Method and catalyst for producing 1,3-butadiene from ethanol
By using a catalyst composed of zeolite, alumina and layered double hydroxide or mixed metal oxide, the problem of insufficient catalyst activity and selectivity when converting ethanol into 1,3-butadiene is solved, and an efficient and stable process is achieved. catalytic effect.
Patent Information
- Application Number
- CN202080019580.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-02-13
- Filing Date
- 2020-02-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When converting ethanol into 1,3-butadiene, the existing technology has low catalyst activity, low selectivity and low yield, and the reaction is complex, making it difficult to achieve efficient conversion under mild conditions.
Using a catalyst containing component A of zeolite, alumina or a combination thereof and layered double hydroxide (LDH) or mixed metal oxide, the catalyst precursor and catalyst are prepared by a co-precipitation method to form a core-shell structure to improve the catalyst The acid-base properties are balanced to improve catalytic activity and selectivity.
High catalytic activity, high yield and high selectivity for the conversion of ethanol into 1,3-butadiene under mild conditions are achieved, and the stability of the catalyst and reaction efficiency are improved.
Smart Images

Figure BDA0003251608370000201 
Figure HDA0003251608380000011 
Figure HDA0003251608380000012
Abstract
Description
Technical Field
[0001] The present invention relates to a method for converting ethanol into 1,3-butadiene, comprising component A and component B. cat Catalyst and composition for preparing the catalyst comprising component A and component B pre Furthermore, the present invention relates to a method for producing 1,3-butadiene from ethanol and the use of the catalyst for converting ethanol into 1,3-butadiene. Background Art
[0002] Since butadiene is used as a monomer in the production of synthetic rubbers such as butadiene rubber, nitrile rubber, styrene butadiene rubber, etc., there is a great demand for butadiene. Currently, the major amount of butadiene produced worldwide is produced as a by-product of steam cracking to produce ethylene.
[0003] In one of the two main industrial processes, butadiene is extracted from oil pyrolysis products. In the second method, butadiene is obtained by catalytic dehydrogenation of n-butane and butene contained in refineries and oil well gas, which is carried out in one or two steps. However, with the rise in oil prices, alternative methods for the production of butadiene from non-petroleum feedstocks are becoming increasingly attractive.
[0004] One of the most promising non-petroleum feedstocks is ethanol. The catalytic conversion of ethanol to 1,3-butadiene is well known. From 1920 to the early 1960s, ethanol was converted to 1,3-butadiene, hydrogen and water in a one-step process at 400 to 450 °C.
[0005] However, the mechanism of ethanol conversion to 1,3-butadiene is extremely complex. The main reason for its complexity is that the pathway of ethanol conversion to 1,3-butadiene contains multiple reaction steps, including simultaneous acid, base and redox reactions.
[0006] The main pathway for the conversion of ethanol to 1,3-butadiene consists of five key reaction steps, namely, ethanol dehydrogenation, acetaldehyde aldol condensation, butanediol dehydration, Meerwein-Ponndorf-Verley (MPV) reduction, and crotyl alcohol dehydration. For these reaction pathways, the balance between the acid-base properties of the catalyst is a key success factor for improving catalyst activity as well as the selectivity and yield of the desired 1,3-butadiene product.
[0007] Therefore, there remains a need to find improved processes and catalysts for converting ethanol to 1,3-butadiene having improved turnover numbers, selectivities and yields, as well as catalysts for converting ethanol to 1,3-butadiene having improved activity and selectivity for the reaction.
[0008] Problems to be solved
[0009] Therefore, an object of the present invention is to provide a catalyst having high catalytic activity, high yield and high selectivity for catalyzing the conversion of ethanol to 1,3-butadiene under mild conditions. Another object of the present invention is to provide a method for producing 1,3-butadiene from ethanol with improved selectivity and yield. Summary of the invention
[0010] The above purpose is achieved by having component A and component B cat A specific combination of catalysts is achieved.
[0011] Therefore, the present invention provides a catalyst precursor for preparing a catalyst for converting ethanol into 1,3-butadiene, which comprises a component A selected from zeolite, silica, alumina or any combination thereof, and a component B comprising a layered double hydroxide (LDH). pre .
[0012] In addition, the present invention provides a catalyst for converting ethanol into 1,3-butadiene, which comprises a component A selected from zeolite, silica, alumina or any combination thereof and a component B comprising a mixed metal oxide. cat .
[0013] In addition, the present invention also provides a method for producing 1,3-butadiene, which comprises contacting an ethanol stream with a catalyst, wherein the catalyst comprises a component A selected from zeolite, silica, alumina or any combination thereof, and a component B comprising a mixed metal oxide. cat .
[0014] Finally, the present invention provides a component A comprising a zeolite, a silica, an alumina or any combination thereof and a component B comprising a layered double hydroxide (LDH). pre Use of a catalyst precursor for preparing a catalyst for converting ethanol into 1,3-butadiene, and a component A selected from zeolite, silica, alumina or any combination thereof and a component B comprising a mixed metal oxide cat The catalyst is used for converting ethanol into 1,3-butadiene.
[0015] definition
[0016] Layered double hydroxides (LDHs) are a class of synthetic or natural two-dimensional nanostructured layered materials with two metal cations in the main layer and in the interlayer regions containing anionic species. The general molecular description of layered double hydroxides (LDHs) is provided by chemical formula (I):
[0017] [M z+ (1-x) M' y+ x (OH)2]a+ A n- a / n ·bH2O (I)
[0018] in
[0019] M and M' are charged metal cations, and M is different from M';
[0020] z is 1 or 2;
[0021] y is 3 or 4;
[0022] A n- is an interlayer anion with n>0, preferably n=1-5;
[0023] 0 <x<0.9
[0024] b=0-10
[0025] a=z(1-x)+xy−2 and is greater than 0.
[0026] Mixed metal oxide refers to an oxidized form of a mixture of at least two or more metals, an oxidized form of a mixture of at least two or more metal oxides, or an oxidized form of a combination thereof, and is not limited by any physical properties, chemical properties, or preparation methods. LDO (layered double oxide) is a preferred embodiment of the mixed metal oxide.
