Thermally conductive pad and preparation method and application thereof

By controlling the crosslink density and the direction of freezing treatment in the preparation method of thermal conductivity gasket, the problems of shape integrity and thermal conductivity of thermal conductivity gaskets at high temperatures are solved, and efficient heat dissipation effect is achieved.

CN113698754BActive Publication Date: 2024-11-12NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202110808775.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-16
Publication Date
2024-11-12
Estimated Expiration
2041-07-16

AI Technical Summary

Technical Problem

The existing thermal conductivity gaskets are difficult to maintain their shape when the temperature is higher than the melting point of the phase change material, resulting in the overflow of the phase change material, limiting the increase in the thermal conductivity coefficient and unable to meet the growing heat dissipation needs.

Method used

By providing a preparation method, it includes mixing the phase change material, the thermally conductive filler and the matrix material in the presence of a crosslinking agent to form a preform at a first temperature and freezing treatment at a second temperature to make the thermally conductive filler axial direction The thermally conductive gasket surface is formed with the angle between 60 degrees and 90 degrees, and the cross-linking density of the bonded matrix is ​​controlled between 0.5% and 5%, ensuring the rotation and high-temperature retention of the thermally conductive filler.

Benefits of technology

It realizes excellent thermal conductivity and high-temperature shape retention of thermal gaskets, can maintain shape integrity at high temperatures, solves the problem of phase change material overflow, and is suitable for thermally conductive devices in electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113698754B_ABST
    Figure CN113698754B_ABST
Patent Text Reader

Abstract

The present invention relates to a thermally conductive gasket and a preparation method and application thereof. The preparation method comprises the following steps: providing raw materials, the raw materials comprising a phase change material, a thermally conductive filler, a matrix material and a cross-linking agent, wherein the ratio of the axial length to the radial length of the thermally conductive filler is greater than 1; at a first temperature, mixing the raw materials, the matrix material undergoes a curing cross-linking reaction in the presence of a cross-linking agent to form a matrix, and obtaining a preform, wherein the first temperature is greater than the melting point of the phase change material and less than the boiling point of the phase change material, and the cross-linking density of the matrix is ​​0.5%-5%; and at a second temperature, freezing the preform to obtain a thermally conductive gasket, wherein the second temperature is less than the melting point of the phase change material and the temperature difference reaches more than 30°C, and the angle between the axial direction of the thermally conductive filler in the thermally conductive gasket and the surface of the thermally conductive gasket is 60 degrees-90 degrees. The thermally conductive gasket obtained by the preparation method has excellent thermal conductivity and high-temperature conformability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electronic products, and in particular to a thermally conductive pad and a preparation method and application thereof. Background Art

[0002] As microelectronic devices become more and more integrated, heat dissipation becomes a key issue restricting the development of the industry. Thermal pads, as a key material for improving the thermal conductivity between heat sources and cold sources, are widely used in the electronic and electrical fields.

[0003] In order to improve the thermal conductivity of the thermal pad, the method of adding thermal conductive fillers and phase change materials is usually adopted. However, with the increase in the amount of thermal conductive fillers and phase change materials, when the thermal conductive pad is used, when the temperature is higher than the melting point of the phase change material, it is difficult to maintain the integrity of the shape, and the phase change material is easy to overflow. Therefore, the addition ratio of thermal conductive fillers and phase change materials is limited, and the thermal conductivity cannot be further improved, which cannot meet the growing heat dissipation needs. Summary of the invention

[0004] Based on this, it is necessary to provide a thermally conductive gasket and a preparation method and application thereof to address the above problems. The thermally conductive gasket prepared by the preparation method has excellent thermal conductivity and high-temperature conformal properties, and can be better used as a thermal conductive device in electronic products.

