder and Li2SiO3 were mixed at a molar ratio of 2:1. The element ratio of the mixed powder was Si:Li:O=1:0.67:1. The same method as in Example 1 was used to produce a powder with an average particle size of 5.1 μm. In addition, L1 / L2 and the standard deviation of L2, as well as the amount of Li and the amount of O of the produced powder were determined.
[0068] (Example 4)
[0069] Si powder, SiO2 powder and LiOH powder were mixed in a molar ratio of 4:1:3. The powder was charged into a reaction vessel as a primary raw material and heated to 1400°C and sintered in an Ar atmosphere at atmospheric pressure. A portion of the sintered material was recovered and analyzed, and the result showed that the element ratio was Si:Li:O=1:0.6:1, and it was confirmed that no H component remained.
[0070] Next, the calcined material was used as a secondary raw material, and then heated to 1400°C under reduced pressure in the reaction container, and the generated gas was cooled on the vapor deposition stage arranged at the upper part of the reaction container and recovered. In addition, after the recovered material (precipitate) was powdered in the same manner as in Example 1, the L1 / L2 and L2 standard deviations of the powder, as well as the Li content and the O content were determined. The average particle size of the obtained powder was 5.6 μm.
[0071] (Comparative Example 1)
[0072] Si powder and SiO2 powder were mixed at a molar ratio of 1:1. The element ratio in the mixed powder was Si:Li:O=1:0:1. A powder having an average particle size of 5.1 μm was prepared in the same manner as in Example 1 except that. Since the prepared powder did not contain Li, only the amount of O was measured.
[0073] (Comparative Example 2)
[0074] After adding lithium hydride (LiH) powder to the SiO powder prepared in Comparative Example 1 so that the Li content was 0.4 mol relative to Si and O, the powder was heated to 850° C. in an Ar atmosphere and sintered to obtain a powder having an average particle size of 5.2 μm. The L1 / L2 and standard deviation of L2 of the obtained powder, as well as the Li content and the O content were determined.
[0075] (Comparative Example 3)
[0076] Two reaction containers are prepared, and a mixture of Si powder and SiO2 powder mixed in a molar ratio of 1:1 is placed in one container. The element ratio of the mixed powder is Si:Li:O=1:0:1. In addition, metallic Li is placed in another container under an inert atmosphere. In addition, the weight ratio of the raw materials and the heating temperature in the two containers are adjusted in such a way that the partial pressure of SiO gas generated in one container and Li gas generated in the other container becomes 1:0.4, and the gases generated in the two containers are mixed and cooled and recovered on a common evaporation table.
[0077] Then, the recovered material (precipitate) was powdered in the same manner as in Example 1, and L1 / L2 and the standard deviation of L2 of the powder were determined, as well as the amount of Li and the amount of O. The average particle size of the obtained powder was 5.2 μm.
[0078] (Battery Evaluation)
[0079] Battery evaluation was performed on the powder samples prepared in Examples 1 to 4 and Comparative Examples 1 to 3 in the following procedure.
[0080] The powder sample, PI binder as a non-aqueous (organic) binder, and KB as a conductive additive were mixed in a weight ratio of 80:15:5, and kneaded with organic NMP as a solvent to form a slurry. The prepared slurry was applied to a copper foil and subjected to vacuum heat treatment at 350°C for 30 minutes to form a negative electrode. A button battery was made by combining the negative electrode, the positive electrode (Li foil), an electrolyte (EC:DEC=1:1), an electrolyte (LiPF6 1 mol / L), and a separator (polyethylene porous film 30 μm thick).
[0081] The button battery was subjected to a charge and discharge test. For charging, the battery was charged at a constant current of 0.1C until the voltage between the two electrodes reached 0.005V, and after the voltage reached 0.005V, the battery was charged at a constant voltage until the current reached 0.01C. For discharging, the battery was discharged at a constant current of 0.1C until the voltage between the two electrodes reached 1.5V.
[0082] The initial charge capacity and initial discharge capacity were measured by the charge and discharge test to determine the initial efficiency. The results are shown in Table 1 together with the main specifications of the powder sample (Li content, O content, L1 / L2, and L2 standard deviation).
[0083] [Table 1]
[0084]
[0085] In Comparative Example 1, SiO powder was not doped with Li. In any of Examples 1 to 4, the initial efficiency was improved compared with Comparative Example 1, and the performance improvement effect brought about by Li doping was confirmed. Incidentally, L1 / L2, which is the ratio of the Li concentration inside the particle to the Li concentration on the particle surface, fell within the range of 0.8<L1<L2<1.2 in any example, and the L2 standard deviation also fell below 0.1.
[0086] On the other hand, in Comparative Example 2, Li doping was performed by the solid phase method (calcination method) shown in Patent Document 1. As a tendency unique to this method, Li is relatively dense and unevenly present on the particle surface, and L1 / L2, which is the ratio of the Li concentration inside the particle to the Li concentration on the particle surface, is greater than 1.2 and has a large deviation, so the performance of the binder is deteriorated, and the initial efficiency is also reduced compared with Comparative Example 1.
[0087] On the other hand, in Comparative Example 3, Li doping was performed by the gas phase method (precipitation method) shown in Patent Document 2. Since a mixed gas of SiO gas and Li gas was used, although the difference in Li concentration between the particle surface and the inside of the particle was small, the deviation in Li concentration between the particles was large, resulting in a lower initial efficiency than that of Comparative Example 2. It is believed that this is because particles with a high concentration of Li were generated and the particles reacted with the binder.
[0088] By the way, except for Comparative Example 1 in which Li doping was not performed, the amount of Li (x = Li / Si) and the amount of O (y = O / Si) in the powder all satisfied the range of 0.05 < x < y < 1.2 of the present invention. It can also be seen that L1 / L2 and the standard deviation of L2 are effective performance indicators of the negative electrode material powder.
Claims
1. A method for producing a silicon oxide-based negative electrode material, comprising heating a raw material containing Si, O and Li, generating SiO gas and Li gas from the raw material simultaneously, cooling and recovering the gases on the same surface, Part of Si contained in the raw material exists as Si simple substance, and Li exists as lithium silicate.
2. The method for producing a silicon oxide-based negative electrode material according to claim 1, wherein: The raw material is a mixture of Si element and lithium silicate, or the raw material is a mixture of Si element, lithium silicate and Si oxide.
3. The method for producing a silicon oxide-based negative electrode material according to claim 2, wherein: A primary raw material containing one or both of LiOH and Li2CO3 and Si simple substance is heated and calcined to become a secondary raw material, and the secondary raw material is heated as the raw material.
4. The method for producing a silicon oxide-based negative electrode material according to any one of claims 1 to 3, wherein: With SiLi x O y represents the average composition of the raw materials, and satisfies 0.05<x<0.7 and 0.9<y<1.1.