Electrolyte manufacturing device and electrolyte manufacturing method
By using mesh anode mesh, cathode mesh and carbon fiber layer in the electrolytic solution, combined with electrolytic reduction of circulating sulfuric acid aqueous solution and vanadium-containing liquid, the problems of high resistance and low energy efficiency of the electrolytic solution manufacturing device are solved, and high-efficiency current is achieved Cycling and low pressure loss method.
Patent Information
- Application Number
- CN202080012097.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-02-05
- Filing Date
- 2020-01-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-01-31
AI Technical Summary
The existing electrolyte manufacturing devices have high unit resistance and low energy efficiency. Due to the large heat generation, large cooling devices are required, resulting in increased equipment costs.
An electrolyte manufacturing device is designed, using a mesh anode net and a cathode net between the anode chamber and the cathode chamber, combined with a carbon fiber layer, and circulating an aqueous sulfuric acid solution containing more than 4 valence vanadium in the anode chamber, And through current reduction, the flow of gas oxygen is controlled to reduce cell resistance and pressure loss.
It achieves the effects of small unit resistance, high current efficiency during reduction, and small electrolyte circulation pressure loss, reducing equipment costs.
Smart Images

Figure CN113474492B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrolyte manufacturing device and an electrolyte manufacturing method. Background Art
[0002] As a large-capacity storage battery, a redox flow battery is known. The redox flow battery is charged and discharged by supplying a positive electrolyte and a negative electrolyte to a battery cell having an ion exchange membrane between a positive electrode and a negative electrode. As the positive electrolyte and the negative electrolyte, a solution containing a metal whose valence changes due to an oxidation-reduction reaction is used. An electrolyte containing vanadium is widely used as a positive electrolyte and a negative electrolyte of a redox flow battery. An electrolyte containing vanadium can be manufactured from ammonium metavanadate (NH4VO3), vanadium pentoxide (V2O5), vanadyl sulfate (VOSO4), etc.
[0003] For example, Patent Document 1 discloses an electrolyte manufacturing device, which uses a sulfuric acid solution containing vanadyl sulfate as a cathode electrolyte and a sulfuric acid solution as an anode electrolyte to manufacture an electrolyte containing trivalent vanadium ions by performing a redox reaction. Specifically, the electrolyte manufacturing device of Patent Document 1 comprises: an ion exchange membrane separating the anode electrolyte and the cathode electrolyte; an anode disposed at a position more than 1 mm away from the ion exchange membrane; and a cathode electrolyte in the vicinity of the cathode during the redox reaction so that the current density reaches 50 mA / cm 2 Above and 600mA / cm 2 The electrolyte production apparatus of Patent Document 1 further comprises: a power supply device for supplying electric current in the following manner: 2 Above 2.5 mL / min·cm 2 A cathode side circulation device for circulating the electrolyte in the following manner; and a flow rate of the anolyte near the anode to reach 0.1 mL / min·cm 2 Above 2.5 mL / min·cm 2 An anode side circulation device circulates the anolyte in the following manner.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 5779292 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] The electrolyte production device of Patent Document 1 has high cell resistance and low energy efficiency. In addition, due to the large amount of heat generated, a large cooling device is required to cool the electrolyte production device, which increases the equipment cost.
[0009] The present invention has been made in view of the above circumstances, and an object thereof is to provide an electrolyte manufacturing device and an electrolyte manufacturing method having low cell resistance, high current efficiency during reduction, and low pressure loss during electrolyte circulation.
[0010] Means for solving problems
[0011] In order to achieve the above-mentioned object, the electrolyte manufacturing device according to the first aspect of the present invention comprises:
[0012] An electrolytic cell comprising: an anode chamber in which an anode is arranged, a cathode chamber in which a cathode is arranged, and a diaphragm separating the anode chamber from the cathode chamber,
[0013] a circulation unit that circulates an aqueous sulfuric acid solution as an anolyte in the anode chamber and circulates an aqueous sulfuric acid solution containing tetravalent or higher vanadium as a catholyte in the cathode chamber, and
[0014] a power supply unit, which is electrically connected to the anode and the cathode and supplies current;
[0015] The cathode has a carbon fiber layer on a surface opposite to the separator;
[0016] The electrolytic unit has a mesh-shaped anode net disposed between the anode and the diaphragm and a mesh-shaped cathode net disposed between the cathode and the diaphragm;
[0017] The circulation unit circulates the anolyte at a flow rate greater than the flow rate of the cathode solution and at a flow rate equal to or greater than twice the volume of gaseous oxygen generated per unit time at 0° C. in the anode chamber.
[0018] A method for producing an electrolyte solution according to a second aspect of the present invention comprises:
[0019] a circulation step of circulating an aqueous sulfuric acid solution as an anode liquid in an anode chamber, and circulating an aqueous sulfuric acid solution containing vanadium with a valence of four or more as a cathode liquid in a cathode chamber, wherein the anode chamber is separated by a diaphragm and is provided with an anode and a mesh anode net disposed between the anode and the diaphragm, and the cathode chamber is separated by the diaphragm and is provided with a cathode having a carbon fiber layer on a surface opposite to the diaphragm and a mesh cathode net disposed between the cathode and the diaphragm,
[0020] a reduction step of supplying current between the anode and the cathode to electrolytically reduce the tetravalent or higher vanadium in the cathode chamber;
[0021] In the circulation step, the anolyte is circulated at a flow rate greater than the flow rate of the cathode solution and at least twice the volume of gaseous oxygen generated per unit time at 0° C. in the anode chamber.
