Method for making shielded gate trench device
Through thermal oxygen growth and argon ion implantation technology, combined with the use of high-density plasma liner layer and oxide dielectric filling layer, the problem of high-density plasma filling holes in low-voltage shielded gate trench devices is solved, and the filling process window is improved and device quality.
Patent Information
- Application Number
- CN202110779917.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-07-09
AI Technical Summary
Existing low-voltage shielded gate trench devices are prone to voids during high-density plasma filling, resulting in device defects, especially as the original cell size continues to shrink, the filling depth and aspect ratio is close to the limit of the existing process.
Using thermal oxygen growth technology and argon ion implantation, adjust the lattice structure of the source polycrystalline silicon, reduce the depth-to-width ratio of the critical opening of the trench, and grow the liner layer before filling with high-density plasma, and oxidation is formed by wet etching. The material medium fill layer improves the filling process window.
It effectively reduces the aspect ratio before HDP filling, avoids filling holes, improves the filling quality and reliability of the device, and enhances the adaptability of the process.
Smart Images

Figure CN113571419B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductors, and in particular relates to a method for manufacturing a shielded gate trench device. Background Art
[0002] In low voltage shielded gate trench devices, a high density plasma (HDP) oxide film layer 101 is usually used as a dielectric layer between gate polysilicon (Gate Poly) 102 and source polysilicon (Source Poly) 103. Usually, the shielded gate trench device has a process flow from filling the source polysilicon 103 to filling the HDP as follows: Figure 1 As shown in, it mainly includes:
[0003] Step ①, source polysilicon 103 is deposited;
[0004] Step ②, etching back the source polysilicon 103;
[0005] Step ③, removing the sidewall oxide film layer 105 of the trench 104;
[0006] Step ④, HDP liner growth;
[0007] Step ⑤, HDP filling.
[0008] Through the above process and subsequent process, we finally get Figure 2 The device structure of the prior art is shown.
[0009] The filling capability of HDP is related to the aspect ratio (AR ratio) of the trench structure during filling. The larger the AR ratio, the more difficult it is to fill. Small cell size shielded gate trench devices mean that the critical opening of the trench is reduced, so Figure 3 As shown in , HDP fills have a large depth-to-width ratio, such as Figure 1 As shown in ⑤, HDP filling voids 106 are likely to occur, causing defects in the device. As the size of the device's primitive cell continues to shrink, the HDP filling requirement has approached the limit of existing process capabilities, and the aspect ratio before HDP filling needs to be improved. Summary of the invention
[0010] The present invention aims to provide a method for manufacturing a shielded gate trench device in view of the technical problem that high-density plasma filling cavities easily occurs in the existing process, causing device defects.
[0011] A method for manufacturing a shielded gate trench device comprises the following steps in sequence:
[0012] Step S1, providing a substrate, a source sidewall dielectric layer is grown in an active area trench of an epitaxial layer on the substrate, and a source polysilicon is deposited in the source sidewall dielectric layer;
[0013] Step S2, etching back the source polysilicon;
[0014] Step S3, growing thermal oxide on the source polysilicon to form an oxide layer and removing part of the source sidewall dielectric layer and oxide to form an oxide dielectric thermal oxide layer;
[0015] Step S4, filling to form HDP oxide, and removing the upper HDP oxide to form an oxide dielectric filling layer.
[0016] In step S2, the source polysilicon is etched back, and after the back etching, the center depth of the active area trench: the height of the source polysilicon is 100:48-100:65, preferably 100:51-100:60, and more preferably 100:54.5.
[0017] Before step S3, ion implantation is performed on the source polysilicon after the back etching in step S2 to disperse the lattice structure of the source polysilicon.
[0018] The ion implantation is argon ion implantation.
[0019] The injection energy of the argon ion injection is 20KeV-100KeV, preferably 60KeV;
[0020] The dosage of the argon ion implantation is 1E+12-5E+12, and the preferred dosage is 2E+12.
[0021] In step S3, the source polysilicon is consumed when thermal oxygen is grown on the source polysilicon, so that the center depth of the active area trench: the height of the source polysilicon is 100:50.
[0022] In step S3, when growing thermal oxygen on the source polysilicon, the thermal oxygen is grown at 900° C.-1050° C., preferably at 950° C.
