Superconducting cavity prepared by mixing low-purity niobium and high-purity niobium and preparation method thereof
Patent Information
- Application Number
- CN202111054272.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-09
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-09-09
AI Technical Summary
Existing radio frequency superconducting cavities have deficiencies in terms of mechanical strength and engineering cost. High-purity niobium has high cost and poor mechanical properties. Low-purity niobium is expensive and has poor cavity performance when used on non-high-frequency surfaces.
A mixture of low-purity niobium and high-purity niobium is used to prepare the superconducting cavity. The high-frequency electromagnetic field distribution is determined through finite element analysis. High-purity niobium is used in the strong magnetic field area, and low-purity niobium is used in other areas. A combination of stamping, machining, ultrasonic cleaning, and chemical Cleaning and preparation using vacuum electron beam welding technology.
It reduces the project cost, improves the mechanical strength and stability of the cavity, and achieves a cost-effective balance.
Smart Images

Figure CN113677082B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a superconducting cavity prepared by mixing low-purity niobium and high-purity niobium and a preparation method thereof, and belongs to the field of particle accelerator processing and manufacturing. Background Art
[0002] The radio frequency resonant cavity is a key component of high-energy particle accelerators. The high-intensity electromagnetic field established in the resonant cavity by high-power microwaves (radio frequency) can accelerate or deflect charged particles. Compared with the room temperature resonant cavity made of oxygen-free copper, the radio frequency superconducting cavity made of superconducting materials and working at 2K or 4.2K has a higher quality factor and can increase the energy of particles within the same distance. The radio frequency superconducting resonant cavity is usually made of high-purity niobium (residual resistivity RRR>300, RRR is the ratio of resistance at 300K to resistance at 4.2K) through a series of stamping, machining, surface treatment, frequency control, welding, and weld grinding. High-purity niobium is expensive, about 4,500 yuan / kg, and its mechanical strength is low, with a yield strength of only about 50MPa at room temperature. Low-purity niobium (RRR~30) is cheap, about 2,000 yuan / kg, and has good mechanical strength, with a maximum of 125MPa at room temperature. In the current processing of superconducting cavities, all places in contact with the high-frequency surface are processed and welded with high-purity niobium. Only the processing of the reinforcement ribs that do not contact the high-frequency surface uses low-purity niobium. This processing scheme is costly and has poor mechanical properties of the cavity. In actual engineering operation, the limit of single cavity performance is not pursued, but the mechanical stability of the entire system is more valued. How to improve the mechanical strength of the existing RF superconducting resonant cavity and reduce the engineering cost is an urgent problem to be solved. Summary of the invention
[0003] In view of the above technical problems, the present invention provides a low-purity niobium-high-purity niobium mixed superconducting cavity and a preparation method thereof. The present invention prepares a superconducting cavity by mixing low-purity niobium and high-purity niobium. According to the high-frequency electromagnetic field distribution of the superconducting cavity, niobium materials of different purities are used at different positions to prepare it, thereby reducing the cost of the entire project and improving the mechanical stability of the cavity.
[0004] To achieve the above object, the present invention adopts the following technical solutions:
[0005] A low-purity niobium-high-purity niobium mixed superconducting cavity, comprising:
[0006] The low-purity niobium-high-purity niobium mixed superconducting cavity is preferably prepared by determining the geometric structure of the superconducting cavity, and then obtaining the high-frequency electromagnetic field distribution in the superconducting cavity through finite element analysis. During operation, the area where the cavity heats most seriously is the strong magnetic field area. High-purity niobium plates or rods are used in this area, while low-purity niobium plates or rods are used in other areas.
[0007] The low-purity niobium-high-purity niobium mixed superconducting cavity comprises:
[0008] The outer conductor is a hollow structure, wherein the first end of the outer conductor is fixed on the bottom plate, and two slots are provided near the first end of the outer conductor and are symmetrically arranged along the axial direction thereof, wherein a nose cone is installed in the slot, and a beam pipe is installed on the nose cone;
[0009] The inner conductor is also a hollow structure and is disposed in the cavity of the outer conductor. A drift tube is mounted on the first end of the inner conductor. The drift tube and the beam pipe are located on the same central axis.