[0027] The layered double oxide (LDO) is derived from a layered double hydroxide (LDH), wherein the layered double hydroxide (LDH) is heat-treated to remove interlayer water molecules, anions, and hydroxyl groups. As a result, the structure of the layered double hydroxide (LDH) at least partially collapses to form the layered double oxide (LDO).
[0028] Catalyst activity has the unit [g 1,3-BD g cat -1 h -1 ] and represents the quotient of the weight of 1,3-butadiene produced in one hour and the weight of the catalyst.
[0029] As used herein, weight hourly space velocity (WHSV) defines the weight of a feed stream per unit weight of catalyst per hour.
[0030] The term on-stream time refers to the period of time that the catalyst is in contact with the ethanol feed stream.
[0031] As used herein, the term zeolite refers to a crystalline material having a structure characterized by a framework of linked tetrahedra, each tetrahedron consisting of four atoms of O. The framework contains open cavities in the form of channels and cages that are usually occupied by H2O molecules and usually exchangeable extra-framework cations.
[0032] Description of the Invention
[0033] The invention provides a catalyst precursor, a catalyst and a method for preparing 1,3-butadiene from ethanol using the catalyst, as well as use of the catalyst for producing 1,3-butadiene from ethanol and use of the catalyst precursor for preparing the catalyst.
[0034] A. Catalyst Precursors
[0035] The present invention provides a catalyst precursor for preparing a catalyst for converting ethanol into 1,3-butadiene, comprising:
[0036] i) component A selected from zeolite, silica, alumina or any combination thereof; and
[0037] ii) Component B comprising a layered double hydroxide (LDH) pre .
[0038] Catalyst Precursor Component B pre
[0039] In one embodiment, component B pre Contains at least 70 wt % LDH, preferably at least 80 wt % LDH, more preferably at least 90 wt % LDH. In a preferred embodiment, component B pre It is composed of layered double hydroxide (LDH).
[0040] Preferably, component A and component B pre The weight ratio of component A to component B is in the range of 1:0.1 to 1:5, more preferably 1:0.2 to 1:5, and even more preferably 1:0.3 to 1:5. pre The weight ratio balances the acid-base properties of the catalyst precursor, thereby improving the yield and selectivity of the catalyst derived from the catalyst precursor according to the present invention for converting ethanol to 1,3-butadiene.
[0041] In a preferred embodiment, the LDH comprises a first metal DM and a second metal TM. The first metal DM is at least one monovalent metal cation, a divalent metal cation, or a combination thereof. Preferably, the first metal DM is at least one divalent metal cation. In addition, the second metal TM is at least one trivalent metal cation, a tetravalent metal cation, or a combination thereof. Preferably, the second metal TM is at least one trivalent metal cation.
[0042] In one embodiment, the LDH further comprises an intercalation anion. The intercalation anion is selected from CO3 2- 、OH-、F-、Cl - Br -,I - 、SO4 2- 、NO3 - and PO4 3- In a preferred embodiment, the interlayer anion is selected from CO3 2- and NO3 - In a first most preferred embodiment, the intercalation anion is CO3 2- In a second most preferred embodiment, the intercalation anion is NO3 - .
[0043] Preferably, the molar ratio of the first metal DM to the second metal TM is in the range of 1:1 to 10:1, more preferably 2:1 to 7:1, and most preferably 2:1 to 5:1.
[0044] In a preferred embodiment, the first metal DM is selected from Li, Ca, Mg, Zn, Fe, Co, Cu, Ni and combinations thereof, preferably selected from Ca, Mg, Zn, Cu, Ni and combinations thereof, more preferably selected from Mg, Cu, Ni, Zn and combinations thereof. In a first most preferred embodiment, the first metal DM comprises Mg, preferably consists of Mg. In a second most preferred embodiment, the first metal DM comprises, preferably consists of a combination of Mg, Cu and Ni.
[0045] In embodiments where the first metal DM comprises, preferably consists of, a combination of Mg, Cu and Ni, preferably the molar ratio of Mg:Cu:Ni is in the range of 1-5:0.01-3:0.01-3, preferably 1.5-4.5:0.02-2.5:0.02-2.5, more preferably 1.8-4:0.02-1.5:0.02-1.5.
[0046] In a preferred embodiment, the second metal TM is selected from Al, Ga, In, Y, Fe, Co, Mn, Cr, Ti, V, La, Sn, Zr and combinations thereof, preferably selected from Al, Ga, In, Fe, Co, Sn, Zr and combinations thereof, more preferably selected from Al, Zr and combinations thereof. In a first most preferred embodiment, the second metal TM comprises Al, preferably consists of Al. In a second most preferred embodiment, the second metal TM comprises, preferably consists of a combination of Al and Zr.
[0047] In embodiments where the second metal TM comprises, preferably consists of, a combination of Al and Zr, the molar ratio of Al:Zr is in the range of 0.05-1.5:0.02-1.5, preferably 0.1-1.2:0.05-1.5, and more preferably 0.25-1.15:0.05-1.15.
[0048] In a specific embodiment, the first metal DM comprises, preferably consists of, Mg, and the second metal TM comprises, preferably consists of, Al and Zr.
[0049] In another specific embodiment, the first metal DM comprises, preferably consists of, Mg, Cu and Ni, and the second metal TM comprises, preferably consists of Al.
[0050] Preferably, the first metal DM and the second metal TM are selected from different metal cations.
[0051] In an alternative preferred embodiment, component B pre Also comprising an active metal deposited on the surface of a layered double hydroxide (LDH). For example, the deposited LDH can be obtained by impregnating the LDH with an active metal. The active metal can be selected from Li, Ca, Zn, Fe, Co, Cu, Ni, Ga, In, Y, Fe, Co, Mn, Cr, Ti, V, La, Sn, Zr and combinations thereof, preferably selected from Cu, Ni, Zr and combinations thereof.
[0052] Component A of the catalyst precursor
[0053] Component A is selected from zeolite, silica, alumina and combinations thereof. In a preferred embodiment, component A is selected from zeolite, silica and alumina. In another preferred embodiment, component A is selected from zeolite, silica and combinations thereof. In the first most preferred embodiment, component A comprises, preferably at least 80wt%, more preferably at least 90wt% silica, and even more preferably consists of silica. In the second most preferred embodiment, component A comprises, preferably at least 80wt%, more preferably at least 90wt% zeolite, and even more preferably consists of zeolite.
