A method for manufacturing a circuit board by separately processing electroplating holes, circuit masks and conductive patterns using lasers

The non-photosensitive mask material is removed by laser, and the hole wall and line coating thickness of the circuit board are independently controlled, which solves the problem of inconsistent thickness of the conductive layer, improves the quality of electrical signal transmission, and simplifies the manufacturing process, making it suitable for multi-variety production.

CN113747673BActive Publication Date: 2024-10-25德中(天津)技术发展股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111001586.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-30
Publication Date
2024-10-25
Estimated Expiration
2041-08-30

AI Technical Summary

Technical Problem

In the existing circuit board manufacturing technology, the coating thickness of the hole wall and the line is difficult to control independently, resulting in inconsistent thickness of the conductive layer, which affects the quality of electrical signal transmission. Moreover, the traditional etching method is complex and inefficient. The direct laser removal method has a small spot diameter and low speed. Slow and inefficient.

Method used

The laser is used to remove the non-photosensitive mask material respectively to prepare the plating hole wall and circuit pattern. The laser is used to remove the copper foil in the non-circuit area to achieve fine manufacturing of the conductive pattern, and the solder mask pattern is laser cleaned at the assembly site.

Benefits of technology

It achieves independent control of hole wall and line coating thickness, improves the fineness and efficiency of conductive patterns, simplifies the manufacturing process, reduces costs, and is suitable for large-volume and small-volume production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113747673B_ABST
    Figure CN113747673B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a circuit board by using a laser to process a plating hole, a circuit mask and a conductive pattern respectively, drilling a hole and depositing a thin metal layer on the hole and the board surface, attaching a non-photosensitive masking film, and removing the masking layer covering the hole wall by laser to expose the hole wall, and then only plating and thickening the conductive layer in the hole, and then using a laser to make a plating-resistant pattern for the circuit part and electroplating the pattern, and using a laser to make a conductive pattern and a solder resist pattern; the present invention can optimize and shorten the manufacturing process of the circuit board as a whole, improve the quality and efficiency, reduce the cost, and be environmentally friendly. Using non-photosensitive materials as plating-resistant materials can reduce costs; plating holes and circuits differently, and the thickness of the plating layer can be easily controlled; using lasers to manufacture plating hole patterns and plating circuit patterns in steps, and using lasers to manufacture conductive patterns, there are fewer steps, and more sophisticated conductive patterns can be manufactured. The present invention is suitable for mass production of various circuit boards, and is also suitable for circuit board samples and small batch, multi-variety production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a circuit board by using laser to separately process electroplating holes, circuit masks and conductive patterns. The laser is used to directly remove mask materials step by step to form a pattern of only electroplating hole walls, and then the hole walls and circuit patterns are electroplated simultaneously. The hole walls and circuits are electroplated differently, and then the conductive pattern and solder resist pattern are manufactured by laser. The method belongs to the technical field of circuit board manufacturing. Background Art

[0002] The present invention uses laser direct material removal technology to manufacture circuit boards, differentially electroplates hole walls and circuits, and directly manufactures conductive patterns and solder resist patterns without a graphic transfer process.

[0003] The manufacturing process is as follows: depositing an initial conductive layer on the semi-finished product of a double-sided, multi-layer circuit board with completed drilling, chemically plating or electroplating thin copper → pasting an anti-plating masking film → making a pattern on the electroplated hole wall, laser removing the anti-plating masking film layer on the hole area, opening a window for the liquid to enter the hole → electroplating, depositing copper on the hole wall to thicken the hole wall → laser removing the anti-plating masking film layer on the line, adding a line plating window on the hole plating window → electroplating, and depositing copper and other metals on the line and on the hole wall at the same time → laser removing the anti-plating masking film and the copper foil under the masking in the non-line area at one time or in steps to make a conductive pattern → coating the entire board and curing the solder resist material at one time → using a laser to remove the organic material on the conductor in the welding area at the assembly site to make a solder resist pattern, and cleaning and solderability treatment of the welding area surface → adding solder to the connection pad, mounting and inserting components, and performing remelting soldering and / or wave soldering.

[0004] The present invention can be used to replace various subtractive hole-making metal printed circuit board technologies. The starting raw material is a conductive metal foil material, including various rigid copper-clad boards, flexible copper-clad boards, or rigid-flexible boards. The present invention uses laser processing technology and the same non-photosensitive material mask to separately make patterns for electroplating only the hole wall and patterns for electroplating the hole wall and the circuit at the same time. The copper thickness of the hole wall and the copper thickness of the circuit can be controlled separately, and the electrical requirements of electronic products for the circuit board can be better met. It is suitable for small-batch and multi-variety production of circuit boards, and is also suitable for batch manufacturing of circuit boards.

[0005] From concept to finished product, electronic products generally go through three stages: design, material preparation, and assembly.

[0006] After the physical design is completed, material preparation is required, including the selection and customization of various components, connectors, display modules, and other functional modules. Among them, one of the most important materials is the bare circuit board, because the bare circuit board is used to support components and play the role of electrical interconnection between the pins of components. It is a key factor affecting the quality and reliability of electronic products and the difficulty, cost, and speed of the entire manufacturing process. It must be customized according to the design requirements and product properties. Bare circuit board, referred to as bare board, refers to a circuit board that has not yet been installed with components. It is also called printed circuit board, printed circuit board, printed circuit board, printed board, circuit board, circuit board, printed board. Bare boards are generally customized on demand by manufacturers specializing in the manufacture of printed circuit boards. Taking a multi-layer circuit board as an example, the process flow of bare board manufacturing is roughly as follows: making inner conductive patterns - blackening / browning and lamination - drilling holes on a multi-layer copper-clad insulating substrate - performing hole metallization - making outer conductive patterns and removing metal anti-corrosion film or organic anti-corrosion film - applying solder resist - making solder resist patterns and generating welding areas - applying solderability coating to the surface of the welding area - making marking symbols - shipping to manufacturers in the assembly stage.

[0007] The assembly of electronic products is to assemble, match and combine various materials together, and to achieve the fixation of the positions of the materials and the corresponding electrical connections and functional coordination through connection means such as soldering, fastening and bonding. In a narrow sense, the assembly process of installing and soldering components to the circuit board is often called assembly. The product after the components are assembled is generally called an assembled board. In situations where no distinction is needed, bare circuit boards and assembled boards are generally called circuit boards.

[0008] In the past, the assembly technology was mainly based on the through-hole method, that is, the pins of various components, connectors, functional modules, etc. were inserted into the mounting holes of the bare board, and then the pins were brazed with the hole wall and the pads with solder, so that the components were fixed on the circuit board, and the electrical interconnection between the pins of the components was achieved through the pads, interconnection wires, and relay holes on the circuit board. At present, electronic products are more often assembled using surface mounting technology, that is, firstly, solder paste is applied on the connection pad of the circuit board, that is, the pad, and then the pins of various components, connectors, functional modules, etc. are placed on the solder paste layer of the connection pad, and finally the circuit board is heated to melt the powdered or granular solid metal tin / tin alloy in the solder paste, and the molten solder infiltrates the terminal electrodes / pins of the components and the circuit board pads. When cooled into solid metal, the terminal electrodes of the components are brazed with the connection pads, so that the components are mounted and fixed on the surface of the circuit board, and the electrical interconnection between the components is achieved through the conductive channel formed by the pads, wires, and holes on the circuit board. The assembly of circuit boards is either done by professional assembly factories or by electronic product development organizations. Taking SMT technology as an example, the assembly process of circuit boards is roughly as follows: circuit boards from bare board manufacturers - solder paste is printed on the soldering pads - components are picked up and attached to the surface of the circuit board - heating is performed to reflow the solder paste to achieve soldering of pins and pads.