[0022] Effects of the Invention
[0023] According to the present invention, it is possible to provide an electrolyte production device and an electrolyte production method having low cell resistance, high current efficiency during reduction, and low pressure loss during circulation of the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram showing an electrolytic solution production apparatus according to an embodiment of the present invention.
[0025] Figure 2 It is a cross-sectional view showing an electrolytic cell according to an embodiment of the present invention.
[0026] Figure 3 It is a schematic diagram showing the mesh of the anode mesh according to the embodiment of the present invention.
[0027] Figure 4 It is a schematic diagram showing the mesh of the cathode mesh according to the embodiment of the present invention.
[0028] Figure 5 This is a flowchart showing a method for producing an electrolytic solution according to an embodiment of the present invention.
[0029] Figure 6 It is a graph showing the measurement results of Examples and Comparative Examples. DETAILED DESCRIPTION
[0030] Reference Figure 1 to Figure 4 An electrolytic solution production apparatus 10 according to an embodiment of the present invention will be described.
[0031] In the electrolyte manufacturing device 10, an aqueous sulfuric acid solution as an anolyte is circulated in the anode chamber 105a, and an aqueous sulfuric acid solution containing tetravalent or higher vanadium as a cathode chamber 105c is circulated. The electrolyte manufacturing device 10 manufactures an electrolyte containing trivalent vanadium by electrolytically reducing tetravalent or higher vanadium. In the present embodiment, the concentration of tetravalent or higher vanadium in the aqueous sulfuric acid solution containing tetravalent or higher vanadium is, for example, greater than 1.0 mol / L and less than 3.0 mol / L. In addition, the aqueous sulfuric acid solution as the anolyte preferably has an osmole concentration greater than the osmole concentration (osmol) of the cathode solution. In this specification, pentavalent vanadium means a vanadium compound ion (for example, metavanadate ion (VO3 - ), peroxyvanadium ion (VO2 +)) or vanadium ion. The tetravalent vanadium means a vanadium compound ion having a valence of tetravalent vanadium (e.g., vanadyl ion (VO 2+ )) or vanadium ion. Trivalent vanadium means a vanadium compound ion or vanadium ion having a valence of three.
[0032] like Figure 1 As shown, the electrolyte manufacturing device 10 includes: an electrolytic unit 100 having an anode chamber 105a and a cathode chamber 105c separated by a diaphragm 110; and a circulation unit 300 having an anode liquid circulation unit 300a for circulating an anode liquid in the anode chamber 105a and a cathode liquid circulation unit 300c for circulating a cathode liquid in the cathode chamber 105c. In addition, the electrolyte manufacturing device 10 includes a power supply unit 500 for supplying current for causing a reduction reaction in the cathode chamber 105c. The electrolyte manufacturing device 10 further includes an anode liquid storage tank 610a for storing an anode liquid and a cathode liquid storage tank 610c for storing a cathode liquid.
[0033] In addition, the electrolytic cell 100 has an anode 145a disposed in the anode chamber 105a and a cathode 145c disposed in the cathode chamber 105c and having a carbon fiber layer 148c on the surface opposite to the diaphragm 110. The electrolytic cell 100 further has an anode mesh 154a disposed between the anode 145a and the diaphragm 110 and a cathode mesh 154c disposed between the cathode 145c and the diaphragm 110.
[0034] The anolyte circulation section 300a of the circulation section 300 has an anode pump 310a for circulating the anolyte between the anode chamber 105a and the anolyte storage tank 610a, an anode liquid supply pipe 312a for supplying the anolyte to the anode chamber 105a, and an anode liquid recovery pipe 314a for recovering the anolyte from the anode chamber 105a. The cathode liquid circulation section 300c of the circulation section 300 has a cathode pump 310c for circulating the cathode liquid between the cathode chamber 105c and the cathode liquid storage tank 610c, a cathode liquid supply pipe 312c for supplying the cathode liquid to the cathode chamber 105c, and a cathode liquid recovery pipe 314c for recovering the cathode liquid from the cathode chamber 105c.
[0035] First, the specific structure of the electrolysis unit 100 is described. Figure 2 As shown, the electrolytic cell 100 is composed of an anode frame 120a, an anode portion 140a having an anode 145a, an anode mesh portion 150a having an anode mesh 154a, a diaphragm 110, a cathode mesh portion 150c having a cathode mesh 154c, a cathode portion 140c having a cathode 145c, and a cathode frame 120c stacked in this order. Figure 2 In the description, the upward direction on the paper is referred to as upward, and the downward direction on the paper is referred to as downward.
[0036] The anode frame 120a of the electrolytic cell 100 forms the outer shape of the electrolytic cell 100. The anode frame 120a and the cathode frame 120c hold the anode part 140a, the anode mesh part 150a, the diaphragm 110, the cathode mesh part 150c and the cathode part 140c. The anode frame 120a can be formed into a flat plate shape by synthetic resin (such as polyvinyl chloride).
[0037] The anode frame 120a is provided with a flow path (not shown) at the end below, and the flow path has an inlet 122a and a plurality of outlets (not shown) connected to the anolyte supply pipe 312a of the anolyte circulation unit 300a. In addition, the anode frame 120a is provided with a flow path (not shown) at the end above, and the flow path has an outlet 124a and a plurality of inlets (not shown) connected to the anolyte recovery pipe 314a of the anolyte circulation unit 300a. The flow path below the anode frame 120a is connected to a plurality of through holes (not shown) below the anode part 140a, forming a manifold for supplying anolyte to the anode chamber 105a. The flow path above the anode frame 120a is connected to a plurality of through holes (not shown) above the anode part 140a, forming a manifold for recovering anolyte from the anode chamber 105a.