[0054] Silicon dioxide (SiO2) of component A of the catalyst precursor
[0055] In the case where component A comprises silicon dioxide, SiO according to the present invention can have any shape, size (diameter) and purity. In a preferred embodiment, the silicon dioxide comprises more than 75 wt% SiO, preferably more than 85 wt% SiO, more preferably more than 95 wt% SiO, and most preferably more than 98 wt% SiO.
[0056] Preferably, the silicon dioxide has a spherical shape. SiO2 spheres can be prepared by any method known in the art. For example, SiO2 spheres can be prepared by modified The method involves the ammonia-catalyzed hydrolysis and condensation of tetraethyl orthosilicate (TEOS) using ethanol as solvent and cetyltrimethylammonium bromide as a surfactant porogen, as is well known in the art.
[0057] Preferably, the SiO 2 spheres are SiO 2 spheres, wherein the average diameter of the SiO 2 spheres is between 100 nm and 1000 nm, preferably between 200 nm and 600 nm, more preferably between 300 nm and 550 nm.
[0058] Zeolite of component A of the catalyst precursor
[0059] Preferably, the zeolite of component A of the catalyst precursor of the present invention is selected from ZSM-5, X-zeolite, Y-zeolite, USY-zeolite, β-zeolite, MCM-22, ferrierite, chabazite and combinations thereof, more preferably selected from ZSM-5, X-zeolite, Y-zeolite, USY-zeolite and combinations thereof.
[0060] Preferably, the zeolite is present in the form of particles having an average diameter of at least 100 nm, preferably at least 300 nm, more preferably at least 500 nm.
[0061] In a preferred embodiment of the present invention, the zeolite has a silicon to aluminum (Si:Al) molar ratio of 1:1 to 5000:1, preferably 15:1 to 2000:1, more preferably 40:1 to 1500:1, and most preferably 250:1 to 1300:1.
[0062] Alumina of component A of the catalyst precursor
[0063] Alumina is a compound comprising aluminum and oxygen. Preferably, the aluminum oxide used in the present invention comprises aluminum-(III)-oxide (Al2O3), preferably consists of aluminum-(III)-oxide (Al2O3).
[0064] Alumina according to the present invention can have any shape, size (diameter) and purity. In a preferred embodiment, the alumina contains more than 75wt% Al2O3, preferably more than 85wt% Al2O3, more preferably more than 95wt% Al2O3, and most preferably more than 98wt% Al2O3.
[0065] Preferably, the aluminum oxide according to the present invention comprises, preferably consists of, Al2O3 having a spherical shape.
[0066] In a further preferred embodiment of the present invention, the aluminum oxide of the present invention is an Al2O3 sphere. The Al2O3 sphere can be prepared by any method known in the art.
[0067] Structure of catalyst precursor
[0068] The catalyst precursor according to the present invention comprises component A and component B pre , whereby component A and component B pre Can be structurally combined in a variety of ways. For example, component A can be combined with component B pre Physical mixing or component A can be made from component B pre support.
[0069] In a preferred embodiment of the present invention, the catalyst precursor has a core-shell structure, wherein the core-shell structure means that one component (core) is substantially or completely surrounded by another component (shell). In another explanation, the core-shell structure is defined as having an outer boundary of one component (shell) substantially or completely covering another component (core). Preferably, for the present invention, the core-shell structure has a core whose outer surface is at least 10%, more preferably at least 20%, and even more preferably at least 30% covered by the shell.
[0070] According to a preferred embodiment of the catalyst precursor of the present invention, the core comprises component A, preferably consists of component A, and the shell comprises component B pre , preferably composed of component B pre In another preferred embodiment of the present invention, the core consists of component A. In another preferred embodiment of the present invention, the shell consists of component B pre composition.
[0071] Preferably, the catalyst precursor of the present invention is present as particles, the primary particle size (average diameter) of which is between 200 nm and 3000 nm, preferably between 300 nm and 2500 nm, more preferably between 400 nm and 2000 nm, as measured by transmission electron microscopy (TEM).
[0072] B. Catalyst
[0073] The present invention provides a catalyst for converting ethanol into 1,3-butadiene, comprising:
[0074] i) component A selected from zeolite, silica, alumina or any combination thereof; and
[0075] ii) Component B comprising mixed metal oxides cat .
[0076] Catalyst component B cat
[0077] In a preferred embodiment, component B catContains at least 70 wt% of mixed metal oxides, preferably at least 80 wt% of mixed metal oxides, more preferably at least 90 wt% of mixed metal oxides. In a more preferred embodiment, component B cat Composed of mixed metal oxides. In a most preferred embodiment, the mixed metal oxide is a layered double oxide (LDO).
[0078] Preferably, component A and component B cat The weight ratio of component A to component B is in the range of 1:0.05 to 1:2.5, more preferably in the range of 1:0.1 to 1:2.5, and even more preferably in the range of 1:0.15 to 1:2.5. cat The weight ratio of the catalyst balances the acid-base properties of the catalyst, thereby improving the yield and selectivity of converting ethanol to 1,3-butadiene using the catalyst of the present invention.
[0079] In a preferred embodiment, if the mixed metal oxide comprises LDO, preferably consists of LDO, then the LDO comprises a first metal DM and a second metal TM. The first metal DM is at least one monovalent metal cation, one divalent metal cation or a combination thereof. Preferably, the first metal DM is at least one divalent metal cation. Furthermore, the second metal TM is at least one trivalent metal cation, one tetravalent metal cation or a combination thereof. Preferably, the second metal TM is at least one trivalent metal cation.
[0080] Preferably, the molar ratio of the first metal DM to the second metal TM is in the range of 1: 1 to 10: 1, more preferably 2: 1 to 7: 1, and most preferably 2: 1 to 5: 1. In a preferred embodiment, the LDO has the same molar ratio of the first metal DM to the second metal DM as the LDH of the catalyst precursor from which the LDO of the catalyst is derived.
[0081] In a preferred embodiment, the first metal DM is selected from Li, Ca, Mg, Zn, Fe, Co, Cu and Ni and combinations thereof, preferably selected from Ca, Mg, Zn, Cu, Ni and combinations thereof, more preferably selected from Mg, Cu, Ni, Zn and combinations thereof. In a first most preferred embodiment, the first metal DM comprises Mg, preferably consists of Mg. In a second most preferred embodiment, the first metal DM comprises, preferably consists of a combination of Mg, Cu and Ni.
