Optical film and method for producing the same, polarizing plate, and image display device
By forming a slippery layer containing binder resin and particles on a transparent film substrate, the dispersion of particles and alkaline components are improved, and the optical defects of polarizers in high temperature and high humidity environments are solved, and excellent sliding is achieved and adhesiveness, suitable for polarizer protection of image display devices.
Patent Information
- Application Number
- CN202110949132.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-19
- Filing Date
- 2019-07-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2039-07-22
AI Technical Summary
In the image display device, the polarizer is prone to optical defects in a high temperature and high humidity environment, resulting in a decrease in display characteristics.
It forms an easy-sliding layer on the surface of the transparent film base material. The easy-sliding layer contains binder resin and fine particles. By improving the dispersion of the fine particles and the management of alkaline components, an excellent sliding and adhesive optical film is formed to reduce the need for a better optical film. Adhesions and optical defects.
The durability and adhesion of the optical film in high temperature and high humidity environment are achieved, and optical defects of the polarizing plate are avoided, and are suitable for polarizing member protection films.
Smart Images

Figure CN113759455B_ABST
Abstract
Description
[0001] This application is a divisional application of an application with a filing date of July 22, 2019, an application number of 201980006223.X, and an invention name of “Optical film and method for manufacturing the same, polarizing plate, and image display device”. Technical Field
[0002] The present invention relates to an optical film having an easy-slip layer on the surface of a transparent film substrate and a method for producing the same. Furthermore, the present invention relates to a polarizing plate having an optical film having an easy-slip layer bonded to the surface of a polarizer and an image display device having the polarizing plate. Background Art
[0003] Liquid crystal display devices and organic EL display devices are widely used as various image display devices such as mobile devices, car navigation devices, personal computer displays, and televisions. From the perspective of its display principle, a liquid crystal display device is provided with a polarizing plate on the surface of the identification side of the liquid crystal unit. In a transmission-type liquid crystal display device, polarizing plates are provided on both sides of the liquid crystal unit. In an organic EL display device, in order to suppress external light from being reflected by a metal electrode (cathode) and being identified as a mirror surface, a circular polarizing plate (typically a laminate of a polarizing plate and a 1 / 4 wavelength plate) is sometimes provided on the surface of the identification side.
[0004] Polarizing plates generally have a transparent film (polarizer protective film) on one or both sides of a polarizer for the purpose of protecting the polarizer, etc. As a polarizer, a polyvinyl alcohol (PVA) film adsorbed with iodine and oriented in molecules by stretching or the like is widely used.
[0005] As a polarizer protective film bonded to the surface of the polarizer, a polarizing plate bonded with a low moisture permeability film formed of a resin material such as acrylic, polyester, polycarbonate, cyclic polyolefin, etc., tends to have little change in optical properties and excellent durability even when exposed to a high humidity environment for a long time. Patent document 1 records that by providing an easy-slip layer containing microparticles and a binder resin on the surface of an acrylic film, adhesion when the film is wound into a roll can be suppressed. The embodiment of patent document 1 discloses a polarizer protective film having a urethane resin layer with an average thickness of 400nm (thickness range 300-500nm) containing 1-7% by weight of silica microparticles provided on the surface of an acrylic film.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 5354733 Summary of the invention
[0009] Problem that the invention aims to solve
[0010] In the process of increasing the size and brightness of image display devices, the polarizing plate constituting the image display device is required to have small changes in optical properties even in more severe environments (e.g., higher temperature and higher humidity conditions). The following problem has been newly discovered about the polarizing plate with a polarizer protective film disclosed in Patent Document 1: if exposed to a high humidity environment for a long time, optical defects such as stripe-like unevenness may occur, resulting in a decrease in display properties.
[0011] In view of the above problems, an object of the present invention is to provide an optical film which is less likely to cause blocking and less likely to cause optical defects even when exposed to a high temperature and high humidity environment for a long time.
