Semiconductor structure and method for forming the same
By forming a diffusion barrier structure layer in the semiconductor structure to ensure direct contact between the through-hole interconnection structure and the first interconnection line, the problem of high contact resistance between the through-hole interconnection structure and the lower interconnection line is solved, and the performance of the semiconductor structure is improved. .
Patent Information
- Application Number
- CN202010285657.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-04-13
AI Technical Summary
The contact resistance between the through-hole interconnection structure and the underlying interconnection lines in existing semiconductor devices is high, resulting in poor device performance. As the feature size of the device shrinks, the diffusion barrier layer has an increasing impact on interconnection performance.
In the method of forming a semiconductor structure, a diffusion barrier structure layer is formed on the bottom surface and sidewalls of the interconnection trench and on the sidewalls of the conductive via hole. The diffusion barrier structure layer exposes the interconnection line at the bottom of the conductive via hole to avoid conduction. A diffusion barrier layer is formed at the bottom of the through hole, so that the through hole interconnection structure is in direct contact with the first interconnection line.
The contact resistance between the through-hole interconnection structure and the first interconnection line is reduced, the contact performance between the through-hole interconnection structure and the first interconnection line is improved, and the performance of the semiconductor structure is optimized.
Smart Images

Figure CN113539941B_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a method for forming the same. Background Art
[0002] As the manufacturing of integrated circuits develops towards ultra-large-scale integrated circuits (ULSI), the internal circuit density is getting higher and higher, and the number of components contained is increasing, so that the surface of the chip cannot provide enough area to manufacture the required interconnection lines. In order to meet the increased demand for interconnection lines after the components are reduced, the design of multi-layer metal interconnection structures with more than two layers realized by metal interconnection lines and through-hole interconnection structures has become a method that must be adopted in ultra-large-scale integrated circuit technology.
[0003] In the back-end manufacturing process of semiconductor devices, a metal interconnection structure forming process is usually required. The metal interconnection structure forming process is usually carried out on a semiconductor substrate, which usually has an active area, and semiconductor devices such as transistors and capacitors are formed on the active area. In the metal interconnection structure, there can usually be multiple layers of through-hole interconnection structures and metal interconnection lines, and the multiple layers of metal interconnection lines can be electrically connected through the through-hole interconnection structure. When forming a subsequent layer of metal interconnection lines on a previous layer of through-hole interconnection structures, or forming a subsequent layer of through-hole interconnection structures on a previous layer of metal interconnection lines, an interlayer dielectric layer is usually first formed on the previous layer of through-hole interconnection structures or metal interconnection lines, and then a via and an interconnection trench are formed in the interlayer dielectric layer. Finally, the via and the interconnection trench are filled with metal to form a subsequent layer of through-hole interconnection structures or metal interconnection lines.
[0004] After forming the through hole or the interconnection trench, before filling the through hole and the trench with metal, a diffusion barrier layer is usually formed on the bottom surface and sidewall of the through hole or the interconnection trench. Summary of the invention
[0005] The problem solved by the embodiments of the present invention is to provide a semiconductor structure and a method for forming the same, which are beneficial to optimizing the performance of the semiconductor structure.
[0006] To solve the above problems, an embodiment of the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate; forming a first dielectric layer and a first interconnection line located in the first dielectric layer on the substrate, wherein the first dielectric layer exposes the top surface of the first interconnection line; forming a second dielectric layer covering the first dielectric layer and the first interconnection line; etching a portion of the thickness of the second dielectric layer to form an interconnection groove in the second dielectric layer; forming a conductive through hole penetrating the second dielectric layer at the bottom of the interconnection groove, wherein the bottom of the conductive through hole exposes the first interconnection line, and the conductive through hole is connected to the interconnection groove; forming a diffusion barrier structure layer located on the bottom surface and sidewalls of the interconnection groove and on the sidewalls of the conductive through hole, wherein the diffusion barrier structure layer exposes the first interconnection line located at the bottom of the conductive through hole; and forming a through hole interconnection structure located in the conductive through hole and a second interconnection line located in the interconnection groove on the diffusion barrier structure layer through a filling process, wherein the through hole interconnection structure is in direct contact with the first interconnection line.
[0007] Correspondingly, an embodiment of the present invention also provides a semiconductor structure, comprising: a substrate; a first dielectric layer, located on the substrate; a first interconnection line, located in the first dielectric layer; a second dielectric layer, covering the first dielectric layer and the first interconnection line; a through-hole interconnection structure, located in the second dielectric layer above the first interconnection line and in direct contact with the first interconnection line; a second interconnection line, located in the second dielectric layer above the through-hole interconnection structure and in contact with the through-hole interconnection structure; a diffusion barrier structure layer, located between the second interconnection line and the second dielectric layer, and between the side wall of the through-hole interconnection structure and the second dielectric layer.
[0008] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:
[0009] In the method for forming a semiconductor structure provided by an embodiment of the present invention, a diffusion barrier structure layer is formed on the bottom surface and side walls of the interconnection groove and on the side walls of the conductive through hole, and the diffusion barrier structure layer exposes the first interconnection line located at the bottom of the conductive through hole; therefore, the bottom of the conductive through hole in the embodiment of the present invention is not formed with a diffusion barrier structure layer, so that in the step of forming a through-hole interconnection structure located in the conductive through hole, the through-hole interconnection structure can directly contact the first interconnection line, which is beneficial to reducing the contact resistance between the through-hole interconnection structure and the first interconnection line, and further beneficial to improving the contact performance between the through-hole interconnection structure and the first interconnection line, and correspondingly optimizing the performance of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figures 1 to 4 It is a schematic structural diagram corresponding to each step in a method for forming a semiconductor structure;
[0011] Figures 5 to 15 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention. DETAILED DESCRIPTION
[0012] In the interconnection process, a through-hole interconnection structure is usually used to connect the upper and lower interconnection lines. However, the contact resistance between the through-hole interconnection structure and the interconnection line of the lower layer is relatively high, resulting in poor performance of the device. The reasons for the poor performance of the device are analyzed in combination with a method for forming a semiconductor structure.
[0013] Figures 1 to 4 A structural schematic diagram corresponding to each step in a method for forming a semiconductor structure is shown.
[0014] refer to Figure 1 , providing a substrate 1; forming a first dielectric layer 2 and a first interconnection line 3 located in the first dielectric layer 2 on the substrate 1, wherein the first dielectric layer 2 exposes the top surface of the first interconnection line 3; and forming a second dielectric layer 4 covering the first dielectric layer 2 and the first interconnection line 3.
[0015] refer to Figure 2 , etching a portion of the thickness of the second dielectric layer 4 to form an interconnection groove 5 in the second dielectric layer 4; forming a conductive through hole 6 in the second dielectric layer 4 penetrating the bottom portion of the interconnection groove 5, wherein the bottom of the conductive through hole 6 exposes the first interconnection line 3, and the conductive through hole 6 is connected to the interconnection groove 5.
