Semiconductor structure and method for forming the same

By using the second side wall, protective layer and dielectric layer of different materials in the semiconductor structure, combined with a specific etching process, the semiconductor structure performance improvement and leakage current problems in the prior art are solved, and better isolation effect is achieved and Integration degree.

CN113707719BActive Publication Date: 2024-11-19SEMICON MFG INT (SHANGHAI) CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010436510.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-05-21
Publication Date
2024-11-19
Estimated Expiration
2040-05-21

AI Technical Summary

Technical Problem

In the process of reducing size and improving integration, the performance of existing semiconductor structures still needs to be improved, especially the conductive structures formed under the self-aligning electrical contact process have leakage current and short connection problems.

Method used

Using the second side wall of different materials, protective layer and dielectric layer in the gate structure, the first and second openings are formed by selecting a process of lower etching rate to ensure isolation effect, avoid leakage current, and improve the structure. performance.

Benefits of technology

Through the combination and process selection of different materials, the etching damage of the second side wall is reduced, the isolation effect is improved, the performance and compatibility of the semiconductor structure is improved, the generation of leakage current is avoided, and the integration and performance of the device is improved. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113707719B_ABST
    Figure CN113707719B_ABST
Patent Text Reader

Abstract

A semiconductor structure and a method for forming the same, wherein the structure comprises: a substrate, a gate structure on the substrate, the gate structure comprising: a gate layer and a protective layer located on a surface of a portion of the gate layer; a first sidewall and a second sidewall located on both sides of the gate structure, the second sidewall being located on the first sidewall, the material of the second sidewall being different from the material of the protective layer; and a dielectric layer located on the substrate, the material of the dielectric layer being different from the material of the second sidewall. The semiconductor structure has good performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to a semiconductor structure and a forming method thereof. Background Art

[0002] With the rapid development of semiconductor manufacturing technology, semiconductor devices are developing towards higher component density and higher integration, for example, flash memory is used as a storage device in electronic devices such as digital cameras, laptops or tablet computers. Therefore, reducing the size of flash memory cells and thereby reducing the cost of flash memory is one of the directions of technological development. For the NOR gate electrically erasable tunneling oxide flash memory, a self-aligned electrical contact process can be used to manufacture the conductive structure on the surface of the source region and the drain region, thereby meeting the demand for manufacturing a smaller size flash memory.

[0003] However, even if the conductive structure on the surface of the source region or the drain region is manufactured using a self-aligned electrical contact process, the performance of the formed semiconductor structure still needs to be improved. Summary of the invention

[0004] The technical problem solved by the present invention is to provide a semiconductor structure and a method for forming the same, so as to improve the performance of the formed semiconductor structure.

[0005] To solve the above technical problems, the technical solution of the present invention provides a semiconductor structure, including: a substrate, a gate structure is provided on the substrate, the gate structure includes: a gate layer and a protective layer located on a surface of a portion of the gate layer; a first side wall and a second side wall located on both sides of the gate structure, the second side wall is located on the first side wall, and the material of the second side wall is different from the material of the protective layer; a dielectric layer is located on the substrate, and the material of the dielectric layer is different from the material of the second side wall.

[0006] Optionally, the material of the first side wall is different from the material of the second side wall.

[0007] Optionally, the material of the first sidewall spacer includes: a low-K dielectric material.

[0008] Optionally, the material of the second sidewall spacer includes: aluminum nitride.

[0009] Optionally, the material of the protective layer includes silicon oxide, silicon nitride, silicon carbide nitride, silicon boron nitride, silicon carbon nitride oxide or silicon nitride oxide.

[0010] Optionally, the top surface of the protection layer is flush with the top surface of the dielectric layer.

[0011] Optionally, the material of the gate layer includes: one or more combinations of copper, tungsten, aluminum, titanium, nickel, titanium nitride and tantalum nitride.

[0012] Optionally, the thickness of the second sidewall spacer is in a range of 3 nanometers to 10 nanometers.

[0013] Optionally, a height ratio between the second side wall and the first side wall is in a range of 1:5 to 1:1.

[0014] Optionally, a bottom surface of the second spacer is lower than a top surface of the gate layer.

[0015] Optionally, it also includes: source-drain doped regions located in the substrate on both sides of the gate structure, the first side wall and the second side wall; a conductive structure located on the source-drain doped regions, the bottom surface of the second side wall is lower than the top surface of the conductive structure; the dielectric layer has a first opening and a second opening, the first opening exposes a portion of the top surface of the conductive structure, and the second opening exposes a portion of the top surface of the gate layer.

[0016] Optionally, the gate structure further includes: a gate dielectric layer located at the bottom and sidewall surface of the gate layer.

[0017] Optionally, the material of the gate dielectric layer includes: a high-K dielectric material.

[0018] Optionally, the base includes a substrate and a fin located on a surface of the substrate, the gate structure spans the fin, and the gate structure is located on a portion of a top surface and a sidewall surface of the fin.

[0019] Correspondingly, the present invention also provides a method for forming a semiconductor structure, comprising: providing a substrate; forming a pseudo gate structure and a dielectric layer on the substrate, the side wall surface of the pseudo gate structure having an initial side wall, the substrate on both sides of the pseudo gate structure and the initial side wall having source and drain doping regions, and the dielectric layer being located on the surface of the pseudo gate structure and the surface of the source and drain doping regions; removing part of the initial side wall, forming a groove in the dielectric layer, so that the initial side wall forms a first side wall, and the groove exposes the top surface of the first side wall; forming a second side wall in the groove, the material of the second side wall being different from the material of the dielectric layer; after forming the second side wall, removing the pseudo gate structure, forming a pseudo gate opening in the dielectric layer; forming a gate structure in the pseudo gate opening, the gate structure comprising: a gate layer and a protective layer located on the surface of the gate layer, and the material of the protective layer is different from the material of the second side wall, and the material of the protective layer is different from the material of the dielectric layer.

[0020] Optionally, the material of the second side wall is different from that of the first side wall.

[0021] Optionally, the thickness of the second sidewall spacer is in a range of 3 nanometers to 10 nanometers.

[0022] Optionally, a height ratio between the second side wall and the first side wall is in a range of 1:5 to 1:1.

[0023] Optionally, the top surface of the dielectric layer is flush with the top surface of the initial sidewall.

