Cylinder liner, engine and cylinder liner processing method
By creating annular grooves in the circumferential direction of the cylinder liner inner bore wall and applying a thermal spray coating, the problems of carbon buildup and wear on the piston head are solved, thereby improving the engine's thermal efficiency and extending its service life.
Patent Information
- Application Number
- CN202110875849.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-07-30
AI Technical Summary
In existing technologies, the high temperature of the engine leads to increased carbon deposits on the piston head and severe wear inside the cylinder liner, affecting the engine's thermal efficiency and service life.
An annular groove is made in the circumferential direction of the inner wall of the cylinder liner, and a thermal spray coating, including an iron-based coating or a friction-reducing and wear-resistant coating, is sprayed into the groove to improve the bonding strength and reduce the coefficient of friction.
It effectively removes carbon deposits from the piston head, reduces friction between the piston rings and cylinder liners, improves engine thermal efficiency, and extends service life.
Smart Images

Figure CN113431695B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of engines, and in particular to a cylinder liner, an engine and a cylinder liner processing method. Background Art
[0002] The cylinder is a pneumatic actuator that converts the pressure energy of compressed air into mechanical energy. It is an important component in the engine. Together with the cylinder head, piston, and piston ring, it constitutes the working space of the engine cylinder, which enables the medium in the cylinder to convert thermal energy into mechanical energy through expansion. It is cooled by cooling water outside. The cylinder liner is installed in the cylinder body and is fixed by the cylinder head. The piston reciprocates in its inner hole. As the engine's specific power and explosion pressure increase, the high temperature inside the engine causes the carbon deposits on the piston head to gradually increase. At the same time, the wear inside the cylinder liner also gradually increases, which greatly affects the thermal efficiency of the engine and shortens the service life of the engine.
[0003] Therefore, how to effectively improve the thermal efficiency of the engine and extend the service life of the engine is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0004] In view of this, an object of the present invention is to provide a cylinder liner that can effectively improve the thermal efficiency of the engine and extend the service life of the engine.
[0005] Another object of the present invention is to provide an engine.
[0006] Another object of the present invention is to provide a cylinder liner processing method.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A cylinder liner comprises a cylinder liner body. At least one annular groove is provided along the circumference of the inner hole wall of the cylinder liner body. A thermal spray coating is sprayed in the annular groove.
[0009] Preferably, the annular groove is a first annular groove arranged on the inner hole wall of the cylinder liner body, one groove wall of the first annular groove is arranged on the top end surface of the inner hole wall of the cylinder liner body, the other groove wall of the first annular groove is arranged above the top dead center position of the inner hole wall of the cylinder liner body, and is 1mm-3mm away from the top dead center position, the thermal spray coating is sprayed in the first annular groove, and the thickness of the thermal spray coating is greater than the depth of the first annular groove.
[0010] Preferably, the first annular groove is a right-angled trapezoidal groove, and the first annular groove includes a first main body groove and a first transition groove arranged at one end of the first main body groove;
[0011] The groove depth of the first main groove is between 0.1mm and 0.3mm, the groove depth of the first transition groove gradually decreases from one end close to the first main groove to one end far from the first main groove, and the groove width of the first transition groove is between 0.1mm and 1.5mm.
[0012] Preferably, the annular groove is a second annular groove arranged on the inner hole wall of the cylinder liner body, one groove wall of the second annular groove is arranged at the bottom of the carbon scraping ring groove of the inner hole wall of the cylinder liner body, and the other groove wall of the second annular groove is arranged below the top dead center position of the inner hole wall of the cylinder liner body and at a distance of 10mm-40mm from the top dead center position.
[0013] Preferably, the second annular groove is a right-angled trapezoidal groove, and the second annular groove includes a second main body groove and a second transition groove arranged at one end of the second main body groove;
[0014] The groove depth of the second main groove is between 0.1 mm and 0.3 mm, the groove depth of the second transition groove gradually decreases from one end close to the second main groove to one end far from the second main groove, and the groove width of the second transition groove is between 0.1 mm and 1.5 mm;
[0015] The thermal spray coating is sprayed in the second annular groove, and the thickness of the thermal spray coating is 0.05 mm-0.2 mm.
[0016] Preferably, the annular groove is a third annular groove, one groove wall of the third annular groove is arranged on the top end surface of the inner hole wall of the cylinder liner body, and the other groove wall of the third annular groove is arranged below the top dead center position of the inner hole wall of the cylinder liner body and at a distance of 10mm-40mm from the top dead center position.
[0017] Preferably, the third annular groove is a right-angled trapezoidal groove, and the third annular groove includes a third main body groove and a third transition groove arranged at one end of the third main body groove;
[0018] The groove depth of the third main groove is between 0.1 mm and 0.3 mm, the groove depth of the third transition groove gradually decreases from one end close to the third main groove to one end far from the third main groove, and the groove width of the third transition groove is between 0.1 mm and 1.5 mm;
[0019] The thermal spray coating is sprayed in the third annular groove, and the thickness of the thermal spray coating is 0.05 mm-0.2 mm.
[0020] Preferably, the annular groove includes a fourth annular groove and a fifth annular groove, one groove wall of the fourth annular groove is arranged above the top dead center position of the inner hole wall of the cylinder liner body and is 2mm-10mm away from the top dead center position, and the other groove wall of the fourth annular groove is arranged below the top dead center position of the inner hole wall of the cylinder liner body and is 10mm-40mm away from the top dead center position;
[0021] One groove wall of the fifth annular groove is arranged above the bottom dead center position of the inner hole wall of the cylinder liner body, and is 10mm-30mm away from the bottom dead center position, and the other groove wall of the fifth annular groove is arranged below the bottom dead center position of the inner hole wall of the cylinder liner body, and is 2mm-15mm away from the bottom dead center position.