[0010] The low-purity niobium-high-purity niobium mixed superconducting cavity is preferably a quarter-wavelength cavity, and the inner conductor is a high-purity niobium cavity.
[0011] The low-purity niobium-high-purity niobium mixed superconducting cavity is preferably composed of the outer conductor being a low-purity niobium cavity, the nose cone being a low-purity niobium nose cone, the beam pipe being a low-purity niobium beam pipe, and the drift tube being a low-purity niobium drift tube.
[0012] In the low-purity niobium-high-purity niobium mixed superconducting cavity, preferably, the second ends of the outer conductor and the inner conductor are equipped with end caps, and the two are connected through the end caps, and the end caps are provided with cleaning ports for cleaning the outer conductor and the inner conductor, and the end caps are high-purity niobium end caps, and the cleaning ports are high-purity niobium cleaning ports.
[0013] The low-purity niobium-high-purity niobium mixed superconducting cavity is preferably provided with a power coupling port on the bottom plate, and a signal extraction port is provided on the outer conductor for collecting signals in the outer conductor and the inner conductor, the power coupling port is a low-purity niobium coupling port, and the signal extraction port is a low-purity niobium port.
[0014] In the low-purity niobium-high-purity niobium mixed superconducting cavity, preferably, reinforcing ribs are arranged on the bottom plate to improve the mechanical strength of the bottom plate, the bottom plate is a low-purity niobium bottom plate, and the reinforcing ribs are low-purity niobium reinforcing ribs.
[0015] Based on the above-mentioned low-purity niobium-high-purity niobium mixed superconducting cavity preparation, the present invention also provides a method for preparing the superconducting cavity, comprising:
[0016] Use high-purity niobium materials with an RRR value greater than 300 to produce parts in the most heated area of the cavity through stamping dies or mechanical processing methods;
[0017] Use low-purity niobium material with an RRR value of 30 to produce parts in areas other than the most severely heated area of the cavity through stamping dies or mechanical processing methods;
[0018] Using an ultrasonic cleaning device to ultrasonically clean the parts processed in the above two steps;
[0019] Use a mixed acid consisting of hydrofluoric acid: nitric acid: phosphoric acid in a volume ratio of 1:1:2 to chemically clean the parts after ultrasonic cleaning. The acid temperature is controlled below 20° and the cleaning time is controlled within 10-40 minutes.
[0020] Use ultrapure water with a resistivity of not less than 18MΩ·cm to clean the parts after chemical cleaning, and dry them in a clean room better than Class 1000;
[0021] The parts dried in the clean room are welded using a vacuum electron beam welder to complete the manufacturing process.
[0022] Based on the above-mentioned low-purity niobium-high-purity niobium mixed superconducting cavity preparation, the present invention also provides a method for preparing a quarter-wave field superconducting cavity, comprising:
[0023] Using high-purity niobium material with an RRR value greater than 300, two semi-inner conductors and the end cap are manufactured by a stamping die;
[0024] High-purity niobium material with an RRR value greater than 300 is used to obtain four cleaning ports through a mechanical processing method;
[0025] Using low-purity niobium material with an RRR value of 30, two semi-outer conductors, two nose cones and one bottom plate are manufactured by a stamping die;
[0026] The beam pipe, the drift tube, the power coupling port, the signal extraction port and the reinforcing rib are obtained by a mechanical processing method using a low-purity niobium material with an RRR value of 30;
[0027] Using an ultrasonic cleaning device to ultrasonically clean the parts processed in the above four steps;
[0028] Use a mixed acid consisting of hydrofluoric acid: nitric acid: phosphoric acid in a volume ratio of 1:1:2 to chemically clean the parts after ultrasonic cleaning. The acid temperature is controlled below 20° and the cleaning time is controlled within 10-40 minutes.