[0038] The anode portion 140a of the electrolytic unit 100 has an anode substrate 142a and an anode 145a. The anode substrate 142a is formed into a plate shape having a recess 143a by, for example, thermoplastic elastomer, synthetic rubber, polyvinyl chloride, etc. In the present embodiment, the anode substrate 142a, the frame 152a of the anode mesh portion 150a and the diaphragm 110 form the anode chamber 105a. The anode 145a is embedded in the recess 143a of the anode portion 140a. The anode 145a is, for example, a platinum-coated electrode formed by forming a plate shape with titanium (Ti) and coated with platinum (Pt). The anode 145a is embedded in the recess 143a of the anode substrate 142a and forms the same plane. The anode 145a is electrically connected to the power supply unit 500. In the anode 145a, electrons enter the anode 145a from the ions contained in the anolyte (aqueous sulfuric acid solution) to generate oxygen. In order to facilitate the discharge of oxygen generated in the anode 145a, the distance D1 between the anode 145a and the separator 110 is preferably 2 mm or more and 5 mm or less. As described later, the distance D1 between the anode 145a and the separator 110 is ensured by the anode mesh 154a.
[0039] A plurality of through holes that penetrate anode substrate 142a and anode 145a are provided at the end below anode portion 140a. These through holes are connected to the flow path below anode frame 120a. In addition, a plurality of through holes that penetrate anode substrate 142a and anode 145a are provided at the end above anode portion 140a. These through holes are connected to the flow path above anode frame 120a.
[0040] The anode mesh part 150a includes a frame part 152a and a mesh-shaped anode mesh 154a. The frame part 152a is formed into a frame shape by synthetic resin (e.g., polypropylene). The frame part 152a of the anode mesh part 150a supports the anode mesh 154a. In addition, the frame part 152a, the anode substrate 142a, and the diaphragm 110 together form the anode chamber 105a.
[0041] The anode mesh 154a of the anode mesh portion 150a is a mesh-shaped mesh having meshes. The anode mesh 154a is disposed between the anode 145a and the diaphragm 110. The anode mesh 154a ensures a gap D1 between the anode 145a and the diaphragm 110. In the present embodiment, since the anode mesh 154a ensures a gap D1 between the anode 145a and the diaphragm 110, oxygen generated in the anode chamber 105a can be easily discharged, and the unit resistance can be reduced. In order to easily discharge oxygen generated in the anode chamber 105a, it is preferred that the anode mesh 154a has a thickness of 50% to 150% relative to the gap D1 between the anode 145a and the diaphragm 110. For example, as the anode mesh 154a, a Figure 3 A net of tortoise shell type mesh made of polyethylene having a mesh pitch of p1 = p2 = 4.5 mm, a diameter of the wire 156a of 0.9 mm, and a thickness of the wire 156a at the intersection 157a of 1.7 mm as shown.
[0042] Back to Figure 2 The diaphragm 110 of the electrolytic unit 100 is an ion exchange membrane. The diaphragm 110 separates the anode chamber 105a and the cathode chamber 105c and allows the specified ions to pass through. From the viewpoint of reducing the amount of water moving from the anode chamber 105a to the cathode chamber 105c and the movement loss of the vanadium compound ions from the cathode chamber 105c to the anode chamber 105a, the thickness of the diaphragm 110 is preferably 100 μm or more.
[0043] The cathode frame 120c of the electrolysis unit 100, like the anode frame 120a, constitutes the outer shape of the electrolysis unit 100. The cathode frame 120c and the anode frame 120a together clamp the anode part 140a, the anode mesh part 150a, the diaphragm 110, the cathode mesh part 150c and the cathode part 140c. The cathode frame 120c is formed into a flat plate shape by synthetic resin (e.g., polyvinyl chloride) like the anode frame 120a.
[0044] The cathode frame 120c is provided with a flow path (not shown) at the lower end, and the flow path has an inlet 122c and a plurality of outlets (not shown) connected to the cathode liquid supply pipe 312c of the cathode liquid circulation unit 300c. In addition, the cathode frame 120c is provided with a flow path (not shown) at the upper end, and the flow path has an outlet 124c and a plurality of inlets (not shown) connected to the cathode liquid recovery pipe 314c of the cathode liquid circulation unit 300c. The lower flow path is connected to the plurality of through holes (not shown) below the cathode part 140c to form a manifold for supplying the cathode liquid to the cathode chamber 105c. The upper flow path is connected to the plurality of through holes (not shown) above the cathode part 140c to form a manifold for recovering the cathode liquid from the cathode chamber 105c.
[0045] The cathode portion 140c of the electrolytic cell 100 includes a cathode substrate 142c, a base cathode 146c, and a carbon fiber layer 148c. The base cathode 146c and the carbon fiber layer 148c constitute a cathode 145c. In the cathode 145c, trivalent vanadium is generated by electrolytically reducing the tetravalent or higher vanadium contained in the cathode liquid (aqueous sulfuric acid solution containing tetravalent or higher vanadium).
[0046] The cathode substrate 142c of the cathode portion 140c is formed into a plate having a recess 143c by thermoplastic elastomer, synthetic rubber, polyvinyl chloride, etc., similarly to the anode substrate 142a. In the present embodiment, the cathode substrate 142c, the frame 152c of the cathode mesh portion 150c, and the diaphragm 110 form a cathode chamber 105c. The base cathode 146c is embedded in the recess 143c of the cathode substrate 142c.
[0047] The base cathode 146c of the cathode portion 140c is formed into a plate shape, for example, of lead (Pb) or a lead alloy. The base cathode 146c is embedded in the recess 143c of the cathode substrate 142c and formed in the same plane. The base cathode 146c is electrically connected to the power supply portion 500.