[0005] The method for preparing the thermally conductive pad provided by the present invention comprises the following steps:

[0006] Providing raw materials, the raw materials include phase change material, thermal conductive filler, matrix material and cross-linking agent, the ratio of the axial length to the radial length of the thermal conductive filler is greater than 1;

[0007] At a first temperature, the raw materials are mixed, and the matrix material undergoes a curing and crosslinking reaction in the presence of the crosslinking agent to form a matrix to obtain a preform, wherein the first temperature is greater than the melting point of the phase change material and less than the boiling point of the phase change material, and the crosslinking density of the matrix is ​​0.5%-5%; and

[0008] The preform is frozen at a second temperature to obtain a thermally conductive gasket, wherein the second temperature is lower than the melting point of the phase change material and the temperature difference is above 30°C, and the angle between the axial direction of the thermally conductive filler in the thermally conductive gasket and the surface of the thermally conductive gasket is 60-90 degrees.

[0009] In one embodiment, the preform has a thickness of 0.3 mm to 3 mm.

[0010] In one embodiment, the thermally conductive filler is selected from a rod-shaped thermally conductive filler, an ellipsoidal thermally conductive filler or a sheet-shaped thermally conductive filler.

[0011] In one embodiment, the particle size of the thermally conductive filler is 0.5 μm-500 μm.

[0012] In one embodiment, the mass fraction of the phase change material in the raw material is 45%-89%;

[0013] And / or, the mass fraction of the thermally conductive filler in the raw material is 5%-49%;

[0014] And / or, the mass fraction of the matrix material in the raw material is 5%-20%;

[0015] And / or, the mass fraction of the cross-linking agent in the raw material is 0.01%-16%.

[0016] In one embodiment, the temperature difference between the first temperature and the melting point of the phase change material is 10°C-20°C.

[0017] In one embodiment, the phase change material includes at least one of polyethylene glycol, polyvinyl alcohol, polypropylene alcohol, octadecyl or paraffin;

[0018] And / or, the thermally conductive filler includes at least one of carbon fiber, carbon nanotube, graphite, graphene, diamond, aluminum oxide, magnesium oxide, silicon oxide, boron nitride, aluminum nitride, copper or silver;

[0019] And / or, the matrix material includes at least one of silicone oil, silicone gel, acrylic acid, acrylic rubber, acrylic ester copolymer resin, ethylene-vinyl acetate copolymer resin, polyurethane rubber or polyvinyl ether resin;

[0020] And / or, the cross-linking agent includes at least one of N,N'-methylenebisacrylamide, hydrogenated silicone oil, dicumyl peroxide, benzoyl peroxide or di-tert-butyl peroxide.

[0021] In one embodiment, the raw material further includes an auxiliary agent, and the auxiliary agent includes at least one of an initiator, a platinum catalyst, a surface modifier, a rheology modifier or an antioxidant.

[0022] A thermally conductive gasket is prepared by the thermally conductive gasket preparation method as described above.

[0023] An application of the thermally conductive pad as described above in electronic products.

[0024] In the preparation method of the thermally conductive gasket of the present invention, the second temperature is lower than the melting point of the phase change material and the temperature difference reaches more than 30°C, so that the preform is rapidly frozen, so that the heat dissipation direction of the preform is perpendicular to the surface of the preform, and thus the solidification direction of the phase change material is perpendicular to the surface of the preform, so that the thermally conductive filler can rotate during the freezing process, and then the axial direction of the thermally conductive filler forms an angle of 60 degrees to 90 degrees with the thermally conductive gasket, and forms a heat conduction path together with the solidified phase change material, so that the thermally conductive gasket has excellent thermal conductivity. At the same time, the cross-linking density of the matrix of the thermally conductive gasket is between 0.5% and 5%, and the mechanical strength is moderate. On the one hand, it does not affect the rotation of the thermally conductive filler, and on the other hand, the prepared thermally conductive gasket has excellent high-temperature conformality, and can be better used as a thermal conductive device in electronic products. Even if the temperature is higher than the melting point of the phase change material, it can still maintain the integrity of the shape, solving the problem of phase change material overflow.