[0082] In embodiments where the first metal DM comprises, preferably consists of, a combination of Mg, Cu and Ni, preferably the molar ratio of Mg:Cu:Ni is in the range of 1-5:0.01-3:0.01-3, preferably 1.5-4.5:0.02-2.5:0.02-2.5, more preferably 1.8-4:0.02-1.5:0.02-1.5.
[0083] In a preferred embodiment, the second metal TM is selected from Al, Ga, In, Y, Fe, Co, Mn, Cr, Ti, V, La, Sn, Zr and combinations thereof, preferably selected from Al, Ga, In, Fe, Co, Sn, Zr and combinations thereof, more preferably selected from Al, Zr and combinations thereof. In a first most preferred embodiment, the second metal TM comprises Al, preferably consists of Al. In a second most preferred embodiment, the second metal TM comprises, preferably consists of a combination of Al and Zr.
[0084] In embodiments where the second metal TM comprises, preferably consists of, a combination of Al and Zr, the molar ratio of Al:Zr is in the range of 0.05-1.5:0.02-1.5, preferably 0.1-1.2:0.05-1.5 and more preferably 0.25-1.15:0.05-1.15.
[0085] In a specific embodiment, the first metal DM comprises, preferably consists of, Mg, and the second metal TM comprises, preferably consists of, a combination of Al and Zr.
[0086] In another specific embodiment, the first metal DM comprises, preferably consists of, Mg, Cu and Ni, and the second metal TM comprises, preferably consists of Al.
[0087] Preferably, the first metal DM and the second metal TM are selected from different metal cations.
[0088] In an alternative preferred embodiment, component B cat Further comprising an active metal deposited on the surface of the layered double hydroxide (LDO). For example, the deposited LDO can be obtained by impregnating the active metal on the LDO. The active metal is selected from Li, Ca, Zn, Fe, Co, Cu, Ni, Ga, In, Y, Fe, Co, Mn, Cr, Ti, V, La, Sn, Zr and combinations thereof, preferably Cu, Ni, Zr and combinations thereof.
[0089] In a preferred embodiment, the LDO of the catalyst has the same combination of first metal DM and second metal TM found in the LDH of the catalyst precursor from which the LDO of the catalyst is derived.
[0090] Catalyst component A
[0091] Component A is selected from zeolite, silica, alumina and combinations thereof. In a preferred embodiment, component A is selected from zeolite, silica and alumina. In another preferred embodiment, component A is selected from zeolite, silica and combinations thereof. In the first most preferred embodiment, component A comprises, preferably at least 80wt%, more preferably at least 90wt% silica, and even more preferably consists of silica. In the second most preferred embodiment, component A comprises, preferably at least 80wt%, more preferably at least 90wt% zeolite, and even more preferably consists of zeolite. Preferably, component A of the catalyst is the same as component A of the catalyst precursor.
[0092] Component A of the catalyst: silicon dioxide (SiO2)
[0093] In the case where component A comprises silicon dioxide, SiO according to the present invention can have any shape, size (diameter) and purity. In a preferred embodiment, the silicon dioxide comprises more than 75 wt% SiO, preferably more than 85 wt% SiO, more preferably more than 95 wt% SiO, and most preferably more than 98 wt% SiO.
[0094] Preferably, the silicon dioxide has a spherical shape. SiO2 spheres can be prepared by any method known in the art. For example, SiO2 spheres can be prepared by modified The method comprises the ammonia catalyzed hydrolysis and condensation of tetraethyl orthosilicate (TEOS) using ethanol as solvent and cetyltrimethylammonium bromide as surfactant porogen, as is well known in the art.
[0095] Preferably, the SiO 2 spheres are SiO 2 spheres, wherein the average diameter of the SiO 2 spheres is between 100 nm and 1000 nm, preferably between 200 nm and 600 nm, more preferably between 300 nm and 550 nm.
[0096] Zeolite of component A of the catalyst
[0097] Preferably, the zeolite of component A of the catalyst of the present invention is selected from ZSM-5, X-zeolite, Y-zeolite, USY-zeolite, β-zeolite, MCM-22, ferrierite, chabazite and combinations thereof, more preferably selected from ZSM-5, X-zeolite, Y-zeolite, USY-zeolite and combinations thereof.
[0098] Preferably, the zeolite is present as particles having an average diameter of at least 100 nm, preferably at least 300 nm, more preferably at least 500 nm.
[0099] In a preferred embodiment of the present invention, the zeolite has a silicon to aluminum (Si:Al) molar ratio of 1:1 to 5000:1, preferably 15:1:1 to 2000:1, more preferably 40:1 to 1500:1, most preferably 250:1 to 1300:1.
[0100] Alumina of component A of the catalyst
[0101] Alumina is a compound comprising aluminum and oxygen. Preferably, the aluminum oxide used in the present invention comprises aluminum-(III)-oxide (Al2O3), preferably consists of aluminum-(III)-oxide (Al2O3).
[0102] Alumina according to the present invention can have any shape, size (diameter) and purity. In a preferred embodiment, the alumina contains more than 75wt% Al2O3, preferably more than 85wt% Al2O3, more preferably more than 95wt% Al2O3, and most preferably more than 98wt% Al2O3.
[0103] Preferably, the aluminum oxide according to the present invention comprises, preferably consists of, Al2O3 having a spherical shape.
[0104] In a further preferred embodiment of the present invention, the aluminum oxide of the present invention is an Al2O3 sphere. The Al2O3 sphere can be prepared by any method known in the art.
[0105] Catalyst structure
[0106] The catalyst according to the invention comprises component A and component B cat , where component A and component B cat Can be structurally combined in a variety of ways. For example, component A can be combined with component B cat Physical mixing or component A can be made from component B cat support.
[0107] In a preferred embodiment of the present invention, the catalyst has a core-shell structure, wherein the core-shell structure means that one component (core) is surrounded by another component (shell). In another explanation, the core-shell structure is defined as having one component (shell) substantially or completely covering the outer boundary of another component (core). Preferably, for the present invention, the core-shell structure has a core whose outer surface is at least 10%, more preferably at least 20%, and even more preferably at least 30% covered by the shell.