[0009] Considering the bare board manufacturing and component assembly process of the circuit board as a whole, it can be seen that the key to bare circuit board manufacturing is the process of conductive pattern production, lamination, drilling and hole metallization, solder mask pattern production and solderability coating, while solder paste coating, component insertion and welding are the key processes in the assembly production stage. Further analysis shows that these processes are essentially for the purpose of achieving the installation and fixation of components and the electrical interconnection between components. Among them, the manufacturing of conductive patterns is related to the fineness and electrical performance of the circuit board circuit; the manufacturing of solder mask patterns and solderability coating are completed at the bare board stage, but they are the basis of production at the assembly stage; and drilling and hole metallization affect the connection density, mechanical properties, application environment, and matching degree of the installation and fixation of the plug-in on the one hand, and determine the electrical performance and reliability of the Z-direction interconnection between the horizontal conductive layers of the circuit board on the other hand, and directly affect the difficulty of the manufacturing process of the conductive pattern of the horizontal electrical connection of the circuit board.

[0010] With the progress of social economy, the requirements for electronic products are getting higher and higher, the components are getting smaller, the functions are getting stronger, the number of pins is increasing, the requirements for conductive patterns and solder mask patterns are becoming more and more precise, and the requirements for holes are getting smaller and deeper. Whether in the bare board manufacturing stage or the component assembly stage, various process problems affect each other, making the technical difficulty of circuit board manufacturing increasingly greater.

[0011] For example, in the current hole metallization process, in order to meet the minimum reliability and electrical requirements of the physical carrier of Z-direction electrical interconnection, that is, the minimum thickness of the hole wall conductive layer, metal copper must be deposited on the hole wall by electroplating technology, and the electroplating process requires a conductive channel. The existing technology, whether it is graphic electroplating, full-board electroplating etching to make conductive graphics, or laser selective removal of copper foil to make conductive patterns, has to use the original copper foil on the substrate as the power line for copper plating on the hole wall. While electroplating copper to thicken the hole wall conductive layer, the thickness of the conductive layer will inevitably increase synchronously with the hole wall on the basis of the inherent copper foil on the board surface. Moreover, due to the step-by-step factors of the power line, and also due to the depth capacity and the plating capacity of the electroplating process, the thickness of the final board surface deposition layer will be greater than the hole wall deposition layer. The IPC-6012 standard has clear requirements for the thickness of the metallized hole wall, which is at least 20μm. The current PCB manufacturing process has limited deep plating capability. When the hole wall copper thickness reaches 20μm, the increased copper thickness on the board exceeds the hole wall copper thickness. When added to the original copper foil thickness of the material of 18um, the total copper thickness exceeds 40μm, or even reaches 50um. However, this electroplating thickened hole must simultaneously thicken the original copper foil on the board. It does not enhance the performance of the PCB due to the consumption of copper resources, nor does it reduce the difficulty of subsequent processes. On the contrary, such a process has a negative impact on the performance and process of the PCB in the following aspects:

[0012] First, the thickness of the hole wall conductive layer is smaller than that of the board surface conductive layer, resulting in inconsistent electrical properties between the Z-direction conductive link and the X and Y plane conductive link. Second, the conductive layer produced by the hole wall electroplating process of the circuit board becomes the top layer of the conductive pattern conductive layer in the future. Under the action of the skin effect, it is the main medium for the transmission of high-frequency electrical signals. The quality of the copper layer deposited by electroplating technology in the production of circuit boards is slightly lower than the purity of the copper foil produced by electroforming or rolling technology. The crystal is slightly rougher, and the electrical and mechanical properties are slightly worse. Therefore, the increase in the thickness of the conductive layer is not conducive to high-speed and high-frequency signal transmission. Third, the increase in the thickness of the copper foil and the lateral etching caused by it are factors that restrict the fineness of the conductive pattern. In the process of manufacturing the conductive pattern by chemical etching technology, the etching liquid contacts the copper foil for etching. In addition to the vertical etching to the depth of the copper foil, the etching liquid contacts the two sides of the wire, so that the etching is also carried out on the two sides of the wire at the same time. The thicker the etched copper layer and the longer the time, the more serious the lateral etching phenomenon. The lateral etching not only reduces the width of the wire, but also causes wire breakage in severe cases. Fourth, the uneven thickness of the copper foil is a bottleneck for the widespread application of laser conductive patterning technology. Obviously, the thicker the copper foil, the greater the laser energy required, the more times the processing is required, and the slower the processing process will be; the more uneven the thickness of the copper foil, the more difficult the photo-etching process is, either the laser power applied to the area with thicker copper foil is too small, the copper is not completely removed, and the residual copper affects the insulation performance, or the laser power applied to the area with thinner copper foil is too large, the insulating material under the copper foil is ablated, affecting the quality of the circuit board.

[0013] The problem with the existing technology in the conductive pattern manufacturing process is that the traditional etching method is complicated and requires the use of a pattern transfer process to manufacture an anti-etching mask. The pattern transfer process requires the use of photosensitive materials, and a mask plate for selective exposure needs to be manufactured first. After the conductive pattern is etched, the anti-etching mask needs to be removed. The under-etching, over-etching, side-etching, and uneven etching that occur with etching often cause the quality control factors to lose sight of each other, and there are many problems. Although the laser directly removes organic materials to make anti-etching masks, anti-plating masks, and solder masks, and directly removes conductive copper foil to make conductive patterns, the process is simple, but because the laser spot diameter is small, it needs to be processed point by point and line by line, which is slow and inefficient. In addition, in the process of directly removing conductive copper foil from the conductive pattern by laser, because the copper foil layer on the substrate becomes thicker and more uneven after the hole metallization, it is difficult for the laser energy to change accordingly in real time, and it is difficult to ensure the removal quality.

[0014] The problem with solder mask pattern making and solderability coating is that, like the manufacturing of conductive patterns, the traditional technology of solder mask pattern making is a pattern transfer process that requires the use of photosensitive materials and the manufacture of masks for selective exposure. The baking and exposure effects interfere with each other, making quality control difficult, and defects such as pads on solder mask frequently appear. Whether it is hot air leveling or chemical nickel-gold technology for solderability coating, the ingredients are complex and the process is cumbersome, which will bring confusion about unclear welding mechanism and affect reliability.

[0015] The inventor of application number CN201410190917.2 has disclosed a method for selectively electroplating conductive holes in a circuit board, which is suitable for the direct electroplating hole metallization process of a polymer conductive film method. The technical solution is to use a material that is resistant to electroplating, resistant to polymer conductive film deposition, and can be peeled off, that is, a polyester film that is peelable and coated with a silicone rubber adhesive, to mask all areas of the board surface, and expose the surface of the hole wall after drilling. Because these materials have the properties of resisting the pretreatment required for the deposition of polymer conductive films and resisting the deposition of polymer conductive films, in the subsequent direct electroplating process of polymer conductive films, polymer conductive films will only be added to the hole walls. During electroplating, the electroplating power supply uses the copper foil on the board surface as a conductive link channel to provide current to the hole walls, thereby realizing electroplating processing that only deposits copper on the hole walls. The problem is that the hole metallization process of direct electroplating of polymer conductive film method needs to be treated with a solution of 100g / L or more permanganate concentration at a temperature of 90 degrees Celsius for 70 seconds, which will produce destructive oxidation effects on both the peelable glue and the adhesive of the polyester film, causing the masking material, which has a weak adhesion to the substrate, to have a lower bonding strength with the copper foil, resulting in bone separation, delamination, seams, and openings, which will inevitably lead to poor masking board surface effects. After the hole wall is thickened by electroplating copper, the problem of uneven thickness of the copper foil on the copper foil board surface will be aggravated due to the infiltration, overflow, and immersion of the solution. In addition, the direct electroplating hole metallization process of polymer conductive film method has a limited scope of application and is not suitable for multi-layer circuit boards. Considering factors such as quality and cost, it is even more necessary to solve the problems of only metallization and electroplating hole wall faced by traditional chemical copper deposition hole metallization technology, black hole direct electroplating hole metallization technology, and palladium film method direct electroplating hole metallization technology. Because these technologies require acid, alkali or organic solvent treatment before hole metallization, it is obvious that the technical solution of using strippable colloidal materials is not strong enough and cannot be applied to mainstream hole metallization technology. It is necessary to find more suitable materials and methods.