[0025] In addition, the preparation method of the present invention is simple and suitable for industrial production; and it has universal applicability, and thermally conductive gaskets with different properties can be obtained by adopting different types of thermally conductive fillers. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A schematic structural diagram of a preform according to an embodiment of the present invention;

[0027] Figure 2 A schematic structural diagram of a thermally conductive gasket according to an embodiment of the present invention.

[0028] In the figure, 10, thermal conductive filler; 20, phase change material; 30, substrate. DETAILED DESCRIPTION

[0029] The thermal conductive pad provided by the present invention and its preparation method and application will be further described below.

[0030] The method for preparing the thermally conductive pad provided by the present invention comprises the following steps:

[0031] S1, providing raw materials, the raw materials including phase change material 20, thermal conductive filler 10, matrix material and cross-linking agent, the ratio of the axial length to the radial length of the thermal conductive filler 10 is greater than 1;

[0032] S2, mixing the raw materials at a first temperature, allowing the matrix material to undergo a curing crosslinking reaction in the presence of a crosslinking agent to form a matrix, thereby obtaining a preform, wherein the first temperature is greater than the melting point of the phase change material and less than the boiling point of the phase change material, and the crosslinking density of the matrix is ​​0.5%-5%; and

[0033] S3, freezing the preform at a second temperature to obtain a thermally conductive gasket, wherein the second temperature is lower than the melting point of the phase change material and the temperature difference is above 30°C, and the angle between the axial direction of the thermally conductive filler 10 in the thermally conductive gasket and the surface of the thermally conductive gasket is 60 degrees to 90 degrees.

[0034] It should be noted that the crosslinking density is equal to the percentage of crosslinked structural units in the total structural units. For example, when the base material is acrylic acid and the crosslinking agent is N,N'-methylenebisacrylamide, the crosslinking density is equal to the percentage of the number of N,N'-methylenebisacrylamide molecules in the total number of N,N'-methylenebisacrylamide and acrylic acid molecules.

[0035] The preparation method of the thermally conductive gasket provided by the present invention, when the cross-linking density of the base 30 is less than 0.5%, the mechanical strength of the base 30 is too small, the high-temperature conformability of the thermally conductive gasket is insufficient, resulting in the thermally conductive gasket being unable to maintain structural integrity during application, and easily causing the phase change material 20 to overflow; when the cross-linking density of the base 30 of the thermally conductive gasket is greater than 5%, the mechanical strength of the base 30 is too large, which will hinder the rotation of the thermally conductive filler 10 during the freezing treatment process. Therefore, the cross-linking density of the base 30 of the present invention is between 0.5%-5%, and the mechanical strength is moderate. On the one hand, it does not affect the rotation of the thermally conductive filler 10, and on the other hand, the prepared thermally conductive gasket has excellent high-temperature conformability. Specifically, the present invention regulates the cross-linking density of the base 30 by the type and amount of the base material, the type of the cross-linking agent, and the amount of the two.

[0036] In one embodiment, in step S1, the matrix material includes a polymer material or a monomer of a polymer material. Specifically, the matrix material includes at least one of a thermosetting resin, a thermosetting resin monomer, rubber or a rubber monomer, and preferably includes at least one of silicone oil, silicone gel, acrylic acid, acrylic rubber, acrylic ester copolymer resin, ethylene-vinyl acetate copolymer resin, polyurethane rubber or polyvinyl ether resin.

[0037] In one embodiment, the mass fraction of the matrix material in the raw material is 5%-20%. It should be noted that the mass fraction of the matrix material in the raw material should be minimized while ensuring that the phase change material does not overflow. Therefore, the mass fraction of the matrix material in the raw material is preferably 5%-10%.

[0038] In one embodiment, the crosslinking agent includes at least one of N,N'-methylenebisacrylamide, hydrogenated silicone oil, dicumyl peroxide, benzoyl peroxide or di-tert-butyl peroxide. The mass fraction of the crosslinking agent in the raw material is 0.01%-16%, more preferably 0.1%-16%.