[0029] Use ultrapure water with a resistivity of not less than 18MΩ·cm to clean the parts after chemical cleaning, and dry them in a clean room better than Class 1000;
[0030] The parts dried in the clean room are welded using a vacuum electron beam welder to complete the manufacturing process.
[0031] The method for preparing a superconducting cavity by mixing low-purity niobium and high-purity niobium is preferably to weld the parts dried in the clean room using a vacuum electron beam welder, and the specific steps are as follows:
[0032] Welding two semi-inner conductors into a complete inner conductor, and inserting the drift tube into the inner conductor and welding them into one body;
[0033] Welding two semi-outer conductors into a complete outer conductor, welding the two nose cones together with the corresponding beam pipes and flanges, and then welding them together with the outer conductor;
[0034] Welding the bottom plate to the outer conductor, and welding the reinforcing ribs, the power coupling port and the flange to the bottom plate;
[0035] splicing the inner conductor, the outer conductor and the end cap together, measuring the frequency of the cavity, and determining the trimming amount of the open ends of the inner conductor and the outer conductor according to the welding allowance and the target frequency;
[0036] The end cover is welded together with the inner conductor and the outer conductor, the cleaning port is welded to the end cover, and the corresponding flange and niobium-titanium alloy sheet are welded to the cleaning port.
[0037] In the method for preparing a superconducting cavity by mixing low-purity niobium and high-purity niobium, preferably, the weld seam of the welded parts in each of the above steps is polished, and the weld seam polishing includes mechanical polishing.
[0038] The present invention adopts the above technical solution, which has the following advantages:
[0039] 1. The present invention prepares a superconducting cavity by mixing low-purity niobium and high-purity niobium. According to the high-frequency electromagnetic field distribution of the superconducting cavity, niobium materials of different purities are used at different positions to prepare it, thereby reducing the cost of the entire project and improving the mechanical strength of the superconducting cavity.
[0040] 2. The present invention obtains the high-frequency electromagnetic field distribution in the superconducting cavity through finite element analysis. During operation, the area where the cavity heats the most is usually in the strong magnetic field area, so high-purity niobium is used in this part, and low-purity niobium is used in other areas, thereby reducing the cost of the entire cavity and improving the mechanical strength of the cavity. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 A three-dimensional schematic diagram of a superconducting cavity prepared by mixing low-purity niobium and high-purity niobium according to an embodiment of the present invention;
[0042] Figure 2 Multiple side views of the low-purity niobium-high-purity niobium mixed superconducting cavity provided in this embodiment of the present invention, wherein a is a side view and b is an internal view;
[0043] Figure 3 A schematic diagram of the distribution of the high-frequency electromagnetic field in the superconducting cavity prepared by mixing low-purity niobium and high-purity niobium provided in this embodiment of the present invention, and a distribution diagram of high-purity niobium and low-purity niobium in the superconducting cavity of the present invention, wherein a is an electric field contour distribution diagram, b is a magnetic field contour distribution diagram, and c is a distribution diagram of high-purity niobium and low-purity niobium in the superconducting cavity of the present invention;
[0044] Figure 4 Schematic diagram of explosion of preparing superconducting cavity by mixing low-purity niobium and high-purity niobium provided in this embodiment of the present invention;
[0045] The marks in the figure are as follows:
[0046] 1-outer conductor; 2-inner conductor; 3-end cap; 4-cleaning port; 5-bottom plate; 6-power coupling port; 7-reinforcement rib; 8-drift tube; 9-nose cone; 10-beam pipe; 11-signal extraction port. DETAILED DESCRIPTION
[0047] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary persons in the art without creative work are within the scope of protection of the present invention.