[0023] In step S3, the central depth of the active area trench: the thickness of a layer of oxide formed by growing thermal oxidation is 100:14.5-100:16.5, preferably 100:15-100:16, and more preferably 100:15.4.
[0024] In step S3, the source sidewall dielectric layer and the formed oxide dielectric thermal oxide layer are flush with each other.
[0025] In step S3, the ratio of the center depth of the active area trench to the thickness of the oxide dielectric thermal oxide layer is 100:8-100:10, preferably 100:8.5-100:9.5, and more preferably 100:9.1.
[0026] In step S3, etching is used to remove part of the source sidewall dielectric layer and oxide.
[0027] The etching is performed by wet etching.
[0028] In step S4, high density plasma is filled in the active area trench to form HDP oxide.
[0029] In step S4, the ratio of the center depth of the active area trench to the thickness of the formed oxide dielectric filling layer is 100:22.7-100:43.1, preferably 100:25-100:41, and more preferably 100:36.4.
[0030] In step S4, the filling depth-to-width ratio of the high-density plasma is 1.0-1.9, preferably 1.1-1.8, and more preferably 1.6.
[0031] In step S4, before filling the active area trench with high-density plasma, a high-density plasma liner layer is first grown in the active area trench.
[0032] The temperature range for growing the high-density plasma liner is 850° C.-1150° C., preferably 950° C.;
[0033] The thickness of the high density plasma liner layer is 200 Å-500 Å, preferably 300 Å.
[0034] In step S4, wet etching is used to remove the upper HDP oxide to form an oxide dielectric filling layer.
[0035] The positive progress of the present invention is that: the present invention adopts a method for manufacturing shielded gate trench devices, adds a thermal oxygen growth method on the basis of the original process, reduces the depth-to-width ratio before HDP filling, and combines argon ion implantation to greatly improve the filling process window. By improving the process flow, the depth-to-width ratio of the critical opening of the trench is reduced, and after filling the HDP, filling voids are avoided. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 A partial flow chart of manufacturing a shielded gate trench device in the prior art;
[0037] Figure 2 A cross-sectional structural diagram of a prior art device;
[0038] Figure 3This is a cross-sectional structure diagram before HDP filling in the prior art;
[0039] Figure 4 A partial flow chart of manufacturing a shielded gate trench device according to the present invention;
[0040] Figure 5 A cross-sectional structural diagram of a device finally obtained by the method for manufacturing a shielded gate trench device of the present invention;
[0041] Figure 6 This is a cross-sectional structural diagram of the present invention before HDP filling. DETAILED DESCRIPTION
[0042] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below with reference to specific illustrations.
[0043] Reference Figure 4 , a method for manufacturing a shielded gate trench device, comprising the following steps in sequence:
[0044] Step ①, source polysilicon deposition: a substrate is provided, a source sidewall dielectric layer 202 is grown in the active region trench 201 of the epitaxial layer on the substrate, and source polysilicon 203 is deposited in the source sidewall dielectric layer 202 .
[0045] This step adopts the same process flow as the prior art.
[0046] Step ②, source polysilicon etching back: source polysilicon 203 is etched back.
[0047] The source polysilicon 203 is etched back. The deposition and etching back thickness of the source polysilicon 203 can be determined according to the device requirements, and the following selection is preferably adopted. After etching back, the center depth of the active area trench 201: the height of the source polysilicon 203 is 100:48-100:65, preferably 100:51-100:60, and more preferably 100:54.5. Figure 4 As shown in ②, line segment AA is defined as the center depth of active area trench 201, and line segment BB is defined as the height of source polysilicon 203, then AA:BB=100:48-100:65, preferably AA:BB=100:51-100:60, and more preferably AA:BB=100:54.5.
[0048] Step ③, thermal oxygen growth: growing thermal oxygen on the source polysilicon 203 to form a layer of oxide 204 .
[0049] Before step ③, ion implantation is performed on the source polysilicon 203 after back etching in step ② to break up the lattice structure of the source polysilicon. The ion implantation is argon ion implantation. The implantation energy and dose of argon ion implantation affect the speed of thermal oxygen growth and the consumption of source polysilicon 203. The following specific parameters can be selected according to the device design requirements: the implantation energy of argon ion implantation is 20KeV-100KeV, and the preferred implantation energy is 60KeV; the dose of argon ion implantation is 1E+12-5E+12, and the preferred dose is 2E+12. The dose of 2E+12 means 2×10 12 / cm 2 .