[0016] refer to Figure 3 , forming a diffusion barrier layer 7 located on the bottom surface and side walls of the interconnection trench 5 and the bottom surface and side walls of the conductive via 6 .
[0017] refer to Figure 4 Through a filling process, a through-hole interconnect structure 8 located in the conductive through-hole 6 and a second interconnect line 9 located in the interconnect trench 5 are formed on the diffusion barrier layer 7 .
[0018] In the above formation method, after forming the conductive through hole 6, a diffusion barrier layer 7 is formed on the bottom surface and side walls of the interconnection groove 5 and on the bottom surface and side walls of the conductive through hole 6. The diffusion barrier layer 7 is also used to prevent the through hole interconnection structure 8 or the second interconnection line 9 from diffusing into the second dielectric layer 4, thereby improving the problem of electromigration.
[0019] However, the diffusion barrier layer 7 is formed between the through-hole interconnect structure 8 and the first interconnect line 3. Compared with the material of the through-hole interconnect structure 8, the first interconnect line 3 or the second interconnect line 9, the material of the diffusion barrier layer 7 has lower electrical conductivity and poorer electrical conductivity. The diffusion barrier layer 7 is formed between the through-hole interconnect structure 8 and the first interconnect line 3, which results in that the through-hole interconnect structure 8 and the first interconnect line 3 cannot be in direct contact, which easily leads to a higher contact resistance between the through-hole interconnect structure 8 and the first interconnect line 3, thereby reducing the contact performance between the through-hole interconnect structure 8 and the first interconnect line 3, resulting in poor performance of the formed semiconductor structure.
[0020] Moreover, as the feature size of devices further decreases, the diffusion barrier layer 7 has an increasingly greater impact on the interconnection performance of the semiconductor structure.
[0021] In order to solve the technical problem, an embodiment of the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate; forming a first dielectric layer and a first interconnection line located in the first dielectric layer on the substrate, wherein the first dielectric layer exposes the top surface of the first interconnection line; forming a second dielectric layer covering the first dielectric layer and the first interconnection line; etching a portion of the thickness of the second dielectric layer to form an interconnection groove in the second dielectric layer; forming a conductive through hole penetrating the second dielectric layer at the bottom of the interconnection groove, wherein the bottom of the conductive through hole exposes the first interconnection line, and the conductive through hole is connected to the interconnection groove; forming a diffusion barrier structure layer located on the bottom surface and sidewalls of the interconnection groove and on the sidewalls of the conductive through hole, wherein the diffusion barrier structure layer exposes the first interconnection line located at the bottom of the conductive through hole; and forming a through hole interconnection structure located in the conductive through hole and a second interconnection line located in the interconnection groove on the diffusion barrier structure layer through a filling process, wherein the through hole interconnection structure is in direct contact with the first interconnection line.
[0022] In the method for forming a semiconductor structure provided by an embodiment of the present invention, a diffusion barrier structure layer is formed on the bottom surface and side walls of the interconnection groove and on the side walls of the conductive through hole, and the diffusion barrier structure layer exposes the first interconnection line located at the bottom of the conductive through hole; therefore, the bottom of the conductive through hole in the embodiment of the present invention is not formed with a diffusion barrier structure layer, so that in the step of forming a through-hole interconnection structure located in the conductive through hole, the through-hole interconnection structure can directly contact the first interconnection line, which is beneficial to reducing the contact resistance between the through-hole interconnection structure and the first interconnection line, and further beneficial to improving the contact performance between the through-hole interconnection structure and the first interconnection line, and correspondingly optimizing the performance of the semiconductor structure.
[0023] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and understandable, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0024] Figures 5 to 15 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention.
[0025] refer to Figure 5 , providing a substrate 100.
[0026] The substrate 100 is used to provide a process platform for a process.
[0027] In this embodiment, semiconductor devices such as transistors and capacitors may be formed in the substrate 100 , and functional structures such as resistor structures and conductive structures may also be formed in the substrate 100 .
[0028] Continue to refer Figure 5 A first dielectric layer 110 and a first interconnection line 111 located in the first dielectric layer 110 are formed on the substrate 100 , and the first dielectric layer 110 exposes a top surface of the first interconnection line 111 .
[0029] In this embodiment, the first dielectric layer 110 is an intermetallic dielectric (IMD) layer. The first dielectric layer 110 is used to achieve electrical isolation between adjacent interconnects in a back end of line (BEOL) process. Specifically, the first dielectric layer 110 is used to electrically isolate adjacent first interconnects 111.
[0030] To this end, the material of the first dielectric layer 110 is a low-k dielectric material (a low-k dielectric material refers to a dielectric material having a relative dielectric constant greater than or equal to 2.6 and less than or equal to 3.9), an ultra-low-k dielectric material (an ultra-low-k dielectric material refers to a dielectric material having a relative dielectric constant less than 2.6), silicon oxide, silicon nitride or silicon oxynitride, etc.
[0031] In this embodiment, the material of the first dielectric layer 110 is an ultra-low-k dielectric material, so as to reduce the parasitic capacitance between the back-end interconnection structures, thereby reducing the back-end RC delay. Specifically, the ultra-low-k dielectric material can be SiOCH.
[0032] In this embodiment, the first dielectric layer 110 is taken as a single-layer structure as an example. In other embodiments, the first dielectric layer may also be a multi-layer structure.
[0033] The first interconnection line 111 is electrically connected to the substrate 100 , for example, the first interconnection line 111 is electrically connected to a transistor in the substrate 100 , so that the transistor is electrically connected to an external circuit or other interconnection structures.
[0034] The first dielectric layer 110 exposes the top surface of the first interconnection line 111 , so as to subsequently form an interconnection structure electrically connected to the first interconnection line 111 .
[0035] In this embodiment, the first interconnection line 111 is a metal line.
[0036] As an example, in this embodiment, the first interconnection line 111 is a single-layer structure, and the material of the first interconnection line 111 is copper. Copper has a low resistivity, which is beneficial to improving the signal delay of the back-end RC and increasing the processing speed of the chip, and is also beneficial to reducing the resistance of the first interconnection line 111, thereby reducing power consumption accordingly.
[0037] In other embodiments, the material of the first interconnection line may also be a conductive material such as cobalt, tungsten, aluminum, etc., and the first interconnection line may also be a multi-layer structure.
[0038] In this embodiment, a third diffusion barrier layer 112 is further formed on the bottom surface and sidewall of the first interconnection line 111. The third diffusion barrier layer 112 is used to improve the adhesion between the first interconnection line 111 and the first dielectric layer 110, and the third diffusion barrier layer 112 is also used to reduce the probability of the material of the first interconnection line 111 diffusing into the first dielectric layer 110. In this embodiment, the material of the third diffusion barrier layer 112 is tantalum nitride.
[0039] In this embodiment, the first dielectric layer 110 and the first interconnection line 111 are formed on the substrate 100 as an example. In actual processes, one or more dielectric layers can be formed between the first dielectric layer 110 and the substrate 100, and interconnection lines or conductive plugs can be formed in each dielectric layer.