[0048] The carbon fiber layer 148c of the cathode portion 140c is a layer formed by processing carbon fibers into a non-woven fabric, felt, textile, sheet, or the like, such as carbon felt. The carbon fiber layer 148c is arranged on the base cathode 146c opposite to the diaphragm 110 and in close contact. Then, the cathode liquid is caused to flow along the carbon fiber layer 148c. By causing the cathode liquid to flow along the carbon fiber layer 148c, the side reaction of generating hydrogen can be suppressed, thereby improving the current efficiency during reduction (hereinafter referred to as reduction current efficiency). In the present embodiment, in order to allow the cathode liquid to fully flow into the carbon fiber layer 148c, it is preferred to adjust the interval D2 between the diaphragm 110 and the base cathode 146c and the thickness of the carbon fiber layer 148c before being loaded into the electrolytic cell 100 in such a manner that the filling rate of the carbon fiber layer 148c is greater than 70% and less than 120%. Here, the filling rate of the carbon fiber layer 148 c refers to the ratio of the thickness of the carbon fiber layer 148 c before being installed in the electrolytic cell 100 to the distance D2 between the separator 110 and the base cathode 146 c.
[0049] In addition, in the cathode portion 140c, a plurality of through holes constituting a manifold for supplying cathode liquid to the cathode chamber 105c are provided below the carbon fiber layer 148c. In addition, a plurality of through holes constituting a manifold for recovering cathode liquid from the cathode chamber 105c are provided above the carbon fiber layer 148c. Thus, the cathode liquid easily flows into the carbon fiber layer 148c.
[0050] The cathode mesh 150c of the electrolysis unit 100 includes a frame 152c and a mesh cathode mesh 154c. The frame 152c is formed into a frame shape by synthetic resin (e.g., polypropylene) similarly to the frame 152a of the anode mesh 150a. The frame 152c of the cathode mesh 150c supports the cathode mesh 154c. The frame 152c, the cathode substrate 142c, and the diaphragm 110 together form the cathode chamber 105c.
[0051] The cathode mesh 154c of the cathode mesh part 150c is a mesh-shaped mesh having meshes similar to the anode mesh 154a. The cathode mesh 154c is arranged between the carbon fiber layer 148c of the cathode part 140c and the diaphragm 110. The cathode mesh 154c ensures a gap (interval) between the carbon fiber layer 148c and the diaphragm 110. Thus, the cathode liquid flows along the gap between the carbon fiber layer 148c and the diaphragm 110 in the cathode part 140c and through the cathode mesh 154c. By making the cathode liquid flow along the gap between the carbon fiber layer 148c and the diaphragm 110 ensured by the cathode mesh 154c, the reduction current efficiency can be improved, and the circulation pressure loss of the cathode liquid can be reduced.
[0052] In order to maintain high reduction current efficiency by using the carbon fiber layer 148c and reduce the pressure loss of the cathode liquid circulation, the cathode mesh 154c is preferably a large mesh and a thin mesh (for example, a thickness of 0.4 mm to 1.0 mm). Specifically, the cathode mesh 154c is preferably a mesh with a larger mesh spacing than the anode mesh 154a and a thinner thickness at the intersection. For example, as the cathode mesh 154c, Figure 4 The net shown is a polyethylene net with deformed diamond meshes having mesh spacings: p1 = 7.0 mm, p2 = 2.9 mm, diameter of wire 156c: 0.25 mm, thickness of wire 156c at intersection 157c: 0.63 mm.
[0053] Next, the circulation unit 300 of the electrolyte production device 10 will be described. Figure 1 As shown, the circulation section 300 includes an anolyte circulation section 300a and a cathode liquid circulation section 300c.
[0054] The anolyte circulation section 300a of the circulation section 300 circulates the anolyte in the anode chamber 105a. The anolyte circulation section 300a circulates the anolyte in a manner such that the bubble rate (bubble rate: the ratio of the volume of gaseous oxygen generated in the anode chamber 105a to the amount of anolyte supplied to the anode chamber 105a) of the anode chamber 105a at 0°C and 1 atmosphere is 50% or less. That is, the anolyte circulation section 300a circulates the anolyte at a flow rate that is more than twice the volume of gaseous oxygen generated per unit time in the anode chamber at 0°C and 1 atmosphere. In this way, the voltage rise between the anode 145a and the cathode 145c caused by the gaseous oxygen can be suppressed, and the unit resistance can be reduced.
[0055] In addition, if the current value supplied by the power supply unit 500 is set to I (ampere), the gas constant is set to R (L·atm / K / mol), the Faraday constant is set to F (c / mol), and the unit time is set to 1 (sec), then the volume V (L / sec) of gaseous oxygen generated per unit time at 0°C (273.15 (K)) and 1 atmosphere is V = (I×R×273.15) / (4×F).
[0056] In addition, the anolyte circulation section 300a circulates the anolyte in a manner where the flow rate is greater than the flow rate of the cathode liquid circulating in the cathode liquid circulation section 300c. As a result, since the pressure in the anode chamber 105a is higher than the pressure in the cathode chamber 105c, the volume of the cathode chamber 105c becomes narrower, thereby increasing the uniformity of the flow of the cathode liquid and improving the reduction current efficiency. The ratio of the flow rate of the anolyte to the flow rate of the cathode liquid is preferably greater than 1.25 and less than 3.4. When the ratio of the flow rate of the anolyte to the flow rate of the cathode liquid is less than 1.25, the uniformizing effect of the flow of the cathode liquid is reduced. In addition, when the ratio of the flow rate of the anolyte to the flow rate of the cathode liquid is greater than 3.4, the volume of the cathode chamber 105c becomes too narrow, and the pressure loss of the circulation of the cathode liquid increases. In addition, the flow rate of the cathode liquid will be described later.