[0012] Solutions for solving problems
[0013] In view of the above problems, the present inventors have found that the alkaline components such as ammonia and amines added to the easy-slip layer-forming composition for the purpose of improving the dispersibility of fine particles remain in the easy-slip layer, which is one of the reasons for the reduction in durability in a humid environment. The above problems can be solved by controlling the amount of residual alkali in the easy-slip layer to be within a specified range.
[0014] The present invention relates to an optical film having a slippery layer on the surface of a transparent film substrate and a method for producing the same. The slippery layer contains a binder resin and microparticles. The average primary particle size of the microparticles is, for example, 10 to 250 nm, preferably 10 to 100 nm. The content of alkaline components in the slippery layer is preferably 5 to 75 ppm. The thickness of the slippery layer is preferably 40 to 280 nm.
[0015] As the transparent film substrate, an acrylic film or the like is used. As the binder resin of the easy-slip layer, a urethane resin or the like is used. The content of the fine particles in the easy-slip layer is preferably about 3 to 50% by weight, more preferably 10 to 50% by weight. The fine particles of the easy-slip layer may be embedded in the transparent film substrate.
[0016] The slippery layer is formed by applying a slippery layer-forming composition to the surface of a transparent film substrate and heating the composition. The slippery layer-forming composition comprises a binder resin or a precursor thereof, microparticles, an alkaline component, and a solvent. By making the slippery layer-forming composition comprise an alkaline component, the dispersibility of the microparticles is improved, and an optical film having excellent slipperiness can be obtained. In addition, the alkaline component can also function as a catalyst for promoting the reaction of the binder resin (precursor). From the viewpoint of promoting the volatilization of the alkaline component by heating, the boiling point of the alkaline component is preferably below 150°C. Examples of the alkaline component include amines, ammonia, and the like.
[0017] By increasing the heating temperature after applying the easy-slip layer-forming composition, the volatilization of the alkaline components can be promoted to form an easy-slip layer with less residual alkaline components. For example, the easy-slip layer-forming composition can be heated at a temperature 10°C or higher than the glass transition temperature of the transparent film substrate. By increasing the heating temperature, the region where the particles of the easy-slip layer are buried in the transparent film substrate tends to be formed, and the adhesion between the transparent film substrate and the easy-slip layer tends to be improved.
[0018] After coating the easy-slip layer-forming composition on the transparent film substrate, the transparent film substrate may be stretched while being heated. In particular, by stretching the transparent film substrate while heating the easy-slip layer-forming composition at a temperature 10° C. or higher than the glass transition temperature of the transparent film substrate, the adhesion between the transparent film substrate and the easy-slip layer tends to be improved.
[0019] The slippery layer can also help improve the adhesion with other films, glass substrates, etc. The optical film can be used as a polarizer protective film, for example. For example, by laminating the optical film on the surface of a polyvinyl alcohol-based polarizer with the aid of an adhesive layer, a polarizing plate can be obtained. For the optical film, the surface on which the easy-adhesive layer is formed and any surface on which the easy-adhesive layer is not formed can be laminated to the polarizer. By configuring a polarizing plate on the surface of an image display unit such as a liquid crystal display unit and an organic EL unit, an image display device can be formed.
[0020] Effects of the Invention
[0021] The optical film of the present invention has excellent adhesiveness, is unlikely to cause blocking, and is unlikely to cause optical defects even when exposed to a high humidity environment for a long time. Therefore, it can be suitably used as a film for display devices such as a polarizer protective film. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a cross-sectional view showing a structural example of an optical film including an easy-slip layer.
[0023] Figure 2A It is a cross-sectional view showing a configuration example of a polarizing plate.
[0024] Figure 2B It is a cross-sectional view showing a configuration example of a polarizing plate.
[0025] Figure 3 This is a cross-sectional TEM observation image of an optical film in which an interface layer is formed at the interface between the film substrate and the easy-slip layer.