[0048] Unless otherwise defined, the technical or scientific terms used in the present invention shall have the usual meanings understood by persons with ordinary skills in the field to which the present invention belongs. The words "first", "second", "third", "fourth", "upper", "lower", "left and right" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect.
[0049] Finite element analysis refers to establishing a thin shell model of the RF resonant cavity (or an air body model in the cavity) in the finite element analysis software, setting the material properties of the model to niobium (or vacuum), defining the contact surface between the air body and the niobium shell as the electrical boundary, dividing the model into a finite number of small units, and using the eigenmode solver of the high-frequency analysis in the finite element analysis software to solve the electromagnetic field distribution of the cavity.
[0050] For a radio frequency resonant cavity of a certain shape, the spatial distribution of the electromagnetic field in the cavity is also determined. The high-frequency electromagnetic field in the cavity will generate high-frequency heat, which will be lost on the cavity wall, causing the temperature of the cavity wall to rise. For a superconducting cavity, when working, the superconducting cavity is immersed in liquid helium as a whole, and the high-frequency heat on the cavity wall is taken away by the liquid helium, so that the temperature of the entire cavity is kept below the superconducting transition temperature of niobium, so that the cavity can always maintain a superconducting state. If the high-frequency heat on the cavity wall cannot be taken away by liquid helium in time, the temperature on the cavity wall will rise accordingly. If the cavity wall temperature is higher than the superconducting transition temperature of the niobium material, it will cause the cavity to quench. The heat transfer efficiency of niobium material is closely related to its residual resistivity. Therefore, when processing superconducting cavities, high-purity niobium (RRR>300) is usually used. However, high-purity niobium is expensive and has low mechanical strength. Low-purity niobium (RRR~30) is cheap and has high mechanical strength, and is usually used for reinforcing ribs outside the cavity. In order to reduce the overall cost of a superconducting cavity and improve the mechanical strength of the cavity, the present application proposes a method for preparing a superconducting cavity by mixing high-purity niobium and low-purity niobium, that is, high-purity niobium is used in areas of the cavity where heat generation is more serious, and low-purity niobium is used in other areas.
[0051] The present invention provides a technical solution for preparing a superconducting cavity by mixing low-purity niobium and high-purity niobium, and describes the technical solution in detail by taking a quarter-wavelength accelerating cavity as an example.
[0052] In a preferred embodiment of the present invention, Figure 1 , 2 As shown, the quarter-wave cavity includes: an outer conductor 1, which is a hollow structure, the first end of the outer conductor 1 is fixed on the bottom plate 5, and two slots are symmetrically arranged along the axis of the outer conductor 1 near the first end of the outer conductor 1, a nose cone 9 is installed in the slot, and a beam pipe 10 is installed on the nose cone 9; an inner conductor 2, which is also a hollow structure, is arranged in the cavity of the outer conductor 1, the first end of the inner conductor 2 is equipped with a drift tube 8, the drift tube 8 and the beam pipe 10 are located on the same central axis, the second end of the outer conductor 1 is connected to the second end of the inner conductor 2 through an end cover 3, a cleaning port 4 is opened on the end cover 3, a power coupling port 6 is opened on the bottom plate 5, and a signal extraction port 11 is opened at the first end of the outer conductor 1 near the bottom plate 5.
[0053] In a preferred embodiment of the present invention, Figure 3 As shown, taking a quarter-wavelength superconducting cavity as an example, once the geometric structure of the cavity is determined, the high-frequency electromagnetic field distribution in the cavity is obtained by finite element analysis ( Figure 3As shown in Figures 3a and 3b, through finite element analysis, the maximum surface magnetic field value on the cavity wall can be obtained. We use 1 / 3 of the maximum magnetic field value (Bmax) as the boundary. High-purity niobium is used in areas where the surface field is greater than 1 / 3Bmax of the magnetic field, and low-purity niobium is used in areas where the surface magnetic field is less than 1 / 3Bmax. Other types of cavities can also be divided based on 1 / 3 of the maximum magnetic field value (Bmax) to select high-purity and low-purity niobium. During operation, the area where the cavity heats most severely is usually in the strong magnetic field area. Therefore, high-purity niobium is used in this part, and low-purity niobium is used in other areas, thereby reducing the cost of the entire cavity and improving the mechanical strength of the cavity.