[0057] The anolyte circulation unit 300a includes an anode pump 310a, an anolyte supply pipe 312a, and an anolyte recovery pipe 314a. The anode pump 310a is connected to the anolyte storage tank 610a and the anolyte supply pipe 312a. The anolyte supply pipe 312a is connected to the inlet 122a of the anode frame 120a of the electrolysis unit 100. In addition, the anolyte recovery pipe 314a is connected to the outlet 124a of the anode frame 120a of the electrolysis unit 100 and the anolyte storage tank 610a.
[0058] The cathode liquid circulation section 300c of the circulation section 300 circulates the cathode liquid in the cathode chamber 105c. The cathode liquid circulation section 300c preferably circulates the cathode liquid at a flow rate (SFR: 6 or more) that is 6 times or more of the stoichiometric flow rate (SFR: Specific Flow Rate). Thus, the vanadium with a valence of four or more contained in the cathode liquid is fully supplied to the cathode chamber 105c, and the side reaction of generating hydrogen in the cathode chamber 105c can be suppressed, thereby improving the reduction current efficiency. From the viewpoint of the increase in pressure loss, the operating cost, etc., the flow rate of the cathode liquid is preferably 30 times or less of the stoichiometric flow rate.
[0059] In addition, the stoichiometric flow rate means the theoretically required minimum flow rate of the electrolyte relative to the supplied current. If the current value of the current supplied by the power supply unit 500 is set to I (ampere), the concentration of vanadium with a valence of four or more is set to C (mol / L), the Faraday constant is set to F (c / mol), and the unit time is set to 1 (sec), the stoichiometric flow rate SFR (L / sec) is SFR = I / (C×F).
[0060] The cathode liquid circulation unit 300c includes a cathode pump 310c, a cathode liquid supply pipe 312c, and a cathode liquid recovery pipe 314c. The cathode pump 310c is connected to the cathode liquid storage tank 610c and the cathode liquid supply pipe 312c. The cathode liquid supply pipe 312c is connected to the inlet 122c of the cathode frame 120c of the electrolysis unit 100. In addition, the cathode liquid recovery pipe 314c is connected to the outlet 124c of the cathode frame 120c of the electrolysis unit 100 and the cathode liquid storage tank 610c.
[0061] like Figure 1 As shown, the power supply unit 500 of the electrolyte manufacturing device 10 is electrically connected to the base cathode 146c of the anode 145a and the cathode 145c to supply current. An oxidation reaction occurs in the anode chamber 105a and a reduction reaction occurs in the cathode chamber 105c by the current supplied by the power supply unit 500. In this embodiment, the power supply unit 500 supplies a direct current of 50 amperes, for example.
[0062] The anolyte storage tank 610a of the electrolyte manufacturing device 10 stores the anolyte. Figure 1 As shown, the anolyte storage tank 610a is connected to the anode pump 310a and the anolyte recovery pipe 314a of the anolyte circulation unit 300a. The cathode liquid storage tank 610c of the electrolyte manufacturing device 10 stores the cathode liquid. The cathode liquid storage tank 610c is connected to the cathode pump 310c and the cathode liquid recovery pipe 314c of the cathode liquid circulation unit 300c.
[0063] Next, a method for producing the electrolytic solution will be described. Figure 5 : is a flow chart showing a method for producing an electrolyte. The method for producing an electrolyte comprises: a circulation process (step S10) of circulating an aqueous sulfuric acid solution as an anode liquid in the anode chamber 105a of the electrolysis unit 100, and circulating an aqueous sulfuric acid solution containing tetravalent or higher vanadium as a cathode liquid in the cathode chamber 105c of the electrolysis unit 100; and a reduction process (step S20) of supplying current between the anode 145a and the cathode 145c of the electrolysis unit 100 to electrolytically reduce the tetravalent or higher vanadium in the cathode chamber 105c of the electrolysis unit 100. Figure 2 As shown, an anode 145a and a mesh anode net 154a disposed between the anode 145a and the diaphragm 110 are arranged in the anode chamber 105a separated by the diaphragm 110 of the electrolysis unit 100. In addition, a cathode 145c having a carbon fiber layer 148c on the surface opposite to the diaphragm 110 and a mesh cathode net 154c disposed between the cathode 145c and the diaphragm 110 are arranged in the cathode chamber 105c separated by the diaphragm 110 of the electrolysis unit 100.
[0064] Back to Figure 5In the circulation process (step S10), first, an aqueous sulfuric acid solution is prepared as the anolyte, and an aqueous sulfuric acid solution containing tetravalent or higher vanadium is prepared as the catholyte. As for the aqueous sulfuric acid solution as the anolyte, sulfuric acid is added to pure water and adjusted to a prescribed concentration (an osmotic pressure molar concentration greater than the osmotic pressure molar concentration of the catholyte). As for the aqueous sulfuric acid solution containing tetravalent or higher vanadium as the catholyte, for example, vanadyl sulfate hydrate is added to pure water and adjusted to a prescribed concentration (1.0 mol / L to 3.0 mol / L). Then, the adjusted anolyte is supplied to Figure 1 The anolyte storage tank 610a is shown, and the adjusted catholyte is supplied to the catholyte storage tank 610c.