[0040] refer to Figure 6 , forming a second dielectric layer 120 covering the first dielectric layer 110 and the first interconnection line 111 .
[0041] Subsequent steps also include: forming an interconnection trench in the second dielectric layer 120; forming a conductive through hole in the second dielectric layer 120 penetrating the bottom of the interconnection trench portion; forming a through hole interconnection structure in the conductive through hole, and a second interconnection line in the interconnection trench.
[0042] The second dielectric layer 120 is also a metal interlayer dielectric layer. The second dielectric layer 120 is used to achieve electrical isolation between the through-hole interconnect structures and between the second interconnect lines.
[0043] To this end, the material of the second dielectric layer 120 is a low-k dielectric material, an ultra-low-k dielectric material, silicon oxide, silicon nitride or silicon oxynitride.
[0044] In this embodiment, the material of the second dielectric layer 120 is an ultra-low-k dielectric material, so as to reduce the parasitic capacitance between the back-end interconnection structures, thereby reducing the back-end RC delay. Specifically, the ultra-low-k dielectric material can be SiOCH.
[0045] In this embodiment, the second dielectric layer 120 is taken as a single-layer structure as an example. In other embodiments, the second dielectric layer may also be a multi-layer structure.
[0046] In this embodiment, the second dielectric layer 120 is formed by a deposition process.
[0047] refer to Figure 7 , etching a portion of the thickness of the second dielectric layer 120 to form an interconnection trench 10 in the second dielectric layer 120 .
[0048] The interconnection trench 10 is used to provide a spatial location for forming a second interconnection line.
[0049] In this embodiment, the step of forming the interconnection trench 10 includes: forming a hard mask layer 130 on the second dielectric layer 120 ; and etching a portion of the thickness of the second dielectric layer 120 using the hard mask layer 130 as a mask to form the interconnection trench 10 .
[0050] In this embodiment, the hard mask layer 130 is a metal hard mask layer, and the hard mask layer 130 is used as an etching mask for forming the interconnection trench 10 .
[0051] In this embodiment, the material of the hard mask layer 130 is titanium nitride.
[0052] In this embodiment, a dry etching process, such as an anisotropic dry etching process, is used to etch a portion of the thickness of the second dielectric layer 120 to form the interconnection trench 10 .
[0053] The anisotropic dry etching process has anisotropic etching characteristics, which is beneficial to improving the controllability of the etching profile, and correspondingly beneficial to improving the profile quality of the interconnection trench 10 , and is also beneficial to accurately controlling the depth of the interconnection trench 10 .
[0054] Combined with reference Figure 8 After forming the interconnect trench 10 , the method for forming the semiconductor structure further includes: removing the hard mask layer 130 to expose the top surface of the second dielectric layer 120 .
[0055] Subsequent steps also include: forming a second interconnection line located in the interconnection groove 10. The formation of the second interconnection line generally includes the steps of forming a conductive layer filling the interconnection groove 10 on the second dielectric layer 120, and removing the conductive layer higher than the second dielectric layer 120. In this embodiment, by removing the hard mask layer 130 to expose the top surface of the second dielectric layer 120, the conductive layer only needs to be filled in the interconnection groove 10 formed in the partial thickness of the second dielectric layer 120, and does not need to be filled in the groove surrounded by the hard mask layer 130. This is conducive to reducing the thickness of the conductive layer that needs to be filled, thereby facilitating the improvement of the filling capacity of the conductive layer in the interconnection groove 10, and further facilitating the improvement of the formation quality of the second interconnection line.
[0056] In this embodiment, a dry etching process is used to remove the hard mask layer 130 .
[0057] In this embodiment, removing the hard mask layer after forming the interconnection trench 10 and before forming the first diffusion barrier layer is taken as an example. In other embodiments, according to actual needs, the hard mask layer may be retained after forming the interconnection trench.
[0058] Continue to refer Figure 8 After forming the interconnect trench 10 , the method for forming the semiconductor structure further includes: forming a first diffusion barrier layer 140 on the bottom and sidewalls of the interconnect trench 10 .
[0059] The first diffusion barrier layer 140 is used to prevent the material of the second interconnect line from diffusing into the second dielectric layer 120, thereby improving the problem of electromigration (EM); moreover, the first diffusion barrier layer 140 is also used to prevent impurities such as carbon atoms and oxygen atoms in the second dielectric layer 120 from diffusing into the second interconnect line. Both of the above aspects are conducive to improving the reliability of the semiconductor structure.
[0060] In this embodiment, in the step of forming the first diffusion barrier layer 140 , the first diffusion barrier layer 140 is formed on the bottom and sidewalls of the interconnection trench 10 and the top surface of the second dielectric layer 120 .
[0061] The material of the first diffusion barrier layer 140 includes one or more of tantalum, tantalum nitride, titanium, titanium nitride, cobalt, manganese, manganese oxide, ruthenium nitride and ruthenium. In this embodiment, the material of the first diffusion barrier layer 140 is tantalum.
[0062] In this embodiment, in the step of forming the first diffusion barrier layer 140, the first diffusion barrier layer 140 located at the bottom of the interconnection trench 10 has a first thickness, and the first diffusion barrier layer 140 located at the sidewall of the interconnection trench 10 has a second thickness, and the first thickness is greater than the second thickness.
[0063] Subsequent steps also include: forming a conductive via of the second dielectric layer 120 penetrating a portion of the bottom of the interconnection groove 10; forming a second diffusion barrier layer on the sidewalls of the conductive via and the interconnection groove 10, the second diffusion barrier layer and the first diffusion barrier layer 140 being used to constitute a diffusion barrier structure layer; wherein the step of forming the second diffusion barrier layer includes: forming a barrier material layer on the bottom and sidewalls of the conductive via, and on the bottom and sidewalls of the interconnection groove 10; and removing the barrier material layer at the bottom of the interconnection groove 10 and the bottom of the conductive via.
[0064] In the present embodiment, by making the first thickness greater than the second thickness, the first diffusion barrier layer 140 located at the bottom of the interconnection groove 10 is made thicker, thereby helping to prevent the problem of the first diffusion barrier layer 140 located at the bottom of the interconnection groove 10 being completely removed in the subsequent step of removing the barrier material layer located at the bottom of the interconnection groove 10 and the bottom of the conductive through hole, thereby helping to ensure that the first diffusion barrier layer 140 located at the bottom of the interconnection groove 10 can retain a portion of its thickness, thereby correspondingly ensuring the anti-diffusion capability of the diffusion barrier structure layer.