[0026] Figure 4 This is a cross-sectional TEM observation image of an optical film in which no interface layer is formed at the interface between the film substrate and the easy-slip layer. DETAILED DESCRIPTION
[0027] Figure 1 1 is a cross-sectional schematic diagram showing an example of the structure of an optical film according to an embodiment of the present invention. The optical film 1 has a slippery layer 15 on at least one side of a film substrate 11. The slippery layer may also be provided on both sides of the film substrate. The optical film may be used by laminating with other films, glass substrates, etc.
[0028] As a usage form of the optical film, a polarizer protective film can be mentioned. Figure 2A and Figure 2B A cross-sectional view showing a configuration example of a polarizing plate including an optical film 1 as a polarizer protective film. Figure 2A The polarizing plate 100 and Figure 2B The polarizing plate 101 shown includes an optical film 1 bonded to one surface (first main surface) of a polarizer 5 via an adhesive layer 6. In the polarizing plate 100, the optical film 1 has an easy-slip layer 15 on the surface of the film substrate 11 bonded to the polarizer 5. Figure 2B In the polarizing plate 101 shown, the polarizer 5 is bonded to the surface of the optical film 1 on which the easy-slip layer 15 is not provided. Figure 2A The polarizing plate 100 and Figure 2B In the polarizing plate 101 shown, a transparent protective film 2 is bonded to the other surface (second main surface) of the polarizer 5 via an adhesive layer 7 .
[0029] [Optical Film]
[0030] The optical film 1 includes an easy-slip layer 15 on at least one surface of a film substrate 11 .
[0031] <Film substrate>
[0032] As the film substrate 11, a transparent film is preferred. The total light transmittance of the transparent film substrate is preferably 80% or more, more preferably 85% or more, and further preferably 90% or more. As the resin material constituting the film substrate 11, acrylic resins, polyester resins, polycarbonate resins, polyolefin resins, cyclic polyolefin resins, polystyrene resins, polyamide resins, polyimide resins, etc. can be cited. When the optical film is used as an optically isotropic polarizer protective film, as the resin material of the film substrate 11, acrylic resins or cyclic polyolefin resins are preferred from the aspect of small birefringence, and acrylic resins are particularly preferred.
[0033] Examples of cyclic polyolefin resins include polynorbornene. Examples of commercially available cyclic polyolefin resins include ZEONOR and ZEONEX manufactured by Zeon Corporation, ARTON manufactured by JSR Corporation, APEL manufactured by Mitsui Chemicals, Inc., and TOPAS manufactured by TOPAS Advanced Polymers. The cyclic polyolefin film preferably contains 50% by weight or more of the cyclic olefin resin.
[0034] Examples of acrylic resins include poly(meth)acrylates such as polymethyl methacrylate, methyl methacrylate-(meth)acrylic acid copolymers, methyl methacrylate-(meth)acrylic acid ester copolymers, methyl methacrylate-(meth)acrylic acid ester copolymers, methyl methacrylate-acrylate-(meth)acrylic acid copolymers, methyl (meth)acrylate-styrene copolymers (MS resins, etc.), and polymers having an alicyclic hydrocarbon group (e.g., methyl methacrylate-cyclohexyl methacrylate copolymers, methyl methacrylate-norbornyl (meth)acrylate copolymers, etc.).
[0035] In the present specification, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid. The acrylic resin includes a resin containing acrylic acid or a derivative thereof as a monomer component and a resin containing methacrylic acid or a derivative thereof as a monomer component.
[0036] As the acrylic resin, the acrylic resin with glutaric anhydride structure described in Japanese Patent Publication No. 2006-283013, Japanese Patent Publication No. 2006-335902, Japanese Patent Publication No. 2006-274118, etc. can be used; and / or the acrylic resin with lactone ring structure described in Japanese Patent Publication No. 2000-230016, Japanese Patent Publication No. 2001-151814, Japanese Patent Publication No. 2002-120326, Japanese Patent Publication No. 2002-254544, Japanese Patent Publication No. 2005-146084, etc. The acrylic resin with glutaric anhydride structure and the acrylic resin with lactone ring structure are suitable for manufacturing polarizing plates with high polarization degree and excellent durability because they have high heat resistance, high transparency, and high mechanical strength.