[0039] In order to make the heat conductive filler 10 rotate more smoothly during the freezing process, so that the longitudinal thermal conductivity of the heat conductive pad is improved, in one embodiment, the heat conductive filler 10 is selected from a rod-shaped heat conductive filler, an ellipsoidal heat conductive filler or a sheet-shaped heat conductive filler. The particle size of the heat conductive filler 10 is 0.5 μm-500 μm, and more preferably 1 μm-200 μm.

[0040] It can be understood that when the thermally conductive filler 10 is a rod-shaped thermally conductive filler or an ellipsoidal thermally conductive filler, the axial direction of the thermally conductive filler 10 is the length direction of the thermally conductive filler 10, and the radial direction is the diameter direction perpendicular to the axial direction; when the thermally conductive filler 10 is selected from a sheet-shaped thermally conductive filler, the axial direction of the thermally conductive filler 10 is the extension direction of the thermally conductive filler 10, and the radial direction is the thickness direction perpendicular to the axial direction.

[0041] In one embodiment, the thermally conductive filler 10 includes at least one of carbon fiber, carbon nanotube, graphite, graphene, diamond, aluminum oxide, magnesium oxide, silicon oxide, boron nitride, aluminum nitride, copper or silver. The mass fraction of the thermally conductive filler 10 in the raw material is 5%-49%, more preferably 30%-49%.

[0042] In one embodiment, the phase change material 20 includes at least one of polyethylene glycol, polyvinyl alcohol, polypropylene alcohol, octadecyl or paraffin.

[0043] In order to improve the thermal conductivity of the thermally conductive gasket as much as possible and avoid the problem of overflow of the phase change material 20, in one embodiment, the mass fraction of the phase change material 20 in the raw material is 45%-89%, and more preferably 45%-70%.

[0044] In one embodiment, the raw material further includes an auxiliary agent, and the auxiliary agent includes at least one of an initiator, a platinum catalyst, a surface modifier, a rheology modifier or an antioxidant.

[0045] The initiator can cause the curing cross-linking reaction. When the auxiliary agent includes the initiator, the initiator includes peroxides and azo initiators, such as ammonium persulfate, benzoyl peroxide, and azobisisobutyronitrile. In one embodiment, the mass fraction of the initiator in the raw material is 0.05%-1%, and more preferably 0.1%-0.5%.

[0046] When the auxiliary agent includes a platinum catalyst, in one embodiment, the mass fraction of the platinum catalyst in the raw material is 1%-5%, more preferably 1%-2%.

[0047] The surface additive can make the thermal conductive filler 10 more dispersed. When the additive includes a surface modifier, the surface modifier includes at least one of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent or stearic acid. In one embodiment, the mass fraction of the surface modifier in the raw material is 0.05%-2%, and more preferably 0.1%-1%.

[0048] When the auxiliary agent includes a rheology modifier, the rheology modifier includes at least one of ethyl acetate, toluene, ethylbenzene, acetone, ethanol, isopropanol or an alkane solvent; in one embodiment, the mass fraction of the rheology modifier in the raw material is 0.5%-10%, more preferably 1%-5%.

[0049] When the auxiliary agent includes an antioxidant, the antioxidant includes at least one of a hindered phenol antioxidant, a hindered amine antioxidant, a thioester or a phosphite; in one embodiment, the mass fraction of the antioxidant in the raw material is 0.01%-0.1%, more preferably 0.05%-0.1%.

[0050] In step S2, in order to prevent the base material from volatilizing at the first temperature and causing local crystallization, in one embodiment, the temperature difference between the first temperature and the melting point of the phase change material 20 is 10°C-20°C.

[0051] In one embodiment, in order to allow the matrix 30 to better wrap the phase change material 20 and prevent the phase change material 20 from overflowing, the step of mixing the raw materials includes: firstly melting the phase change material 20 to a molten state, then adding the remaining raw materials to mix, and finally adding the matrix material and the cross-linking agent in the remaining raw materials.