[0065] The difference between the second thickness and the first thickness should not be too small or too large. If the difference between the second thickness and the first thickness is too small, when the thickness of the first diffusion barrier layer 140 located on the side wall of the interconnection trench 10 is small, the thickness of the first diffusion barrier layer 140 located at the bottom of the interconnection trench 10 is also small. In the subsequent step of removing the barrier material layer located at the bottom of the interconnection trench 10 and the bottom of the conductive via, it is difficult to ensure that the first diffusion barrier layer 140 located at the bottom of the interconnection trench 10 can retain part of its thickness; if the difference between the second thickness and the first thickness is too large, it is easy to cause the thickness of the first diffusion barrier layer 140 located at the bottom of the interconnection trench 10 to be too large, and the first diffusion barrier layer 140 located at the bottom of the interconnection trench 10 is easy to occupy more space, thereby easily reducing the subsequent formation space of the second interconnection line. For this reason, in this embodiment, the difference between the second thickness and the first thickness is 1 angstrom to 30 angstroms.
[0066] The thickness of the first diffusion barrier layer 140 is formed by one or more processes including a physical vapor deposition process, an atomic layer deposition process, and a chemical vapor deposition process.
[0067] In this embodiment, a physical vapor deposition (PVD) process is used to form the first diffusion barrier layer 140. The PVD process has low cost and high compatibility with the back-end interconnection process, and the step coverage capability of the PVD process is low. By selecting the PVD process, it is beneficial to make the second thickness greater than the first thickness. Specifically, the PVD process can be a sputtering process or the like.
[0068] refer to Figures 9 to 11 , forming a conductive via 20 penetrating the second dielectric layer 120 at the bottom of the interconnection trench 10 , the bottom of the conductive via 20 exposes the first interconnection line 111 , and the conductive via 20 is connected to the interconnection trench 10 .
[0069] The conductive through-hole 20 is used to provide a spatial position for forming a through-hole interconnection structure.
[0070] The conductive via 20 is connected to the interconnection trench 10, so that the subsequently formed via interconnection structure and the second interconnection line are an integrated structure.
[0071] In this embodiment, the step of forming the conductive via 20 includes: etching the first diffusion barrier layer 140 and the second dielectric layer 120 at the bottom of the interconnection groove 10, and forming a conductive via 20 exposing the first interconnection line 140 in the second dielectric layer 120 and the first diffusion barrier layer 140 at the bottom of the interconnection groove 10.
[0072] Specifically, in this embodiment, the step of forming the conductive via 20 includes:
[0073] like Fig. 9 As shown, a pattern layer 142 filling the interconnection trench 10 is formed on the second dielectric layer 120 , and the pattern layer 142 has a pattern opening 30 located above a portion of the first interconnection line 111 .
[0074] The pattern layer 142 is used as an etching mask for forming conductive through holes.
[0075] In this embodiment, the material of the pattern layer 142 includes photoresist. The pattern layer 142 can be formed by photolithography processes such as photoresist coating, exposure, and development.
[0076] In this embodiment, before forming the pattern layer 142 , the method for forming a semiconductor structure further includes: forming a filling layer 141 filling the interconnection trench 10 . Accordingly, the pattern layer 142 is formed on the filling layer 141 .
[0077] The filling layer 141 is used to provide a flat surface for forming the pattern layer 142 , thereby facilitating improving the pattern quality and dimensional accuracy of the pattern layer 142 .
[0078] In this embodiment, the material of the filling layer 141 includes spin-on-carbon (SOC), which has good filling performance and a simple formation process.
[0079] like Fig.10 As shown, the first diffusion barrier layer 140 is etched along the pattern opening 30 using the pattern layer 142 as a mask to form an initial through hole (not shown) penetrating the first diffusion barrier layer 140 .
[0080] After forming the initial through hole penetrating the first diffusion barrier layer 140, the remaining first diffusion barrier layer 140 can be used as a self-aligned stop layer for etching the second dielectric layer 120 to form a conductive through hole. Specifically, the interconnection trench 10 extends in a direction parallel to the substrate 100, and the top view of the interconnection trench 10 is a long strip structure. After forming the initial through hole, the remaining first diffusion barrier layer 140 can be used as a self-aligned stop layer in a direction parallel to the substrate 100 and in a width direction of the interconnection trench 10, thereby defining a formation area of the conductive through hole 20, so that the conductive through hole can be formed in the interconnection trench 10.
[0081] In this embodiment, the pattern layer 142 is used as a mask to etch the filling layer 141 and the first diffusion barrier layer 140 along the pattern opening 30 to form an initial through hole.
[0082] In this embodiment, a dry etching process, for example, an anisotropic dry etching process, is used to etch the filling layer 141 and the first diffusion barrier layer 140 along the pattern opening 30 to form the initial through hole.
[0083] like Fig.10 As shown, the second dielectric layer 120 below the initial through hole is etched to form the conductive through hole 20 .
[0084] In the process of etching the second dielectric layer 120 below the initial through hole, the process of etching the second dielectric layer 120 has a low etching rate on the first diffusion barrier layer 140, so that the first diffusion barrier layer 140 can define the position of the conductive through hole 20 along the width direction parallel to the substrate 100 and along the interconnection groove 10, which is beneficial to reduce the process difficulty of forming the conductive through hole 20 and increase the process window for forming the conductive through hole 20.
[0085] In this embodiment, a dry etching process is adopted to etch the second dielectric layer 120 below the initial through hole.
[0086] Specifically, by adjusting the etching gas type and etching parameters, in the same reaction chamber, the first diffusion barrier layer 140 is sequentially etched to form the initial through hole, and the second dielectric layer 120 below the initial through hole is etched to form the conductive through hole 20 .
[0087] As an example, in this embodiment, the pattern layer 142 is used as a mask to sequentially etch the first diffusion barrier layer 140 and the second dielectric layer 120 along the pattern opening 30 to form the conductive via 20 .
[0088] In other embodiments, after etching the first diffusion barrier layer along the pattern opening to form an initial through hole, in the second dielectric layer below the initial through hole, even if the pattern layer is lost, the remaining first diffusion barrier layer can continue to serve as a mask for etching the second dielectric layer to form a conductive through hole, so that the remaining first diffusion barrier layer can serve as a self-aligned stop layer in a direction parallel to the substrate and along the width of the interconnection groove, thereby defining a formation area for the conductive through hole, aligning the conductive through hole with the interconnection groove in the width direction of the interconnection groove, and thereby facilitating improved process stability.
[0089] In other embodiments, when a hard mask layer is still retained on the second dielectric layer, during the process of forming the conductive via, the hard mask layer can also define the formation area of the conductive via in a direction parallel to the substrate and along the width of the interconnection groove, so that the conductive via is aligned with the interconnection groove along the width of the interconnection groove.
[0090] Combined with reference Fig.11 After forming the conductive via 20, the pattern layer 141 and the filling layer 142 are removed. Specifically, the pattern layer 141 and the filling layer 142 are removed by an ashing process or a wet stripping process.
[0091] refer to Figure 12 to Figure 13 , forming a diffusion barrier structure layer 160 (such as a diffusion barrier layer 160) located on the bottom surface and sidewalls of the interconnect trench 10 and the sidewalls of the conductive via 20 Fig.13 As shown), the diffusion barrier structure layer 160 exposes the first interconnection line 111 located at the bottom of the conductive through hole 20.