[0022] Preferably, the fourth annular groove and the fifth annular groove are both trapezoidal grooves;
[0023] The fourth annular groove includes a fourth main groove and fourth transition grooves respectively arranged at both ends of the fourth main groove;
[0024] The groove depth of the fourth main groove is between 0.1 mm and 0.3 mm, the groove depth of the fourth transition groove gradually decreases from one end close to the main groove to one end far from the main groove, and the groove width of the fourth transition groove is between 0.1 mm and 1.5 mm;
[0025] The fifth annular groove includes a fifth main groove and fifth transition grooves respectively arranged at two ends of the fifth main groove;
[0026] The groove depth of the fifth main groove is between 0.1 mm and 0.3 mm, the groove depth of the fifth transition groove gradually decreases from one end close to the main groove to one end far from the main groove, and the groove width of the fifth transition groove is between 0.1 mm and 1.5 mm;
[0027] The thermal spray coating is sprayed in the fourth annular groove or the fifth annular groove, and the thickness of the thermal spray coating is 0.05 mm-0.2 mm.
[0028] Preferably, the annular groove is the sixth annular groove, one groove wall of the sixth annular groove is placed above the top dead center position of the inner hole wall of the cylinder liner body, and is 2mm-10mm away from the top dead center position, and the other groove wall of the sixth annular groove is arranged below the bottom dead center position of the inner hole wall of the cylinder liner body, and is 2mm-15mm away from the bottom dead center position.
[0029] Preferably, the sixth annular groove includes a sixth main body groove and sixth transition grooves respectively arranged at both ends of the sixth main body groove;
[0030] The groove depth of the sixth main groove is between 0.1 mm and 0.3 mm, the groove depth of the sixth transition groove gradually decreases from one end close to the main groove to one end far from the main groove, and the groove width of the sixth transition groove is between 0.1 mm and 1.5 mm;
[0031] The sixth annular groove is sprayed with the thermal spray coating, and the thickness of the thermal spray coating is 0.05 mm-0.2 mm.
[0032] Preferably, the thermal spray coating is an iron-based coating or a friction-reducing and wear-resistant coating.
[0033] Preferably, the mass percentage of each component of the iron-based coating is:
[0034] C: 1.2%-1.5%, Mn: 1.3%-1.55%, Cr: 1.2%-1.7%, the rest is Fe;
[0035] The mass percentage of each component of the friction-reducing and wear-resistant coating is:
[0036] C: 0.3%-0.6%, Mn: 0.45%-0.9%, Cr: 12.5%-15%, Al2O3 / ZrO2: 35%, the rest is Fe; or
[0037] C: 1.2%-1.5%, Mn: 1.3%-1.55%, Cr: 1.2%-1.7%, Al2O3 / ZrO2: 35%, the rest is Fe; or
[0038] Mn: ≤0.6%, Cr: 26%-28%, Mo: 3.5%-4.1%, Ni≤0.33%, Al2O3 / ZrO2: 35%, the rest is Fe; or TiO2: 100%.
[0039] Preferably,
[0040] The hardness of the iron-based coating is ≥300HV0.3, the bonding strength of the iron-based coating is ≥30MPa, the porosity of the iron-based coating is ≤5%, and the surface roughness of the iron-based coating is not greater than Rz100μm;
[0041] The hardness of the anti-friction and wear-resistant coating is ≥300HV0.3, the bonding strength of the anti-friction and wear-resistant coating is ≥30MPa, the porosity of the anti-friction and wear-resistant coating is ≤5%, and the surface roughness of the anti-friction and wear-resistant coating is not greater than Rz100μm.
[0042] An engine comprises a cylinder liner, wherein the cylinder liner is any one of the cylinder liner described above.
[0043] A cylinder liner processing method, comprising:
[0044] Step 100: performing rough machining on the inner hole wall of the cylinder liner body;
[0045] Step 200: at least one annular groove is formed along the circumferential direction of the inner hole wall of the cylinder liner body;
[0046] Step 300: performing pre-spraying treatment on the annular groove;
[0047] Step 400: spraying a thermal spray coating in the annular groove.
[0048] Preferably, the step 300 includes:
[0049] S301: using volatile solvent alcohol or acetone to clean the inner hole wall of the cylinder liner body and the annular groove and blow dry;
[0050] S302: performing mechanical roughening and sandblasting treatment on the annular groove to form a roughening and sandblasting area;
[0051] S303: Clean the roughened sandblasted surface of the annular groove to remove impurity particles.
[0052] Preferably, the step 400 includes:
[0053] S401: Melting the thermal spray coating material to be sprayed at high temperature into a molten or semi-molten state;
[0054] S402: using compressed air to blow the thermal spray coating in a molten or semi-molten state toward the surface of the annular groove, wherein the thickness of the thermal spray coating is greater than the groove depth of the annular groove, and the spraying length of the thermal spray coating is greater than the groove width of the annular groove and less than the sandblasting length of the roughening sandblasting area;
[0055] S403: naturally cooling the sprayed cylinder liner body.
[0056] Preferably, when the annular groove is the second annular groove arranged on the inner hole wall of the cylinder liner body, or when the annular groove is the third annular groove arranged on the inner hole wall of the cylinder liner body, or when the annular groove is the fourth annular groove and the fifth annular groove arranged on the inner hole wall of the cylinder liner body, or when the annular groove is the sixth annular groove arranged on the inner hole wall of the cylinder liner body, step 500 is also included: processing the inner hole wall of the cylinder liner body and the thermal spray coating.
[0057] Preferably, the step 500 includes:
[0058] Step S501: performing a rough honing process on the thermal spray coating, honing a portion of the thermal spray coating protruding from the annular groove until it is consistent with the inner hole wall surface of the cylinder liner body;
[0059] Step S502: performing overall rough honing processing on the inner hole wall of the cylinder liner body;
[0060] Step S503: performing fine honing on the inner hole wall of the cylinder liner body.