[0054] In a preferred embodiment of the present invention, Figure 3 As shown in c, taking a quarter-wavelength superconducting cavity as an example, the inner conductor 2 is a high-purity niobium cavity.
[0055] In a preferred embodiment of the present invention, Figure 3 As shown in c, taking a quarter-wavelength superconducting cavity as an example, the outer conductor 1 is a low-purity niobium cavity, the nose cone 9 is a low-purity niobium nose cone, the beam pipe 10 is a low-purity niobium beam pipe, and the drift tube 8 is a low-purity niobium drift tube.
[0056] In a preferred embodiment of the present invention, Figure 1 , 2 As shown in FIG. 4 , the second ends of the outer conductor 1 and the inner conductor 2 are equipped with an end cap 3 , and a cleaning port 4 is provided on the end cap 3 for cleaning the outer conductor 1 and the inner conductor 2 . The end cap 3 and the cleaning port 4 are made of high-purity niobium.
[0057] In a preferred embodiment of the present invention, Figure 1 , 2 As shown in FIG. 4 , a power coupling port 6 is provided on the bottom plate 5, and a signal extraction port 11 is provided on the outer conductor 1 for extracting the signal in the cavity. The bottom plate 5, the power coupling port 6 and the signal extraction port 11 are made of low-purity niobium.
[0058] In a preferred embodiment of the present invention, Figure 1 , 2 As shown in Figures 4 and 5, a reinforcing rib 7 is provided on the bottom plate 5 to improve the mechanical strength of the bottom plate 5. The reinforcing rib 7 is made of low-purity niobium.
[0059] Based on the above-mentioned low-purity niobium-high-purity niobium mixed superconducting cavity preparation, the present invention also provides a method for preparing the superconducting cavity, comprising:
[0060] High-purity niobium material with an RRR value greater than 300 is used to produce two semi-inner conductors and an end cap 3 by a stamping die, wherein the two semi-inner conductors have a trimming margin at the connection with the end cap 3, and the die forming method includes but is not limited to stamping, spinning, hydraulic pressure, etc.;
[0061] High-purity niobium material with an RRR value greater than 300 is used to obtain four cleaning ports 4 through a mechanical processing method, and the mechanical processing method includes but is not limited to a CNC lathe, a wire cutting machine, a water cutting machine, a machining center, etc.; the cleaning port 4 is equipped with a niobium-titanium alloy flange and a niobium-titanium alloy disc;
[0062] Low-purity niobium material with an RRR value of about 30 is used to produce two semi-outer conductors, two nose cones 9, and a bottom plate 5 through a stamping die, wherein the two semi-outer conductors have a trimming margin at the connection with the end cover 3, and the forming method includes but is not limited to stamping, spinning, hydraulic pressure, etc.;
[0063] A low-purity niobium material with an RRR value of about 30 is used to obtain a beam pipe 10, a drift tube 8, a power coupling port 6, a signal extraction port 11 and a reinforcing rib 7 by a mechanical processing method, and the mechanical processing method includes but is not limited to a CNC lathe, a wire cutting, a water cutting, a machining center, etc.; a niobium-titanium alloy flange and a niobium-titanium alloy disc are assembled on the beam pipe 10, the power coupling port 6 and the signal extraction port 11;
[0064] Use an ultrasonic cleaning device to perform ultrasonic cleaning on the parts processed in the above four steps, and the cleaning time shall not be less than 40 minutes;
[0065] A mixed acid consisting of hydrofluoric acid (40wt%): nitric acid (68wt%): phosphoric acid (85wt%) = 1:1:2 is used to chemically clean the parts after ultrasonic cleaning, the acid solution temperature is controlled below 20°, and the cleaning time is controlled within 10-40 minutes;
[0066] Use ultrapure water with a resistivity of not less than 18MΩ·cm to clean the parts after chemical cleaning, and dry them in a clean room better than Class 1000;
[0067] The parts dried in the clean room are welded using a vacuum electron beam welder. The welding methods include but are not limited to electron beam welding, laser welding, etc.