[0092] In the method for forming a semiconductor structure provided by an embodiment of the present invention, a diffusion barrier structure layer 160 is formed on the bottom surface and sidewalls of the interconnection trench 10 and on the sidewalls of the conductive via 20, and the diffusion barrier structure layer 160 exposes the first interconnection line 111 located at the bottom of the conductive via 20; therefore, the diffusion barrier structure layer 160 is not formed at the bottom of the conductive via 20 in the embodiment of the present invention, so that in the step of forming a through-hole interconnection structure located in the conductive via 20, the through-hole interconnection structure can directly contact the first interconnection line 111, which is beneficial to reducing the contact resistance between the through-hole interconnection structure and the first interconnection line 111, and further beneficial to improving the contact performance between the through-hole interconnection structure and the first interconnection line 111, and correspondingly optimizing the performance of the semiconductor structure.
[0093] The diffusion barrier structure layer 160 is used to prevent the material of the second interconnection line and the through-hole interconnection structure from diffusing into the second dielectric layer 120, thereby improving the problem of electromigration (EM); moreover, the diffusion barrier structure layer 160 is also used to prevent impurities such as carbon atoms and oxygen atoms in the second dielectric layer 120 from diffusing into the second interconnection line and the through-hole interconnection structure. Both of the above aspects are conducive to improving the reliability of the semiconductor structure.
[0094] In this embodiment, the step of forming the diffusion barrier structure layer 160 includes: forming a second diffusion barrier layer 150 on the side walls of the conductive via 20 and the interconnection groove 10, the second diffusion barrier layer 150 exposing the first interconnection line 111 at the bottom of the conductive via 20, and the second diffusion barrier layer 150 and the first diffusion barrier layer 140 are used to constitute the diffusion barrier structure layer 160.
[0095] The material of the second diffusion barrier layer 150 includes one or more of tantalum, tantalum nitride, titanium, titanium nitride, cobalt, manganese, manganese oxide, ruthenium nitride and ruthenium. In this embodiment, the material of the second diffusion barrier layer 150 is tantalum nitride.
[0096] The thickness of the second diffusion barrier layer 150 should not be too small or too large. If the thickness of the second diffusion barrier layer 150 is too small, it is easy to cause the second diffusion barrier layer 150 located on the side wall of the conductive through hole 20 to have too low anti-diffusion barrier capability; if the thickness of the second diffusion barrier layer 150 is too large, it is easy to cause the second diffusion barrier layer 150 to occupy too much space of the conductive through hole 20, which is easy to cause the volume of the subsequent through-hole interconnection structure to be too small, and correspondingly, it is easy to increase the resistance of the through-hole interconnection structure. For this reason, in this embodiment, the thickness of the second diffusion barrier layer 150 is 5 angstroms to 30 angstroms.
[0097] Specifically, in this embodiment, the step of forming the second diffusion barrier layer 150 includes:
[0098] like Fig.12 As shown, a barrier material layer 145 is formed on the bottom and sidewalls of the conductive via 20 and the bottom and sidewalls of the interconnect trench 10 .
[0099] The barrier material layer 145 is used to form the second diffusion barrier layer 150 .
[0100] In this embodiment, the barrier material layer 145 is also formed on the first diffusion barrier layer 140 located on the second dielectric layer 120 .
[0101] In the step of forming the barrier material layer 145, the barrier material layer 145 located at the bottom of the interconnection groove 10 and the bottom of the conductive via 20 has a third thickness, and the barrier material layer 145 located at the sidewall of the interconnection groove 10 and the sidewall of the conductive via 20 has a fourth thickness, the third thickness is greater than or equal to the fourth thickness, and the difference between the third thickness and the fourth thickness is less than the difference between the first thickness and the second thickness.
[0102] The difference between the third thickness and the fourth thickness is smaller than the difference between the first thickness and the second thickness, that is, compared with the first diffusion barrier layer 140 located at the bottom and sidewall of the interconnection groove 10, the thickness difference between the barrier material layer 145 located at the sidewall of the interconnection groove 10 and the conductive via 20 and the barrier material layer 145 located at the bottom of the interconnection groove 10 and the conductive via 20 is smaller, which is beneficial to ensure that the thickness of the barrier material layer 145 located at the sidewall of the conductive via 20 is not too small, and further helps to ensure the anti-diffusion barrier capability of the subsequent second diffusion barrier layer 150 located on the sidewall of the conductive via 20.
[0103] The process of forming the barrier material layer 145 includes one or more of an atomic layer deposition process, a physical vapor deposition process, and a chemical vapor deposition process.
[0104] In this embodiment, an atomic layer deposition process is used to form the barrier material layer 145. The atomic layer deposition process has a strong step coverage capability, which is conducive to improving the conformal coverage capability of the barrier material layer 145, and correspondingly is conducive to improving the thickness uniformity of the barrier material layer 145, so that the difference between the third thickness and the fourth thickness is small, and the atomic layer deposition process includes performing multiple atomic layer deposition cycles, which is conducive to improving the density of the barrier material layer 145, and further conducive to improving the anti-diffusion barrier capability of the second diffusion barrier layer.
[0105] like Fig.13As shown, the barrier material layer 145 located at the bottom of the interconnect trench 10 and the bottom of the conductive via 20 is removed, and the remaining barrier material layer 145 located at the sidewalls of the interconnect trench 10 and the sidewalls of the conductive via 20 is used as the second diffusion barrier layer 150 .
[0106] In this embodiment, an anisotropic dry etching process is used to remove the barrier material layer 145 located at the bottom of the interconnection trench 10 and the bottom of the conductive via 20 .
[0107] The anisotropic dry etching process has the characteristic of anisotropic etching, which is beneficial to reducing the lateral etching of the barrier material layer 145 located on the side walls of the interconnection groove 10 and the conductive via 20, so that while removing the barrier material layer 145 located at the bottom of the interconnection groove 10 and the bottom of the conductive via 20, the barrier material layer 145 located on the side walls of the interconnection groove 10 and the conductive via 20 can be retained as the second diffusion barrier layer 150. In addition, in the process of forming the second diffusion barrier layer 150 in this embodiment, there is no need to form an additional mask, which is beneficial to cost saving.
[0108] In this embodiment, in the step of removing the barrier material layer 145 located at the bottom of the interconnection trench 10 and the bottom of the conductive via 20, a partial thickness of the first diffusion barrier layer 140 located at the bottom of the interconnection trench 10 and the barrier material layer 145 located above the second dielectric layer 120 are also removed.
[0109] refer to Fig.14 and Fig.15 , through a filling process, a through-hole interconnect structure 170 (such as Fig.15 ), and a second interconnection line 180 (as shown in FIG. Fig.15 As shown), the through-hole interconnect structure 170 is in direct contact with the first interconnect line 111.