[0061] It can be seen from the above technical scheme that the cylinder liner disclosed in the embodiment of the present invention includes a cylinder liner body, at least one annular groove is opened along the circumferential direction of the inner hole wall of the cylinder liner body, and a thermal spray coating is sprayed in the annular groove. Compared with the prior art, spraying the thermal spray coating in the annular groove can not only play the effect of scraping the carbon ring, thereby effectively removing the carbon deposits on the piston head and extending the service life of the engine, but also effectively reduce the friction coefficient between the piston ring and the cylinder liner body and the wear amount of the inner hole wall surface of the cylinder liner body. Therefore, the cylinder liner greatly reduces the friction work loss between the piston ring and the cylinder liner, improves the thermal efficiency of the engine, and extends the service life of the engine. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0063] Figure 1 It is a schematic structural diagram of a cylinder liner provided with a first annular groove disclosed in an embodiment of the present invention;
[0064] Figure 2 It is a schematic diagram of a structure in which a thermal spray coating is sprayed in a first annular groove according to an embodiment of the present invention;
[0065] Figure 3 It is a schematic structural diagram of a cylinder liner provided with a second annular groove after spraying disclosed in an embodiment of the present invention;
[0066] Figure 4 A schematic diagram of a structure in which a thermal spray coating is sprayed in a second annular groove according to an embodiment of the present invention;
[0067] Figure 5 It is a schematic structural diagram of a cylinder liner provided with a third annular groove after spraying disclosed in an embodiment of the present invention;
[0068] Figure 6 It is a schematic diagram of a structure in which a thermal spray coating is sprayed in a third annular groove according to an embodiment of the present invention;
[0069] Figure 7 It is a schematic structural diagram of a cylinder liner provided with a fourth annular groove and a fifth annular groove after spraying according to an embodiment of the present invention;
[0070] Figure 8 A schematic diagram of a structure in which a thermal spray coating is sprayed in a fourth annular groove and a fifth annular groove according to an embodiment of the present invention;
[0071] Fig. 9 It is a schematic structural diagram of a cylinder liner provided with a sixth annular groove after spraying according to an embodiment of the present invention;
[0072] Fig.10 It is a schematic diagram of a structure in which a thermal spray coating is sprayed in a sixth annular groove according to an embodiment of the present invention;
[0073] Fig.11 It is a schematic structural diagram of the annular groove before spraying disclosed in an embodiment of the present invention;
[0074] Fig.12 It is a schematic diagram of the ring spraying structure of Examples 1 to 3 disclosed in the embodiments of the present invention;
[0075] Fig.13 This is a schematic diagram of the ring spraying structure of Example 4 and Example 5 disclosed in the embodiments of the present invention.
[0076] The names of the components are as follows:
[0077] 100 is a cylinder liner body, 101 is a first annular groove, 1011 is a first main groove, 1012 is a first transition groove, 102 is a second annular groove, 1021 is a second main groove, 1022 is a second transition groove, 103 is a third annular groove, 1031 is a third main groove, 1032 is a third transition groove, 104 is a fourth annular groove, 1041 is a fourth main groove, 1042 is a fourth transition groove, 105 is a fifth annular groove, 1051 is a fifth main groove, 1052 is a fifth transition groove, 106 is a fifth annular groove, 1061 is a sixth main groove, 1062 is a sixth transition groove, 200 is a thermal spray coating, 300 is a coarse sandblasting area, 301 is a coarse sandblasting main area, 302 is a coarse sandblasting extension area, and α is a transition angle. DETAILED DESCRIPTION
[0078] In view of this, the core of the present invention is to provide a cylinder liner that can effectively improve the thermal efficiency of the engine and extend the service life of the engine.
[0079] Another object of the present invention is to provide an engine.
[0080] Another object of the present invention is to provide a cylinder liner processing method.
[0081] In order to enable those skilled in the art to better understand the solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0082] The cylinder liner disclosed in the embodiment of the present invention comprises a cylinder liner body 100, at least one annular groove is provided along the circumferential direction of the inner hole wall of the cylinder liner body 100, and a thermal spray coating 200 is sprayed in the annular groove. Compared with the prior art, spraying the thermal spray coating 200 in the annular groove can not only play the effect of scraping the carbon ring, thereby effectively removing the carbon deposits on the piston head and extending the service life of the engine, but also effectively reduce the friction coefficient between the piston ring and the cylinder liner body 100 and the wear amount of the inner hole wall surface of the cylinder liner body 100, so the cylinder liner greatly reduces the friction work loss between the piston ring and the cylinder liner, improves the thermal efficiency of the engine, and extends the service life of the engine.
[0083] It should be noted that, multiple annular grooves can be provided, or only one annular groove can be provided, that is, multiple annular grooves can be simultaneously opened at different positions in the cylinder liner body 100, and then the thermal spray coating 200 can be sprayed in the annular groove; or only one annular groove can be provided at any position in the cylinder liner body 100, and then the thermal spray coating 200 can be sprayed in the annular groove.
[0084] The embodiments of the present invention do not limit the specific number and location of the annular grooves. As long as the structure meets the use requirements of the present invention, it is within the protection scope of the present invention, and those skilled in the art can make a selection according to actual needs.
[0085] Please refer to Figure 1 to Figure 2 As a first embodiment, in the cylinder liner disclosed in the embodiment of the present invention, the annular groove is a first annular groove 101 arranged on the inner hole wall of the cylinder liner body 100, wherein one groove wall of the first annular groove 101 is arranged on the top surface of the inner hole wall of the cylinder liner body 100, and the other groove wall of the first annular groove 101 is arranged above the top dead center position of the inner hole wall of the cylinder liner body 100, and is 1mm-3mm away from the top dead center position. A thermal spray coating 200 is sprayed in the first annular groove 101, and the thickness of the thermal spray coating 200 is greater than the depth of the first annular groove 101. Such a setting can effectively achieve the effect of scraping the carbon ring.