[0016] In summary, it is not difficult to see that the current circuit board manufacturing technology includes a series of indirect processing, chemical treatment, and wet manufacturing processes. These single-function processes have their own inherent technical limitations, and they are mutually restrained and mutually dependent, which is the fundamental reason for limiting higher quality, higher efficiency, and more environmentally friendly. It is necessary to improve and update each single-function process, and also to optimize and upgrade it as a whole. Summary of the invention

[0017] In view of the deficiency of the prior art that the thickened holes and circuits cannot be plated separately, the present invention has developed a new manufacturing method. The technical solution of the present invention is as follows:

[0018] A method for making a circuit board by using laser to process electroplated holes, circuit masks and conductive patterns respectively, drilling holes and depositing a thin metal layer in the holes and on the board surface, pasting a non-photosensitive masking film, laser removing the masking layer covering the hole wall to expose the hole wall, only electroplating to thicken the conductive layer in the hole, and then using laser to make a circuit part anti-plating pattern and pattern electroplating, and using laser to make a conductive pattern and a solder resist pattern; the steps are:

[0019] (1) Depositing an initial conductive layer on a double-sided, multi-layer circuit board in production after drilling, and electroplating copper to a thickness that can withstand subsequent processes;

[0020] (2) Affixing a non-photosensitive organic film to the board surface as an anti-plating masking film;

[0021] (3) using a laser to remove the masking material covering the hole wall area to produce an anti-plating pattern, and using a laser to remove the anti-plating masking film layer on the surface of the clamping point of the electroplating fixture to expose the copper surface in the contact area with the electroplating fixture;

[0022] (4) electroplating, depositing copper on the hole wall to thicken the conductive layer to the required thickness;

[0023] (5) Use laser to remove the anti-plating masking film layer on the pad area and the circuit area, and add the plating window of the pad and circuit area on the hole plating window;

[0024] (6) Electroplating: deposit copper on the hole wall, pad and circuit to the thickness required for final inspection and add other metals.

[0025] (7) Use laser to remove the anti-plating masking film on the non-circuit area;

[0026] (8) Use laser to remove the copper foil in the non-circuit area to produce a conductive pattern;

[0027] (9) Full board coating and one-time curing of solder resist material;

[0028] (10) Use laser to remove organic materials on the conductors in the welding area at the assembly site, create solder resist patterns, and clean and treat the surface of the welding area for solderability;

[0029] (11) Add solder to the connection pads, mount and insert components, and perform reflow soldering and / or wave soldering.

[0030] The non-photosensitive organic film in step (2) is composed of several layers of different shapes and compositions, wherein the layer in contact with the circuit board has viscosity and fluidity. Step (2) includes depositing non-photosensitive organic film-forming substances on the board surface and hole wall by electrophoresis, vacuum coating, vapor deposition and other technologies; including coating liquid photosensitive materials and dry photosensitive films by using existing technologies.

[0031] The step (9) comprises attaching a dry photosensitive film and a dry non-photosensitive film under a certain pressure and temperature.

[0032] The step (9) or (10) includes removing organic materials on the conductors in the welding area by laser at the bare board manufacturing site to produce a solder resist pattern and clean the surface of the welding area.

[0033] The step (9) or (10) further includes continuing the circuit board manufacturing process at the bare board manufacturing site using existing technologies and materials.

[0034] The present invention discloses a method for manufacturing a circuit board by using laser to process electroplated holes, circuit masks and conductive patterns respectively. After chemical copper plating or electroplating thin copper, a non-photosensitive anti-plating mask is attached, and the mask material is directly removed by laser to form a pattern of only electroplated holes and then electroplating is performed; then, the mask material on the pad area and the circuit area is directly removed by laser, and then the holes, pads and circuits are electroplated at the same time; then, the conductive pattern and solder resist pattern are manufactured by laser.

[0035] Step (1) deposits an initial conductive layer on the finished product of the double-sided, multi-layer circuit board after drilling, and electroplates copper to a thickness that can withstand subsequent processes. The purpose of making a thin copper on the initial conductive layer is to increase the reliability of the process, and its thickness can reach the lower limit of ensuring process reliability, for example, after traditional chemical copper deposition, or after black hole formation using a carbon film method, electroplating 1μm-5μm thin copper.

[0036] Step (2) affixing a non-photosensitive organic film to the board surface as an anti-plating masking film. The prior art generally uses a photosensitive dry film as an anti-plating mask. The photosensitive dry film is a three-layer structure. The photosensitive adhesive coating is between the carrier film and the protective film. It is composed of an adhesive and a photopolymerizable monomer, etc. The pattern forming process is relatively complicated and requires the steps of photo-drawing, film pasting, exposure, and development. Moreover, it is expensive, has low strength, and is relatively thick, generally above 20 μm. The resolution is limited and the masking effect is poor. The masking film of the present invention does not need to have photosensitive properties. A general pre-coated pressure-sensitive coating film or a heat-sensitive coating film can meet the requirements. The film is hot-pressed and directly removed by laser to form a pattern. The process is simple. Moreover, the film has high resolution, low price, high strength, good masking ability, can be removed in steps, and can withstand multiple electroplating processes. For example, a 20 μm thick heat-sensitive PI, PVC, PC, PET, or PP film can be hot-pressed as an anti-plating mask. Parylene can also be used as an anti-plating mask.

[0037] The anti-plating masking film includes a dry film made of single-component, multi-component, composite thermosetting, photosetting, heat-pressing attachable, photosensitive and non-photosensitive materials, and its thickness is greater than the total metal thickness thickened on the circuit, ranging from 2μm to 1000μm. It is preferably a thermosetting dry film that can be heat-pressed and has solder resistance, and the preferred film thickness is 5μm-500μm.

[0038] The non-photosensitive organic film in step (2) is composed of several layers of different shapes and compositions, wherein the layer in contact with the circuit board has viscosity and fluidity; step (2) includes depositing non-photosensitive organic film-forming substances on the board surface and hole walls by electrophoresis, vacuum coating, vapor deposition and other technologies; including using existing technologies to coat liquid photosensitive materials and dry photosensitive films.

[0039] Step (3) uses a laser to remove the masking material covering the hole wall area to produce an anti-electroplating pattern, and uses a laser to remove the anti-electroplating masking film layer on the surface of the clamping point of the electroplating fixture to expose the copper surface of the contact area with the electroplating fixture. The laser removes the anti-electroplating masking film layer on the hole area to open a window for the liquid to enter the hole. For example, a pulsed IR laser with a wavelength of 1064nm is used, with the inner diameter of the hole as the outer contour, to remove the masking film covering the hole wall by ring cutting into blocks or photoetching point by point to expose the hole wall. In order to solve the problems of too small total area, uneven distribution of electric lines, and difficult control of current density when electroplating the hole wall, when making the hole wall electroplating pattern, a laser can be used to remove the dead copper area with no electrical function in the non-circuit part, or the area where its conductive layer needs to be removed and does not have a negative impact on the subsequent removal process, or the area where the copper thickness does not affect its function, or the area where increasing the copper thickness has a positive impact on the function, so as to increase the conductive area area, disperse the electric lines, and form a pattern that is conducive to the balanced electroplating process of the plated hole wall.