[0024] Optionally, the method for forming the second sidewall in the groove includes: forming a sidewall material film in the groove and on the surface of the dielectric layer; and planarizing the sidewall material film until the top surface of the dielectric layer is exposed to form the second sidewall.

[0025] Optionally, the dummy gate structure includes: a dummy gate dielectric layer located on the surface of the substrate, a dummy gate layer located on the surface of the dummy gate dielectric layer, and a blocking layer located on the surface of the dummy gate layer; the method for removing the dummy gate structure includes: removing the blocking layer, the dummy gate layer and the dummy gate dielectric layer.

[0026] Optionally, the gate structure also includes: a gate dielectric layer located at the bottom and side wall surfaces of the gate layer, and the gate dielectric layer is located at the bottom and side wall surfaces of the pseudo gate opening; the method for forming the gate structure includes: forming a gate dielectric material layer at the bottom and side wall surfaces of the pseudo gate opening and on the surface of the dielectric layer; forming a gate material layer on the surface of the gate dielectric material layer, and the gate material layer fills the pseudo gate opening; flattening the gate material layer and the gate dielectric material layer until the surface of the dielectric layer is exposed, forming an initial gate dielectric layer and an initial gate layer located on the surface of the initial gate dielectric layer in the pseudo gate opening; etching back part of the initial gate dielectric layer and the initial gate layer to form a gate dielectric layer and a gate layer located on the surface of the gate dielectric layer, and the dielectric layer has a gate opening exposing the gate dielectric layer and the top of the gate layer; forming a protective layer in the gate opening.

[0027] Optionally, the top surface of the protection layer is flush with the top surface of the dielectric layer.

[0028] Optionally, it also includes: after forming the second side wall, forming source and drain openings in the dielectric layer, and the source and drain openings expose the surface of the source and drain doped regions; forming a conductive structure in the source and drain openings; forming a first opening and a second opening in the dielectric layer, and the first opening exposes a portion of the top surface of the conductive structure, and the second opening exposes a portion of the top surface of the gate layer.

[0029] Optionally, the source / drain openings also expose sidewall surfaces of the first sidewall spacer and the second sidewall spacer.

[0030] Optionally, the method for forming the source and drain openings includes: forming a first mask layer on the surface of the dielectric layer, the surface of the protective layer, and the surface of the second side wall; forming a first patterned layer on the surface of the first mask layer, the first patterned layer exposing the surface of the first mask layer on the source and drain doped regions; using the first patterned layer as a mask, etching the first mask layer and the dielectric layer until the top surface of the source and drain doped regions is exposed to form the source and drain openings.

[0031] Optionally, the method for forming the conductive structure includes: forming a conductive material layer in the source and drain openings and on the surface of the first mask layer; flattening the conductive material layer until the surface of the first mask layer is exposed, and forming an initial conductive structure in the first mask layer and the dielectric layer; and etching back part of the initial conductive structure so that the initial conductive structure forms the conductive structure, and the top surface of the conductive structure is lower than the top surface of the dielectric layer.

[0032] Optionally, the method for forming the first opening includes: forming a second mask layer on the surfaces of the dielectric layer, the protective layer and the conductive structure; forming a second patterned layer on the surface of the second mask layer, the second patterned layer exposing a portion of the surface of the second mask layer on the conductive structure; using a first etching process, using the second patterned layer as a mask, etching the second mask layer and the second side wall until the top surface of the conductive structure is exposed, thereby forming a first opening in the dielectric layer; after forming the first opening, removing the second mask layer and the second patterned layer.

[0033] Optionally, the etching rate of the second mask layer and the dielectric layer by the first etching process is greater than the etching rate of the second sidewall; the parameters of the first etching process include: the pressure is 20 mTorr to 50 mTorr, the bias power is 300 W to 800 W, and the etching gas includes C 4 F 6 , O 2 , Ar, C 4 F 6 The flow rate is 10 standard ml / min to 20 standard ml / min, the O 2 The flow rate of Ar is 10 standard ml / min to 25 standard ml / min, and the flow rate of Ar is 1000 standard ml / min to 2000 standard ml / min.

[0034] Optionally, the method for forming the second opening includes: forming a third mask layer on the surfaces of the dielectric layer, the protective layer and the conductive structure; forming a third patterned layer on the surface of the third mask layer, the third patterned layer exposing a portion of the surface of the third mask layer on the second protective layer; using a second etching process, using the third patterned layer as a mask, etching the third mask layer, the second side wall, the protective layer and the dielectric layer until the top surface of the gate layer is exposed, and forming a second opening in the dielectric layer; after forming the second opening, removing the third mask layer and the third patterned layer.

[0035] Optionally, the etching rate of the second etching process on the third mask layer, the protective layer and the dielectric layer is greater than the etching rate on the second sidewall; the parameters of the second etching process include: the second etching process includes: a first etching step and a second etching step, the parameters of the first etching step include: a pressure of 20 mTorr to 50 mTorr, a bias power of 300 W to 800 W, and an etching gas including C 4 F 6 , O 2 and Ar, the C 4 F 6 The flow rate is 10 standard ml / min to 20 standard ml / min, the O 2 The flow rate of Ar is 10 standard ml / min to 25 standard ml / min, the flow rate of Ar is 1000 standard ml / min to 2000 standard ml / min, and the second etching step includes: the pressure is 10 mTorr to 20 mTorr, the bias voltage is 100 W to 500 W, and the etching gas includes H 2 and CH 3 F,H 2 The flow rate is 50 standard ml / min to 300 standard ml / min, the CH 3 The flow rate of F is 10 standard ml / min to 30 standard ml / min.

[0036] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0037] In the semiconductor structure provided by the technical solution of the present invention, since the materials of the second sidewall, the protective layer in the gate structure and the dielectric layer are all different, it is advantageous to select an etching process with a lower etching rate for the second sidewall, so that in the subsequent process of forming the first opening and the second opening in the dielectric layer, the etching damage to the second sidewall is small, thereby ensuring that the second sidewall can play a good isolation role between the gate structure and the conductive structure, avoiding the generation of leakage current. At the same time, the morphology of the first opening and the second opening is good, thereby improving the performance of the formed semiconductor structure.