[0086] The embodiment of the present invention does not specifically limit the shape of the first annular groove 101, which may be rectangular, trapezoidal, or other shapes. As long as the structure meets the use requirements of the present invention, it is within the protection scope of the present invention.
[0087] In order to further optimize the above embodiment, the first annular groove 101 disclosed in the embodiment of the present invention is a right-angled trapezoidal groove, wherein the first annular groove 101 includes a first main body groove 1011 and a first transition groove 1012 disposed at one end of the first main body groove 1011 .
[0088] It should be noted that the groove depth of the first main groove 1011 is between 0.1mm and 0.3mm, the groove depth of the first transition groove 1012 gradually decreases from one end close to the first main groove 1011 to the end away from the first main groove 1011, and the groove width of the first transition groove 1012 is 0.1mm-1.5mm.
[0089] The thickness of the thermal spray coating 200 of the first annular groove is 0.2 mm-0.6 mm. After spraying, the surface of the thermal spray coating 200 is 0.1 mm-0.3 mm more protruding than the surface of the cylinder liner body 100 .
[0090] As a preferred embodiment, the groove depth of the first transition groove 1012 disclosed in the embodiment of the present invention gradually decreases from one end close to the first main groove 1011 to the end away from the first main groove 1011 until it reaches 0. Such a setting can further improve the bonding strength between the thermal spray coating 200 and the inner hole wall of the engine cylinder liner body 100. Such a setting can effectively remove carbon deposits on the piston head, thereby extending the service life of the engine.
[0091] Please refer to Figure 3 to Figure 4 As a second embodiment, in the cylinder liner disclosed in the embodiment of the present invention, the annular groove is a second annular groove 102 arranged on the inner hole wall of the cylinder liner body 100, one groove wall of the second annular groove 102 is arranged at the bottom of the carbon scraping ring groove of the inner hole wall of the cylinder liner body 100, and the other groove wall of the second annular groove 102 is arranged below the top dead center position of the inner hole wall of the cylinder liner body 100, and at a distance of 10mm-40mm from the top dead center position.
[0092] The embodiment of the present invention does not specifically limit the shape of the second annular groove 102, which may be rectangular, trapezoidal, or other shapes. As long as the structure meets the use requirements of the present invention, it is within the protection scope of the present invention.
[0093] In order to further optimize the above embodiment, the second annular groove 102 disclosed in the embodiment of the present invention is preferably a right-angled trapezoidal groove, and the second annular groove 102 includes a second main body groove 1021 and a second transition groove 1022 disposed at one end of the second main body groove 1021;
[0094] Among them, the groove depth of the second main groove 1021 is between 0.1mm and 0.3mm, the groove depth of the second transition groove 1022 gradually decreases from one end close to the second main groove 1021 to the end away from the second main groove 1021, and the groove width of the second transition groove 1022 is 0.1mm-1.5mm.
[0095] A thermal spray coating 200 is sprayed in the second annular groove 102 , and the thickness of the thermal spray coating 200 is preferably 0.05 mm-0.2 mm.
[0096] It should be noted that, as a preferred embodiment, the groove depth of the second transition groove 1022 disclosed in the embodiment of the present invention gradually decreases from one end close to the second main groove 1021 to the end away from the second main groove 1021 until it reaches 0. Such a setting can further enhance the bonding strength between the thermal spray coating 200 and the inner hole wall of the cylinder liner.
[0097] Please refer to Figures 5 and 6 As a third embodiment, the annular groove disclosed in the embodiment of the present invention is a third annular groove 103, wherein one groove wall of the third annular groove 103 is arranged on the top surface of the inner hole wall of the cylinder liner body 100, and the other groove wall of the third annular groove 103 is arranged below the top dead center position of the inner hole wall of the cylinder liner body 100, and at a distance of 10mm-40mm from the top dead center position.
[0098] The embodiment of the present invention does not specifically limit the shape of the third annular groove 103, which may be rectangular, trapezoidal, or other shapes. As long as the structure meets the use requirements of the present invention, it is within the protection scope of the present invention.
[0099] In order to further optimize the above embodiment, the third annular groove 103 disclosed in the embodiment of the present invention is a right-angled trapezoidal groove, and the third annular groove 103 includes a third main body groove 1031 and a third transition groove 1032 arranged at one end of the third main body groove 1031;
[0100] Among them, the groove depth of the third main groove 1031 is between 0.1mm and 0.3mm, the groove depth of the third transition groove 1032 gradually decreases from one end close to the third main groove 1031 to the end far away from the third main groove 1031, and the groove width of the third transition groove 1032 is 0.1mm-1.5mm.
[0101] The third annular groove 103 is sprayed with a thermal spray coating 200 , and the thickness of the thermal spray coating 200 is preferably 0.05 mm-0.2 mm.
[0102] It should be noted that, as a preferred embodiment, the groove depth of the third transition groove 1032 disclosed in the embodiment of the present invention gradually decreases from the three ends close to the third main groove 1031 to the three ends away from the third main groove 1031 until it reaches 0. Such a setting can further enhance the bonding strength between the thermal spray coating 200 and the inner hole wall of the engine cylinder liner body.