[0108] According to a preferred embodiment of the catalyst of the present invention, the core comprises component A, preferably consists of component A, and the shell comprises component B cat , preferably composed of component B catIn another preferred embodiment of the present invention, the core consists of component A. In yet another preferred embodiment of the present invention, the shell consists of component B. cat composition.
[0109] Preferably, the catalyst of the present invention is present as particles having a primary particle size (average diameter) of 200 nm to 3000 nm, preferably 300 nm to 2500 nm, more preferably 400 nm to 2000 nm, as measured by transmission electron microscopy (TEM).
[0110] C. Preparation of Catalyst Precursor
[0111] The catalyst precursor of the present invention can be prepared by a coprecipitation method to form a preferred core-shell structure. The coprecipitation method comprises the following steps:
[0112] a) by mixing component A with i) a solution containing an anionic salt, ii) a solution containing a metal ion (preferably component B) pre metal ions DM and TM) an aqueous solution of a metal precursor and iii) a base to prepare a suspension,
[0113] b) filtering the solid compound from the suspension obtained in step a), and washing the solid compound with deionized water to obtain a wet cake, and
[0114] c) drying the wet cake of solid compound obtained from step b).
[0115] For example, to obtain a core-shell structure (wherein the core comprises component A and the shell comprises component B pre ), the following method can be used. Component A is dispersed as a powder in deionized water using ultrasonic treatment. Subsequently, anionic salt Na2CO3 is added under further ultrasonic treatment. Then, component B is added under vigorous stirring. pre The aqueous solution of metal precursors of metal ions DM and TM is added to a mixture of deionized water, component A and Na2CO3, while the pH value of the mixture is maintained at pH 10 by adding NaOH at a temperature of about 25°C. The obtained suspension is then filtered using vacuum filtration, and the obtained solid compound is washed with deionized water until pH 7 is reached. The solid compound will then exist in the form of a wet cake. The wet cake of the solid compound is then heated and dried overnight at a temperature of at least 80°C to obtain a dry powder of the catalyst precursor according to the present invention having a core-shell structure.
[0116] D. Preparation of Catalyst
[0117] The core-shell structure of the catalyst according to the present invention can be prepared by a method comprising homogeneous coprecipitation. In a preferred embodiment, LDH is precipitated on component A. Therefore, the first step of the method for preparing the catalyst according to the present invention can include the preparation of the catalyst precursor according to the present invention.
[0118] Therefore, preferably, the catalyst according to the present invention is preferably prepared by the preparation of a catalyst precursor and an additional calcination step. cat The mixed metal oxide, preferably LDO, found in the catalyst precursor is preferably prepared by calcining component B as in pre It is derived from LDH found in
[0119] Therefore, the preparation method of the catalyst comprises the coprecipitation method of the catalyst precursor according to the present invention, comprising steps a) to c), and component B pre Component B in the catalyst cat , further comprising a calcination step d), preferably performed after step c).
[0120] In a preferred embodiment, the calcination step d) of the catalyst preparation process is carried out at a temperature between 300 and 700 °C, preferably 400 and 600 °C, more preferably 450 and 550 °C.
[0121] In an even more preferred embodiment of the present invention, the calcination step d) of the catalyst preparation process is carried out for at least 1 h, preferably at least 2 h, more preferably at least 3 h. Preferably, the calcination step d) is carried out for 1 h to 6 h, more preferably 2 h to 5.5 h.
[0122] Most preferably, the calcination step d) is carried out at a temperature between 450°C and 550°C for at least 2h.
[0123] The core-shell structure of the catalyst according to the present invention can be demonstrated by scanning electron microscopy (SEM), transmission electron microscopy (TEM) and X-ray powder diffraction (XRD).
[0124] It has been found that the core-shell structure of the catalyst of the invention consists of layers of active components which are exposed in sequence.
[0125] In one embodiment, the method for preparing the catalyst according to the present invention may further include step e) of molding the catalyst powder into a shape suitable for a commercial reactor. Step e) may be performed before or after step d). Preferably, step e) is performed before step d) and after step c).
[0126] Shapes suitable for commercial reactors may include pellets, extrudates, spheres, etc. Sufficient binder material may be further added to the ethanol conversion catalyst composition to facilitate the shaping of the catalyst. Providing a catalyst in a specific shape facilitates its use.
[0127] In one embodiment, the catalyst according to the invention has a specific surface area of at least 50 m 2 / g, preferably at least 100m 2 / g, more preferably at least 150m 2 / g, even more preferably at least 200m 2 Preferably, the specific surface area of the catalyst according to the present invention is less than 700 m 2 / g, more preferably less than 600m 2 / g, most preferably less than 500m 2 The specific surface area is measured after calcination by using Brunauer-Emmett-Teller (BET) surface area analysis.
[0128] In a particularly preferred embodiment of the present invention, the catalyst has a core-shell structure, with the core comprising component A, preferably consisting of component A, and the shell comprising component B. cat , preferably composed of component B cat The specific surface area of the catalyst is at least 50 m 2 / g and less than 700m 2 / g, wherein the specific surface area is preferably measured after calcination.
[0129] In a preferred embodiment, the shell of the core-shell ethanol conversion catalyst has a thickness greater than 5 nm, preferably greater than 10 nm, more preferably greater than 20 nm, preferably the thickness is measured after calcination.
[0130] E. Conversion of ethanol to 1,3-butadiene
[0131] The method for producing 1,3-butadiene comprises contacting an ethanol stream with a catalyst according to the present invention, whereby the method can be operated under a wide range of operating conditions. However, a specific range of operating conditions can improve the production efficiency of 1,3-butadiene.
[0132] In a preferred embodiment, the process is carried out at a temperature in the range of 250°C to 500°C, preferably in the range of 300°C to 500°C, more preferably in the range of 320°C to 450°C.
[0133] In another preferred embodiment, the process for producing 1,3-butadiene from ethanol is carried out at atmospheric pressure.
[0134] The contact time required to obtain a desired yield of 1,3-butadiene product depends on several factors, such as operating temperature, operating pressure and catalyst activity.