[0038] Furthermore, the materials of the first side wall and the second side wall are different. The material of the first side wall is a low-K dielectric material, which can ensure that the formed device has better performance and has better compatibility with existing processes, thereby facilitating improving the performance of the formed semiconductor structure.

[0039] In the method for forming a semiconductor structure provided by the technical solution of the present invention, by forming a second sidewall on the sidewall of the gate structure, and the materials of the second sidewall, the protective layer in the gate structure and the dielectric layer are all different, it is beneficial to select an etching process with a lower etching rate for the second sidewall, so that in the subsequent process of forming the first opening and the second opening in the dielectric layer, the etching damage to the second sidewall is small, thereby ensuring that the second sidewall can play a good isolation role for the gate structure and the conductive structure, avoiding the generation of leakage current. At the same time, the morphology of the first opening and the second opening is good, thereby improving the performance of the formed semiconductor structure.

[0040] Furthermore, the materials of the first side wall and the second side wall are different. The material of the first side wall is a low-K dielectric material, which can ensure that the formed device has better performance and has better compatibility with existing processes, thereby facilitating improving the performance of the formed semiconductor structure.

[0041] Furthermore, the thickness of the second sidewall spacer ranges from 3 nanometers to 10 nanometers. If the thickness is greater than 10 nanometers, while the second sidewall spacer can still have a good isolation effect after forming the first opening and the second opening, it takes extra process time to form the thicker second sidewall spacer, which is not conducive to improving production efficiency, and a second sidewall spacer that is too thick will take up a large space, which is not conducive to improving device integration; if the thickness is less than 3 nanometers, the thinner second sidewall spacer is easily etched through during the subsequent formation of the first opening and the second opening, resulting in a short circuit between the gate structure and the conductive structure on both sides of the second sidewall spacer, thereby generating leakage current, which is not conducive to the performance of the semiconductor structure.

[0042] Furthermore, the height ratio of the second sidewall to the first sidewall is in the range of 1:5 to 1:1. If the ratio is greater than 1:1, the volume of the first sidewall located on the sidewall of the gate structure is too small, which is not conducive to maintaining the performance of the formed device; if the ratio is less than 1:5, the height of the second sidewall located on the sidewall of the gate structure is too small, resulting in the subsequent formation of the first opening and the second opening. The first sidewall located at the bottom of the second sidewall is still susceptible to etching damage, making it easy for the gate structure and the conductive structure to be short-circuited, thereby generating leakage current, which is not conducive to the performance of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1It is a schematic diagram of the structure of a semiconductor structure;

[0044] Figure 2 It is a schematic diagram of the structure of a semiconductor structure;

[0045] Figures 3 to 14 It is a structural schematic diagram of each step of a method for forming a semiconductor structure in one embodiment of the present invention. DETAILED DESCRIPTION

[0046] As described in the background art, semiconductor structures have poor performance.

[0047] The following is a detailed description of the reasons for the poor performance of the semiconductor structure with reference to the accompanying drawings. Figure 1 It is a structural diagram of a semiconductor structure.

[0048] Please refer to Figure 1 , providing a substrate 100, forming a gate structure 102 on the substrate 100, the gate structure 102 extending along a first direction Y, the gate structure 102 including a first region I and a second region II extending along the first direction Y; a source-drain doped layer 103 in the substrate 100 on both sides of the gate structure 102 in the first region I; forming a first conductive structure 104 on the source-drain doped layer 103; and forming a second conductive structure 101 on the gate structure 102 in the second region II.

[0049] However, in this embodiment, in order to avoid short circuit between the first conductive structure 104 and the second conductive structure 101, the second conductive structure 101 is formed on the second region II of the gate structure 102, which results in a larger distance between the first conductive structure 104 and the second conductive structure 101. This results in a larger space occupied by the first conductive structure 104 and the second conductive structure 101, thereby reducing the integration of the semiconductor structure element finally formed.

[0050] In order to solve the above problems, a semiconductor structure is proposed, which will be described in detail below with reference to the accompanying drawings.

[0051] Please refer to Figure 2 , providing a substrate 200; forming a gate structure 202 on the substrate 200, the gate structure 202 extending along a first direction Y, the gate structure 202 including a first region I and a second region II extending along the first direction Y; forming a source-drain doped layer 203 in the substrate 200 on both sides of the gate structure 202 in the first region I; forming a first conductive structure 204 on the source-drain doped layer 203; and forming a second conductive structure 201 on the gate structure 202 in the first region I.

[0052] In this embodiment, by forming the second conductive structure 201 on the gate structure 202 located in the first region I, the distance between the first conductive structure 204 and the second conductive structure 201 can be effectively reduced, thereby improving the integration of the components of the semiconductor structure finally formed. However, in this embodiment, the first conductive opening and the second conductive opening (not shown) corresponding to the first conductive structure 204 and the second conductive structure 201 are formed by exposing the mask with an extreme ultraviolet light source at one time. As the device density of the semiconductor structure increases, the short circuit problem between the first conductive structure 204 and the second conductive structure 201 is likely to occur in the subsequent process of forming the first conductive structure 204 and the second conductive structure 201, thereby affecting the performance of the semiconductor structure.

[0053] To solve the above technical problems, an embodiment of the present invention provides a method for forming a semiconductor structure, comprising: removing a portion of the initial sidewall, forming a groove in the dielectric layer, so that the initial sidewall forms a first sidewall, and the groove exposes the top surface of the first sidewall; forming a second sidewall in the groove, the material of the second sidewall is different from the material of the dielectric layer, and the material of the second sidewall is different from the material of the subsequently formed protective layer, which is conducive to selecting an etching process with a lower etching rate for the second sidewall, thereby improving the performance of the formed semiconductor structure.

[0054] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0055] Figures 3 to 14 It is a structural schematic diagram of each step of a method for forming a semiconductor structure in one embodiment of the present invention.

[0056] Please refer to Figure 3 , providing a substrate.

[0057] In this embodiment, the base includes: a substrate 300 and a fin 301 located on the substrate 300 .

[0058] The method for forming the base 300 and the fin 301 includes: forming a mask layer (not shown) on the initial substrate; and etching the substrate using the mask layer as a mask to form the base 300 and the fin 301 .

[0059] In this embodiment, the material of the substrate 300 is single crystal silicon. In other embodiments, the material of the substrate may also be polycrystalline silicon or amorphous silicon; the material of the substrate may also be semiconductor materials such as germanium, silicon germanium, and gallium arsenide.