[0040] The pattern of the electroplated hole wall made by laser also includes removing dead copper areas with no electrical function that are not circuits and are spaced more than 30μm from the circuits, preferably more than 50μm apart, or areas where the conductive layer needs to be removed and does not have a negative impact on the subsequent removal process, or areas where the copper thickness does not affect its function, or areas where increasing the copper thickness has a positive effect on the function. The anti-plating mask film forms a balanced electroplating pattern that is beneficial to the plated hole wall.

[0041] When using a laser to remove an anti-plating mask film, the focused laser light power density should be set to a level greater than the minimum power density required to remove the material, for example, greater than 1.2 times the minimum light power density required for the material, but lower than or close to the minimum light power density required to remove the underlying metal copper layer.

[0042] Step (4) electroplating, depositing copper on the hole wall to thicken the conductive layer to the required thickness. The control point of this step is the electroplating time. At this time, all areas on the board surface except the hole wall and the electroplating balance block are covered with a mask. The mask is an insulating material. Although it is in contact with the electroplating solution, copper cannot be deposited on the surface. Therefore, only the hole wall and the balance block can deposit copper during the electroplating process. If the electroplating time is sufficient, a copper deposition layer of sufficient thickness can be obtained on the hole wall, achieving the purpose of selectively controlling the copper thickness of the hole wall.

[0043] Step (5) Use laser to remove the anti-plating masking film layer on the pad area and the circuit area, and add a plating window for the pad and circuit area on the hole plating window.

[0044] Step (6) electroplating, depositing copper on the hole wall, pad and circuit to the thickness required for final inspection and adding other metals. This step includes electroplating copper metal first, and then electroplating tin, nickel gold and other solderability protection metals. The control point of the process is the electroplating time. The current circuit board manufacturing technology generally uses photosensitive dry film as an anti-electroplating mask. The material is mostly UV-curable. The thickness of the masking pattern formed by it is within a certain range and cannot be too thin or too thick. Because the material is cross-linked and polymerized during hot pressing and UV exposure to become a mask, and it must be relatively easy to be decomposed by the film removal chemical solution later, the mask produced by such technology can only be an imperfect sub-solid to some extent. If it is too thick, the resolution is low, and the required exposure is large. On the one hand, the thin layer close to the light source is overexposed, and on the other hand, the thin layer far from the light source is underexposed; if the inherently fragile sub-solid material is too thin, it will not reach the mechanical strength required for masking, resulting in infiltration.

[0045] The present invention uses laser to directly remove and manufacture masking patterns, and non-photosensitive materials can be used. The material itself is a fully polymerized solid, and has sufficient masking ability regardless of thickness. Even if the electroplating time is long, it will not fall off or dissolve. For circuit boards that require thicker circuit copper, a thicker material can be selected in step (2), for example, a mask with a thickness of 300 μm is selected. After the mask material on the surface of the required circuit is removed by laser, the electroplating time is controlled until the thickness of the single metal or multiple metal coating approaches or reaches 300 μm.

[0046] Steps (5) and (6) are used to simultaneously electroplate metal copper on the line and on the hole wall for thickening, and to electroplate metals such as nickel, gold or tin as a solderability protective layer. When the copper foil thickness on the copper-clad board can meet the requirements of the electrical design for the copper thickness of the line, steps (5) and (6) can be skipped and step (7) can be performed directly.

[0047] Step (7) uses laser to remove the anti-plating masking film on the non-circuit area; when using laser to remove the anti-plating masking film on the non-circuit area, when the ratio of the perimeter of the area to be removed to the diameter of the focused laser beam is small, preferably less than 10, the masking film on the surface of the substrate and the conductive metal copper thereunder are removed by point-by-point and line-by-line photolithography using a focused laser beam; when the ratio of the perimeter of the area to be removed to the diameter of the focused laser beam is large, preferably greater than 15, the masking film on the surface of the substrate and the conductive metal copper thereunder are first removed by point-by-point photolithography using a focused laser beam along the inner side of the envelope of the area to be removed and with the envelope as the boundary, until a closed insulating channel is formed around the unremoved portion of the area, and then a laser beam with a diameter lower than the minimum optical power density required to remove the metal copper is used to heat the unremoved area, so that the anti-plating masking film thereon and the conductive metal copper thereunder are simultaneously detached from the substrate surface and removed.

[0048] When using laser to remove the anti-plating masking film on the non-circuit area, the focused laser light power density used is kept greater than the minimum power density required to remove the organic material, preferably greater than 1.2 times the minimum light power density required to remove the organic material and lower than or close to the minimum light power density required to remove the metal layer covered thereunder, and the focused laser beam diameter is changed according to the shape and size of the removed area to reduce or remove the overlap of the laser processing area and improve the processing efficiency. When laser removing the anti-plating masking film on the non-circuit area, lasers of the same wavelength and pulse width, as well as lasers of different wavelengths and pulse widths, can be used to complete the process under different parameters such as spot diameter, focal depth, and light power density.

[0049] Step (8) uses a laser to remove the copper foil in the non-circuit area to produce a conductive pattern. Because the present invention can selectively electroplate holes, the technology of using a laser to remove the conductive material in the non-circuit area is easier to implement. In the current common circuit board manufacturing technology, after the hole metallization electroplating process, due to the limitation of the hole plating capacity of the hole system, the deposition rate of copper is different in different areas on the same substrate material, resulting in a large difference in the thickness of the total conductive layer. In this way, when using laser photoetching to remove the conductive layer of the non-circuit part, if the laser parameters do not change with the copper thickness, either the copper is not completely removed from the area with a large total copper thickness, and the residual copper affects the insulation performance, or excessive energy is applied to the area with a small total copper thickness, resulting in a problem of ablation of the insulating material.

[0050] The technical solution of selectively electroplating holes and conductive patterns of the present invention can avoid copper deposition in non-circuit areas, especially in the laser photoetching removal path, so that the conductive layer under the laser photoetching path is kept as the original copper foil with uniform thickness, thereby reducing the difficulty of laser processing. The present invention adopts the striping and stripping method / Striping & Stripping of German-Chinese technology, firstly using laser photoetching to vaporize the conductive material point by point and layer by layer to form a closed dividing line, and subdividing the conductive layer area to be removed into small pieces with mutually insulated areas within a certain range, which is called striping; then, using laser to heat the small pieces to reduce the bonding force between the small pieces and the substrate, so that the small pieces are separated from the substrate in pieces, which is called stripping.

[0051] When implementing laser striping and stripping technology, it is not necessary to remove the anti-plating masking film in the non-circuit area first. For example, when using ultraviolet laser processing or picosecond laser striping, the masking film and the copper foil layer underneath it can be vaporized by laser photo-erosion until the insulating substrate layer is stopped, forming an insulating channel; when stripping, the masking film and the copper foil layer underneath it are heated together, and the pieces are stripped off through thermal deformation and reduced bonding strength with the insulating substrate. In order to be suitable for laser processing, the anti-plating masking film can be selected from colored materials to produce better absorption effects.

[0052] When laser removal of copper foil on non-circuit areas, the focused laser light power density used is kept greater than the minimum light power density required to remove the conductive metal copper layer, and less than 3 times the minimum light power density required to remove the conductive metal copper layer. The focused laser beam diameter is changed according to the shape and size of the removed area to reduce or remove the overlap of the laser processing area and improve the processing efficiency. When laser removal of copper foil on non-circuit areas, lasers with the same wavelength and pulse width, as well as lasers with different wavelengths and pulse widths, can be used under different parameters such as spot diameter, focal depth, and light power density.

[0053] Step (9) coating the entire board with solder resist material and curing it at one time.