[0135] In a preferred embodiment, the method is carried out in 0.1h -1 Up to 40h -1 In the range, preferably in 0.3h -1 Until 20h -1 In the range of 0.5h -1 Until 10h -1 The reaction was carried out at a weight hourly space velocity (WHSV) within a certain range.
[0136] The method can be carried out batchwise or continuously. For commercial scale, it is advantageous to use a fixed bed to operate the method continuously. Particularly preferably, the method is carried out continuously in a one-step process and / or a single-stage reactor.
[0137] The catalytic activity of the catalyst used in the process for producing 1,3-butadiene is preferably at least 0.1 g 1,3-BD g cat -1 h -1 , more preferably 0.2g 1,3-BD g cat -1 h -1 , most preferably 0.3g 1,3-BD g cat -1 h -1 Furthermore, the catalytic activity of the catalyst used in the method for producing 1,3-butadiene is preferably not more than 10 g 1,3-BD g cat -1 h -1 .
[0138] The product stream obtained by the process for producing 1,3-butadiene preferably comprises at least 12 wt% 1,3-butadiene, more preferably at least 15 wt% 1,3-butadiene, and most preferably at least 20 wt% 1,3-butadiene. In addition, the product stream obtained by the process for producing 1,3-butadiene preferably may comprise no more than 95 wt% 1,3-butadiene.
[0139] The product stream obtained by the process for producing 1,3-butadiene preferably comprises no more than 20 wt% ethylene, more preferably no more than 15 wt% ethylene. Furthermore, the product stream obtained by the process for producing 1,3-butadiene preferably may comprise at least 0.1 wt% ethylene.
[0140] In a particularly preferred embodiment, the process for converting ethanol to 1,3-butadiene is carried out by contacting an ethanol feed stream with a catalyst according to the present invention at a temperature of 320° C. to 400° C., atmospheric pressure and a WHSV of 1.55 h -1 under the reaction conditions.
[0141] The ethanol feed stream of the process according to the invention can be of any purity. In a preferred embodiment, the ethanol feed stream comprises more than 75 wt% ethanol, preferably more than 85 wt% ethanol, more preferably more than 95 wt% ethanol, and most preferably more than 98 wt% ethanol.
[0142] After contacting the catalyst of the present invention with the ethanol feed stream under the operating conditions discussed, some harmful substances and coke may be deposited on the surface of the catalyst. This usually affects the activity of the catalyst, causing it to gradually decrease over time. The spent catalyst can be appropriately regenerated to restore at least some of its activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0143] Figure 1 :XRD patterns of pure SiO2 and core-shell SiO2-Mg3Al-CO3 LDH(IE1)
[0144] Figure 2 :SEM and TEM images of SiO2 spheres
[0145] Figure 3 : TEM image of zeolite ZA
[0146] Figure 4 :SEM and TEM images of core-shell SiO2-Mg3Al-LDH(IE1) with SiO2 spheres as core
[0147] Figure 5 :SEM and TEM images of core-shell zeolite ZA-Mg3Al-LDH(IE2) with zeolite ZA as core
[0148] Figure 1 The XRD patterns of pure SiO2 and core-shell SiO2-Mg3Al-CO3 LDH are shown. The image shows that the core-shell SiO2-Mg3Al-CO3 LDH sample was successfully synthesized because the characteristic peaks of Mg3Al-CO3 LDH can be observed, which are sharp and strong (003), (006), (009), (015), (018), (110) and (113) reflections at 2θ = 11.50°, 22.90°, 34.74°, 39.13°, 46.28°, 60.46° and 61.80°. SiO2 can be found at 2θ = 22.6°.
[0149] Figure 4 The SEM and TEM images of the core-shell SiO2-Mg3Al-LDH with SiO2 spheres as the core are shown. Figure 2 Shown is the formation of an LDH shell on a silica sphere core.
[0150] Figure 5 The SEM and TEM images of the core-shell zeolite ZA-Mg3Al-LDH with zeolite ZA as the core are shown. Figure 3 Shown is the formation of an LDH shell on a zeolite ZA core. DETAILED DESCRIPTION
[0151] Determination method
[0152] a) X-ray powder diffraction (XRD)
[0153] The X-ray powder diffraction (XRD) patterns of the samples were characterized using an X-ray powder diffractometer (RikaguTTRAX III) with a monochromator and Cu-Kα radiation at λ=0.15405 nm, with a 2θ range from 5° to 80°, a scanning speed of 3° / min, and a scanning step of 0.02°.
[0154] b) Scanning electron microscopy (SEM)
[0155] Scanning electron microscopy (SEM) analysis was performed on a JEOL JSM 6610 scanning electron microscope. The particles were dispersed in water and cast onto a clean silicon dioxide wafer. Energy dispersive X-ray spectroscopy (EDX), also performed on this instrument, was used to determine the relative amounts of constituent elements on the sample surface.
[0156] c) Transmission electron microscopy (TEM)
[0157] Transmission electron microscopy (TEM) analysis was performed on a JEOL 2100Plus microscope at an accelerating voltage of 200 kV. The particles were dispersed in water or ethanol using sonication and then cast onto a copper grid coated with a carbon film and then dried.
[0158] d) Gas chromatography (GC)
[0159] The gaseous products were analyzed by gas chromatography (Agilent Technologies 6890 Network GC system) using a HP-PLOT Al2O3 column (50 m×0.32 mm ID and 20 μm film thickness) equipped with a flame ionization detector (FID) to determine the hydrocarbon gases. The GC operating conditions were set as follows:
[0160] Initial temperature: 40°C (holding time 10 minutes)
[0161] Gradient 1:
[0162] Heating rate: 10℃ / min
[0163] Final temperature: 120°C and holding time 10 minutes
[0164] Gradient 2:
[0165] Heating rate: 5℃ / min
[0166] Final temperature: 180°C (holding time 10 minutes)
[0167] e) Gas chromatography-mass spectrometry, time of flight (GC-TOF)
[0168] Liquid products were analyzed using a gas chromatograph equipped with a time-of-flight mass spectrometer (GC×GC TOF / MS), Agilent 7890. Helium was used as a carrier gas and nitrogen was used for cooling the system. The conditions were set as follows:
[0169] Initial temperature: 40°C (holding time 2 minutes)
[0170] Heating rate: 2.5℃ / min
[0171] Final temperature: 250°C (holding time 5 minutes)
[0172] Split ratio: 1:25
[0173] Experimental Section
[0174] Material
[0175] ZA is a ZSM-5 zeolite having a Si:Al ratio of 250-700.