[0060] In this embodiment, the material of the fin 301 is single crystal silicon. In other embodiments, the material of the fin may also be single crystal silicon germanium or other semiconductor materials.

[0061] In other embodiments, the substrate may also be a structure without the fin.

[0062] The substrate also has an isolation layer (not shown in the figure), which covers part of the sidewall of the fin 301, and the top surface of the isolation layer is lower than the top surface of the fin 301. The isolation layer is used to achieve electrical isolation between different devices.

[0063] Please refer to Figure 4 A dummy gate structure 310 and a dielectric layer 320 are formed on the substrate, the sidewall surface of the dummy gate structure 310 has an initial sidewall 330, and the substrate on both sides of the dummy gate structure 310 and the initial sidewall 330 has a source-drain doped region 340, and the dielectric layer 320 is located on the surface of the dummy gate structure 310 and the surface of the source-drain doped region 340.

[0064] In this embodiment, the top surface of the dielectric layer 320 is flush with the top surface of the initial spacer 330 .

[0065] The dummy gate structure 310 includes: a dummy gate dielectric layer (not shown) located on the surface of the substrate, a dummy gate layer (not shown) located on the surface of the dummy gate dielectric layer, and a blocking layer (not shown) located on the surface of the dummy gate layer.

[0066] The method for forming the pseudo gate structure 310 includes: forming a pseudo gate dielectric material layer on the substrate; forming a pseudo gate material layer on the surface of the pseudo gate dielectric material layer; forming a blocking material layer on the surface of the pseudo gate material layer; and patterning the pseudo gate dielectric material layer, the pseudo gate material layer and the blocking material layer until the substrate surface is exposed to form the pseudo gate structure 310.

[0067] The method for forming the initial spacer 330 includes: forming an initial spacer material layer on the surface of the substrate and the surface of the dummy gate structure 310; and etching back the initial spacer material layer until the surface of the substrate and the top surface of the dummy gate structure are exposed to form the initial spacer 330.

[0068] The material of the initial spacer 330 includes: a low-k dielectric material (a low-k dielectric material refers to a dielectric material with a relative dielectric constant lower than 3.9).

[0069] In this embodiment, the material of the initial sidewall spacer 330 is silicon oxycarbide.

[0070] The method for forming the dielectric layer 320 includes: forming an initial dielectric film (not shown in the figure) on the dummy gate structure 310 and the source-drain doped region 340, the initial dielectric film covering the top surface and side wall surface of the dummy gate structure 310 and the initial sidewall 330; and planarizing the initial dielectric film until the top surface of the dummy gate structure 310 is exposed to form the dielectric layer 320.

[0071] The material of the dielectric layer 320 includes silicon oxide.

[0072] Please refer to Figure 5 , removing part of the initial sidewall 330 , forming a groove 341 in the dielectric layer 320 , so that the initial sidewall 330 forms a first sidewall 351 , and the groove 341 exposes the top surface of the first sidewall 351 .

[0073] The groove 341 provides space for subsequently forming a second sidewall 352 .

[0074] The process of removing part of the initial sidewall spacer 330 includes: one of a wet etching process and a dry etching process or a combination of the two.

[0075] Please refer to Figure 6 A second sidewall 352 is formed in the groove 341 , and the material of the second sidewall 352 is different from the material of the dielectric layer 320 .

[0076] The second spacer 352 is used for subsequent self-alignment to form a first opening and a second opening.

[0077] The method for forming the second sidewall 352 in the groove 341 includes: forming a sidewall material film (not shown) in the groove 341 and on the surface of the dielectric layer 320 ; and planarizing the sidewall material film until the top surface of the dielectric layer 320 is exposed to form the second sidewall 352 .

[0078] In this embodiment, the material of the second sidewall 352 is different from the material of the first sidewall 351 .

[0079] In this embodiment, the material of the first sidewall spacer 351 is silicon oxycarbide, and the material of the second sidewall spacer 352 is aluminum nitride.

[0080] The thickness of the second spacer 352 is in a range of 3 nanometers to 10 nanometers.

[0081] If the thickness is greater than 10 nanometers, while the second side wall 352 can still have a good isolation effect after the first opening and the second opening are subsequently formed, it will take extra process time to form the thicker second side wall 352, which is not conducive to improving production efficiency. In addition, a second side wall 352 that is too thick will occupy a large space, which is not conducive to improving device integration. If the thickness is less than 3 nanometers, the thinner second side wall 352 will easily be etched through during the subsequent formation of the first opening and the second opening, resulting in a short circuit between the gate structure and the conductive structure on both sides of the second side wall 352, thereby generating leakage current, which is not conducive to the performance of the semiconductor structure.

[0082] The height ratio of the second side wall 352 to the first side wall 351 is in the range of 1:5 to 1:1.

[0083] If the ratio is greater than 1:1, the volume of the first side wall 351 located on the side wall of the gate structure is too small, which is not conducive to maintaining the performance of the formed device; if the ratio is less than 1:5, the height of the second side wall 352 located on the side wall of the gate structure is too small, resulting in the subsequent process of forming the first opening and the second opening. The first side wall 351 located at the bottom of the second side wall 352 is still susceptible to etching damage, making it easy for a short circuit to occur between the gate structure and the conductive structure, thereby generating leakage current, which is not conducive to the performance of the semiconductor structure.

[0084] Since the material of the initial side wall 330 is a low-K dielectric material, the first side wall 351 is formed by the initial side wall 330, and thus the material of the first side wall 351 is a low-K dielectric material. The material can ensure that the formed device has better performance and has better compatibility with the existing process, which is beneficial to improving the performance of the formed semiconductor structure.

[0085] Please refer to Figure 7 After forming the second sidewall spacer 352 , the dummy gate structure 310 is removed, and a dummy gate opening 311 is formed in the dielectric layer 320 .

[0086] The dummy gate opening 311 provides space for subsequently forming a gate structure.

[0087] The method for removing the dummy gate structure 310 includes: removing the barrier layer, the dummy gate layer and the dummy gate dielectric layer.

[0088] The process of removing the dummy gate structure 310 includes: one of a wet etching process and a dry etching process or a combination of the two.