[0054] The step (9) comprises attaching a dry photosensitive film and a dry non-photosensitive film under a certain pressure and temperature.

[0055] The prior art generally uses liquid photosensitive ink as solder resist, which contains adhesives and photopolymerizable monomers. The pattern forming process is very complicated and requires multiple processes such as coating, pre-baking, exposure, development, and curing. Moreover, it is expensive, has low resolution, and is difficult to ensure the coating quality between fine pitch connection pads. The solder resist of the present invention does not need to have photosensitive properties. General pre-coated pressure-sensitive coating films and heat-sensitive coating films can meet the requirements. It is cheap and has high resolution, and can produce fine pattern structures. In addition, the present invention uses hot pressing coating, which does not require an additional curing process. The solder resist pattern is left to be produced on-site by laser before component assembly, and the process is simple. For example, a heat-pressed paste with a thickness of 20μm-200μm of thermal-sensitive PI, PVC, PC, PET, and PP films is used as a solder resist, and parylene can also be used as a solder resist.

[0056] The step (9) includes removing organic materials on the conductors in the soldering area with a laser at the bare board manufacturing site, manufacturing a solder mask pattern, and cleaning the soldering area surface. The step also includes continuing the circuit board manufacturing process at the bare board manufacturing site using existing technology and materials.

[0057] Step (10) uses a laser to remove organic materials on the conductor of the welding area at the assembly site to produce a solder resist pattern, and cleans and treats the surface of the welding area for solderability. This step can be completed in one step on the same equipment, or it can be carried out in two steps on different equipment, namely, the first step: making a solder resist pattern and generating a welding area: using a laser to selectively photoetch to remove the solder resist coating on the welding area to produce a solder resist pattern and generate a welding area; the second step is to clean and treat the surface of the welding area for solderability, using another laser to remove the solder resist residue on the surface of the welding area, and slightly photoetching the metal surface layer of the welding area to remove metal oxides, expose a fresh metal surface, and produce solderability that is easily wetted by molten solder.

[0058] The step (10) includes removing organic materials on the conductors in the soldering area with a laser at the bare board manufacturing site, manufacturing a solder resist pattern, and cleaning the soldering area surface. The step (10) also includes continuing the circuit board manufacturing process at the bare board manufacturing site using existing technology and materials.

[0059] Step (11) adds solder to the connection pad, performs component mounting and insertion, performs remelting soldering and / or wave soldering. In the method of the present invention, since the solderable coating layer of the welding area is replaced with a fresh copper surface treated by laser, after step (10), step (11) should be performed in the shortest possible time to avoid oxidation of the connection pad surface, and complete component assembly under the condition of excellent solderability after laser treatment, including performing component insertion and directly applying solder to the laser treated welding area to complete component welding; or directly printing solder paste on the laser treated welding area, and then performing component mounting and reflow soldering; or assembling components according to other technologies.

[0060] The present invention can optimize and shorten the circuit board manufacturing process as a whole, improve quality and efficiency, reduce costs, and be environmentally friendly. Using non-photosensitive materials as anti-plating materials can reduce costs; differentiating the holes and lines for plating makes it easy to control the thickness of the coating; using lasers to step-by-step manufacture the plating hole pattern and the plating line pattern, and using lasers to manufacture the conductive pattern, with fewer steps, more sophisticated conductive patterns can be manufactured. The present invention is suitable for mass production of various circuit boards, and is also suitable for circuit board samples and small batch, multi-variety production.

[0061] The advantages and effects of the present invention are:

[0062] 1. The present invention can selectively electroplate holes and circuits, and the coating thickness can be easily controlled. In particular, only thickened holes can be electroplated, which can solve the problem of thin coating thickness on the hole wall and the problem of inconsistency between the coating thickness on the hole wall and the copper plating thickness on the circuit.

[0063] 2. The present invention uses a laser direct removal method to manufacture electroplated hole walls and electroplated circuit patterns. Non-photosensitive materials can be used as anti-plating materials to reduce costs. In addition, the electroplating resistance is good, and thicker hole wall conductive layers and circuit conductive layers can be manufactured.

[0064] 3. The present invention realizes electroplating of only holes and circuits, and the thickness of the conductive layer of the non-circuit part does not increase. It is suitable for using laser to directly remove the copper foil of the non-circuit part to manufacture conductive patterns. There is no need to remove the anti-plating material, and the steps are few, so that more sophisticated conductive patterns can be manufactured.

[0065] 4. In the laser pattern manufacturing process of the present invention, the focused laser beam diameter is changed according to the shape and size of the removed area, so that the focused beam diameter or its multiple is exactly equal to the width of the area to be removed, which can reduce or eliminate the overlap of the laser processing area and improve the processing efficiency.

[0066] 5. The present invention removes the anti-plating mask at the same time when laser manufacturing the conductive pattern, and no longer requires a special film removal process, which reduces the number of steps.

[0067] 6. The present invention uses a film pre-coated with heat-sensitive and pressure-sensitive solder resist materials as a solder resist, and uses lasers with different wavelengths, pulse widths, and power densities to manufacture solder resist patterns and clean welding areas and perform solderability treatment, which is more efficient and has better treatment effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0068] Figure 1 : Process flow chart of embodiment 1;

[0069] Figure 2 : Process flow chart of embodiment 2;

[0070] Wherein: 1. Insulating substrate 2. Copper layer of copper clad plate 3. Initial conductive layer 4. Electroplated thin copper 5. Anti-electroplating masking film 6. Electroplated hole layer 7. Electroplated copper layer on hole wall, pad and circuit 8. Other metal layers on hole wall, pad and circuit 9. Solder resist material layer 10. Cleaned and solderable surface 11. Solder 11. Components

[0071] In the attached drawings, each letter A\B\C\D\E\F\G\H corresponds to a partial enlarged schematic diagram of each step. DETAILED DESCRIPTION

[0072] The present invention will be further described below in conjunction with the following embodiments. The following embodiments are illustrative, not restrictive, and the protection scope of the present invention cannot be limited by the following embodiments.

[0073] Example 1

[0074] In the electronics industry, copper clad laminate is often used as a basic material to make circuit boards. The copper clad laminate includes an insulating substrate 1 and a copper layer 2 of the copper clad laminate.

[0075] This embodiment takes a double-sided printed circuit board as an example, and the specific processing steps are as follows:

[0076] (1) The copper-clad laminate, a substrate of the circuit board, comprises an insulating substrate 1 and a copper layer 2 of the copper-clad laminate. The copper-clad laminate is drilled, and an initial conductive layer 3 is deposited on the semi-finished product of the double-sided circuit board after the drilling. The copper is electroplated to a thickness that can withstand subsequent processes, thereby forming an electroplated thin copper 4.

[0077] The purpose of making a thin copper layer on the initial conductive layer is to increase the reliability of the process, and the thickness of the thin copper layer only needs to reach the lower limit of ensuring the reliability of the process.

[0078] Chemical copper is deposited on the double-sided board after drilling, and copper electroplating is performed. Specifically, the double-sided board after drilling is brushed to remove the burrs at the hole mouth and clean the board surface. Then normal copper electroplating is performed, and the electroplating parameters are: 10ASF*30min, and the coating thickness is about 5um.

