A polyurethane adhesive defect measurement method and system based on ultrasonic detection
Through ultrasonic detection method, the vertical wave straight probe and ultrasonic coupling agent are used to solve the problem that the internal defects of the polyurethane adhesive cannot be effectively detected in the prior art, and fast and accurate defect positioning and detection are achieved, which improves detection efficiency and safety .
Patent Information
- Application Number
- CN202110877053.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-07-31
AI Technical Summary
The existing non-destructive testing methods cannot effectively detect internal defects in polyurethane adhesives, and have problems such as high cost, slow speed, and harmful to the human body. It is difficult to detect and judge defects in the adhesive structure in a timely manner, which may lead to deterioration of mechanical properties and Overall failure.
Using ultrasonic detection method, ultrasonic signals are collected through vertical wave straight probes, the near field area length is calculated, ultrasonic coupling agent is used for detection, the defects of ultrasonic echo signal are judged, the distance of defects is calculated, and a polyurethane adhesive defect measurement is provided. Methods and systems, including digital ultrasonic flaw detectors, longitudinal wave straight probes and PC terminals, achieve fast and accurate defect positioning.
Accurate detection of defect locations in polyurethane materials. The equipment is light, low detection cost and high sensitivity. It can quickly and accurately detect defects in polyurethane materials, avoid misjudgment and missed inspection, and improve the bonding structure. Inspection efficiency and safety.
Smart Images

Figure CN113671039B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polyurethane adhesive defect measurement method and system based on ultrasonic detection, belonging to the technical field of non-destructive detection. Background Art
[0002] Adhesive connection has the advantages of simple structure, light weight, small size and good processability, and is widely used in industrial production and life. Polyurethane adhesive has become one of the most commonly used adhesives due to its high strength, strong wear resistance, low temperature resistance, oil resistance and chemical corrosion resistance.
[0003] During the production process, adhesive bonding structures may have defects such as lack of adhesive, contamination of the bonding surface, incomplete curing and partial bonding; during the service process, problems such as aging, cracking, adhesion failure and cohesive failure may occur, thereby destroying the integrity of the adhesive structure. In adhesive bonding structures, interface debonding defects pose the greatest hidden danger. These defects in adhesive bonding structures will seriously reduce the bonding strength. Under the action of external forces, there are residual stresses in the interface and the influence of the use environment. The mechanical properties of the adhesive structure will deteriorate and may eventually lead to overall failure. If these defects are not discovered in time and the harmfulness of the defects cannot be accurately judged, huge losses will be incurred.
[0004] At present, the non-destructive testing methods commonly used to detect bonded structures are: infrared thermal imaging, radiography, and penetration testing. Due to the high application cost of infrared thermal imaging and its sensitivity to external environmental factors such as temperature, it is subject to strict environmental factors in practical applications. The detection cost of radiography is high, the detection speed is slow, and it is harmful to the human body, so protective measures need to be taken. The penetration method can only be used to detect defects exposed on the surface of the workpiece by openings, and cannot detect hidden defects inside. Compared with the above detection methods, the ultrasonic detection method has been widely used due to its advantages such as light equipment, low detection cost, fast speed, strong penetration ability, accurate defect positioning, high sensitivity, harmlessness to the human body and the environment, a wide range of objects to be inspected, and convenient on-site use.
[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgement or any form of suggestion that the information constitutes the prior art already known to ordinary technicians in this field. Summary of the invention
[0006] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a polyurethane adhesive defect measurement method and system based on ultrasonic detection, which deeply analyzes the defect signals in the polyurethane material through ultrasonic non-destructive testing, thereby accurately detecting the defect location in the polyurethane material.
[0007] To achieve the above object, the present invention is implemented by adopting the following technical solutions:
[0008] On the one hand, the present invention provides a polyurethane adhesive defect measurement method based on ultrasonic detection, comprising the following steps:
[0009] S1: Select the longitudinal wave straight probe and ultrasonic parameters for detection, and calculate the length of the near field area according to the ultrasonic parameters;
[0010] S2: using a longitudinal wave straight probe to collect ultrasonic signals at multiple different positions of the polyurethane adhesive to be tested outside the near field area, wherein the surface of the polyurethane adhesive to be tested is coated with an ultrasonic coupling agent;
[0011] S3: Determine whether the ultrasonic echo signals collected at each position have defects;
[0012] S4: Acquire the arrival times t1 and t2 of the defect echo and the defect bottom wave corresponding to the defective ultrasonic echo signal, and the arrival times t1' and t2' of the initial wave and the bottom wave corresponding to the defect-free ultrasonic echo signal;
[0013] S5: Obtain the thickness of the polyurethane adhesive to be tested at each position, and calculate the distance T between the defective part of the polyurethane adhesive and the upper surface according to the thickness, and the arrival times t1, t2 and the arrival times t1', t2'.