[0050] In step ③, when thermal oxygen is grown on the source polysilicon 203, the source polysilicon is consumed, so that the center depth of the active area trench 201: the height of the source polysilicon 203 reaches 100:50.
[0051] In step ③, when growing thermal oxide on the source polysilicon 203, the thermal oxide is grown at 900°C-1050°C, preferably at 950°C.
[0052] In step ③, the depth of the center of the active area trench 201: the thickness of the oxide layer 204 formed by the growth of thermal oxidation is 100:14.5-100:16.5, preferably 100:15-100:16, and more preferably 100:15.4. Figure 4 As shown in ③, the line segment AA is defined as the center depth of the active area trench 201, and the line segment CC is defined as the thickness of the oxide 204, then AA:CC=100:14.5-100:16.5, preferably AA:CC=100:15-100:16, and more preferably AA:CC=100:15.4.
[0053] Step ④, removing part of the oxide: removing part of the source sidewall dielectric layer 202 and the oxide 204 to form an oxide dielectric thermal oxide layer 205.
[0054] In step ④, the source sidewall dielectric layer 202 and the formed oxide dielectric thermal oxide layer 205 are flush with each other.
[0055] In step ④, the center depth of the active area trench 201: the thickness of the oxide dielectric thermal oxide layer 205 is 100:8-100:10, preferably 100:8.5-100:9.5, and more preferably 100:9.1. Figure 4 As shown in ④, the line segment AA is defined as the center depth of the active area trench 201, and the line segment DD is defined as the thickness of the oxide dielectric thermal oxide layer 205, then AA:DD=100:8-100:10, preferably AA:DD=100:8.5-100:9.5, and more preferably AA:DD=100:9.1.
[0056] In step ④, etching is used to remove part of the source sidewall dielectric layer and oxide. The etching is performed by wet etching.
[0057] Step ⑤, HDP filling: filling to form HDP oxide 206, and removing the upper HDP oxide to form an oxide dielectric filling layer 207.
[0058] In this step, high density plasma is filled in the active region trench 201 to form HDP oxide 206. The filling depth-to-width ratio of the high density plasma filling is 1.0-1.9, preferably 1.1-1.8, and more preferably 1.6.
[0059] In this step, before high-density plasma is filled in the active region trench 201, a high-density plasma liner layer is first grown in the active region trench 201. The temperature range for growing the high-density plasma liner layer is 850° C.-1150° C., preferably 950° C.; the thickness of the high-density plasma liner layer is 200 Å-500 Å, preferably 300 Å.
[0060] In this step, the thickness of the oxide dielectric filling layer formed can be determined according to the device requirements, and is preferably selected as follows: The center depth of the active area trench 201: the thickness of the oxide dielectric filling layer 207 formed is 100:22.7-100:43.1, preferably 100:25-100:41, and more preferably 100:36.4. Figure 5 As shown, line segment AA is defined as the center depth of active area trench 201, and line segment EE is defined as the thickness of oxide dielectric filling layer 207, then AA:EE=100:22.7-100:43.1, preferably AA:EE=100:25-100:41, and more preferably AA:EE=100:36.4.
[0061] In this step, wet etching is used to remove the upper HDP oxide 206 to form Figure 5 The oxide dielectric filling layer 207 is shown in FIG.
[0062] In Example 1, when the center depth of the active area trench is 2.2 um and the critical opening of the trench is 0.5 um, the following HDP filling steps are adopted:
[0063] Step ①, providing a substrate, growing a source sidewall dielectric layer in an active region trench of an epitaxial layer on the substrate, and depositing source polysilicon in the source sidewall dielectric layer;
[0064] Step ②, the source polysilicon is etched back, and the height of the etched back source polysilicon is 0.8um;
[0065] Step ③, using 950°C to grow thermal oxide on the source polysilicon to form a 0.44um thick oxide layer, the source polysilicon is consumed during the growth of thermal oxide, so that the source polysilicon height is 1.0um;
[0066] Step ④, remove part of the source sidewall dielectric layer and oxide to form an oxide dielectric thermal oxide layer, the thickness of the oxide dielectric thermal oxide layer is 0.3um. At this time, the depth of the active area trench to be filled with high-density plasma is 0.7um, the critical opening of the trench is 0.5um, and the aspect ratio is 1.4.