[0089] Please refer to Figure 8A gate structure 360 ​​is formed in the pseudo gate opening 311 , and the gate structure 360 ​​includes: a gate layer 361 and a protection layer 362 located on the surface of the gate layer 361 , and the material of the protection layer 362 is different from the material of the second sidewall 352 , and the material of the protection layer 362 is different from the material of the dielectric layer 320 .

[0090] The bottom surface of the second spacer 352 is lower than the top surface of the gate layer 361 , so that the second spacer 352 can fully isolate the gate structure 360 ​​from the subsequently formed conductive structure.

[0091] The gate structure 360 ​​further includes: a gate dielectric layer 363 located at the bottom and sidewall surfaces of the gate layer 361 . The gate dielectric layer 363 is located at the bottom and sidewall surfaces of the dummy gate opening 311 .

[0092] The method for forming the gate structure 360 ​​includes: forming a gate dielectric material layer (not shown in the figure) at the bottom and sidewalls of the pseudo gate opening 311 and on the surface of the dielectric layer 320; forming a gate material layer (not shown in the figure) on the surface of the gate dielectric material layer, and the gate material layer fills the pseudo gate opening 311; planarizing the gate material layer and the gate dielectric material layer until the surface of the dielectric layer 320 is exposed, and forming an initial gate dielectric layer (not shown in the figure) and an initial gate layer (not shown in the figure) located on the surface of the initial gate dielectric layer in the pseudo gate opening 311; etching back part of the initial gate dielectric layer and the initial gate layer to form a gate dielectric layer 363 and a gate layer 361 located on the surface of the gate dielectric layer 363, and the dielectric layer 320 has a gate opening (not shown in the figure) exposing the gate dielectric layer 363 and the top of the gate layer 361; forming a protective layer 362 in the gate opening.

[0093] In this embodiment, the top surface of the protection layer 362 is flush with the top surface of the dielectric layer 320 .

[0094] The protection layer 362 is used to protect the top surface of the gate layer 361 to reduce the impact of subsequent processes.

[0095] Please refer to Fig. 9 After forming the second sidewall 352 , a source / drain opening 371 is formed in the dielectric layer 320 , and the source / drain opening 371 exposes the surface of the source / drain doped region 340 .

[0096] The source-drain openings 371 provide space for subsequent formation of a conductive structure.

[0097] In this embodiment, the source / drain openings 371 also expose the sidewall surfaces of the first spacer 351 and the second spacer 352 .

[0098] The method for forming the source-drain opening 371 includes: forming a first mask layer 3711 on the surface of the dielectric layer 320, the surface of the protective layer 362, and the surface of the second side wall 352; forming a first patterned layer (not shown in the figure) on the surface of the first mask layer 3711, the first patterned layer exposing the surface of the first mask layer 3711 on the source-drain doped region 340; using the first patterned layer as a mask, etching the first mask layer 3711 and the dielectric layer 320 until the top surface of the source-drain doped region 340 is exposed to form the source-drain opening 371.

[0099] In this embodiment, the first mask layer 3711 is a single-layer structure, and the material of the first mask layer 3711 is silicon oxide. In other embodiments, the first mask layer may also be a multi-layer structure.

[0100] After forming the source / drain openings 371 , the method further includes: removing the first patterned layer.

[0101] Please refer to Fig.10 , a conductive structure 372 is formed in the source / drain opening 371 .

[0102] The bottom surface of the second spacer 352 is lower than the top surface of the conductive structure 372 , so that the second spacer 352 can fully isolate the conductive structure 372 from the gate structure 360 ​​.

[0103] The method for forming the conductive structure 372 includes: forming a conductive material layer (not shown in the figure) in the source / drain opening 371 and on the surface of the first mask layer 3711; planarizing the conductive material layer until the surface of the first mask layer 3711 is exposed, and forming an initial conductive structure (not shown in the figure) in the first mask layer 3711 and the dielectric layer 320; and etching back a portion of the initial conductive structure so that the initial conductive structure forms the conductive structure 372, and the top surface of the conductive structure 372 is lower than the top surface of the dielectric layer 320.

[0104] The material of the conductive structure includes: one or more combinations of copper, tungsten, aluminum, titanium, nickel, titanium nitride and tantalum nitride.

[0105] In this embodiment, the conductive structure 372 is made of tungsten.

[0106] In this embodiment, the conductive structure 372 is formed after the gate structure 360 ​​is formed. In other embodiments, the gate structure is formed after the conductive structure is formed.

[0107] In this embodiment, after the conductive structure 372 is formed, the remaining material of the first mask layer is continuously used as the material for subsequently forming a first opening mask.

[0108] Next, a first opening and a second opening are formed in the dielectric layer 320, wherein the first opening exposes a portion of the top surface of the conductive structure 372, and the second opening exposes a portion of the top surface of the gate layer 361. For details on the process of forming the first opening and the second opening, please refer to Figure 11 to Figure 12 .

[0109] Please refer to Fig.11 , a second mask layer is formed on the surfaces of the dielectric layer 320 , the protective layer 362 and the conductive structure 372 ; a second patterned layer 382 is formed on the surface of the second mask layer, and the second patterned layer 382 exposes a portion of the second mask layer surface on the conductive structure 372 .

[0110] In this embodiment, the second mask layer includes: a first mask portion 3811 located on the surface of the dielectric layer 320, the protective layer 362 and the conductive structure 372, and a second mask portion 3812 located on the surface of the first mask portion 3811, and the material of the first mask portion 3811 is different from that of the second mask portion 3812.

[0111] In this embodiment, the material of the first mask portion 3811 is silicon oxide, and the material of the second mask portion 3812 is silicon nitride.

[0112] The second mask layer of the multi-layer structure is beneficial to improving the accuracy of etching to form the first opening 381 .

[0113] Please refer to Fig.12 , using a first etching process, with the second patterned layer 382 as a mask, etching the second mask layer and the second sidewall 352 until the top surface of the conductive structure 372 is exposed, and forming a first opening 381 in the dielectric layer 320 .

[0114] The etching rate of the first etching process on the second mask layer and the dielectric layer 320 is greater than the etching rate on the second sidewall 352; the parameters of the first etching process include: the pressure is 20 mTorr to 50 mTorr, the bias power is 300 W to 800 W, and the etching gas includes C 4 F 6 , O 2 , Ar, C 4 F 6 The flow rate is 10 standard ml / min to 20 standard ml / min, the O 2 The flow rate of Ar is 10 standard ml / min to 25 standard ml / min, and the flow rate of Ar is 1000 standard ml / min to 2000 standard ml / min.