[0079] (2) A non-photosensitive organic film is attached to the board surface as an anti-plating masking film 5. The prior art generally uses a photosensitive dry film as an anti-plating mask. The photosensitive dry film is a three-layer structure. The photosensitive adhesive coating is between the carrier film and the protective film. It is composed of an adhesive and a photopolymerizable monomer, etc. The pattern forming process is relatively complicated and requires the steps of photo-drawing, film attachment, exposure, and development. Moreover, it is expensive, has low strength, and is relatively thick, generally above 20 μm. The resolution is limited and the masking effect is poor. The masking film of the present invention does not need to have photosensitive properties. A general pre-coated pressure-sensitive coating film or a heat-sensitive coating film can meet the requirements. The film is hot-pressed and directly removed by laser to form a pattern. The process is simple. Moreover, the film has high resolution, low price, high strength, good masking ability, can be removed in steps, and can withstand multiple electroplating processes. For example, a 20 μm thick heat-sensitive PI, PVC, PC, PET, or PP film is hot-pressed as an anti-plating mask. Parylene can also be used as an anti-plating mask.

[0080] The anti-plating masking film includes a dry film made of single-component, multi-component, composite thermosetting, photosetting, heat-pressing attachable, photosensitive and non-photosensitive materials, and its thickness is greater than the total metal thickness thickened on the circuit, ranging from 2μm to 1000μm. It is preferably a thermosetting dry film that can be heat-pressed and has solder resistance, and the preferred film thickness is 5μm-500μm.

[0081] Specifically, the double-sided copper-plated board is brushed, the double-sided board surface is roughened and cleaned, and the bonding strength between the copper surface and the polymer film to be bonded is enhanced. Then, the BOPET polymer film with anti-electroplating performance is hot-pressed on the double-sided copper-clad board by a film laminating machine. The film thickness is 10um, and the laminating parameters are: pressure 10kg / cm 2 , temperature 90℃, speed 0.1m / min.

[0082] (3) Use laser to remove the masking material covering the hole wall area to produce an anti-plating pattern, and use laser to remove the anti-plating masking film layer on the surface of the clamping point of the electroplating fixture to expose the copper surface in the contact area with the electroplating fixture. Use laser to remove the anti-plating masking film layer on the hole area to open a window for the liquid to enter the hole.

[0083] In order to solve the problems of too small plating area, uneven distribution of electric lines, and difficult control of current density when electroplating hole walls, laser is used to remove dead copper areas with no electrical function in non-circuit parts when making hole wall electroplating patterns, increase the conductive area, and disperse the electric lines.

[0084] Specifically, this embodiment uses a 20W ultraviolet nanosecond laser machine to remove the BOPET film on the hole wall area, the clamping point of the electroplating fixture, and the electroplating balance block. The circuit board is placed on the laser equipment adsorption table, the engineering data of the laser processing is imported, the circuit board is accurately aligned with the processing data, and the BOPET film is removed by laser photoetching. After the top surface processing is completed, the circuit board is turned over, and the film on the bottom surface of the copper clad board is removed in the same way. The processing parameters are as follows:

[0085] Power / W Frequency / kHz Pulse width / ns Processing speed / mm / s Processing times 5 150 20 800 1

[0086] (4) Electroplating: deposit copper on the hole wall to thicken the conductive layer to the required thickness, forming the hole electroplating layer 6. The control point of this step is the electroplating time. At this time, all areas on the board except the hole wall and the electroplating balance block are covered with a mask. The mask is an insulating material. Although it is in contact with the electroplating solution, copper cannot be deposited on the surface. Therefore, only the hole wall and the balance block can deposit copper during the electroplating process. If the electroplating time is sufficient, a copper deposition layer of sufficient thickness can be obtained on the hole wall, achieving the purpose of selectively controlling the copper thickness of the hole wall.

[0087] Specifically, since the electroplating area is small, a low current density is used for electroplating in this step, and the electroplating parameters are: 10ASF*50min, and the coating thickness is about 15um.

[0088] (5) Use laser to remove the anti-plating masking film layer on the pad area and the circuit area, and add plating windows for the pad and circuit area on the hole plating windows.

[0089] Specifically, the processing method and processing parameters are the same as step (3).

[0090] (6) Electroplating: depositing copper on the hole wall, pad and circuit to the required thickness for final inspection and adding other metals to form electroplated copper layer 7 on the hole wall, pad and circuit and other metal layers 8 on the hole wall, pad and circuit.

[0091] This step includes electroplating copper metal first, and then electroplating solderability protective metals such as tin, nickel and gold. The control point of the process is the electroplating time. The current circuit board manufacturing technology generally uses photosensitive dry film as an anti-plating mask. The material is mostly UV-curable. The thickness of the masking pattern formed is within a certain range, and it cannot be too thin or too thick. Because the material is cross-linked and polymerized during hot pressing and UV exposure to become a mask, and it must be able to be easily decomposed by the film removal chemical solution later, so the mask produced by such technology can only be an imperfect sub-solid to some extent. If it is too thick, the resolution is low, and the required exposure is large. On the one hand, the thin layer close to the light source will be overexposed, and on the other hand, the thin layer far away from the light source will be underexposed; if the sub-solid material, which is already fragile, is too thin, it will not reach the mechanical strength required for masking, resulting in infiltration.

[0092] Specifically, this step includes electroplating copper metal first, and then electroplating nickel and gold. The electroplating copper parameters are: 12ASF*60min, and the plating thickness is about 20um.

[0093] After further copper electroplating, soft gold is electroplated on the hole wall, pads and circuits as a solderable metal protective layer. Soft gold electroplating parameters: 0.3ASD*10min, coating thickness is about 2um.

[0094] (7) Remove the BOPET anti-plating masking film on the non-circuit area with laser. Specifically, the processing method and processing parameters are the same as step (3).

[0095] (8) Use laser to remove the copper foil in the non-circuit area to produce a conductive pattern. Because the present invention can selectively plate holes, the technology of using laser to remove the conductive material in the non-circuit area is easier to implement. In the current common circuit board manufacturing technology, after the hole metallization electroplating process, due to the limitation of the hole plating capacity of the hole system, the deposition rate of copper is different in different areas on the same substrate material, resulting in a large difference in the thickness of the total conductive layer. In this way, when using laser photoetching to remove the conductive layer of the non-circuit part, if the laser parameters do not change with the copper thickness, either the copper is not completely removed from the area with a large total copper thickness, and the residual copper affects the insulation performance, or excessive energy is applied to the area with a small total copper thickness, resulting in a problem of ablation of the insulating material.

[0096] The technical solution of selectively electroplating holes and conductive patterns of the present invention can avoid copper deposition in non-circuit areas, especially in the laser photoetching removal path, so that the conductive layer under the laser photoetching path is kept as the original copper foil with uniform thickness, thereby reducing the difficulty of laser processing. The present invention adopts the striping and stripping method / Striping & Stripping of German-Chinese technology, firstly using laser photoetching to vaporize the conductive material point by point and layer by layer to form a closed dividing line, and subdividing the conductive layer area to be removed into small pieces with mutually insulated areas within a certain range, which is called striping; then, using laser to heat the small pieces to reduce the bonding force between the small pieces and the substrate, so that the small pieces are separated from the substrate in pieces, which is called stripping.

[0097] When implementing laser striping and stripping technology, it is not necessary to remove the anti-plating masking film in the non-circuit area first. For example, when using ultraviolet laser processing or picosecond laser striping, the masking film and the copper foil layer underneath it can be vaporized by laser photo-erosion until the insulating substrate layer is stopped, forming an insulating channel; when stripping, the masking film and the copper foil layer underneath it are heated together, and the pieces are stripped off through thermal deformation and reduced bonding strength with the insulating substrate. In order to be suitable for laser processing, the anti-plating masking film can be selected from colored materials to produce better absorption effects.

[0098] When laser removal of copper foil on non-circuit areas, the focused laser light power density used is kept greater than the minimum light power density required to remove the conductive metal copper layer, and less than 3 times the minimum light power density required to remove the conductive metal copper layer. The focused laser beam diameter is changed according to the shape and size of the removed area to reduce or remove the overlap of the laser processing area and improve the processing efficiency. When laser removal of copper foil on non-circuit areas, lasers with the same wavelength and pulse width, as well as lasers with different wavelengths and pulse widths, can be used under different parameters such as spot diameter, focal depth, and light power density.