[0052] It should be noted that when the matrix material is a polymer monomer, the polymer monomer can be polymerized in situ at the first temperature and undergo a curing and cross-linking reaction to form the matrix 30 .

[0053] like Figure 1 , which is a schematic structural diagram of a preform according to an embodiment of the present invention, wherein the thermal conductive filler 10 is arranged irregularly in the preform.

[0054] In order to make the thermally conductive filler 10 in the preform more easily rotate during the freezing process so that the prepared thermally conductive gasket has a better heat dissipation effect, in one embodiment, the thickness of the preform is 0.3mm-3mm, and more preferably 0.3mm-2mm.

[0055] In step S3, the second temperature is lower than the melting point of the phase change material 20 and the temperature difference is more than 30°C. Therefore, the preform will be rapidly frozen during the freezing process, so that the heat dissipation direction of the preform is perpendicular to the surface of the preform. Therefore, the solidification direction of the phase change material 20 is perpendicular to the surface of the preform, so that the thermally conductive filler 10 can rotate during the freezing process, and then the axial direction of the thermally conductive filler 10 forms an angle of 60 degrees to 90 degrees with the thermally conductive gasket, and forms a thermal conductive path together with the solidified phase change material 20, so that the thermally conductive gasket has excellent thermal conductivity. It should be noted that when the second temperature is lower than the melting point of the phase change material 20 but the temperature difference is less than 30°C, the thermally conductive filler 10 cannot rotate during the freezing process.

[0056] In order to further accelerate the freezing speed of the preform and make the heat conductive filler 10 rotate better, the temperature difference between the second temperature and the melting point of the phase change material 20 is greater than or equal to 50°C, and more preferably greater than or equal to 70°C.

[0057] It should be noted that, if conditions permit, the temperature difference between the second temperature and the melting point of the phase change material 20 should be increased as much as possible to accelerate the freezing speed of the preform.

[0058] The preparation method of the present invention is simple and suitable for industrial production. It is also universal and can obtain thermally conductive gaskets with different properties by using different types of thermally conductive fillers 10.

[0059] The present invention also provides a thermally conductive gasket prepared by the thermally conductive gasket preparation method as described above.

[0060] like Figure 2 , which is a schematic diagram of a thermally conductive gasket according to an embodiment of the present invention, wherein the angle between the axial direction of the thermally conductive filler 10 in the thermally conductive gasket and the surface of the thermally conductive gasket is 60 degrees to 90 degrees.

[0061] The present invention also provides an application of the thermally conductive gasket as described above in an electronic product. Specifically, the thermally conductive gasket is used as a thermally conductive device in the electronic product.

[0062] In one embodiment, the electronic product includes a heating device and a heat dissipation device. Preferably, a thermally conductive pad is provided as a thermally conductive device between the heating device and the heat dissipation device to conduct heat generated by the heating device to the heat dissipation device.

[0063] The thermally conductive gasket provided by the present invention has excellent thermal conductivity and high-temperature conformality, and can be better used as a thermal conductive device in electronic products. Even if the temperature is higher than the melting point of the phase change material 20, it can still maintain the integrity of its shape, thus solving the problem of overflow of the phase change material 20.

[0064] Hereinafter, the thermal conductive pad and its preparation method and application will be further described through the following specific embodiments.

[0065] Example 1

[0066] The raw materials provided are: 10 g polyethylene glycol (melting point 63° C.), 10 g carbon fiber (length 250 μm), 1.48 g acrylic acid, 0.44 g water, 0.03 g ammonium persulfate and 0.07 g N,N′-methylenebisacrylamide.

[0067] At 70°C, polyethylene glycol was melted to a molten state, and then the remaining raw materials were added, among which acrylic acid was added last, to obtain a first mixture; after the first mixture was stirred at 1000 rpm for 2 minutes to be evenly mixed, it was poured into a 1 mm thick mold, and the mold was placed in an oven at 80°C for 2 hours to allow the acrylic acid to be in-situ polymerized and cured and cross-linked to complete, to obtain a preform with a cross-linking density of 2.2%.