[0103] Please refer to Figures 7 and 8 As a fourth embodiment, the annular groove disclosed in the embodiment of the present invention includes a fourth annular groove 104 and a fifth annular groove 105, wherein one groove wall of the fourth annular groove 104 is arranged above the top dead center position of the inner hole wall of the cylinder liner body 100, and is 2mm-10mm away from the top dead center position, and the other groove wall of the fourth annular groove 104 is arranged below the top dead center position of the inner hole wall of the cylinder liner body 100, and is 10mm-40mm away from the top dead center position;
[0104] One groove wall of the fifth annular groove 105 is arranged above the bottom dead center position of the inner hole wall of the cylinder liner body 100, and is 10mm-30mm away from the bottom dead center position, and the other groove wall of the fifth annular groove 105 is arranged below the bottom dead center position of the inner hole wall of the cylinder liner body 100, and is 2mm-15mm away from the bottom dead center position.
[0105] The embodiment of the present invention does not specifically limit the shapes of the fourth annular groove 104 and the fifth annular groove 105, which may be rectangular, trapezoidal, or other shapes. As long as the structures meet the use requirements of the present invention, they are within the protection scope of the present invention.
[0106] In order to further optimize the above embodiment, the fourth annular groove 104 and the fifth annular groove 105 disclosed in the embodiment of the present invention are both trapezoidal grooves, wherein the fourth annular groove 104 includes a fourth main groove 1041 and fourth transition grooves 1042 respectively arranged at both ends of the fourth main groove 1041;
[0107] It should be noted that the groove depth of the fourth main groove 1041 is between 0.1 mm and 0.3 mm, the groove depth of the fourth transition groove 1042 gradually decreases from one end close to the main groove to the end far from the main groove, and the groove width of the fourth transition groove 1042 is 0.1 mm to 1.5 mm;
[0108] The fifth annular groove 105 includes a fifth main groove 1051 and a fifth transition groove 1052 respectively arranged at both ends of the fifth main groove 1051; the groove depth of the fifth main groove 1051 is between 0.1mm and 0.3mm, the groove depth of the fifth transition groove 1052 gradually decreases from one end close to the main groove to the end away from the main groove, and the groove width of the fifth transition groove 1052 is 0.1mm-1.5mm.
[0109] The fourth annular groove 104 or the fifth annular groove 105 is sprayed with a thermal spray coating 200 , and the thickness of the thermal spray coating 200 is 0.05 mm-0.2 mm.
[0110] Please refer to Figures 9 and 10 As the fifth embodiment, the annular groove disclosed in the embodiment of the present invention is the sixth annular groove 106, one groove wall of the sixth annular groove is placed above the top dead center position of the inner hole wall of the cylinder liner body, and is 2mm-10mm away from the top dead center position, and the other groove wall of the sixth annular groove is arranged below the bottom dead center position of the inner hole wall of the cylinder liner body, and is 2mm-15mm away from the bottom dead center position.
[0111] The embodiment of the present invention does not specifically limit the shape of the sixth annular groove 106, which may be rectangular, trapezoidal, or other shapes. As long as the structure meets the use requirements of the present invention, it is within the protection scope of the present invention.
[0112] In order to further optimize the above embodiment, the sixth annular groove 1061 disclosed in the embodiment of the present invention includes a sixth main groove 1061 and sixth transition grooves 1062 respectively arranged at both ends of the sixth main groove 1061;
[0113] The groove depth of the sixth main groove 1061 is between 0.1mm and 0.3mm, the groove depth of the sixth transition groove 1062 gradually decreases from one end close to the main groove to the end far from the main groove, and the groove width of the sixth transition groove 1062 is between 0.1mm and 1.5mm.
[0114] The sixth annular groove 106 is sprayed with a thermal spray coating 200 , and the thickness of the thermal spray coating 200 is 0.05 mm-0.2 mm.
[0115] It should be noted that in Examples 2 to 5, the thickness of the thermal spray coating is preferably the same as the depth of the annular groove. This arrangement more effectively reduces the friction coefficient between the piston ring and the cylinder liner body and the wear amount of the inner hole wall surface of the cylinder liner body.
[0116] It should be explained that the “above” and “below” disclosed in the embodiments of the present invention both refer to the side away from the ground being the above and the side close to the ground being the below when the engine is in working state.
[0117] It should be noted that the thermal spray coating 200 disclosed in the embodiment of the present invention is an iron-based coating, or a friction-reducing and wear-resistant coating, wherein the friction-reducing and wear-resistant coating may be a ceramic coating, or a coating formed by a mixture of a ceramic coating and an iron-based coating.
[0118] Among them, the embodiments of the present invention do not specifically limit the mass percentage of each component of the iron-based coating and the mass percentage of each component of the friction-reducing and wear-resistant coating. As long as the structure meets the use requirements of the present invention, it is within the protection scope of the present invention.
[0119] The preferred mass percentages of the components of the iron-based coating in the embodiment of the present invention are C: 1.2%-1.5%, Mn: 1.3%-1.55%, Cr: 1.2%-1.7%, and the rest is Fe; the preferred mass percentages of the components of the anti-friction and wear-resistant coating in the embodiment of the present invention are:
[0120] C: 0.3%-0.6%, Mn: 0.45%-0.9%, Cr: 12.5%-15%, Al2O3 / ZrO2: 35%, and the rest is Fe; or C: 1.2%-1.5%, Mn: 1.3%-1.55%, Cr: 1.2%-1.7%, Al2O3 / ZrO2: 35%, and the rest is Fe; Mn: ≤0.6%, Cr: 26%-28%, Mo: 3.5%-4.1%, Ni≤0.33%, Al2O3 / ZrO2: 35%, and the rest is Fe; or TiO2: 100%.