[0099] Specifically, this embodiment uses a 20W infrared nanosecond laser to remove the copper foil on the non-circuit area to produce a conductive pattern. In this embodiment, the conductive layer in the laser-removed area is the original copper foil with uniform thickness, which greatly reduces the difficulty of laser processing. The processing parameters are as follows:

[0100] stage Power / W Frequency / kHz Pulse width / ns Processing speed / mm / s Processing times Remark Envelope insulation 15 200 100 800 1 Focus Striping and Sharding 15 200 100 800 1 Focus Heating stripping 30 200 100 900 1 Defocus

[0101] (9) The entire board is coated with solder resist material and cured at one time to form a solder resist material layer 9. The prior art generally uses liquid photosensitive ink as a solder resist. The solder resist contains adhesives and photopolymerizable monomers. The pattern forming process is very complicated and requires multiple steps such as coating, pre-baking, exposure, development, and curing. Moreover, it is expensive and has low resolution. It is difficult to ensure the coating quality between fine pitch connection pads. The solder resist of the present invention does not need to have photosensitive properties. General pre-coated pressure-sensitive coating films and heat-sensitive coating films can meet the requirements. They are cheap and have high resolution, and can produce fine pattern structures. In addition, the present invention uses hot pressing coating, which does not require an additional curing process. The solder resist pattern is left to be produced on-site by laser before component assembly, and the process is simple. For example, a heat-sensitive PI, PVC, PC, PET, or PP film with a thickness of 20μm-200μm is used as a solder resist, and parylene can also be used as a solder resist.

[0102] Specifically, the KSM-386 thermosetting ink produced by Suzhou Guangxin Photosensitive New Materials Co., Ltd. is printed on the double-sided board by screen printing and fully cured at one time. The curing conditions are: 150° C.*30 min. The thickness of the solder resist ink is about 20 um.

[0103] (10) At the assembly site, a laser is used to remove organic materials on the conductor of the welding area to produce a solder resist pattern, and the surface of the welding area is cleaned and treated for solderability to form a cleaned and solderable surface 10; this step can be completed in one step on the same equipment, or it can be performed in two steps on different equipment, namely, the first step: making a solder resist pattern to generate a welding area: using a laser to selectively photoetch to remove the solder resist coating on the welding area to produce a solder resist pattern and generate a welding area; the second step is to clean and treat the surface of the welding area for solderability, using another laser to remove the solder resist residue on the surface of the welding area, and slightly photoetching the metal surface layer of the welding area to remove metal oxides, exposing a fresh metal surface, and producing solderability that is easily wetted by molten solder.

[0104] Specifically, this embodiment first uses a 20W infrared nanosecond laser machine to remove the solder resist ink in the welding area, places the circuit board on the laser equipment adsorption table, imports the engineering data of laser processing, accurately aligns the circuit board with the processing data, and removes the solder resist ink by laser photoetching. After the top surface processing is completed, turn the circuit board over and use the same method to remove the ink on the bottom surface of the copper clad board. The processing parameters are as follows:

[0105] Power / W Frequency / kHz Pulse width / ns Processing speed / mm / s Processing times 6 200 100 1000 1

[0106] Then, a UV picosecond laser with lower single pulse energy was used to clean and treat the weld area. The processing parameters were as follows:

[0107] Power / W Frequency / kHz Pulse width / ps Processing speed / mm / s Processing times 10 1000 12 2000 1

[0108] (11) Add solder 11 to the connection pad, mount and insert the component 12, and perform remelting soldering and / or wave soldering. In the method of the present invention, since the solderable coating layer of the welding area is replaced by the fresh copper surface treated by laser, after the completion of step (10), step (11) should be performed in the shortest possible time to avoid oxidation of the connection pad surface, and complete the component assembly under the condition of excellent solderability after laser treatment, including inserting components and directly applying solder to the laser treated welding area to complete component welding; or directly printing solder paste on the laser treated welding area, and then mounting components and reflow soldering; or assembling components according to other technologies.

[0109] Example 2

[0110] In the electronics industry, copper clad laminate is often used as a basic material to make circuit boards. The copper clad laminate includes an insulating substrate 1 and a copper layer 2 of the copper clad laminate.

[0111] This embodiment takes a four-layer circuit board with inner layer circuits fabricated as an example, and the specific processing steps are as follows:

[0112] (1) The copper-clad laminate of the circuit board substrate comprises an insulating substrate 1 and a copper layer 2 of the copper-clad laminate. The copper-clad laminate is drilled, and chemical copper is deposited on the four-layer circuit board with the holes drilled and the inner layer circuits completed to form an initial conductive layer 3, and copper is electroplated to form an electroplated thin copper 4;

[0113] Specifically, the drilled circuit board is brushed to remove the burrs at the hole and clean the board surface. Then, copper electroplating is performed after removing the glue residue. The electroplating parameters are: 10ASF*35min, and the coating thickness is about 5um.

[0114] (2) A non-photosensitive polymer film is attached to the board surface as an anti-plating masking film 5.

[0115] Specifically, the four-layer circuit board after thin copper electroplating is brushed and dried, and then hot-pressed with anti-electroplating polymer film BOPP, the film thickness is 10um, and the bonding parameters are: pressure 15kg / cm 2 , temperature 100℃, speed 0.1m / min.

[0116] (3) Use laser to remove the masking material covering the hole wall area to produce an anti-plating pattern, and use laser to remove the anti-plating masking film layer on the surface of the clamping point of the electroplating fixture to expose the copper surface in the contact area with the electroplating fixture.

[0117] Specifically, this embodiment uses a 20W ultraviolet nanosecond laser machine to remove the BOPP film on the hole wall area, the clamping point of the electroplating fixture, and the electroplating balance block. The circuit board is placed on the laser equipment adsorption table, the engineering data of the laser processing is imported, the circuit board is accurately aligned with the processing data, and the BOPP film is removed by laser photoetching. After the top surface processing is completed, the circuit board is turned over and the bottom surface film is removed in the same way. The processing parameters are as follows:

[0118] Power / W Frequency / kHz Pulse width / ns Processing speed / mm / s Processing times 6 200 20 600 1

[0119] (4) Electroplating of the exposed holes: depositing copper on the hole wall to thicken the conductive layer to the thickness required for final inspection, thereby forming a hole electroplating layer 6.

[0120] The control point of this step is the electroplating time. At this time, except for the hole wall and the electroplating balance block, all areas on the board are covered with a mask. The mask is an insulating material. Although it is in contact with the electroplating solution, copper cannot be deposited on the surface. Therefore, only the hole wall and the balance block can deposit copper during the electroplating process. If the electroplating time is sufficient, a copper deposition layer of sufficient thickness can be obtained on the hole wall, achieving the purpose of selectively controlling the copper thickness of the hole wall.

[0121] Since the electroplating area is small, a low current density is used for electroplating in this step. The electroplating parameters are: 10ASF*55min, and the coating thickness is about 15um.

[0122] (5) Use laser to remove the anti-plating masking film layer on the pad area and the circuit area, and add plating windows for the pad and circuit area on the hole plating windows.

[0123] Specifically, the processing method and processing parameters are the same as step (3).

[0124] (6) Electroplating: depositing copper on the hole wall, pad and circuit to the required thickness for final inspection and adding other metals to form electroplated copper layer 7 on the hole wall, pad and circuit and other metal layers 8 on the hole wall, pad and circuit.