[0115] The first etching process has a high etching selectivity for the second side wall 352. In the process of etching to form the first opening 381, the etching damage to the second side wall 352 is small. On the one hand, the accuracy of the size of the first opening 381 is improved, and the morphology of the first opening 381 is better. On the other hand, the second side wall 352 can play a good isolation role between the gate structure 360 ​​and the conductive structure 372 to avoid the generation of leakage current.

[0116] In this embodiment, after the first opening 381 is formed, the second patterned layer 382 and the second mask portion 3812 are removed.

[0117] In this embodiment, after the first opening 381 is formed, the remaining material of the first mask portion 3811 in the second mask layer is continuously used as the material for subsequently forming a second opening mask.

[0118] At this point, a first opening 381 is formed in the dielectric layer 320 , and the first opening 381 exposes a portion of the top surface of the conductive structure 372 .

[0119] Please refer to Fig.13 , forming a third mask layer on the surfaces of the dielectric layer 320 , the protective layer 362 and the conductive structure 372 ; forming a third patterned layer 392 on the surface of the third mask layer, wherein the third patterned layer 392 exposes a portion of the surface of the third mask layer on the protective layer 362 .

[0120] Specifically, in this embodiment, after the first opening 381 is formed, the second opening is formed, and the third mask layer is still located in the first opening 381 .

[0121] In this embodiment, the third mask layer includes: a third mask portion 3813 located in the first opening 381, on the surface of the dielectric layer 320, the protective layer 362 and the conductive structure 372, and a fourth mask portion 3814 located on the surface of the third mask portion 3813, and the material of the fourth mask portion 3814 is different from that of the third mask portion 3813.

[0122] In this embodiment, the third mask portion 3813 is the first mask portion 3811 remaining after the first opening 381 is formed.

[0123] In this embodiment, the material of the third mask portion 3813 is silicon oxide, and the material of the fourth mask portion 3814 is silicon nitride.

[0124] The third mask layer of the multi-layer structure is beneficial to improving the accuracy of etching to form the second opening 391 .

[0125] Please refer to Fig.14, using a second etching process, with the third patterned layer 392 as a mask, etching the third mask layer, the second sidewall 352 , the protection layer 362 and the dielectric layer 320 until the top surface of the gate layer 361 is exposed, and forming the second opening 391 in the dielectric layer 320 .

[0126] The etching rate of the second etching process on the third mask layer, the protective layer 362 and the dielectric layer 320 is greater than the etching rate on the second sidewall 352; the parameters of the second etching process include: the second etching process includes: a first etching step and a second etching step, the parameters of the first etching step include: a pressure of 20 mTorr to 50 mTorr, a bias power of 300 W to 800 W, and an etching gas including C 4 F 6 , O 2 and Ar, the C 4 F 6 The flow rate is 10 standard ml / min to 20 standard ml / min, the O 2 The flow rate of Ar is 10 standard ml / min to 25 standard ml / min, the flow rate of Ar is 1000 standard ml / min to 2000 standard ml / min, and the second etching step includes: the pressure is 10 mTorr to 20 mTorr, the bias power is 100 W to 500 W, and the etching gas includes H 2 and CH 3 F,H 2 The flow rate is 50 standard ml / min to 300 standard ml / min, the CH 3 The flow rate of F is 10 standard ml / min to 30 standard ml / min.

[0127] The second etching process has a high etching selectivity for the second side wall 352. In the process of etching to form the second opening 391, the etching damage to the second side wall 352 is small. On the one hand, the accuracy of the size of the second opening 391 is improved, and the morphology of the second opening 391 is better. On the other hand, the second side wall 352 can play a better isolation role between the gate structure 360 ​​and the conductive structure 372, thereby avoiding the generation of leakage current.

[0128] In this embodiment, after the second opening 391 is formed, the third patterned layer 392 and the third mask layer are removed.

[0129] At this point, a second opening 391 is formed in the dielectric layer 320 , and the second opening 391 exposes a portion of the top surface of the gate layer 361 .

[0130] In other embodiments, the first opening may be formed after the second opening is formed.

[0131] Accordingly, the embodiment of the present invention further provides a semiconductor structure formed by the above method, please continue to refer to Fig.14 , comprising: a substrate, the substrate having a gate structure 360, the gate structure 360 ​​comprising: a gate layer 361 and a protective layer 362 ( Figure 8 as shown in ); a first side wall 351 and a second side wall 352 located on both sides of the gate structure 360, the second side wall 352 is located on the first side wall 351, and the material of the second side wall 352 is different from the material of the protective layer 362; a dielectric layer 320 located on the substrate, and the material of the dielectric layer 320 is different from the material of the second side wall 352.

[0132] Since the second sidewall 352, the protective layer 362 in the gate structure 360 ​​and the dielectric layer 320 are made of different materials, it is advantageous to select an etching process with a lower etching rate for the second sidewall 352, so that in the subsequent process of forming the first opening 381 and the second opening 391 in the dielectric layer 320, the second sidewall 352 is less damaged by etching, thereby ensuring that the second sidewall 352 can play a good isolation role between the gate structure 360 ​​and the conductive structure 372, thereby avoiding the generation of leakage current. At the same time, the morphology of the first opening 381 and the second opening 391 is good, thereby improving the performance of the formed semiconductor structure.

[0133] The following is a detailed description with reference to the accompanying drawings.

[0134] The base includes a substrate 300 and a fin 301 located on a surface of the substrate 300 . The gate structure 360 ​​spans across the fin 301 , and the gate structure 360 ​​is located on a portion of a top surface and a sidewall surface of the fin 301 .

[0135] The material of the first sidewall 351 is different from the material of the second sidewall 352 .

[0136] The material of the first sidewall spacer 351 includes: a low-K dielectric material.

[0137] The materials of the first sidewall 351 and the second sidewall 352 are different. The material of the first sidewall 351 is a low-K dielectric material, which can ensure that the formed device has better performance and has better compatibility with the existing process, thereby facilitating improving the performance of the formed semiconductor structure.