[0067] Step ⑤, filling to form HDP oxide, and removing the upper HDP oxide to form an oxide dielectric filling layer, the thickness of the oxide dielectric filling layer is 0um.
[0068] In Example 2, when the center depth of the active area trench is 2.2 um and the critical opening of the trench is 0.5 um, the following HDP filling steps are adopted:
[0069] Step ①, providing a substrate, growing a source sidewall dielectric layer in an active region trench of an epitaxial layer on the substrate, and depositing source polysilicon in the source sidewall dielectric layer;
[0070] Step ②, the source polysilicon is etched back, and the height of the etched back source polysilicon is 0.92um;
[0071] Step ③, using 950°C conditions to grow thermal oxide on the source polysilicon to form a 0.19um oxide layer, the source polysilicon is consumed during the growth of thermal oxide, so that the source polysilicon height is 1.0um;
[0072] Step ④, remove part of the source sidewall dielectric layer and oxide to form an oxide dielectric thermal oxide layer, the thickness of the oxide dielectric thermal oxide layer is 0.05um. At this time, the depth of the active area trench to be filled with high-density plasma is 0.95um, the critical opening of the trench is 0.5um, and the aspect ratio is 1.9.
[0073] Step ⑤, filling to form HDP oxide, and removing the upper HDP oxide to form an oxide dielectric filling layer, the thickness of the oxide dielectric filling layer is 0.25um.
[0074] In Example 3, when the center depth of the active area trench is 2.2 um and the critical opening of the trench is 0.5 um, the following HDP filling steps are adopted:
[0075] Step ①, providing a substrate, growing a source sidewall dielectric layer in an active region trench of an epitaxial layer on the substrate, and depositing source polysilicon in the source sidewall dielectric layer;
[0076] Step ②, the source polysilicon is etched back, and the height of the etched back source polysilicon is 0.85um;
[0077] Step ③, using 950°C conditions to grow thermal oxide on the source polysilicon to form a 0.34um thick oxide layer, 0.15um thick source polysilicon is consumed during the growth of thermal oxide, so that the source polysilicon height is 1.0um;
[0078] Step ④, remove the source sidewall dielectric layer and 0.14um thick oxide in the active area trench to form an oxide dielectric thermal oxide layer with a thickness of 0.2um. At this time, the depth of high-density plasma to be filled in the active area trench is 0.8um, the critical opening of the trench is 0.5um, and the aspect ratio is 1.6.
[0079] Step ⑤, filling to form HDP oxide, and removing the upper HDP oxide to form an oxide dielectric filling layer, the thickness of the oxide dielectric filling layer is 0.1 um.
[0080] By Example 3, Figure 6 The active area trench structure before HDP filling is shown in the figure. At this time, the depth D (depth) of the active area trench that needs to be filled with high-density plasma is 0.8um, the critical opening W (width) of the trench is 0.5um, and the aspect ratio is 1.6. Figure 1 The active area trench obtained under the existing process flow is as follows: Figure 3 As shown in , the critical opening W of the trench before HDP filling is 0.5um, the depth D of the trench to be filled is 1.0um, and the aspect ratio is 2. Compared with the prior art, since the present invention adds step ③ before step ⑤ and accurately controls the process parameters, a smaller aspect ratio is obtained, which greatly improves the filling process window and avoids the occurrence of filling voids.
[0081] Reference Figure 5 The device finally obtained by the method of manufacturing the shielded gate trench device of the present invention has a two-layer structure in the dielectric layer between the source polysilicon 203 and the gate polysilicon 208, which are an oxide dielectric thermal oxide layer 205 and an oxide dielectric filling layer 207 from bottom to top, and the oxide dielectric thermal oxide layer 205 is located in the source sidewall dielectric layer 202.