[0068] The preform was frozen at -24°C for 1 minute to obtain a thermally conductive gasket with a thickness of 1 mm, wherein the angle between the length direction of the carbon fiber and the surface of the thermally conductive gasket was 60 degrees to 90 degrees.

[0069] Example 2

[0070] The raw materials provided are: 10 g polyethylene glycol (melting point 63° C.), 5 g carbon fiber (length 250 μm), 1.48 g acrylic acid, 0.44 g water, 0.03 g ammonium persulfate and 0.07 g N,N′-methylenebisacrylamide.

[0071] At 70°C, polyethylene glycol was melted to a molten state, and then the remaining raw materials were added, among which acrylic acid was added last, to obtain a first mixture; after the first mixture was stirred at 1000 rpm for 2 minutes to be evenly mixed, it was poured into a 1 mm thick mold, and the mold was placed in an oven at 80°C for 2 hours to allow the acrylic acid to be in-situ polymerized and then cured and cross-linked to completely form polyacrylic rubber, thereby obtaining a preform with a cross-linking density of 2.2%.

[0072] The preform was frozen at -24°C for 1 minute to obtain a thermally conductive gasket with a thickness of 1 mm, wherein the angle between the length direction of the carbon fiber and the surface of the thermally conductive gasket was 60 degrees to 90 degrees.

[0073] Example 3

[0074] The raw materials provided are: 10 g paraffin (melting point is 60° C.), 10 g boron nitride (particle size is 10 μm), 3 g silicone oil, 3 g hydrogenated silicone oil, and 0.3 g platinum catalyst.

[0075] At 80°C, paraffin is melted to a molten state, and then the remaining raw materials are added, among which the platinum catalyst is added last, to obtain a first mixture; after the first mixture is stirred at 1000 rpm for 2 minutes to be evenly mixed, it is poured into a 1 mm thick mold, and the mold is placed in an oven at 80°C for 12 hours to complete the curing and cross-linking reaction of the silicone oil and the hydrogenated silicone oil to obtain a preform with a cross-linking density of 0.05%.

[0076] The preform was frozen at -24°C for 1 minute to obtain a thermally conductive gasket with a thickness of 1 mm, wherein the angle between the extension direction of the boron nitride and the surface of the thermally conductive gasket was 60 degrees to 90 degrees.

[0077] Example 4

[0078] The raw materials provided are: 10 g paraffin (melting point is 60° C.), 3 g boron nitride (particle size is 10 μm), 3 g silicone oil, 3 g hydrogenated silicone oil, and 0.3 g platinum catalyst.

[0079] At 80°C, paraffin is melted to a molten state, and then the remaining raw materials are added, among which the platinum catalyst is added last, to obtain a first mixture; after the first mixture is stirred at 1000 rpm for 2 minutes to be evenly mixed, it is poured into a 1 mm thick mold, and the mold is placed in an oven at 80°C for 12 hours to complete the curing and cross-linking reaction of the silicone oil and the hydrogenated silicone oil to obtain a preform with a cross-linking density of 0.05%.

[0080] The preform was frozen at -24°C for 1 minute to obtain a thermally conductive gasket with a thickness of 1 mm, wherein the angle between the extension direction of the boron nitride and the surface of the thermally conductive gasket was 60 degrees to 90 degrees.

[0081] Example 5

[0082] The raw materials provided are: 10 g polyethylene glycol (melting point 63° C.), 5 g carbon fiber (length 250 μm), 1.48 g acrylic acid, 0.44 g water, 0.03 g ammonium persulfate and 0.07 g N,N′-methylenebisacrylamide.