[0138] The material of the second sidewall spacer 352 includes aluminum nitride.

[0139] The material of the protection layer 362 includes silicon oxide, silicon nitride, silicon carbide nitride, silicon boron nitride, silicon carbon nitride oxide or silicon nitride oxide.

[0140] In this embodiment, the material of the protection layer 362 is silicon nitride.

[0141] In this embodiment, the top surface of the protection layer 362 is flush with the top surface of the dielectric layer 320 .

[0142] The material of the gate layer 361 includes: one or more combinations of copper, tungsten, aluminum, titanium, nickel, titanium nitride and tantalum nitride. In this embodiment, the material of the gate layer 361 is tungsten.

[0143] The thickness of the second spacer 352 is in a range of 3 nanometers to 10 nanometers.

[0144] The height ratio of the second side wall 352 to the first side wall 351 is in the range of 1:5 to 1:1.

[0145] A bottom surface of the second spacer 352 is lower than a top surface of the gate layer 361 .

[0146] A bottom surface of the second spacer 352 is lower than a top surface of the conductive structure 372 .

[0147] The semiconductor structure further includes: source-drain doped regions 340 located in the substrate on both sides of the gate structure 360, the first sidewall 351 and the second sidewall 352; a conductive structure 372 located on the source-drain doped region 340, the bottom surface of the second sidewall 352 is lower than the top surface of the conductive structure 272; the dielectric layer 320 has a first opening 381 and a second opening 391, the first opening 381 exposes part of the top surface of the conductive structure 272, and the second opening 391 exposes part of the top surface of the gate layer 361. The gate structure 360 ​​further includes: a gate dielectric layer 363 located at the bottom and sidewall surface of the gate layer 362.

[0148] The material of the gate dielectric layer 363 includes: a high-K dielectric material, and the high-K dielectric material includes: hafnium oxide, zirconium oxide, hafnium silicon oxide, lanthanum oxide, zirconium silicon oxide, titanium oxide, tantalum oxide, barium strontium titanium oxide, barium titanium oxide, strontium titanium oxide or aluminum oxide. In this embodiment, the material of the gate dielectric layer 363 is hafnium oxide.

[0149] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A semiconductor structure, characterized in that: include: A substrate having a gate structure thereon, wherein the gate structure comprises: a gate layer and a protective layer located on a surface of a portion of the gate layer; A first sidewall spacer and a second sidewall spacer located on both sides of the gate structure, wherein the second sidewall spacer is located on the first sidewall, and a material of the second sidewall spacer is different from a material of the protective layer; A dielectric layer located on the substrate, wherein the material of the dielectric layer is different from the material of the second sidewall; a source-drain doped region located in the substrate on both sides of the gate structure, the first sidewall and the second sidewall; a conductive structure located on the source-drain doped region, wherein the bottom surface of the second sidewall is lower than the top surface of the conductive structure; a first opening and a second opening are provided in the dielectric layer, wherein the first opening exposes a portion of the top surface of the conductive structure, and the second opening exposes a portion of the top surface of the gate layer; The second sidewall spacer is used to ensure the opening morphology and isolate the gate structure from the conductive structure during the process of forming the first opening and the second opening.

2. The semiconductor structure according to claim 1, wherein: The material of the first sidewall spacer is different from the material of the second sidewall spacer.

3. The semiconductor structure according to claim 1, wherein: The material of the first sidewall spacer includes: a low-K dielectric material.

4. The semiconductor structure according to claim 1, wherein: The material of the second sidewall spacer includes aluminum nitride.

5. The semiconductor structure according to claim 1, wherein: The material of the protective layer includes silicon oxide, silicon nitride, silicon carbide nitride, silicon boron nitride, silicon carbon nitride oxide or silicon nitride oxide.

6. The semiconductor structure according to claim 1, wherein: The top surface of the protection layer is flush with the top surface of the dielectric layer.

7. The semiconductor structure according to claim 1, wherein: The material of the gate layer includes: one or more combinations of copper, tungsten, aluminum, titanium, nickel, titanium nitride and tantalum nitride.

8. The semiconductor structure according to claim 1, wherein: The thickness of the second spacer is in a range of 3 nanometers to 10 nanometers.

9. The semiconductor structure according to claim 1, wherein: The height ratio of the second side wall to the first side wall is in the range of 1:5 to 1:

1.

10. The semiconductor structure according to claim 1, wherein: A bottom surface of the second spacer is lower than a top surface of the gate layer.

11. The semiconductor structure according to claim 1, wherein: The gate structure further includes: a gate dielectric layer located at the bottom and side wall surface of the gate layer.

12. The semiconductor structure according to claim 11, wherein: The material of the gate dielectric layer includes: high-K dielectric material.

13. The semiconductor structure according to claim 1, wherein: The base includes a substrate and a fin located on a surface of the substrate. The gate structure spans across the fin, and the gate structure is located on a portion of a top surface and a sidewall surface of the fin.

14. A method for forming a semiconductor structure, characterized in that: include: providing a substrate; A dummy gate structure and a dielectric layer are formed on the substrate, wherein the sidewall surface of the dummy gate structure has an initial sidewall, the substrate on both sides of the dummy gate structure and the initial sidewall has a source-drain doped region, and the dielectric layer is located on the surface of the dummy gate structure and the surface of the source-drain doped region; Removing part of the initial sidewall spacer to form a groove in the dielectric layer, so that the initial sidewall spacer forms a first sidewall spacer, and the groove exposes the top surface of the first sidewall spacer; forming a second sidewall spacer in the groove, wherein the material of the second sidewall spacer is different from the material of the dielectric layer; After forming the second sidewall spacer, removing the dummy gate structure, and forming a dummy gate opening in the dielectric layer; A gate structure is formed in the dummy gate opening, wherein the gate structure comprises: a gate layer and a protection layer located on the surface of the gate layer, wherein the material of the protection layer is different from the material of the second sidewall, and the material of the protection layer is different from the material of the dielectric layer; After forming the second sidewall, forming source and drain openings in the dielectric layer, wherein the source and drain openings expose the surface of the source and drain doped regions; forming a conductive structure in the source and drain openings; forming a first opening and a second opening in the dielectric layer, wherein the first opening exposes a portion of the top surface of the conductive structure, and the second opening exposes a portion of the top surface of the gate layer; The second sidewall spacer is used to ensure the opening morphology and isolate the gate structure from the conductive structure during the process of forming the first opening and the second opening.