[0176] ZB is a ZSM-5 zeolite having a Si:Al ratio of 800-1300.
[0177] Comparative Example 1 (CE1): Mg3Al-CO3 LDH (chemical formula: Mg 0.75 Al 0.25 (OH)2(CO3) 0.125 )
[0178] Mg3Al-CO3 LDH was synthesized by adding 700 ml of an aqueous metal precursor solution containing 1.575 mol Mg(NO3)2·6H2O and 0.525 mol Al(NO3)3·9H2O to 700 ml of a solution of 0.315 mol Na2CO3. The pH of the resulting solution was controlled at pH 10 by adding 4 M NaOH dropwise under vigorous stirring. Subsequently, the resulting solution was aged at a temperature of about 25°C for 3 hours. After aging, the precipitated solid compound was filtered out of the solution and washed with deionized water until the filtrate pH = 7 was reached. Finally, the wet cake of the solid compound was dried in an oven at 110°C overnight. Comparative Example 1 represents an example of a Mg3Al-CO3LDH shell without a core.
[0179] Comparative Example 2 (CE2): Cu 0.5 Ni 0.2 Mg 2.3 Al-CO3 LDH (chemical formula: Cu 0.125 Ni 0.05 Mg 0.575 Al 0.25 (OH)2(CO3) 0.125 )
[0180] Cu 0.5 Ni 0.2 Mg 2.3 Al-CO3 LDH was synthesized by adding 700 ml of an aqueous metal precursor solution containing 1.208 mol Mg(NO3)2·6H2O, 0.2625 mol Cu(NO3)2·6H2O, 0.105 mol Ni(NO3)2·6H2O and 0.525 mol Al(NO3)3·9H2O to 700 ml of a solution of 0.315 mol Na2CO3. The pH of the resulting solution was controlled at pH 10 by adding 4 M NaOH dropwise under vigorous stirring. Subsequently, the resulting solution was aged at a temperature of about 25°C for 3 hours. After aging, the precipitated solid compound was filtered out of the solution and washed with deionized water until the filtrate pH = 7 was reached. Finally, the wet cake of the solid compound was dried in an oven at 80°C overnight. Comparative Example 2 represents a solid compound without a core and only Cu 0.5 Ni 0.2 Mg 2.3 Example of Al-CO3 LDH shell.
[0181] Inventive Example 1 (IE1): SiO2 core-Mg3Al-CO3 LDH shell (chemical formula: Mg 0.75 Al 0.25 (OH)2(CO3) 0.125 )
[0182] Spherical silica with a particle size of 500 nm was used as the core for the synthesis of IE1. IE1 was synthesized by a coprecipitation method as described below: 5 g of spherical silica was dispersed in 1000 ml of deionized water using ultrasonic treatment for 30 minutes. Subsequently, 27 mmol Na2CO3 was added and further treated by ultrasonic treatment for 5 minutes. Then, 1000 ml of an aqueous solution of a metal precursor containing 81 mmol Mg(NO3)2·6H2O and 27 mmol Al(NO3)3·9H2O ml was added to a mixture of deionized water, silica and Na2CO3 under vigorous stirring to obtain a suspension. The pH of the suspension was controlled at pH 10 by dropping 1 M NaOH. After aging for 120 minutes under stirring at a temperature of about 25°C, the obtained solid compound was filtered out of the suspension using vacuum filtration and washed with deionized water until the filtrate pH = 7 was reached. Finally, the wet cake of the solid compound was dried overnight at 110°C in an oven.
[0183] Inventive Example 2 (IE2): Zeolite ZA core-Mg3Al-CO3 LDH shell (chemical formula: Mg 0.75 Al 0.25 (OH)2(CO3) 0.125 )
[0184] IE2 was also synthesized using the coprecipitation method: 5 g of zeolite ZA was dispersed in 1000 ml of deionized water using ultrasonic treatment for 30 min. Subsequently, 27 mmol of Na2CO3 was added and further treated by ultrasonic treatment for 5 min. Then, 1000 ml of an aqueous metal precursor solution containing 81 mmol of Mg(NO3)2·6H2O and 27 mmol of Al(NO3)3·9H2O ml was added to the mixture of deionized water, zeolite ZA and Na2CO3 under vigorous stirring to obtain a suspension. The pH of the suspension was controlled at pH 10 by dropwise addition of 1 M NaOH. After aging with stirring at a temperature of about 25°C for 120 min, the obtained solid compound was filtered out of the suspension using vacuum filtration and washed with deionized water until the filtrate pH = 7 was reached. Finally, the wet cake of the solid compound was dried in an oven at 110°C overnight.
[0185] Inventive Example 3 (IE3): SiO2 Core-Mg3Al 0.9 Zr 0.1 -CO3 LDH shell (chemical formula Mg 0.75 Al 0.225 Zr 0.025 (OH)2(CO3) 0.125 )
[0186] Spherical silica with a particle size of 500 nm was used as the core for the synthesis of IE3. IE3 was synthesized again by coprecipitation: 5 g of spherical silica was dispersed in 1000 ml of deionized water using ultrasonic treatment for 30 minutes. Subsequently, 27 mmol Na2CO3 was added and further treated by ultrasonic treatment for 5 minutes. Then, 1000 ml of a metal precursor aqueous solution containing 81 mmol Mg(NO3)2·6H2O, 24.3 mmol Al(NO3)3·9H2O and 2.7 mmol ZrN2O7·9H2O was added to a mixture of deionized water, silica and Na2CO3 under vigorous stirring to obtain a suspension. The pH of the suspension was controlled at pH 10 by dropping 1 M NaOH. After stirring and aging for 120 minutes at a temperature of about 25°C, the obtained solid compound was filtered out from the suspension using vacuum filtration and washed with deionized water until the filtrate pH = 7 was reached. Finally, the wet cake of the solid compound was dried overnight at 80°C in an oven.