[0065] In the circulation process (step S10), then, Figure 1 The circulation unit 300 shown circulates the anolyte stored in the anolyte storage tank 610a and the cathode liquid stored in the cathode liquid storage tank 610c in the anode chamber 105a and cathode chamber 105c, respectively. At this time, the anolyte is circulated at a flow rate greater than the flow rate of the cathode liquid and at least twice the volume of gaseous oxygen generated per unit time in the anode chamber 105a at 0°C and 1 atmosphere.
[0066] In this embodiment, by making the flow rate of the anolyte greater than the flow rate of the cathode liquid, the pressure in the anode chamber 105a is higher than the pressure in the cathode chamber 105c, and the volume of the cathode chamber 105c is narrowed, so the uniformity of the flow of the cathode liquid is improved, and the reduction current efficiency can be improved. By circulating the anolyte at a flow rate of more than twice the volume of the gaseous oxygen generated per unit time in the anode chamber 105a at 0°C and 1 atmosphere, the voltage rise between the anode 145a and the cathode 145c caused by the gaseous oxygen can be suppressed, and the cell resistance can be reduced. In addition, since the anode mesh 154a ensures the gap D1 between the anode 145a and the diaphragm 110, the oxygen generated in the anode chamber 105a can be easily discharged, and the cell resistance can be reduced. In addition, since the cathode liquid flows along the carbon fiber layer 148c of the cathode part 140c and along the gap between the carbon fiber layer 148c and the diaphragm 110 ensured by the cathode mesh 154c, the pressure loss of the circulation of the cathode liquid can be reduced while maintaining the high reduction current efficiency obtained by the carbon fiber layer 148c.
[0067] Back to Figure 5 In the reduction process (step S20), current is supplied between the anode 145a and the cathode 145c to electrolytically reduce the tetravalent or higher vanadium contained in the cathode liquid in the cathode chamber 105c to produce trivalent vanadium. If the tetravalent vanadium and trivalent vanadium contained in the cathode liquid are approximately equivalent, the reduction process (step S20) is terminated. Thus, an electrolyte can be manufactured.
[0068] As described above, in the electrolyte manufacturing device 10, since the electrolytic cell 100 has the anode mesh 154a between the anode 145a and the diaphragm 110, it is easy to discharge the oxygen generated in the anode chamber 105a, and the cell resistance is reduced. In addition, since the electrolytic cell 100 has the cathode mesh 154c between the cathode 145c having the carbon fiber layer 148c opposite to the diaphragm 110 and the diaphragm 110, the cathode liquid flows along the inside of the carbon fiber layer 148c and along the gap between the carbon fiber layer 148c and the diaphragm 110 ensured by the cathode mesh 154c, and the electrolyte manufacturing device 10 can maintain the high reduction current efficiency obtained by the carbon fiber layer 148c while reducing the pressure loss of the circulation of the cathode liquid.
[0069] In addition, in the electrolyte manufacturing device 10, since the flow rate of the anolyte is greater than the flow rate of the cathode liquid through the circulation unit 300, the volume of the cathode chamber 105c is narrowed, so the uniformity of the flow of the cathode liquid is improved, and the reduction current efficiency can be improved. In addition, since the circulation unit 300 circulates the anolyte at a flow rate of more than twice the volume of the gaseous oxygen generated per unit time in the anode chamber 105a at 0°C and 1 atmosphere, the voltage rise between the anode 145a and the cathode 145c caused by the gaseous oxygen can be suppressed, and the unit resistance can be reduced.
[0070] Although a plurality of embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments, and various modifications can be made within the scope not departing from the gist of the present invention.
[0071] For example, the anode 145a is not limited to a platinum-coated titanium electrode, and may be an iridium (Ir)-coated titanium electrode, a platinum-iridium-coated titanium electrode, etc. The base cathode 146c is not limited to a lead electrode, and may be a platinum-coated titanium electrode, an iridium-coated titanium electrode, etc. In addition, from the viewpoint of uniform flow distribution, the shape of the anode 145a and the cathode 145c (base cathode 146c, carbon fiber layer 148c) is preferably a rectangular parallelepiped whose length in the longitudinal direction (vertical direction) of the flow path of the anode liquid or cathode liquid is longer than the length in the width direction of the flow path of the anode liquid or cathode liquid.
[0072] In addition, the carbon fiber layer 148c is not limited to carbon felt, and may be any one as long as it is an aggregate of carbon fibers.
[0073] The anode mesh 154a and cathode mesh 154c are not limited to polyethylene, and may be formed of polypropylene, ethylene vinyl acetate, polyvinylidene fluoride, etc. In addition, the meshes of the anode mesh 154a and cathode mesh 154c are not limited to tortoise shell or deformed diamond meshes, and may be diamond meshes, square meshes, etc.
[0074] From the perspective of the pressure resistance and operating costs of the electrolysis unit 100, the anode liquid circulation unit 300a preferably circulates the anode liquid in a manner such that the bubble rate of the anode chamber 105a is greater than 5% at 0°C and 1 atmosphere, that is, at a flow rate of less than 20 times the volume of gaseous oxygen generated per unit time in the anode chamber at 0°C and 1 atmosphere.
[0075] The electrolyte manufacturing device 10 may also include a plurality of electrolytic units 100. The anode chambers 105a of the plurality of electrolytic units 100 may also be connected in series, and the cathode chambers 105c may be connected in series. In addition, the plurality of electrolytic units 100 may also connect the anode liquid supply pipe 312a and the anode liquid recovery pipe 314a of the anode liquid circulation unit 300a, and the cathode liquid supply pipe 312c and the cathode liquid recovery pipe 314c of the cathode liquid circulation unit 300c in parallel.
[0076] Example
[0077] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to the examples.