[0014] Furthermore, step S1 also includes, before the detection begins, initializing the parameters of the ultrasonic signal acquisition device, wherein the initialization parameters include oscilloscope channel, detection mode, output pulse width, initial gain, sound path and working mode; and selecting a standard echo test block for calibration and adjusting the gain, so that the detection process can better distinguish defect signals.
[0015] Furthermore, the above working mode is selected as a single probe self-transmitting and self-receiving, and a one-transmitting and one-receiving method is adopted to collect ultrasonic signals.
[0016] Furthermore, when using the standard echo test block for calibration, the initial wave signal and the bottom wave signal of the standard echo test block are respectively overlapped with the 0th and 8th grids of the horizontal scale of the ultrasonic detector screen, and the gain is adjusted so that the amplitude of the echo signal reaches 60% of the vertical scale. This setting can make the scale where the signal appears appear on the screen as much as possible, and the waveform displayed on the screen at the same time is as complete as possible.
[0017] For the longitudinal wave sound field radiated by a circular disk wave source, a series of areas with maximum and minimum sound pressure appear near the wave source due to wave interference, which is called the near field of the ultrasonic field, also known as the Fresnel zone.
[0018] Considering that when measuring in the near field, the echo of a larger defect at the minimum sound pressure may be lower, while the echo of a smaller defect at the maximum sound pressure may be higher, this may cause misjudgment or even missed detection. Therefore, the present invention designs the wedge thickness of the longitudinal wave straight probe to avoid measuring in the near field during the detection process.
[0019] Therefore, in the method of the present invention, S1 also includes determining the wedge thickness of the longitudinal wave straight probe according to the length of the near field zone; S2 uses the longitudinal wave straight probe with the corresponding wedge thickness to collect ultrasonic signals.
[0020] Furthermore, the ultrasonic parameters include the wave source radius and the ultrasonic wavelength, and the calculation formula of the near field length is:
[0021]
[0022] Where N is the length of the near field, Rs is the radius of the wave source, and λ is the wavelength of the ultrasonic wave;
[0023] in:
[0024] Where C is the preset wave velocity and f is the frequency of the longitudinal wave straight probe.
[0025] Furthermore, before the detection, the present invention firstly evenly applies CG-98 ultrasonic coupling agent on the surface of the polyurethane adhesive to be detected. The coupling agent has good coupling performance, can effectively reduce the loss of ultrasonic sound energy, is easy to clean, is harmless to the human body, and does not pollute the environment.
[0026] Further, in step S3, the step of determining whether the ultrasonic echo signal collected at each position has a defect includes:
[0027] If the initial wave and bottom wave echoes in the collected ultrasonic echo signal are clearly visible, and there is no obvious defect echo signal, then the ultrasonic echo signal has no defects; if there is an obvious defect echo signal between the initial wave and the bottom wave of the collected ultrasonic echo signal, and the bottom wave signal is attenuated, then the ultrasonic echo signal has defects.
[0028] Further, in step S5, according to the thickness of the polyurethane adhesive to be tested at the ultrasonic echo signal acquisition point, as well as the arrival times t1, t2 and the arrival times t1', t2', the distance T between the defective part of the polyurethane adhesive and the upper surface is calculated, including:
[0029] Calculate the sound velocity C of ultrasonic wave in the polyurethane adhesive to be tested L , the formula is:
[0030]
[0031] Where, D is the thickness of the polyurethane adhesive to be tested at the point where the ultrasonic echo signal is collected;
[0032] Calculate the distance T between the defective part of the polyurethane adhesive and the upper surface using the following formula:
[0033]
[0034] On the other hand, the present invention provides a polyurethane adhesive defect measurement system based on the aforementioned polyurethane adhesive defect measurement method, which includes a digital ultrasonic flaw detector, a longitudinal wave straight probe, a polyurethane adhesive to be measured and a PC end; the longitudinal wave straight probe is connected to a wedge block whose thickness matches the length of the near field zone, and is connected to the digital ultrasonic flaw detector through a channel line; the digital ultrasonic flaw detector is connected to a PC end provided with a display unit.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. The present invention studies the sonic velocity characteristics of polyurethane adhesives. By analyzing the ultrasonic signals of polyurethane adhesives, the defect locations in polyurethane materials can be accurately and quickly detected.