[0110] In the present embodiment, the diffusion barrier structure layer 160 exposes the first interconnection line 111 at the bottom of the conductive through hole 20. Therefore, in the process of forming the through-hole interconnection structure 170, the through-hole interconnection structure 170 can directly contact the first interconnection line 111, which is beneficial to reduce the contact resistance between the through-hole interconnection structure 170 and the first interconnection line 111, and correspondingly helps to improve the contact performance between the interconnection structure 170 and the first interconnection line 111, and further helps to improve the RC performance of the back-end interconnection.
[0111] The through-hole interconnection structure 170 is used to realize the electrical connection between the first interconnection line 111 and other interconnection structures or external circuits. Specifically, the through-hole interconnection structure 170 realizes the electrical connection between the first interconnection line 111 and the second interconnection line 180.
[0112] The second interconnection line 180 is used to electrically connect the through-hole interconnection structure 170 with an external circuit or other interconnection structures.
[0113] In this embodiment, the conductive through hole 20 is connected to the interconnection groove 10, so the through hole interconnection structure 170 and the second interconnection line 180 are an integrated structure, which is beneficial to improve the contact performance between the through hole interconnection structure 170 and the second interconnection line 180, and further improve the signal response speed between the through hole interconnection structure 170 and the second interconnection line 180.
[0114] In this embodiment, the material of the through hole interconnection structure 170 is the same as that of the second interconnection line 180. The material of the through hole interconnection structure 170 and the second interconnection line 180 is copper. In other embodiments, the material of the through hole interconnection structure and the second interconnection line can also be a conductive material such as cobalt, tungsten, aluminum, etc.
[0115] In this embodiment, the steps of forming the through hole interconnect structure 170 and the second interconnect line 180 include: Fig.14 As shown, a conductive layer 165 is formed to fill the conductive via 20 and the interconnection groove 10, and the conductive layer 165 also covers the first diffusion barrier layer 140 located on the second dielectric layer 120; the conductive layer 165 and the first diffusion barrier layer 140 above the second dielectric layer 120 are removed, and the remaining conductive layer 165 located in the conductive via 20 is used as the through-hole interconnection structure 170, and the remaining conductive layer 165 located in the interconnection groove 10 is used as the second interconnection line 180.
[0116] In this embodiment, the conductive layer 165 is formed by an electrochemical plating process.
[0117] In this embodiment, a chemical mechanical polishing process is used to remove the conductive layer 165 and the first diffusion barrier layer 140 that are higher than the second dielectric layer 120 .
[0118] In this embodiment, the through hole interconnect structure 170 and the second interconnect line 180 are taken as a single-layer structure as an example. In other embodiments, according to actual process requirements, the through hole interconnect structure and the second interconnect line can also be a multi-layer structure, and the materials of the through hole interconnect structure and the second interconnect line can include a variety of conductive materials.
[0119] Accordingly, the present invention also provides a semiconductor structure. Fig.15, showing a schematic structural diagram of an embodiment of a semiconductor structure of the present invention.
[0120] The semiconductor structure includes: a substrate 100; a first dielectric layer 110, located on the substrate 100; a first interconnection line 111, located in the first dielectric layer 110; a second dielectric layer 120, covering the first dielectric layer 110 and the first interconnection line 111; a through-hole interconnection structure 170, located in the second dielectric layer 120 above the first interconnection line 111 and in direct contact with the first interconnection line 111; a second interconnection line 180, located in the second dielectric layer 120 above the through-hole interconnection structure 170 and in contact with the through-hole interconnection structure 170; and a diffusion barrier structure layer 160, located between the second interconnection line 180 and the second dielectric layer 120, and between the sidewall of the through-hole interconnection structure 170 and the second dielectric layer 120.
[0121] The diffusion barrier structure layer 160 is located between the second interconnection line 180 and the second dielectric layer 120, and between the side wall of the through-hole interconnection structure 170 and the second dielectric layer 120. The semiconductor structure does not directly set a diffusion barrier structure layer between the through-hole interconnection structure 170 and the first interconnection line 111, so that the through-hole interconnection structure 170 is in direct contact with the first interconnection line 111, which is beneficial to reducing the contact resistance between the through-hole interconnection structure 170 and the first interconnection line 111, and correspondingly beneficial to improving the contact performance between the interconnection structure 170 and the first interconnection line 111, and further beneficial to improving the RC performance of the back-end interconnection.
[0122] The substrate 100 is used to provide a process platform for a process.
[0123] In this embodiment, semiconductor devices such as transistors and capacitors may be formed in the substrate 100 , and functional structures such as resistor structures and conductive structures may also be formed in the substrate 100 .
[0124] In this embodiment, the first dielectric layer 110 is an intermetallic dielectric (IMD) layer. The first dielectric layer 110 is used to achieve electrical isolation between adjacent interconnects in a back end of line (BEOL) process. Specifically, the first dielectric layer 110 is used to electrically isolate adjacent first interconnects 111.
[0125] To this end, the material of the first dielectric layer 110 is a low-k dielectric material, an ultra-low-k dielectric material, silicon oxide, silicon nitride or silicon oxynitride.
[0126] In this embodiment, the material of the first dielectric layer 110 is an ultra-low-k dielectric material, so as to reduce the parasitic capacitance between the back-end interconnection structures, thereby reducing the back-end RC delay. Specifically, the ultra-low-k dielectric material can be SiOCH.
[0127] In this embodiment, the first dielectric layer 110 is taken as a single-layer structure as an example. In other embodiments, the first dielectric layer may also be a multi-layer structure.
[0128] The first interconnection line 111 is electrically connected to the substrate 100 , for example, the first interconnection line 111 is electrically connected to a transistor in the substrate, so that the transistor is electrically connected to an external circuit or other interconnection structures.
[0129] The first dielectric layer 110 exposes the top surface of the first interconnection line 111 , so as to subsequently form an interconnection structure electrically connected to the first interconnection line 111 .
[0130] In this embodiment, the first interconnection line 111 is a metal line.
[0131] As an example, in this embodiment, the first interconnection line 111 is a single-layer structure, and the material of the first interconnection line 111 is copper. Copper has a low resistivity, which is beneficial to improving the signal delay of the back-end RC and increasing the processing speed of the chip, and is also beneficial to reducing the resistance of the first interconnection line 111, thereby reducing power consumption accordingly.
[0132] In other embodiments, the material of the first interconnection line may also be a conductive material such as cobalt, tungsten, aluminum, etc., and the first interconnection line may also be a multi-layer structure.
[0133] In this embodiment, the semiconductor structure further includes: a third diffusion barrier layer 112 located between the first interconnect line 111 and the first dielectric layer 110 .
[0134] The third diffusion barrier layer 112 is used to improve the adhesion between the first interconnection line 111 and the first dielectric layer 110, and also to reduce the probability of the material of the first interconnection line 111 diffusing into the first dielectric layer 110. In this embodiment, the material of the third diffusion barrier layer 112 is tantalum nitride.