[0078] In the embodiment, a sulfuric acid aqueous solution with a concentration of 1.8 mol / L of tetravalent or higher vanadium was used as the anolyte of the electrolyte manufacturing device 10. A sulfuric acid aqueous solution with a concentration of 4.0 mol / L of sulfuric acid was used as the catholyte of the electrolyte manufacturing device 10. SELEMION (registered trademark) CMF manufactured by AGC Co., Ltd. was used as the diaphragm 110 of the electrolytic cell 100. In addition, the interval D1 between the anode 145a and the diaphragm 110 was set to 3.0 mm, and a Figure 3 The cathode mesh 154c shown has a tortoise-shell mesh with a mesh spacing of p1=p2=4.5 mm, a diameter of the wire 156a of 0.9 mm, and a thickness of the wire 156a at the intersection 157a of 1.7 mm. In addition, carbon felt AAF304ZS manufactured by Toyobo Co., Ltd. of Japan (thickness before being loaded into the electrolytic cell 100: 4.3 mm) is used as the carbon fiber layer 148c of the cathode 145c. A Figure 4 The cathode mesh 154c shown has a deformed diamond mesh with mesh spacing: p1 = 7.0 mm, p2 = 2.9 mm, a diameter of wire 156c: 0.25 mm, and a thickness of wire 156c at intersection 157c: 0.63 mm. The effective area of the anode 145a and cathode 145c is 100 cm 2 .
[0079] In the embodiment, the inter-electrode voltage, cathode potential, and membrane potential (liquid membrane potential) in the electrolysis cell 100 were measured by supplying a current of 50 amperes from the power supply unit 500. In addition, as an index of pressure loss, the inlet pressure at the inlet 122c of the cathode frame 120c of the electrolysis cell 100 was measured. In addition, the potential was based on a saturated calomel electrode.
[0080] As a comparative example, an electrolytic solution production apparatus including an electrolytic cell obtained by removing the cathode mesh 154 c from the electrolytic cell 100 of the example was prepared, and the same measurement as in the example was performed.
[0081] (Example 1)
[0082] In Example 1, the filling rate of the carbon fiber layer 148c ((the thickness of the carbon fiber layer 148c before being loaded into the electrolytic cell 100 / the interval D2 between the diaphragm 110 and the base cathode 146c)×100) is set to 86%. In addition, the flow rate of the anolyte is set to 4.55 times the volume of the gaseous oxygen generated per unit time in the anode chamber at 0°C and 1 atmosphere. In addition, the flow rate of the cathode liquid is set to 20 times the stoichiometric flow rate (flow rate of the anolyte / flow rate of the cathode liquid=2.27).
[0083] In the following, for ease of understanding, X times the volume of gaseous oxygen produced per unit time in the anode chamber at 0°C and 1 atmosphere in the flow rate of the anolyte is recorded as gas ratio: X. In addition, Y times the stoichiometric flow rate in the flow rate of the cathode liquid is recorded as SFR: Y. The flow rate of the anolyte / the flow rate of the cathode liquid is recorded as the flow ratio. In this embodiment, the filling rate of the carbon fiber layer 148c is 86%, the flow rate of the anolyte is gas ratio: 4.55, the flow rate of the cathode liquid is SFR: 20, and the flow ratio is 2.27.
[0084] (Example 2)
[0085] In Example 2, the filling rate of the carbon fiber layer 148c was set to 86%. In addition, the flow rate of the anolyte was set to gas ratio: 4.55, the flow rate of the catholyte was set to SFR: 6, and the flow rate ratio was set to 7.69.
[0086] (Comparative Example 1)
[0087] In Comparative Example 1, the filling rate of the carbon fiber layer 148c was set to 86%, the flow rate of the anode liquid was set to gas ratio: 4.55, the flow rate of the cathode liquid was set to SFR: 20, and the flow ratio was set to 2.27.
[0088] (Comparative Example 2)
[0089] In Comparative Example 2, the filling rate of the carbon fiber layer 148c was set to 74%, the flow rate of the anode liquid was set to gas ratio: 4.55, the flow rate of the cathode liquid was set to SFR: 15, and the flow ratio was set to 2.86.
[0090] (Comparative Example 3)
[0091] In Comparative Example 3, the filling rate of the carbon fiber layer 148c was set to 172%, the flow rate of the anode liquid was set to gas ratio: 4.55, the flow rate of the cathode liquid was set to SFR: 20, and the flow rate ratio was set to 2.13.
[0092] (Comparative Example 4)
[0093] In Comparative Example 4, the filling rate of the carbon fiber layer 148c was set to 86%, the flow rate of the anode liquid was set to gas ratio: 1.25, the flow rate of the cathode liquid was set to SFR: 8, and the flow ratio was set to 1.52.
[0094] Figure 6 The measurement results in Example 1, Example 2 and Comparative Examples 1 to 4 are shown in FIG.
[0095] like Figure 6 As shown, in Example 1 and Example 2, the membrane potential and inter-electrode voltage representing the unit resistance are small, and in the electrolyte manufacturing device 10 of Example 1 and Example 2, the unit resistance is reduced. In addition, since the cathode potential is small, the reduction current efficiency is improved in the electrolyte manufacturing device 10 of Example 1 and Example 2. In addition, compared with Comparative Example 1, the inlet pressure of Example 1 is smaller, and the pressure loss is reduced by configuring the cathode mesh 154c between the cathode 145c and the diaphragm 110. In addition, in Comparative Example 4, oxygen gas accumulation is observed between the anode 145a and the diaphragm 110.
[0096] As described above, in the electrolyte production apparatus 10 of Example 1 and Example 2, the cell resistance is small, the current efficiency during reduction is high, and the pressure loss in the circulation of the electrolyte is reduced.