[0121] In order to further optimize the above-mentioned embodiments, the technical indicators of the iron-based coating and the wear-resistant and friction-reducing coating disclosed in the embodiments of the present invention are preferably: the hardness of the iron-based coating ≥300HV0.3, the bonding strength of the iron-based coating ≥30MPa, the porosity of the iron-based coating ≤5%, and the surface roughness of the iron-based coating is not greater than Rz100μm; the hardness of the friction-reducing and wear-resistant coating ≥300HV0.3, the bonding strength of the friction-reducing and wear-resistant coating ≥30MPa, the porosity of the friction-reducing and wear-resistant coating ≤5%, and the surface roughness of the friction-reducing and wear-resistant coating is not greater than Rz100μm.
[0122] An embodiment of the present invention further discloses an engine, including a cylinder liner, wherein the cylinder liner is the cylinder liner disclosed in any one of the above embodiments.
[0123] Since the engine disclosed in the embodiment of the present invention adopts the above-mentioned cylinder liner, the engine disclosed in the embodiment of the present invention has the technical advantages of the above-mentioned cylinder liner, and this application will not elaborate on this.
[0124] The embodiment of the present invention also discloses a cylinder liner processing method, including step 100: rough machining the inner hole wall of the cylinder liner body 100; step 200: opening at least one annular groove along the circumference of the inner hole wall of the cylinder liner body 100; step 300: pre-spraying the annular groove; step 400: spraying a thermal spray coating in the annular groove.
[0125] Compared with the prior art, spraying the thermal spray coating 200 in the annular groove can not only scrape the carbon ring, thereby effectively removing the carbon deposits on the piston head and improving the service life of the engine, but also effectively reduce the friction coefficient between the piston ring and the cylinder liner body 100 and the wear amount of the inner hole wall surface of the cylinder liner body 100. Therefore, the cylinder liner reduces the friction work loss between the piston ring and the cylinder liner, improves the thermal efficiency of the engine, and extends the service life of the engine.
[0126] Among them, in Example 1, during the rough machining process of the inner hole wall of the cylinder liner body 100 , it is necessary to machine the inner and outer circles of the cylinder liner body 100 to the finished size, and then machine an annular groove on the inner hole wall of the cylinder liner body 100 .
[0127] In implementation 2 to embodiment 5, the allowances of the inner and outer circles of the casting blank of the cylinder liner body 100 need to be removed. After the allowances of the inner and outer circles are removed, a 0.5-1.5mm allowance is left after the total length is cut into the finished product, a 0.3-1.5mm allowance is left after the outer circle of the cylinder liner body 100 is roughly machined into the finished product, and a 0.15-0.4mm allowance is left after the inner hole wall of the cylinder liner body 100 is roughly machined into the finished product, and then an annular groove is machined on the inner hole wall of the cylinder liner body 100.
[0128] When processing the annular groove, a circular arc smooth transition is preferably set between the first main groove 1011 and the first transition groove 1012, and the angle of the transition angle α formed between the first main groove 1011 and the first transition groove 1012 is preferably not more than 45 degrees; a circular arc smooth transition is preferably set between the second main groove 1021 and the second transition groove 1022, and the angle of the transition angle α formed between the second main groove 1021 and the second transition groove 1022 is preferably not more than 45 degrees; a circular arc smooth transition is preferably set between the third main groove 1031 and the third transition groove 1032, and the angle of the transition angle α formed between the third main groove 1031 and the third transition groove 1032 is preferably not more than 45 degrees ; A circular arc smooth transition is preferably set between the fourth main groove 1041 and the fourth transition groove 1042, and the angle of the transition angle α formed between the fourth main groove 1041 and the fourth transition groove 1042 is preferably not more than 45 degrees; the angle of the transition angle α formed between the fifth main groove 1051 and the fifth transition groove 1052 is preferably set to a circular arc smooth transition, and the angle of the transition angle α formed between the fifth main groove 1051 and the fifth transition groove 1052 is preferably not more than 45 degrees; an arc smooth transition is preferably set between the sixth main groove 1061 and the sixth transition groove 1062, and the angle of the transition angle α formed between the sixth main groove 1061 and the sixth transition groove 1062 is preferably not more than 45 degrees.
[0129] In the embodiment of the present invention, the present invention does not specifically limit the roughness of the annular groove. As long as the structure meets the use requirements of the present invention, it is within the protection scope of the present invention. The embodiment of the present invention preferably sets the roughness of the annular groove to be less than Ra4.0μm.
[0130] After the inner hole wall and the annular groove of the cylinder liner body 100 are processed, the inner hole wall and the annular groove of the cylinder liner body 100 need to be cleaned to ensure that there is no residue on the inner hole wall and the annular groove surface of the cylinder liner body 100.
[0131] It should be noted that step 300 includes the following three steps: S301: first, the inner hole wall and the annular groove of the cylinder liner body 100 are cleaned and dried with volatile solvent alcohol or acetone; S302: then the annular groove is subjected to mechanical roughening sandblasting to form a roughened sandblasting area 300; S303: finally, the roughened sandblasting surface of the annular groove is cleaned to remove impurity particles.
[0132] It should be noted that the roughening sandblasting area 300 includes a roughening sandblasting main area 301 and a roughening sandblasting extension area 302, wherein the roughening sandblasting main area 301 is placed in the annular groove area, and the roughening sandblasting extension area 302 is placed outside the annular groove, and the length of the roughening sandblasting extension area 302 is preferably less than or equal to 10 mm.
[0133] In step 400, the following three steps are specifically included: S401: melting the thermal spray coating 200 material to be sprayed at high temperature into a molten or semi-molten state; S402: using compressed air to blow the molten or semi-molten thermal spray coating 200 to the surface of the annular groove, wherein the thickness of the thermal spray coating 200 is greater than the groove depth of the annular groove, and the spraying length of the thermal spray coating is greater than the groove width of the annular groove and less than the sandblasting length of the roughening sandblasting area; S403: naturally cooling the cylinder liner body 100 after spraying.