[0083] At 70°C, polyethylene glycol was melted to a molten state, and then the remaining raw materials were added, among which acrylic acid was added last, to obtain a first mixture; after the first mixture was stirred at 1000 rpm for 2 minutes to be evenly mixed, it was poured into a 1 mm thick mold, and the mold was placed in an oven at 80°C for 2 hours to allow the acrylic acid to be in-situ polymerized and then cured and cross-linked to completely form polyacrylic rubber, thereby obtaining a preform with a cross-linking density of 2.2%.

[0084] The preform was frozen at -10°C for 1 minute to obtain a thermally conductive gasket with a thickness of 1 mm, wherein the angle between the length direction of the carbon fiber and the surface of the thermally conductive gasket was 60 degrees to 90 degrees.

[0085] Comparative Example 1

[0086] The raw materials provided are: 10 g polyethylene glycol (melting point 63° C.), 10 g carbon fiber (length 250 μm), 1.48 g acrylic acid, 0.44 g water, 0.03 g ammonium persulfate and 0.07 g N,N′-methylenebisacrylamide.

[0087] At 70°C, polyethylene glycol was melted to a molten state, and then the remaining raw materials were added, among which acrylic acid was added last, to obtain a first mixture; after the first mixture was stirred at 1000 rpm for 2 minutes to be evenly mixed, it was poured into a 1 mm thick mold, and the mold was placed in an oven at 80°C for 2 hours to polymerize the acrylic acid in situ and cure the cross-linking reaction to completely form polyacrylic acid rubber, thereby obtaining a preform with a cross-linking density of 2.2%.

[0088] The preform was cooled at 35° C. for 20 minutes to obtain a thermally conductive gasket with a thickness of 1 mm, wherein the angle between the length direction of the carbon fiber and the surface of the thermally conductive gasket was 0 degrees to 90 degrees.

[0089] Comparative Example 2

[0090] The raw materials provided are: 10 g paraffin (melting point is 60° C.), 10 g boron nitride (particle size is 10 μm), 3 g silicone oil, 3 g hydrogenated silicone oil, and 0.3 g platinum catalyst.

[0091] At 80°C, paraffin is melted to a molten state, and then the remaining raw materials are added, among which the platinum catalyst is added last, to obtain a first mixture; after the first mixture is stirred at 1000 rpm for 2 minutes to be evenly mixed, it is poured into a 1 mm thick mold, and the mold is placed in an oven at 80°C for 12 hours to complete the curing and cross-linking reaction of the silicone oil and the hydrogenated silicone oil to obtain a preform with a cross-linking density of 0.5%.

[0092] The preform was cooled at 35° C. for 20 minutes to obtain a thermally conductive gasket with a thickness of 1 mm, wherein the angle between the extension direction of the boron nitride and the surface of the thermally conductive gasket was 0 degrees to 90 degrees.

[0093] Comparative Example 3

[0094] The raw materials provided are: 10 g polyethylene glycol (melting point 63° C.), 10 g carbon fiber (length 250 μm), 1.48 g acrylic acid, 0.44 g water, 0.03 g ammonium persulfate and 0.07 g N,N′-methylenebisacrylamide.

[0095] At 70°C, polyethylene glycol was melted to a molten state, and then the remaining raw materials were added, among which acrylic acid was added last, to obtain a first mixture; after the first mixture was stirred at 1000 rpm for 2 minutes to be evenly mixed, it was poured into a 5 mm thick mold, and the mold was placed in an oven at 80°C for 2 hours to polymerize the acrylic acid in situ and cure the cross-linking reaction to completely form polyacrylic acid rubber, thereby obtaining a preform with a cross-linking density of 2.2%.

[0096] The preform was frozen at -24°C for 1 minute to obtain a thermally conductive gasket with a thickness of 1 mm, wherein the angle between the length direction of the carbon fiber and the surface of the thermally conductive gasket was 30 degrees to 90 degrees.