[0097] The present invention can be implemented in various embodiments and variations without departing from the broad spirit and scope of the present invention. In addition, the above-mentioned embodiments are used to illustrate the present invention and are not intended to limit the scope of the present invention. In other words, the scope of the present invention is not represented by the embodiments, but by the scope of the claims. In addition, various variations implemented within the scope of the claims and within the scope of the invention meanings equivalent thereto are deemed to be included within the scope of the present invention.
[0098] This application is based on Japanese Patent Application No. 2019-018747 filed on February 5, 2019. The specification, claims, and all drawings of Japanese Patent Application No. 2019-018747 are cited in this specification as a reference.
[0099] Explanation of symbols
[0100] 10-Electrolyte manufacturing device
[0101] 100 - Electrolysis unit
[0102] 105a-Anode chamber
[0103] 105c - cathode chamber
[0104] 110 - Diaphragm
[0105] 120a-Anode frame
[0106] 120c-Cathode frame
[0107] 122a, 122c-Inlet
[0108] 124a, 124c - discharge port
[0109] 140a-Anode
[0110] 142a-Anode substrate
[0111] 143a - concave part
[0112] 145a-Anode
[0113] 140c-Cathode
[0114] 142c-Cathode substrate
[0115] 143c-concave
[0116] 145c - cathode
[0117] 146c-Base cathode
[0118] 148c - Carbon fiber layer
[0119] 150a-Anode mesh
[0120] 152a-Frame
[0121] 154a-Anode mesh
[0122] 156a, 156c - Line
[0123] 157a, 157c - Intersection
[0124] 150c-Cathode mesh
[0125] 152c-Frame
[0126] 154c-Cathode screen
[0127] 300-Circulation Department
[0128] 300a-Anolyte circulation unit
[0129] 310a - Anode pump
[0130] 312a-Anolyte supply pipe
[0131] 314a-Anolyte recovery pipe
[0132] 300c-Cathode liquid circulation unit
[0133] 310c - cathode pump
[0134] 312c - cathode liquid supply pipe
[0135] 314c-Cathode liquid recovery pipe
[0136] 500-Power Supply Department
[0137] 610a - Anolyte Storage Tank
[0138] 610c - Catholyte storage tank
[0139] D1 - the distance between anode and diaphragm
[0140] D2 - the distance between the diaphragm and the base cathode
[0141] p1, p2 - spacing
Claims
1. An electrolyte manufacturing device, in, have: An electrolytic cell having an anode chamber provided with an anode, a cathode chamber provided with a cathode, and a diaphragm separating the anode chamber from the cathode chamber, a circulation unit that circulates an aqueous sulfuric acid solution as an anolyte in the anode chamber and circulates an aqueous sulfuric acid solution containing vanadium with a valence of four or more as a cathode solution in the cathode chamber, a power supply unit, which is electrically connected to the anode and the cathode and supplies current; The cathode has a carbon fiber layer on a surface opposite to the separator; The electrolytic unit has a mesh-shaped anode net disposed between the anode and the diaphragm and a mesh-shaped cathode net disposed between the cathode and the diaphragm; The anode mesh has a thickness of 50% to 150% relative to the distance between the anode and the separator, The thickness of the cathode mesh is thinner than that of the anode mesh, The circulation unit circulates the anolyte at a flow rate greater than the flow rate of the cathode solution and at a flow rate that is twice or more the volume of gaseous oxygen generated per unit time at 0° C. in the anode chamber.
2. The electrolyte manufacturing device according to claim 1, in, The ratio of the flow rate of the anolyte to the flow rate of the catholyte is 1.25 or more and 3.4 or less.
3. The electrolyte manufacturing device according to claim 1, in, The filling rate of the carbon fiber layer is 70% or more and 120% or less.
4. The electrolyte manufacturing device according to claim 1, in, The circulation unit circulates the cathode liquid at a flow rate that is six times or more of the stoichiometric flow rate.
5. The electrolyte manufacturing device according to claim 1, in, The concentration of the tetravalent or higher-valent vanadium in the aqueous sulfuric acid solution containing tetravalent or higher-valent vanadium is 1.0 mol / L or more and 3.0 mol / L or less.
6. A method for producing an electrolyte, in, Include: a circulation step, wherein an aqueous sulfuric acid solution as an anode liquid is circulated in an anode chamber, and an aqueous sulfuric acid solution containing vanadium with a valence of four or more as a cathode liquid is circulated in a cathode chamber; the anode chamber is separated by a diaphragm, and is provided with an anode and a mesh anode net disposed between the anode and the diaphragm; the cathode chamber is separated by the diaphragm, and is provided with a cathode having a carbon fiber layer on a surface opposite to the diaphragm, and a mesh cathode net disposed between the cathode and the diaphragm, a reduction step of supplying current between the anode and the cathode to electrolytically reduce the tetravalent or higher vanadium in the cathode chamber; In the circulation step, the anolyte is circulated at a flow rate greater than the flow rate of the cathode liquid and at least twice the volume of gaseous oxygen generated per unit time in the anode chamber at 0° C., The anode mesh has a thickness of 50% to 150% relative to the distance between the anode and the separator, The cathode mesh is thinner than the anode mesh.
7. The method for producing an electrolyte according to claim 6, in, In the circulation step, the anolyte is circulated at a flow rate ratio of 1.25 times or more and 3.4 times or less compared to the catholyte.
8. The method for producing an electrolyte according to claim 6, in, In the circulation step, the cathode liquid is circulated at a flow rate that is six times or more of the stoichiometric flow rate.