[0134] When spraying the annular groove, the sprayed length of the thermal spray coating 200 is preferably greater than the groove width of the annular groove, but does not exceed the range of the roughened sandblasting extension area 301. The setting of the roughened sandblasting extension area 301 can effectively prevent the coating from falling off during the subsequent honing process.
[0135] When the thermal spray coating 200 in a molten or semi-molten state is cooled and solidified on the surface of the annular groove, the particles are mechanically interlocked with each other in a cake shape to form the thermal spray coating 200 .
[0136] It should be noted that in Examples 1 to 3, at the end of spraying, the end area of the spray coating is a smooth transition without any sharp edges; in Examples 4 and 5, at the start and end of spraying, there are start and end areas of the spray coating, both of which are smooth transitions without any sharp edges.
[0137] The embodiment of the present invention does not specifically limit the thickness of the thermal spray coating 200. As long as the structure meets the use requirements of the present invention, it is within the protection scope of the present invention.
[0138] For the needs of subsequent processing, in the embodiment of the present invention, the thickness of the thermal spray coating 200 is preferably greater than the depth of the annular groove, wherein the thickness of the thermal spray coating 200 is preferably greater than the depth of the annular groove by 0.1 mm-0.4 mm.
[0139] The spraying length of the thermal spray coating 200 disclosed in the embodiment of the present invention is greater than the width of the annular groove, wherein the length of the thermal spray coating 200 is preferably greater than the width of the annular groove by no more than 10 mm. The processing method can effectively prevent the spray coating from falling off.
[0140] In the cylinder liner processing method disclosed in Example 1 of the present invention, the cylinder liner body 100 does not need to be honed after spraying, but the coating radiated by the first transition groove 1012 needs to be cleaned, and a tool retraction avoidance groove needs to be processed under the first transition groove 1012, wherein the depth of the tool retraction avoidance groove is 0.02mm-0.1mm, and the width of the tool retraction avoidance groove is not greater than 1.5mm. After the processing is completed, the surface of the thermal spray coating 200 protrudes 0.1mm-0.3mm more than the surface of the inner wall of the cylinder liner body.
[0141] In the cylinder liner processing method disclosed in Embodiments 2 to 5 of the present invention, when the annular groove is the second annular groove provided on the inner hole wall of the cylinder liner body, or when the annular groove is the third annular groove provided on the inner hole wall of the cylinder liner body, or when the annular groove is the fourth annular groove and the fifth annular groove provided on the inner hole wall of the cylinder liner body, or when the annular groove is the sixth annular groove provided on the inner hole wall of the cylinder liner body, step 500 is also included, in which the inner hole wall and the thermal spray coating of the cylinder liner body 100 are processed, and the specific process flow includes:
[0142] Step S501: performing a rough honing process on the thermal spray coating, honing the portion of the thermal spray coating protruding from the annular groove until it is consistent with the inner hole wall surface of the cylinder liner body; Step S502: performing an overall rough honing process on the inner hole wall of the cylinder liner body; Step S503: performing a fine honing process on the inner hole wall of the cylinder liner body.
[0143] In step S501, the thermal spray coating 200 is roughly honed using a short grinding head, and the portion of the thermal spray coating 200 protruding from the annular groove is honed to be consistent with the inner hole wall surface of the cylinder liner body 100;
[0144] In step S502, a conventional grinding head is used to perform overall rough honing on the inner hole wall of the cylinder liner body 100, so as to remove the honing margin for the subsequent fine honing of the inner hole wall of the cylinder liner body 100 and correct the shape of the inner hole wall of the cylinder liner body 100;
[0145] In step S503, honing parameters are input into a numerically controlled honing device, and the inner hole wall of the cylinder liner body 100 obtained by pre-honing the inner hole wall of the cylinder liner body 100 is finely honed by the numerically controlled honing device, wherein the honing parameters are texture parameters of a smooth texture; specifically, the following steps are included:
[0146] a. Select appropriate honing strips (the selected sand strips are suitable for the surface of the iron-based coating or the wear-resistant and friction-reducing coating and the inner hole wall surface of the cylinder liner body 100, including mesh, flat-top and polishing sand strips, 12 strips each in a pair, 24 strips in total, and the length of the sand strip is 100 mm), and bond the honing strips to the sand strip plate, assemble them into a honing head, and install them to the CNC honing equipment;
[0147] b. Set the processing parameters in the CNC honing equipment, including stroke, rotation speed, reciprocating speed, basic honing pressure, net drawing pressure, flat top, polishing pressure and time;
[0148] c. The CNC honing equipment performs precision honing on the inner hole wall of the cylinder liner according to the set texture parameters, so that the inner hole wall has a qualified mesh texture;
[0149] The honing texture parameters are: Rz≤6.5μm, Rpk≤0.25μm, Rk≤0.5μm, Rvk≤2μm, Mr1≤10%, Mr2≥65%, Ra≤0.65μm, and the texture transition angle is 45°±5°.
[0150] Among them, Rz represents the average peak-to-valley height, Rpk represents the reduction of the peak top, Rk represents the core roughness, Rvk represents the reduction of the valley bottom, Mr1 represents the minimum metal material rate of the roughness center profile, Mr2 represents the maximum metal material rate of the roughness center profile, and Ra represents the surface roughness.
[0151] After the honing of the inner hole wall of the engine is completed, the coating thickness of the finished iron-based coating or wear-resistant and friction-reducing coating is preferably 0.05-0.2 mm, and the coating porosity of the iron-based coating or wear-resistant and friction-reducing coating is preferably 3-20%.