[0068] The specific welding includes the following steps:
[0069] Weld the two semi-inner conductors into a complete inner conductor 2, and insert the central drift tube 8 into the inner conductor 2 and weld them into one;
[0070] The two semi-outer conductors are welded into a complete outer conductor 1, and the two nose cones 9 are welded together with the corresponding beam pipes 10 and flanges, and then welded together with the outer conductor 1 into one body;
[0071] The bottom plate 5 is welded to the outer conductor 1, and the reinforcing rib 7, the power coupling port 6 and the flange are welded to the bottom plate 5;
[0072] The complete inner conductor 2 and the outer conductor 1 and the end cap 5 are spliced together by the tooling, the frequency of the cavity is measured, and the trimming amount of the open ends of the inner and outer conductors is determined according to the welding allowance and the target frequency;
[0073] The end cover 3 is welded together with the inner conductor 2 and the outer conductor 1, the cleaning port 4 is welded to the end cover 3, and the corresponding flange and the niobium-titanium alloy sheet are welded to the cleaning port 4;
[0074] The weld seam of the welded parts in each step of the above welding process is polished, and the weld seam polishing includes but is not limited to mechanical polishing and the like.
[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A superconducting cavity prepared by mixing low-purity niobium and high-purity niobium, characterized in that: After the geometric structure of the superconducting cavity is determined, the high-frequency electromagnetic field distribution in the superconducting cavity is obtained by finite element analysis. During operation, the area where the cavity heats most seriously is the strong magnetic field area. High-purity niobium plates or rods are used in this area, while low-purity niobium plates or rods are used in other areas. The superconducting cavity comprises: An outer conductor (1) having a hollow structure, wherein a first end of the outer conductor (1) is fixed on a bottom plate (5), and two slots are provided near the first end of the outer conductor (1) and are symmetrically arranged along the axis thereof, wherein a nose cone (9) is installed in the slot, and a beam pipe (10) is installed on the nose cone (9); An inner conductor (2), which is also a hollow structure, is disposed in the cavity of the outer conductor (1); a drift tube (8) is mounted on a first end of the inner conductor (2); the drift tube (8) and the beam pipe (10) are located on the same central axis; The superconducting cavity is a quarter-wavelength cavity, and the inner conductor (2) is a high-purity niobium cavity; The outer conductor (1) is a low-purity niobium cavity, the nose cone (9) is a low-purity niobium nose cone, the beam pipe (10) is a low-purity niobium beam pipe, and the drift tube (8) is a low-purity niobium drift tube.
2. The low-purity niobium-high-purity niobium mixed superconducting cavity according to claim 1, characterized in that: The second ends of the outer conductor (1) and the inner conductor (2) are equipped with end caps (3), and the two are connected via the end caps (3). The end caps (3) are provided with cleaning ports (4) for cleaning the outer conductor (1) and the inner conductor (2). The end caps (3) are high-purity niobium end caps, and the cleaning ports (4) are high-purity niobium cleaning ports.
3. The low-purity niobium-high-purity niobium mixed superconducting cavity according to claim 2, characterized in that: The base plate (5) is provided with a power coupling port (6), and the outer conductor (1) is provided with a signal extraction port (11) for collecting signals in the outer conductor (1) and the inner conductor (2), the power coupling port (6) being a low-purity niobium coupling port, and the signal extraction port (11) being a low-purity niobium port.