[0135] In this embodiment, the first dielectric layer 110 and the first interconnection line 111 are located on the substrate 100 as an example. In actual processes, one or more dielectric layers can be formed between the first dielectric layer 110 and the substrate 100, and interconnection lines or conductive plugs can be formed in each dielectric layer.
[0136] The second dielectric layer 120 is also a metal interlayer dielectric layer. The second dielectric layer 120 is used to achieve electrical isolation between the through-hole interconnect structures 170 and the second interconnect lines 180 .
[0137] To this end, the material of the second dielectric layer 120 is a low-k dielectric material, an ultra-low-k dielectric material, silicon oxide, silicon nitride or silicon oxynitride, etc. In this embodiment, the material of the second dielectric layer 120 is an ultra-low-k dielectric material, thereby reducing the parasitic capacitance between the back-end interconnection structures, thereby reducing the back-end RC delay. Specifically, the ultra-low-k dielectric material can be SiOCH.
[0138] In this embodiment, the second dielectric layer 120 is taken as a single-layer structure as an example. In other embodiments, the second dielectric layer may also be a multi-layer structure.
[0139] The through-hole interconnection structure 170 is used to realize the electrical connection between the first interconnection line 111 and other interconnection structures or external circuits. Specifically, the through-hole interconnection structure 170 realizes the electrical connection between the first interconnection line 111 and the second interconnection line 180.
[0140] The second interconnection line 111 is used to electrically connect the through-hole interconnection structure 170 with an external circuit or other interconnection structures.
[0141] In this embodiment, the through-hole interconnect structure 170 and the second interconnect line 180 are an integrated structure, which is beneficial to improving the contact performance between the through-hole interconnect structure 170 and the second interconnect line 180, and further beneficial to improving the signal response speed between the through-hole interconnect structure 170 and the second interconnect line 180.
[0142] In this embodiment, the material of the through hole interconnection structure 170 is the same as that of the second interconnection line 180. The material of the through hole interconnection structure 170 and the second interconnection line 180 is copper. In other embodiments, the material of the through hole interconnection structure and the second interconnection line can also be a conductive material such as cobalt, tungsten, aluminum, etc.
[0143] In this embodiment, the through hole interconnect structure 170 and the second interconnect line 180 are taken as a single-layer structure as an example. In other embodiments, according to actual process requirements, the through hole interconnect structure and the second interconnect line can also be a multi-layer structure, and the materials of the through hole interconnect structure and the second interconnect line can include a variety of conductive materials.
[0144] The diffusion barrier structure layer 160 is used to prevent the materials of the second interconnection line 180 and the through-hole interconnection structure 170 from diffusing into the second dielectric layer 120, thereby improving the problem of electromigration (EM); moreover, the diffusion barrier structure layer 160 is also used to prevent impurities such as carbon atoms and oxygen atoms in the second dielectric layer 120 from diffusing into the second interconnection line 180 and the through-hole interconnection structure 170. Both of the above aspects are conducive to improving the reliability of the semiconductor structure.
[0145] In this embodiment, the diffusion barrier structure layer 160 includes: a first diffusion barrier layer 140, which is located on the sidewall of the second interconnect line 180 and in contact with the second dielectric layer 120, and between the bottom of the second interconnect line 180 and the second dielectric layer 120 at the periphery of the through-hole interconnect structure 170; a second diffusion barrier layer 150, which is located between the sidewall of the second interconnect line 180 and the first diffusion barrier layer 140, and between the sidewall of the through-hole interconnect structure 170 and the second dielectric layer 120.
[0146] The first diffusion barrier layer 140 is used to prevent the material of the second interconnect line 180 from diffusing into the second dielectric layer 120 , thereby improving the problem of electromigration; moreover, the first diffusion barrier layer 140 is also used to prevent impurities such as carbon atoms and oxygen atoms in the second dielectric layer 120 from diffusing into the second interconnect line 180 .
[0147] The material of the first diffusion barrier layer 140 includes one or more of tantalum, tantalum nitride, titanium, titanium nitride, cobalt, manganese, manganese oxide, ruthenium nitride and ruthenium. In this embodiment, the material of the first diffusion barrier layer 140 is tantalum.
[0148] In this embodiment, the first diffusion barrier layer 140 at the bottom of the second interconnect line 180 has a first thickness, and the first diffusion barrier layer 140 at the sidewall of the second interconnect line 180 has a second thickness, and the first thickness is greater than the second thickness.
[0149] Since the diffusion barrier structure layer 160 located on the side wall of the second interconnect line 180 includes the first diffusion barrier layer 140 and the second diffusion barrier layer 150, and the diffusion barrier structure layer 160 located at the bottom of the second interconnect line 180 only includes the first diffusion barrier layer 140, by making the first thickness greater than the second thickness, the difference in thickness of the diffusion barrier structure layer 160 located on the side wall and bottom of the second interconnect line 180 is smaller.
[0150] The material of the second diffusion barrier layer 150 includes one or more of tantalum, tantalum nitride, titanium, titanium nitride, cobalt, manganese, manganese oxide, ruthenium nitride and ruthenium. In this embodiment, the material of the second diffusion barrier layer 150 is tantalum nitride.
[0151] The thickness of the second diffusion barrier layer 150 should not be too small or too large. If the thickness of the second diffusion barrier layer 150 is too small, it is easy to cause the second diffusion barrier layer 150 located on the side wall of the conductive through hole 20 to have too low anti-diffusion barrier capability; if the thickness of the second diffusion barrier layer 150 is too large, it is easy to cause the second diffusion barrier layer 150 to occupy too much space of the conductive through hole 20, which is easy to cause the volume of the subsequent through-hole interconnection structure to be too small, and correspondingly, it is easy to increase the resistance of the through-hole interconnection structure. For this reason, in this embodiment, the thickness of the second diffusion barrier layer 150 is 5 angstroms to 30 angstroms.
[0152] The semiconductor structure can be formed by the formation method described in the above embodiment, or by other formation methods. For the specific description of the semiconductor structure described in this embodiment, reference can be made to the corresponding description in the above embodiment, and this embodiment will not be repeated here.
[0153] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor structure, characterized in that: include: providing a substrate; forming a first dielectric layer and a first interconnection line in the first dielectric layer on the substrate, wherein the first dielectric layer exposes a top surface of the first interconnection line; forming a second dielectric layer covering the first dielectric layer and the first interconnection line; Etching a portion of the thickness of the second dielectric layer to form interconnection trenches in the second dielectric layer; forming a conductive through hole of the second dielectric layer penetrating through the bottom of the interconnection trench portion, wherein the bottom of the conductive through hole exposes the first interconnection line, and the conductive through hole is connected to the interconnection trench; After forming the interconnect trench and before forming the conductive via, the method for forming the semiconductor structure further comprises: forming a first diffusion barrier layer at the bottom and sidewalls of the interconnect trench; in the step of forming the conductive via, etching the first diffusion barrier layer above the first interconnect line; forming a diffusion barrier structure layer located on the bottom surface and sidewalls of the interconnection trench and on the sidewalls of the conductive through hole, wherein the diffusion barrier structure layer exposes the first interconnection line located at the bottom of the conductive through hole; Through a filling process, a through-hole interconnection structure located in the conductive through-hole and a second interconnection line located in the interconnection trench are formed on the diffusion barrier structure layer, and the through-hole interconnection structure is in direct contact with the first interconnection line.