[0152] In the description of the present application, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present application. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0153] Unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0154] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A cylinder liner, characterized in that: It comprises a cylinder liner body, at least one annular groove is provided along the circumference of the inner hole wall of the cylinder liner body, and a thermal spray coating is sprayed in the annular groove; The thermal spray coating is an iron-based coating or a friction-reducing and wear-resistant coating, the hardness of the iron-based coating is ≥300HV0.3, the bonding strength of the iron-based coating is ≥30MPa, the porosity of the iron-based coating is ≤5%, and the surface roughness of the iron-based coating is not greater than Rz100μm; the mass percentages of the components of the iron-based coating are: C: 1.2%-1.5%, Mn: 1.3%-1.55%, Cr: 1.2%-1.7%, and the rest is Fe; The annular groove includes a fourth annular groove and a fifth annular groove; One groove wall of the fourth annular groove is arranged above the top dead center position of the inner hole wall of the cylinder liner body and is 2mm-10mm away from the top dead center position, and the other groove wall of the fourth annular groove is arranged below the top dead center position of the inner hole wall of the cylinder liner body and is 10mm-40mm away from the top dead center position, the fourth annular groove includes a fourth main body groove and fourth transition grooves respectively arranged at both ends of the fourth main body groove, the groove depth of the fourth transition groove gradually decreases from one end close to the main body groove to one end away from the main body groove, and a circular arc smooth transition is arranged between the fourth transition groove and the fourth main body groove, and a transition angle formed between the fourth transition groove and the fourth main body groove is not greater than 45°; One groove wall of the fifth annular groove is arranged above the lower dead center position of the inner hole wall of the cylinder liner body and is 10mm-30mm away from the lower dead center position, and the other groove wall of the fifth annular groove is arranged below the lower dead center position of the inner hole wall of the cylinder liner body and is 2mm-15mm away from the lower dead center position, the fifth annular groove includes a fifth main body groove and a fifth transition groove respectively arranged at both ends of the fifth main body groove, the groove depth of the fifth transition groove gradually decreases from one end close to the main body groove to one end away from the main body groove, and a circular arc smooth transition is arranged between the fifth transition groove and the fifth main body groove, and a transition angle formed between the fifth transition groove and the fifth main body groove is not greater than 45°; The thermal spray coating is sprayed inside the fourth annular groove or the fifth annular groove.
2. The cylinder liner according to claim 1, characterized in that: The fourth annular groove and the fifth annular groove are both trapezoidal grooves; The groove depth of the fourth main groove is between 0.1 mm and 0.3 mm, and the groove width of the fourth transition groove is between 0.1 mm and 1.5 mm; The groove depth of the fifth main body groove is between 0.1mm-0.3mm, and the groove width of the fifth transition groove is 0.1mm-1.5mm; The thickness of the thermal spray coating is 0.05 mm-0.2 mm.
3. The cylinder liner according to claim 1, characterized in that: The mass percentage of each component of the friction-reducing and wear-resistant coating is: C: 0.3%-0.6%, Mn: 0.45%-0.9%, Cr: 12.5%-15%, Al2O3 / ZrO2: 35%, the rest is Fe; or C: 1.2%-1.5%, Mn: 1.3%-1.55%, Cr: 1.2%-1.7%, Al2O3 / ZrO2: 35%, the rest is Fe; or Mn: ≤0.6%, Cr: 26%-28%, Mo: 3.5%-4.1%, Ni≤0.33%, Al2O3 / ZrO2: 35%, the rest is Fe; or TiO2: 100%.
4. The cylinder liner according to claim 1, characterized in that: The hardness of the anti-friction and wear-resistant coating is ≥300HV0.3, the bonding strength of the anti-friction and wear-resistant coating is ≥30MPa, the porosity of the anti-friction and wear-resistant coating is ≤5%, and the surface roughness of the anti-friction and wear-resistant coating is not greater than Rz100μm.
5. An engine, characterized in that: It comprises a cylinder liner, wherein the cylinder liner is the cylinder liner according to any one of claims 1 to 4.
6. A cylinder liner processing method, applied to the cylinder liner according to any one of claims 1 to 4, characterized in that: include: Step 100: performing rough machining on the inner hole wall of the cylinder liner body; Step 200: at least one annular groove is formed along the circumferential direction of the inner hole wall of the cylinder liner body; Step 300: performing pre-spraying treatment on the annular groove; Step 400: spraying a thermal spray coating in the annular groove.
7. The cylinder liner processing method according to claim 6, characterized in that: The step 300 includes: S301: using volatile solvent alcohol or acetone to clean the inner hole wall of the cylinder liner body and the annular groove and blow dry; S302: performing mechanical roughening and sandblasting treatment on the annular groove to form a roughening and sandblasting area; S303: Clean the roughened sandblasted surface of the annular groove to remove impurity particles.
8. The cylinder liner processing method according to claim 7, characterized in that: The step 400 includes: S401: Melting the thermal spray coating material to be sprayed at high temperature into a molten or semi-molten state; S402: using compressed air to blow the thermal spray coating in a molten or semi-molten state toward the surface of the annular groove, wherein the thickness of the thermal spray coating is greater than the groove depth of the annular groove, and the spraying length of the thermal spray coating is greater than the groove width of the annular groove and less than the sandblasting length of the roughening sandblasting area; S403: naturally cooling the sprayed cylinder liner body.
9. The cylinder liner processing method according to claim 8, characterized in that: When the annular groove is a fourth annular groove and a fifth annular groove provided on the inner hole wall of the cylinder liner body, the method further includes step 500: processing the inner hole wall of the cylinder liner body and the thermal spray coating.
10. The cylinder liner processing method according to claim 9, characterized in that: The step 500 includes: Step S501: performing a rough honing process on the thermal spray coating, honing a portion of the thermal spray coating protruding from the annular groove until it is consistent with the inner hole wall surface of the cylinder liner body; Step S502: performing overall rough honing processing on the inner hole wall of the cylinder liner body; Step S503: performing fine honing on the inner hole wall of the cylinder liner body.