4. The low-purity niobium-high-purity niobium mixed superconducting cavity according to claim 3, characterized in that: The bottom plate (5) is provided with reinforcing ribs (7) for improving the mechanical strength of the bottom plate (5); the bottom plate (5) is a low-purity niobium bottom plate, and the reinforcing ribs (7) are low-purity niobium reinforcing ribs.
5. A method for preparing a superconducting cavity by mixing low-purity niobium and high-purity niobium as claimed in claim 1, characterized in that: include: Use high-purity niobium materials with an RRR value greater than 300 to produce parts in the most heated area of the cavity through stamping dies or mechanical processing methods; Use low-purity niobium material with an RRR value of 30 to produce parts in areas other than the most severely heated area of the cavity through stamping dies or mechanical processing methods; Using an ultrasonic cleaning device to ultrasonically clean the parts processed in the above two steps; Using hydrofluoric acid: A mixed acid consisting of nitric acid and phosphoric acid in a volume ratio of 1:1:2 is used to chemically clean the parts after ultrasonic cleaning. The acid temperature is controlled below 20° and the cleaning time is controlled within 10-40 minutes. Use ultrapure water with a resistivity of not less than 18MΩ·cm to clean the parts after chemical cleaning, and dry them in a clean room better than Class 1000; The parts dried in the clean room are welded using a vacuum electron beam welder to complete the manufacturing process.
6. A method for preparing a superconducting cavity by mixing low-purity niobium and high-purity niobium as claimed in claim 4, characterized in that: include: Using high-purity niobium material with an RRR value greater than 300, two semi-inner conductors and the end cap (3) are manufactured by a stamping die; Using high-purity niobium material with an RRR value greater than 300, four cleaning ports (4) are obtained by mechanical processing; Using low-purity niobium material with an RRR value of 30, two semi-outer conductors, two nose cones (9) and one base plate (5) are manufactured by a stamping die; The beam pipe (10), the drift tube (8), the power coupling port (6), the signal extraction port (11) and the reinforcing rib (7) are obtained by a mechanical processing method using a low-purity niobium material with an RRR value of 30; Using an ultrasonic cleaning device to ultrasonically clean the parts processed in the above four steps; Using hydrofluoric acid: A mixed acid consisting of nitric acid and phosphoric acid in a volume ratio of 1:1:2 is used to chemically clean the parts after ultrasonic cleaning. The acid temperature is controlled below 20° and the cleaning time is controlled within 10-40 minutes. Use ultrapure water with a resistivity of not less than 18MΩ·cm to clean the parts after chemical cleaning, and dry them in a clean room better than Class 1000; The parts dried in the clean room are welded using a vacuum electron beam welder to complete the manufacturing process.
7. The method for preparing a superconducting cavity by mixing low-purity niobium and high-purity niobium according to claim 6, characterized in that: Use a vacuum electron beam welder to weld the parts dried in the clean room. The specific steps are as follows: Welding two semi-inner conductors into a complete inner conductor (2), and inserting the drift tube (8) into the inner conductor (2) and welding them into one piece; Welding two semi-outer conductors into a complete outer conductor (1), welding the two nose cones (9) together with the corresponding beam pipes (10) and flanges, and then welding them together with the outer conductor (1); Welding the bottom plate (5) onto the outer conductor (1), and welding the reinforcing rib (7), the power coupling port (6) and the flange onto the bottom plate (5); The inner conductor (2), the outer conductor (1) and the end cap (3) are spliced together, the frequency of the cavity is measured, and the trimming amount of the open ends of the inner conductor (2) and the outer conductor (1) is determined according to the welding allowance and the target frequency; The end cover (3) is welded together with the inner conductor (2) and the outer conductor (1), the cleaning port (4) is welded to the end cover (3), and the corresponding flange and niobium-titanium alloy sheet are welded to the cleaning port (4).
Citation Information
Patent Citations
Port member of superconductive acceleration cavity
CN103026801A
Superconducting cavity prepared by mixing low-purity niobium and high-purity niobium
CN215773681U