[0037] 2. The ultrasonic detection method adopted in the present invention has light equipment, low detection cost, accurate defect positioning, high sensitivity, and a wide range of objects to be inspected. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is a schematic flow chart of an embodiment of the measuring method of the present invention;
[0039] Figure 2 It is the design drawing of the simulated specimen;
[0040] Figure 3 is a schematic diagram of the waveform obtained by measuring a defect-free ultrasonic signal;
[0041] Figure 4 It is a schematic diagram of the waveform obtained by measuring the defective ultrasonic signal. DETAILED DESCRIPTION
[0042] The present invention will be further described below in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.
[0043] Example 1
[0044] This embodiment introduces a polyurethane adhesive defect measurement method based on ultrasonic detection. Figure 1 , including the following steps:
[0045] S1: Select the longitudinal wave straight probe and ultrasonic parameters for detection, and calculate the length of the near field area according to the ultrasonic parameters;
[0046] S2: using a longitudinal wave straight probe to collect ultrasonic signals at multiple different positions of the polyurethane adhesive to be tested outside the near field area, wherein the surface of the polyurethane adhesive to be tested is coated with an ultrasonic coupling agent;
[0047] S3: Determine whether the ultrasonic echo signals collected at each position have defects;
[0048] S4: Acquire the arrival times t1 and t2 of the defect echo and the defect bottom wave corresponding to the defective ultrasonic echo signal, and the arrival times t1' and t2' of the initial wave and the bottom wave corresponding to the defect-free ultrasonic echo signal;
[0049] S5: Obtain the thickness of the polyurethane adhesive to be tested at each position, and calculate the distance T between the defective part of the polyurethane adhesive and the upper surface according to the thickness, and the arrival times t1, t2 and the arrival times t1', t2'.
[0050] By using this embodiment, the defect position of the polyurethane adhesive can be measured quickly and accurately.
[0051] Example 2
[0052] This embodiment specifically introduces a polyurethane adhesive defect measurement method based on ultrasonic detection based on the same inventive concept as that of Embodiment 1, and specifically involves the following contents.
[0053] S1. Preparation before testing
[0054] 1.1 Set the initialization parameters of the ultrasonic signal acquisition device, where the initialization parameters include oscilloscope channel, detection mode, output pulse width, initial gain, sound path and working mode; and select a standard echo test block for calibration and adjust the gain. This allows the detection process to better distinguish defect signals. The working mode can be selected as a single probe self-transmitting and self-receiving, using a one-transmitting and one-receiving method to collect ultrasonic signals.
[0055] When using the standard echo test block for calibration, make the initial wave signal and bottom wave signal of the standard echo test block coincide with the 0th and 8th grids of the horizontal scale of the ultrasonic detector screen respectively, and adjust the gain so that the amplitude of the echo signal reaches 60% of the vertical scale. This setting can make the scale where the signal appears appear on the screen as much as possible, and the waveform displayed on the screen at the same time is as complete as possible.
[0056] 1.2 Determination of near field area
[0057] Considering that when measuring in the near field, the echo of a larger defect at the minimum sound pressure may be lower, while the echo of a smaller defect at the maximum sound pressure may be higher, this may cause misjudgment or even missed detection. Therefore, this embodiment designs the wedge thickness of the longitudinal wave straight probe to avoid measurement in the near field during the detection process.
[0058] The length of the near field is determined by the wave source radius and the wavelength of the ultrasonic wave, and the calculation formula is:
[0059]
[0060] Where N is the length of the near field, Rs is the radius of the wave source, and λ is the wavelength of the ultrasonic wave;
[0061] in:
[0062] Where C is the preset wave velocity and f is the frequency of the longitudinal wave straight probe.
[0063] The thickness of the longitudinal wave straight probe wedge can be set to the length N of the near field zone.
[0064] 1.3 Surface treatment of polyurethane to be tested
[0065] Before testing, first evenly apply CG-98 ultrasonic coupling agent on the surface of the polyurethane adhesive to be tested. This coupling agent has good coupling performance, can effectively reduce the loss of ultrasonic sound energy, is easy to clean, is harmless to the human body, and does not pollute the environment.
[0066] S2, ultrasonic flaw detection and signal acquisition: a longitudinal wave straight probe with a wedge is used to collect ultrasonic signals at multiple different positions of the polyurethane adhesive to be tested outside the near field area.
[0067] S3, determine whether the ultrasonic echo signal collected at each position has defects: if the initial wave and the bottom wave echo in the collected ultrasonic echo signal are clearly visible, and there is no obvious defect echo signal, then the ultrasonic echo signal has no defects, as shown in 3; if the collected ultrasonic echo signal has obvious defect echo signals between the initial wave and the bottom wave, and the bottom wave signal is attenuated, then the ultrasonic echo signal has defects, as shown in Figure 4 shown.