[0082] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for manufacturing a shielded gate trench device, characterized in that: The steps are as follows: Step S1, providing a substrate, a source sidewall dielectric layer is grown in an active area trench of an epitaxial layer on the substrate, and a source polysilicon is deposited in the source sidewall dielectric layer; Step S2, etching back the source polysilicon; Step S3, growing thermal oxide on the source polysilicon to form an oxide layer and removing part of the source sidewall dielectric layer and oxide to form an oxide dielectric thermal oxide layer; In step S3, when growing thermal oxygen on the source polysilicon, the source polysilicon is consumed, so that the center depth of the active area trench: the height of the source polysilicon is 100:50; In step S3, the depth of the center of the active area trench: the thickness of a layer of oxide formed by growing thermal oxidation is 100:14.5-100:16.5; In step S3, the center depth of the active area trench: the thickness of the oxide dielectric thermal oxide layer is 100:8-100:10; In step S3, the source sidewall dielectric layer and the formed oxide dielectric thermal oxide layer are flush with each other; Step S4, filling to form HDP oxide, and removing the upper HDP oxide to form an oxide dielectric filling layer; In step S4, high-density plasma is filled in the active region trench to form HDP oxide, and the filling depth-to-width ratio of the high-density plasma is 1.0-1.
9.
2. The method according to claim 1, characterized in that In step S2, the source polysilicon is etched back, and after the back etching, the center depth of the active area trench: the height of the source polysilicon is 100:48-100:
65.
3. The method according to claim 2, characterized in that After back etching, the center depth of the active area trench: the height of the source polysilicon is 100:51-100:
60.
4. The method according to claim 3, characterized in that After back etching, the center depth of the active area trench: the height of the source polysilicon is 100:54.
5.
5. The method according to any one of claims 1 to 4, characterized in that Before step S3, ion implantation is performed on the source polysilicon after the back etching in step S2 to disperse the lattice structure of the source polysilicon.
6. The method according to claim 5, characterized in that The ion implantation is argon ion implantation.
7. The method according to claim 6, characterized in that The injection energy of the argon ion injection is 20KeV-100KeV; The dosage of the argon ion implantation is 1E+12-5E+12.
8. The method according to claim 7, characterized in that The implantation energy during the argon ion implantation is 60 KeV.
9. The method according to claim 7, characterized in that The dosage of the argon ion implantation is 2E+12.
10. The method according to claim 1, characterized in that In step S3, when growing thermal oxide on the source polysilicon, the thermal oxide is grown under the condition of 900° C.-1050° C.
11. The method according to claim 10, characterized in that When growing thermal oxide on the source polysilicon, the thermal oxide is grown under a condition of 950° C.
12. The method according to claim 1, characterized in that In step S3, the depth of the center of the active area trench: the thickness of a layer of oxide formed by growing thermal oxidation is 100:15-100:
16.
13. The method according to claim 12, characterized in that In step S3, the depth of the center of the active area trench: the thickness of a layer of oxide formed by growing thermal oxidation is 100:15.
4.
14. The method according to claim 1, wherein: In step S3, the ratio of the center depth of the active area trench to the thickness of the oxide dielectric thermal oxide layer is 100:8.5-100:9.
5.
15. The method according to claim 14, characterized in that In step S3, the central depth of the active area trench: the thickness of the oxide medium thermal oxide layer is 100:9.
1.
16. The method according to claim 1, wherein: In step S3, etching is used to remove part of the source sidewall dielectric layer and oxide.
17. The method according to claim 16, characterized in that The etching is performed by wet etching.
18. The method of claim 1, wherein: In step S4, the central depth of the active area trench: the thickness of the formed oxide dielectric filling layer is 100:22.7-100:43.
1.
19. The method according to claim 18, characterized in that In step S4, the ratio of the center depth of the active area trench to the thickness of the formed oxide dielectric filling layer is 100:25-100:
41.
20. The method of claim 19, wherein: In step S4, the central depth of the active area trench: the thickness of the formed oxide dielectric filling layer is 100:36.
4.
21. The method of claim 1, wherein: In step S4, the filling depth-to-width ratio of the high-density plasma is 1.1-1.
8.
22. The method according to claim 21, characterized in that In step S4, the filling depth-to-width ratio of the high-density plasma is 1.
6.
23. The method of claim 1, wherein: In step S4, before filling the active area trench with high-density plasma, a high-density plasma liner layer is first grown in the active area trench.
24. The method of claim 23, wherein: The temperature range for growing the high-density plasma liner is 850° C.-1150° C.; The thickness of the high density plasma liner layer growth is 200 Å-500 Å.
25. The method of claim 24, wherein: The temperature range for the growth of the high density plasma liner layer is 950°C.
26. The method of claim 24, wherein: The high density plasma liner layer was grown to a thickness of 300 Å.
27. The method of claim 1, wherein: In step S4, wet etching is used to remove the upper HDP oxide to form an oxide dielectric filling layer.