2. The method for forming a semiconductor structure according to claim 1, wherein: The step of forming the conductive via comprises: etching the first diffusion barrier layer and the second dielectric layer at the bottom of the interconnection trench portion, and forming a conductive via exposing the first interconnection line in the second dielectric layer and the first diffusion barrier layer at the bottom of the interconnection trench portion; The step of forming the diffusion barrier structure layer includes: forming a second diffusion barrier layer on the sidewalls of the conductive via and the interconnection groove, the second diffusion barrier layer exposes the first interconnection line at the bottom of the conductive via, and the second diffusion barrier layer and the first diffusion barrier layer are used to constitute the diffusion barrier structure layer.
3. The method for forming a semiconductor structure according to claim 2, wherein: In the step of forming the first diffusion barrier layer, the first diffusion barrier layer at the bottom of the interconnect trench has a first thickness, and the first diffusion barrier layer at the sidewall of the interconnect trench has a second thickness, and the first thickness is greater than the second thickness.
4. The method for forming a semiconductor structure according to claim 3, wherein: The difference between the second thickness and the first thickness is 1 angstrom to 30 angstroms.
5. The method for forming a semiconductor structure according to claim 2, wherein: The process of forming the first diffusion barrier layer includes one or more of a physical vapor deposition process, an atomic layer deposition process, and a chemical vapor deposition process.
6. The method for forming a semiconductor structure according to claim 2, wherein: The step of forming the second diffusion barrier layer includes: forming a barrier material layer on the bottom and sidewalls of the conductive via and the bottom and sidewalls of the interconnect trench; The barrier material layer at the bottom of the interconnection trench and the bottom of the conductive via is removed, and the remaining barrier material layer at the sidewalls of the interconnection trench and the sidewalls of the conductive via is used as the second Diffusion barrier.
7. The method for forming a semiconductor structure according to claim 6, wherein: The process of forming the barrier material layer includes one or more of an atomic layer deposition process, a physical vapor deposition process, and a chemical vapor deposition process.
8. The method for forming a semiconductor structure according to claim 6, wherein: In the step of forming the first diffusion barrier layer, the first diffusion barrier layer located at the bottom of the interconnect trench has a first thickness, and the first diffusion barrier layer located at the sidewall of the interconnect trench has a second thickness, and the first thickness is greater than the second thickness; In the step of forming the barrier material layer, the barrier material layer located at the bottom of the interconnect groove and the bottom of the conductive through hole has a third thickness, and the barrier material layer located at the sidewall of the interconnect groove and the sidewall of the conductive through hole has a fourth thickness, the third thickness is greater than or equal to the fourth thickness, and the difference between the third thickness and the fourth thickness is less than the difference between the first thickness and the second thickness.
9. The method for forming a semiconductor structure according to claim 6, wherein: An anisotropic dry etching process is adopted to remove the barrier material layer located at the bottom of the interconnection trench and the bottom of the conductive through hole.
10. The method for forming a semiconductor structure according to claim 6, wherein: In the step of removing the barrier material layer at the bottom of the interconnect trench and the bottom of the conductive via, a portion of the thickness of the first diffusion barrier layer at the bottom of the interconnect trench is also removed.
11. The method for forming a semiconductor structure according to claim 2, wherein: The material of the first diffusion barrier layer and the second diffusion barrier layer includes one or more of tantalum, tantalum nitride, titanium, titanium nitride, cobalt, manganese, manganese oxide, ruthenium nitride and ruthenium.
12. The method for forming a semiconductor structure according to claim 2, wherein: The second diffusion barrier layer has a thickness of 5 angstroms to 30 angstroms.
13. The method for forming a semiconductor structure according to claim 2, wherein: The step of forming the interconnection trench comprises: forming a hard mask layer on the second dielectric layer; using the hard mask layer as a mask, etching a portion of the thickness of the second dielectric layer to form the interconnection trench.
14. The method for forming a semiconductor structure according to claim 13, wherein: After forming the interconnect trench and before forming the first diffusion barrier layer, the method for forming the semiconductor structure further includes: removing the hard mask layer to expose the top surface of the second dielectric layer; In the step of forming the first diffusion barrier layer, the first diffusion barrier layer is formed on the bottom and sidewalls of the interconnect trench and the top surface of the second dielectric layer.
15. The method for forming a semiconductor structure according to claim 2, wherein: The step of forming the conductive via comprises: forming a graphic layer filling the interconnection groove on the second dielectric layer, the graphic layer having a graphic opening located above a portion of the first interconnection line; using the graphic layer as a mask, etching the first diffusion barrier layer along the graphic opening to form an initial via hole penetrating the first diffusion barrier layer; etching the second dielectric layer below the initial via hole to form the conductive via hole.
16. A semiconductor structure, characterized in that: The method for forming a semiconductor structure according to any one of claims 1 to 15 comprises: substrate; A first dielectric layer, located on the substrate; A first interconnection line, located in the first dielectric layer; a second dielectric layer, covering the first dielectric layer and the first interconnection line; a through-hole interconnect structure located in the second dielectric layer above the first interconnect line and in direct contact with the first interconnect line; A second interconnection line is located in a second dielectric layer above the through-hole interconnection structure and contacts the through-hole interconnection structure; A diffusion barrier structure layer is located between the second interconnect line and the second dielectric layer, and between the side wall of the through-hole interconnect structure and the second dielectric layer. The diffusion barrier structure layer includes: a first diffusion barrier layer, located on the side wall of the second interconnect line and in contact with the second dielectric layer, and located between the bottom of the second interconnect line at the periphery of the through-hole interconnect structure and the second dielectric layer.
17. The semiconductor structure according to claim 16, wherein: The diffusion barrier structure layer further includes: a second diffusion barrier layer located between the sidewall of the second interconnect line and the first diffusion barrier layer, and between the sidewall of the through hole interconnect structure and the second dielectric layer.
18. The semiconductor structure according to claim 17, wherein: The material of the first diffusion barrier layer and the second diffusion barrier layer includes one or more of tantalum, tantalum nitride, titanium, titanium nitride, cobalt, manganese, manganese oxide, ruthenium nitride and ruthenium.
19. The semiconductor structure according to claim 17, wherein: The second diffusion barrier layer has a thickness of 5 angstroms to 30 angstroms.
20. The semiconductor structure according to claim 16, wherein: The through hole interconnection structure and the second interconnection line are an integrated structure.
Citation Information
Patent Citations
Advanced interconnection for integrated circuits
US20020151165A1
Method of fabricating interconnection line of semiconductor device
US20200083094A1