15. The method for forming a semiconductor structure according to claim 14, wherein: The material of the second sidewall is different from that of the first sidewall.

16. The method for forming a semiconductor structure according to claim 14, wherein: The thickness of the second spacer is in a range of 3 nanometers to 10 nanometers.

17. The method for forming a semiconductor structure according to claim 14, wherein: The height ratio of the second side wall to the first side wall is in the range of 1:5 to 1:

1.

18. The method for forming a semiconductor structure according to claim 14, wherein: The top surface of the dielectric layer is flush with the top surface of the initial sidewall spacer.

19. The method for forming a semiconductor structure according to claim 18, wherein: The method for forming the second sidewall in the groove comprises: forming a sidewall material film in the groove and on the surface of the dielectric layer; and planarizing the sidewall material film until the top surface of the dielectric layer is exposed to form the second sidewall.

20. The method for forming a semiconductor structure according to claim 14, wherein: The dummy gate structure includes: a dummy gate dielectric layer located on the surface of the substrate, a dummy gate layer located on the surface of the dummy gate dielectric layer, and a blocking layer located on the surface of the dummy gate layer; the method for removing the dummy gate structure includes: removing the blocking layer, the dummy gate layer and the dummy gate dielectric layer.

21. The method for forming a semiconductor structure according to claim 14, wherein: The gate structure also includes: a gate dielectric layer located at the bottom and side wall surface of the gate layer, and the gate dielectric layer is located at the bottom and side wall surface of the pseudo gate opening; the method for forming the gate structure includes: forming a gate dielectric material layer at the bottom and side wall of the pseudo gate opening and on the surface of the dielectric layer; forming a gate material layer on the surface of the gate dielectric material layer, and the gate material layer fills the pseudo gate opening; flattening the gate material layer and the gate dielectric material layer until the surface of the dielectric layer is exposed, forming an initial gate dielectric layer and an initial gate layer located on the surface of the initial gate dielectric layer in the pseudo gate opening; etching back part of the initial gate dielectric layer and the initial gate layer to form a gate dielectric layer and a gate layer located on the surface of the gate dielectric layer, and the dielectric layer has a gate opening exposing the gate dielectric layer and the top of the gate layer; forming a protective layer in the gate opening.

22. The method for forming a semiconductor structure according to claim 14, wherein: The top surface of the protection layer is flush with the top surface of the dielectric layer.

23. The method for forming a semiconductor structure according to claim 14, wherein: The source / drain openings also expose the sidewall surfaces of the first sidewall spacer and the second sidewall spacer.

24. The method for forming a semiconductor structure according to claim 14, wherein: The method for forming the source and drain openings includes: forming a first mask layer on the surface of the dielectric layer, the surface of the protective layer, and the surface of the second sidewall; forming a first patterned layer on the surface of the first mask layer, the first patterned layer exposing the surface of the first mask layer on the source and drain doping region; using the first patterned layer as a mask, etching the first mask layer and the dielectric layer until the top surface of the source and drain doping region is exposed to form the source and drain openings.

25. The method for forming a semiconductor structure according to claim 24, wherein: The method for forming the conductive structure includes: forming a conductive material layer in the source and drain openings and on the surface of the first mask layer; flattening the conductive material layer until the surface of the first mask layer is exposed, and forming an initial conductive structure in the first mask layer and the dielectric layer; etching back a portion of the initial conductive structure so that the initial conductive structure forms the conductive structure, and the top surface of the conductive structure is lower than the top surface of the dielectric layer.

26. The method for forming a semiconductor structure according to claim 14, wherein: The method for forming the first opening includes: forming a second mask layer on the surfaces of the dielectric layer, the protective layer and the conductive structure; forming a second patterned layer on the surface of the second mask layer, wherein the second patterned layer exposes a portion of the surface of the second mask layer on the conductive structure; using a first etching process, using the second patterned layer as a mask, etching the second mask layer and the second side wall until the top surface of the conductive structure is exposed, thereby forming a first opening in the dielectric layer; after forming the first opening, removing the second mask layer and the second patterned layer.

27. The method for forming a semiconductor structure according to claim 26, wherein: The etching rate of the second mask layer and the dielectric layer by the first etching process is greater than the etching rate of the second side wall; the parameters of the first etching process include: a pressure of 20 mTorr to 50 mTorr, a bias power of 300 W to 800 W, and etching gases including C4F6, O2, and Ar. The flow rate of C4F6 is 10 standard ml / min to 20 standard ml / min, the flow rate of O2 is 10 standard ml / min to 25 standard ml / min, and the flow rate of Ar is 1000 standard ml / min to 2000 standard ml / min.

28. The method for forming a semiconductor structure according to claim 14, wherein: The method for forming the second opening includes: forming a third mask layer on the surface of the dielectric layer, the protective layer and the conductive structure; forming a third patterned layer on the surface of the third mask layer, wherein the third patterned layer exposes a portion of the surface of the third mask layer on the protective layer; using a second etching process, using the third patterned layer as a mask, etching the third mask layer, the second side wall, the protective layer and the dielectric layer until the top surface of the gate layer is exposed, thereby forming a second opening in the dielectric layer; after forming the second opening, removing the third mask layer and the third patterned layer.

29. The method for forming a semiconductor structure according to claim 28, wherein: The etching rate of the second etching process on the third mask layer, the protective layer and the dielectric layer is greater than the etching rate on the second sidewall; The second etching process includes: a first etching step and a second etching step, the parameters of the first etching step include: a pressure of 20 mTorr to 50 mTorr, a bias power of 300 W to 800 W, etching gases include C4F6, O2 and Ar, the flow rate of C4F6 is 10 standard ml / min to 20 standard ml / min, the flow rate of O2 is 10 standard ml / min to 25 standard ml / min, and the flow rate of Ar is 1000 standard ml / min to 2000 standard ml / min, the second etching step includes: a pressure of 10 mTorr to 20 mTorr, a bias power of 100 W to 500 W, etching gases include H2 and CH3F, the flow rate of H2 is 50 standard ml / min to 300 standard ml / min, and the flow rate of CH3F is 10 standard ml / min to 30 standard ml / min.