[0068] S4, waveform parameter acquisition: obtain the arrival times t1 and t2 of the defect echo and defect bottom wave corresponding to the defective ultrasonic echo signal, and the arrival times t1' and t2' of the initial wave and bottom wave corresponding to the defect-free ultrasonic echo signal. The waveform parameters can be obtained by manual observation, or automatically obtained by the PC after connecting the digital ultrasonic flaw detector to the PC.
[0069] S5, defect location calculation
[0070] The thickness of the polyurethane adhesive to be tested at each position is obtained, and according to the thickness, the arrival time t1, t2 and the arrival time t1', t2', the distance T between the defective part of the polyurethane adhesive and the upper surface is calculated, specifically including:
[0071] Calculate the sound velocity C of ultrasonic wave in the polyurethane adhesive to be tested L , the formula is:
[0072]
[0073] Where, D is the thickness of the polyurethane adhesive to be tested at the point where the ultrasonic echo signal is collected;
[0074] Calculate the distance T between the defective part of the polyurethane adhesive and the upper surface using the following formula:
[0075]
[0076] Example 3
[0077] This embodiment introduces a polyurethane adhesive defect measurement system based on the polyurethane adhesive defect measurement method described in Example 1 or 2, which includes a digital ultrasonic flaw detector, a longitudinal wave straight probe, a polyurethane adhesive to be measured and a PC end; the longitudinal wave straight probe is connected to a wedge block whose thickness matches the length of the near field zone, and is connected to the digital ultrasonic flaw detector through a channel line; the digital ultrasonic flaw detector is connected to a PC end provided with a display unit.
[0078] The digital ultrasonic flaw detector is connected to the PC, transmits the waveform data to the PC, and displays it on the display unit. At the same time, the PC can automatically obtain the waveform parameter data, calculate the defect position and display the output.
[0079] In order to study the effectiveness of the measuring method of the present invention, a self-made polyurethane test block is used for illustration below.
[0080] Figure 2 The figure shows a homemade polyurethane material simulation test block. The size of the polyurethane test block is designed to be 90mm long, 6mm wide and 25mm high. The detection area is inside the polyurethane. At the same time, a rectangular debonding defect is set in the polyurethane. The glue is injected three times, as shown in the figure. Figure 1 From left to right, a rectangular defect is placed each time the glue is injected, and the defect placement depth h is set to 21mm, 10mm, and 4mm. Defects of different sizes are set for further verification, and the defect size is designed to be 1mm×1mm×2mm in length×width×height, 2mm×2mm×2mm, and 3mm×3mm×2mm.
[0081] Using the ultrasonic detection system of Example 3, the testing process is as follows:
[0082] Step 1: Ultrasonic detector selection and setup
[0083] The SF580 pulse reflection ultrasonic detector produced by Mitutoyo Company is selected to generate pulse ultrasonic waves and real-time echo signals.
[0084] According to the test block parameters, the ultrasonic detector parameters are set as follows:
[0085] Channel selection: 2 Detection mode: full wave detection
[0086] Pulse width: 40ns Initial gain: 60dB
[0087] Sound range: 30mm Working mode: Single probe self-transmitting and self-receiving
[0088] Step 2: Standard echo test block calibration
[0089] After the setup is completed, place the probe at a defect-free part of the test block, adjust the ultrasonic detector so that the initial wave signal and bottom wave signal of the standard echo coincide with the 0th and 8th grids of the horizontal scale on the ultrasonic detector screen respectively, and adjust the gain so that the amplitude of the echo signal reaches 60% of the longitudinal scale, at which time the gain is 65dB.
[0090] Step 3: Straight probe selection
[0091] According to the calculation formula of the near field length, a longitudinal wave straight probe with a frequency of 5 MHz and a probe diameter of 10 mm was selected and connected to the ultrasonic detector.
[0092] Step 4: Coupling
[0093] Apply CG-98 ultrasonic coupling agent evenly on the polyurethane interface
[0094] Step 5: Flaw detection and identification
[0095] In the conventional way, a longitudinal wave straight probe was used to collect ultrasonic signals in a one-time transmission and one-reception manner at the polyurethane interface coated with CG-98 ultrasonic coupling agent. Figure 3 The ultrasonic signal shown in the figure clearly shows the initial wave and bottom wave echo signals. At the same time, the probe is placed on the surface of the known pre-embedded defect test block, and the following is obtained: Figure 4 The defect ultrasonic signal is shown. The defect echo signal can be clearly seen between the initial wave signal and the bottom wave signal, and the bottom wave signal is attenuated.