[0125] This step includes electroplating copper metal first, and then electroplating solderability protective metals such as tin, nickel and gold. The control point of the process is the electroplating time. The current circuit board manufacturing technology generally uses photosensitive dry film as an anti-plating mask. The material is mostly UV-curable. The thickness of the masking pattern formed is within a certain range, and it cannot be too thin or too thick. Because the material is cross-linked and polymerized during hot pressing and UV exposure to become a mask, and it must be able to be easily decomposed by the film removal chemical solution later, so the mask produced by such technology can only be an imperfect sub-solid to some extent. If it is too thick, the resolution is low, and the required exposure is large. On the one hand, the thin layer close to the light source will be overexposed, and on the other hand, the thin layer far away from the light source will be underexposed; if the sub-solid material, which is already fragile, is too thin, it will not reach the mechanical strength required for masking, resulting in infiltration.

[0126] The present invention uses laser to directly remove and manufacture masking patterns, and non-photosensitive materials can be used. The material itself is a fully polymerized solid, and has sufficient masking ability regardless of thickness. Even if the electroplating time is long, it will not fall off or dissolve. For circuit boards that require thicker circuit copper, a thicker material can be selected in step (2), for example, a mask with a thickness of 300 μm is selected. After the mask material on the surface of the required circuit is removed by laser, the electroplating time is controlled until the thickness of the single metal or multiple metal coating approaches or reaches 300 μm.

[0127] This step includes electroplating copper metal first, and then electroplating nickel and gold. The electroplating copper parameters are: 12ASF*70min, and the coating thickness is about 20um.

[0128] After the copper plating is completed, soft gold is electroplated on the hole wall, pads and circuits as a solderable metal protective layer. The soft gold plating parameters are: 0.3ASD*15min, and the plating thickness is about 2um.

[0129] (7) Use laser to remove the anti-plating mask film on the non-circuit area.

[0130] Specifically, the BOPP anti-plating masking film on the four-layer circuit board is completely removed by laser, and the removal method and parameters are the same as step (3).

[0131] (8) Laser removes the copper foil on the non-circuit area to produce a conductive pattern.

[0132] Specifically, this embodiment uses a 20W infrared nanosecond laser to remove the copper foil on the non-circuit area to produce a conductive pattern. In this embodiment, the conductive layer in the laser-removed area is the original copper foil with uniform thickness, which greatly reduces the difficulty of laser processing. The processing parameters are as follows:

[0133] stage Power / W Frequency / kHz Pulse width / ns Processing speed / mm / s Processing times Remark Envelope insulation 15 200 100 800 1 Focus Striping and Sharding 15 200 100 800 1 Focus Heating stripping 30 200 100 900 1 Defocus

[0134] (9) The solder resist material is coated on the entire board and cured at one time to form a solder resist material layer 9.

[0135] In this embodiment, a PI film is laminated on the entire four-layer circuit board as a solder resist. Specifically, before laminating the PI film, a laser is used to remove all remaining anti-plating masking films on the board surface. The removal method and parameters are the same as step (3). Then a laminator is used to laminate the completed circuit board and PI film. The PI film is Kapton HN film produced by DuPont with a thickness of 25um. Silicone rubber pads are used as hot pressing pads during lamination. Before lamination, the RPP masking film needs to be completely removed by laser. According to the material properties, the hot pressing stages and parameters are as follows:

[0136] Serial number Pressing pressure (N / cm2) Pressing temperature(℃) Pressing time (minutes) Phase 1 24 80 15 Phase 2 94 140 25 Phase 3 188 180 25 Phase 4 188 220 60 Phase 5 188→0 220 → Room temperature 45

[0137] (10) using a laser to remove organic materials on the conductor of the welding area at the assembly site to produce a solder resist pattern, and cleaning and soldering the surface of the welding area to form a cleaned and soldered surface 10;

[0138] This step can be completed in one step on the same equipment, or it can be carried out in two steps on different equipment, namely, the first step: making a solder resist pattern and generating a welding area: using a laser to selectively photoetch to remove the solder resist coating on the welding area, making a solder resist pattern and generating a welding area; the second step, cleaning and solderability treatment of the welding area surface, using another laser to remove the solder resist residue on the surface of the welding area, and slightly photoetching the metal surface layer of the welding area to remove metal oxides, exposing a fresh metal surface, and creating solderability that is easily wetted by molten solder.

[0139] Specifically, this embodiment uses a 20W ultraviolet nanosecond laser machine to make the solder mask pattern. The circuit board is placed on the laser equipment adsorption table, the engineering data of the laser processing is imported, the circuit board is accurately aligned with the processing data, and the laser photoetching PI forms the solder mask pattern. After the top surface processing is completed, the circuit board is turned over, and the bottom surface solder mask pattern is completed in the same way. The processing parameters are as follows:

[0140] Power / W Frequency / kHz Pulse width / ns Processing speed / mm / s Processing times 6 200 20 600 1

[0141] The welding area was cleaned and welded using a UV picosecond laser. The processing parameters were as follows:

[0142] Power / W Frequency / kHz Pulse width / ps Processing speed / mm / s Processing times 10 1000 12 2000 1

[0143] (11) Add solder 11 to the connection pad, mount and insert the component 12, and perform reflow soldering or wave soldering.

[0144] The technical solutions disclosed and proposed by the present invention can be realized by those skilled in the art by referring to the contents of this article and appropriately changing the conditions, routes and other links. Although the methods and preparation techniques of the present invention have been described through preferred embodiments, relevant technicians can obviously modify or re-combine the methods and technical routes described herein without departing from the content, spirit and scope of the present invention to realize the final preparation technology. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the spirit, scope and content of the present invention.

Claims

1. A method for making a circuit board by using laser to process electroplated holes, circuit masks and conductive patterns respectively, characterized by: drilling holes and depositing a thin metal layer in the holes and on the board surface, attaching a non-photosensitive masking film, laser removing the masking layer covering the hole wall to expose the hole wall, only electroplating to thicken the conductive layer in the hole, then using laser to make a circuit part anti-plating pattern and pattern electroplating, and using laser to make a conductive pattern and a solder resist pattern; the steps are: (1) Depositing the initial conductive layer on the finished double-sided, multi-layer circuit board product, electroplating copper to a thickness that can withstand subsequent processes; (2) A non-photosensitive organic film is attached to the board surface as an anti-plating masking film. The non-photosensitive organic film is composed of several layers of different shapes and compositions, wherein the layer in contact with the circuit board has viscosity and fluidity. The formation method includes depositing non-photosensitive organic film-forming materials on the board surface and hole wall by electrophoresis, vacuum coating or vapor deposition technology; (3) Using a laser to remove the masking material covering the hole wall area to produce an anti-plating pattern, and using a laser to remove the anti-plating masking film layer on the surface of the clamping point of the electroplating fixture to expose the copper surface in the contact area with the electroplating fixture; (4) Electroplating, depositing copper on the hole wall to thicken the conductive layer to the required thickness; (5) Use laser to remove the anti-plating masking film layer on the pad area and the circuit area, and add the plating window of the pad and circuit area on the hole plating window; (6) Electroplating, depositing copper on the hole wall, pad and circuit to the thickness required for final inspection and adding other metals; (7) Use laser to remove the anti-plating masking film on the non-circuit area; (8) Use laser to remove the copper foil in the non-circuit area to produce a conductive pattern; (9) Full-board coating and one-time curing of solder resist material, which also includes attaching a dry photosensitive film and a dry non-photosensitive film under a certain pressure and temperature; (10) At the assembly site, using a laser to remove organic materials on the conductors in the welding area, manufacturing a solder resist pattern, and cleaning and treating the surface of the welding area for solderability. This step also includes using a laser to remove organic materials on the conductors in the welding area, manufacturing a solder resist pattern, and cleaning the surface of the welding area at the bare board manufacturing site; (11) Add solder to the connection pads, perform component placement, insertion, reflow soldering and / or wave soldering.