[0187] Inventive Example 4 (IE4) - Zeolite ZB Core - Cu 0.5 Ni 0.2 Mg 2.3 Al-CO3 LDH shell (chemical formula: Cu 0.125 Ni 0.05 Mg 0.575 Al 0.25 (OH)2(CO3) 0.125 )
[0188] IE4 was also synthesized by coprecipitation: 5 g of zeolite ZB was dispersed in 1000 ml of deionized water using ultrasonic treatment for 30 minutes. Subsequently, 27 mmol of Na2CO3 was added and further ultrasonicated for 5 minutes. Then, 1000 ml of a metal precursor aqueous solution containing 13.5 mmol of Cu(NO3)2·6H2O, 5.4 mmol of Ni(NO3)2·6H2O, 62.1 mmol of Mg(NO3)2·6H2O and 27 mmol of Al(NO3)3·9H2O was added to a mixture of deionized water, zeolite ZB and Na2CO3 under vigorous stirring to obtain a suspension. The pH of the suspension was controlled at pH 10 by dropwise addition of 1 M NaOH. After aging with stirring at a temperature of about 25°C for 120 minutes, the obtained solid compound was filtered out of the suspension using vacuum filtration and washed with deionized water until the filtrate pH = 7 was reached. Finally, the wet cake of the solid compound was dried overnight at 80°C in an oven.
[0189] Ethanol to 1,3-Butadiene
[0190] The catalyst precursors produced in CE1 to CE2 and IE1 to IE4 were calcined at 500°C to convert the LDH of the catalyst precursors into LDO, and then heated to 350°C, atmospheric pressure, and a weight hourly space velocity (WHSV) of 1.55 h -1 The reaction was carried out for 3 h (running time). The obtained products were divided into liquid products and gaseous products. The liquid products were analyzed using a gas chromatograph equipped with a time-of-flight mass spectrometer (GC×GC-TOF / MS). The gaseous products were analyzed by gas chromatography (Agilent Technologies 6890 Network GC system) using an HP-PLOT Al2O3 column (50 m×0.32 mm ID and 20 μm film thickness) equipped with a flame ionization detector (FID) to determine hydrocarbon gases.
[0191] The results of the conversion reaction of ethanol to 1,3-butadiene with a run time of 3 hours are shown in Table 1.
[0192] Table 1
[0193]
[0194] In Table 1, 1,3-butadiene yield % and catalyst activity after the reaction are key parameters indicating the catalyst performance.
[0195] The catalyst of CE1 consists of Mg and Al and does not contain component A (i.e., any core). Although the catalyst at least converts ethanol to 1,3-butadiene, it was found that the 1,3-butadiene yield and catalyst activity of CE1 were the lowest compared to CE2 and IE1 to IE4. Therefore, the catalyst composition of CE1 was used as the baseline for all remaining examples CE2 and IE1 to IE4. The catalyst of CE2 has improved performance compared to the catalyst of CE1. The LDH of CE2 includes Cu and Ni as well as Mg and Al. In addition, the catalyst of CE2 does not contain component A (i.e., any core). Compared to CE1, the 1,3-butadiene yield and catalyst activity are slightly increased.
[0196] The catalyst according to the invention according to IE1 to IE4 comprises component A and component B cat It was found that their 1,3-butadiene yield and catalyst activity were significantly increased compared with those of CE1 and CE2.
Claims
1. A catalyst for converting ethanol into 1,3-butadiene, comprising: i) component A selected from zeolite, silica, alumina or any combination thereof; and ii) Component B comprising mixed metal oxides cat , wherein the mixed metal oxide is a layered double oxide (LDO), wherein the layered double oxide (LDO) comprises a first metal DM and a second metal TM, Features The first metal DM includes a combination of Mg, Cu and Ni.
2. The catalyst according to claim 1, wherein Component A and Component B cat The weight ratio is in the range of 1:0.05 to 1:2.
5.
3. The catalyst according to claim 1, wherein The catalyst has a core-shell structure, wherein the core of the core-shell structure comprises component A and the shell of the core-shell structure comprises component B cat .
4. A catalyst precursor for preparing a catalyst for converting ethanol into 1,3-butadiene, comprising: i) component A selected from zeolite, silica, alumina or any combination thereof; and ii) Component B comprising a layered double hydroxide (LDH) pre , wherein the layered double hydroxide (LDH) comprises a first metal DM and a second metal TM, Features The first metal DM includes a combination of Mg, Cu and Ni.
5. The catalyst precursor according to claim 4, wherein Component A and Component B pre The weight ratio is in the range of 1:0.1 to 1:
5.
6. The catalyst precursor according to claim 4, wherein The catalyst precursor has a core-shell structure, wherein the core of the core-shell structure comprises component A and the shell of the core-shell structure comprises component B. pre .
7. The catalyst according to any one of claims 1 to 3 or the catalyst precursor according to any one of claims 4 to 6, wherein: The second metal TM is selected from Al, Ga, In, Y, Fe, Co, Mn, Cr, Ti, V, La, Sn, Zr and combinations thereof.
8. The catalyst according to any one of claims 1 to 3 or the catalyst precursor according to any one of claims 4 to 6, wherein: The second metal TM is selected from Al, Zr and a combination thereof.
9. The catalyst according to any one of claims 1 to 3 or the catalyst precursor according to any one of claims 4 to 6, wherein Component A is a zeolite selected from the group consisting of ZSM-5, X-zeolite, Y-zeolite, USY-zeolite, β-zeolite, MCM-22, ferrierite, chabazite, and combinations thereof.
10. The catalyst according to claim 9 or the catalyst precursor according to claim 9, wherein The zeolite has a molar ratio of Si to Al in the range of 1:1 to 5000:
1.
11. The catalyst according to any one of claims 1 to 3 and 10 or the catalyst precursor according to any one of claims 4 to 6 and 10, wherein The molar ratio of Mg:Cu:Ni is in the range of 1-5:0.01-3:0.01-3.
12. A process for producing 1,3-butadiene comprising contacting an ethanol stream with a catalyst according to any one of claims 1 to 3 and 7 to 11.
13. Use of the catalyst according to any one of claims 1 to 3 and 7 to 11 for converting ethanol into 1,3-butadiene.
14. Use of a catalyst precursor according to any one of claims 4 to 11 in the preparation of a catalyst for converting ethanol into 1,3-butadiene.