[0096] According to the obtained defect-free ultrasonic signal and defective ultrasonic signal, combined with the formula:
[0097]
[0098]
[0099] The ultrasonic longitudinal wave velocity in the polyurethane binder can be calculated and the embedded defects in the polyurethane can be analyzed. The actual calculation results are basically consistent with the defect injection position.
[0100] In summary, the method of the present invention combines nondestructive testing with ultrasonic testing methods, and can better analyze the propagation conditions and propagation speed of ultrasonic waves in polyurethane adhesives, laying a foundation for the actual detection of debonding defects in the adhesive parts of vehicle windows.
[0101] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the enlightenment of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the purpose of the present invention and the claims, which all fall within the protection of the present invention.
Claims
1. A polyurethane adhesive defect measurement method based on ultrasonic detection, characterized in that: The steps include: S1: Select the longitudinal wave straight probe and ultrasonic parameters for detection, calculate the near field length according to the ultrasonic parameters, and determine the wedge thickness of the longitudinal wave straight probe according to the near field length; select the standard echo test block for calibration, adjust the gain so that the initial wave signal and the bottom wave signal of the standard echo test block coincide with the 0th and 8th grids of the horizontal scale of the ultrasonic detector screen respectively, and adjust the gain so that the amplitude of the echo signal reaches 60% of the longitudinal degree; S2: using a longitudinal wave straight probe with a corresponding wedge thickness to collect ultrasonic signals at multiple different positions of the polyurethane adhesive to be tested outside the near field, wherein the surface of the polyurethane adhesive to be tested is coated with an ultrasonic coupling agent; S3: Determine whether the ultrasonic echo signal collected at each position has defects: if the initial wave and the bottom wave echo in the collected ultrasonic echo signal are clearly visible, and there is no obvious defect echo signal, then the ultrasonic echo signal has no defects; if the collected ultrasonic echo signal has obvious defect echo signals between the initial wave and the bottom wave, and the bottom wave signal is attenuated, then the ultrasonic echo signal has defects; S4: Acquire the arrival times t1 and t2 of the defect echo and the defect bottom wave corresponding to the defective ultrasonic echo signal, and the arrival times t1' and t2' of the initial wave and the bottom wave corresponding to the defect-free ultrasonic echo signal; S5: Obtain the thickness of the polyurethane adhesive to be tested at each position, and calculate the distance T between the defective part of the polyurethane adhesive and the upper surface according to the thickness, and the arrival times t1, t2 and the arrival times t1', t2'.
2. The polyurethane adhesive defect measurement method according to claim 1, characterized in that: S1 also includes: Initialization parameters are set for the ultrasonic signal acquisition device, wherein the initialization parameters include oscilloscope channel, detection mode, output pulse width, initial gain, sound path and working mode.
3. The polyurethane adhesive defect measurement method according to claim 2, characterized in that: The working mode is set to single probe self-transmitting and self-receiving, and ultrasonic signals are collected in a one-transmit-one-receive method.
4. The polyurethane adhesive defect measurement method according to claim 1, characterized in that: The ultrasonic parameters include the wave source radius and the ultrasonic wavelength, and the calculation formula for the near field length is: Where N is the length of the near field, Rs is the radius of the wave source, and λ is the wavelength of the ultrasonic wave; in: Where C is the preset wave velocity and f is the frequency of the longitudinal wave straight probe.
5. The polyurethane adhesive defect measurement method according to claim 1, characterized in that: The surface of the polyurethane adhesive is evenly coated with CG-98 ultrasonic coupling agent.
6. The polyurethane adhesive defect measurement method according to claim 1, characterized in that: In step S5, the distance T between the defective part of the polyurethane adhesive and the upper surface is calculated according to the thickness of the polyurethane adhesive to be tested at the ultrasonic echo signal collection point, as well as the arrival times t1, t2 and the arrival times t1', t2', including: Calculate the sound velocity C of ultrasonic wave in the polyurethane adhesive to be tested L , the formula is: Where, D is the thickness of the polyurethane adhesive to be tested at the point where the ultrasonic echo signal is collected; Calculate the distance T between the defective part of the polyurethane adhesive and the upper surface using the following formula:
7. A polyurethane adhesive defect measurement system based on the polyurethane adhesive defect measurement method according to any one of claims 1 to 6, characterized in that: It includes a digital ultrasonic flaw detector, a longitudinal wave straight probe, a polyurethane adhesive to be tested and a PC terminal; the longitudinal wave straight probe is connected to a wedge block whose thickness matches the length of the near field zone and is connected to the digital ultrasonic flaw detector through a channel line; the digital ultrasonic flaw detector is connected to the PC terminal with a display unit.