[0097] The longitudinal thermal conductivity, phase change temperature and phase change enthalpy of the thermally conductive gaskets made from test examples 1-5 and comparative examples 1-3, the test methods and the test results are shown in Table 1; the leakage value test method is to heat the thermally conductive gasket to above the melting point, weigh it after cooling, calculate the mass difference before and after heating, and the mass difference divided by the mass of the thermally conductive gasket before heating is the leakage value.

[0098] Table 1

[0099]

[0100]

[0101] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0102] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a thermally conductive gasket, characterized in that: The steps include: Providing raw materials, the raw materials include a phase change material, a thermal conductive filler, a matrix material and a cross-linking agent, the ratio of the axial length to the radial length of the thermal conductive filler is greater than 1, the mass fraction of the phase change material in the raw materials is 45%-89%, the mass fraction of the thermal conductive filler in the raw materials is 5%-49%, the mass fraction of the matrix material in the raw materials is 5%-20%, and the mass fraction of the cross-linking agent in the raw materials is 0.01%-16%; At a first temperature, the raw materials are mixed, and the matrix material undergoes a curing crosslinking reaction in the presence of the crosslinking agent to form a matrix, thereby obtaining a preform, wherein the first temperature is greater than the melting point of the phase change material and less than the boiling point of the phase change material, the temperature difference between the first temperature and the melting point of the phase change material is 10° C.-20° C., and the crosslinking density of the matrix is ​​0.5%-5%; and The preform is frozen at a second temperature to obtain a thermally conductive gasket, wherein the second temperature is lower than the melting point of the phase change material and the temperature difference is above 70°C, and the angle between the axial direction of the thermally conductive filler in the thermally conductive gasket and the surface of the thermally conductive gasket is 60-90 degrees.

2. The method for preparing a thermally conductive gasket according to claim 1, characterized in that: The thickness of the preform is 0.3 mm to 3 mm.

3. The method for preparing a thermally conductive pad according to claim 1, characterized in that: The thermally conductive filler is selected from a rod-shaped thermally conductive filler, an ellipsoidal thermally conductive filler or a sheet-shaped thermally conductive filler.

4. The method for preparing a thermally conductive pad according to claim 3, characterized in that: The particle size of the thermal conductive filler is 0.5 μm-200 μm.

5. The method for preparing a thermally conductive gasket according to any one of claims 1 to 4, characterized in that: The phase change material comprises at least one of polyethylene glycol, polyvinyl alcohol, polypropylene alcohol or paraffin; And / or, the thermally conductive filler includes at least one of carbon fiber, carbon nanotube, graphite, graphene, diamond, aluminum oxide, magnesium oxide, silicon oxide, boron nitride, aluminum nitride, copper or silver; And / or, the matrix material includes at least one of silicone oil, silicone gel, acrylic acid, acrylic rubber, acrylic ester copolymer resin, ethylene-vinyl acetate copolymer resin, polyurethane rubber or polyvinyl ether resin; And / or, the cross-linking agent includes at least one of N,N'-methylenebisacrylamide, hydrogenated silicone oil, dicumyl peroxide, benzoyl peroxide or di-tert-butyl peroxide.

6. The method for preparing a thermally conductive gasket according to any one of claims 1 to 4, characterized in that: The raw materials further include an auxiliary agent, and the auxiliary agent includes at least one of an initiator, a platinum catalyst, a surface modifier, a rheology modifier or an antioxidant.

7. A thermally conductive pad, characterized in that: The thermally conductive gasket is prepared by the method for preparing a thermally conductive gasket according to any one of claims 1 to 6.

8. Use of the thermally conductive gasket as claimed in claim 7 in electronic products.

Citation Information

Patent Citations

  • Heat-conducting silica gel composition and preparation method thereof

    CN107043541A

  • Flexible phase-change material for electronic device thermal control

    CN107254297A

  • High-K-value phase change heat conducting sheet and preparation method thereof

    CN108753261A

  • Heat-conduction sizing phase change material for battery thermal management system and preparation method thereof

    CN109401729A

  • Low-thermal-resistance phase-change heat-conducting soft sheet and preparation method thereof