[0037] When the film substrate 11 is an acrylic film, the content of the acrylic resin in the film substrate is preferably 50% by weight or more, more preferably 60 to 98% by weight, and further preferably 70 to 97% by weight. The acrylic film may contain a thermoplastic resin other than the acrylic resin. For example, by blending other thermoplastic resins, the birefringence of the acrylic resin can be eliminated, and an acrylic film with excellent optical isotropy can be obtained. In addition, for the purpose of improving the mechanical strength of the film, a thermoplastic resin other than the acrylic resin may be blended.
[0038] Examples of thermoplastic resins other than acrylic resins include olefin polymers, halogenated vinyl polymers, polystyrene, copolymers of styrene and acrylic monomers, polyesters, polyamides, polyacetals, polycarbonates, polyphenylene ethers, polyphenylene sulfides, polyetheretherketones, polysulfones, polyethersulfones, polyoxybenzylene, polyamideimides, and rubber polymers.
[0039] The film substrate 11 may contain additives such as antioxidants, stabilizers, reinforcing materials, ultraviolet absorbers, flame retardants, antistatic agents, colorants, fillers, plasticizers, lubricants, and fillers. The resin material and the additives may be mixed and pre-formed into a thermoplastic resin composition such as pellets before being formed into a film.
[0040] The thickness of the film substrate 11 is about 5 to 200 μm. From the viewpoint of mechanical strength, transparency, and handling properties, the thickness of the film substrate 11 is preferably 10 to 100 μm, and more preferably 15 to 60 μm.
[0041] The glass transition temperature Tg of the film substrate 11 is preferably 100° C. or higher, more preferably 110° C. or higher. When the film substrate 11 is an acrylic film, as described above, by using an acrylic resin having a glutaric anhydride structure or an acrylic resin having a lactone ring structure as the acrylic resin, the Tg of the acrylic film can be increased, thereby improving heat resistance. The upper limit of the Tg of the film substrate 11 is not particularly limited, but is preferably 170° C. or lower from the viewpoint of moldability.
[0042] As a method for manufacturing the film substrate 11, a solution casting method, a melt extrusion method, a calendaring method, a compression molding method, etc. can be cited. The film substrate 11 can be an unstretched film or a stretched film. When the film substrate 11 is an acrylic film, from the viewpoint of improving mechanical strength, the acrylic film is preferably a stretched film stretched in at least one direction, and a biaxially stretched film is particularly preferred. In order to eliminate the birefringence of the acrylic resin, by blending other thermoplastic resins, an acrylic film with low retardation and excellent optical isotropy can be obtained even when stretched.
[0043] <Slippery layer>
[0044] The slippery layer 15 provided on the surface of the film substrate 11 contains a binder resin and fine particles. The slippery layer 15 contains fine particles, so that fine concavities and convexities are formed on the surface of the slippery layer 15, and the slipperiness of the film is improved. Therefore, it helps to reduce scratches on the optical film 1 during roll transportation and suppress blocking when it is rolled into a roll.
[0045] (Binder resin)
[0046] As the binder resin, from the aspect of excellent adhesion to film substrates such as acrylic films, resins (polymers) having reactive groups such as polyurethane resins, epoxy resins, isocyanate resins, polyester resins, polymers containing amino groups in the molecule, and acrylic resins having crosslinking functional groups such as oxazoline groups can be used. As the binder resin of the easy-slip layer 15, polyurethane resins are particularly preferred. The easy-slip layer 15 containing a polyurethane resin binder has high adhesion to the film substrate 11.
[0047] The urethane resin is typically a reaction product of a polyol and a polyisocyanate. As the polyol component, preferably used is a high molecular weight polyol such as polyacrylic polyol, polyester polyol, polyether polyol, or the like.
[0048] Polyacrylic acid polyols can be obtained by polymerization of (meth)acrylates and monomers containing hydroxyl groups. Examples of (meth)acrylates include methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Examples of monomers containing hydroxyl groups include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxypentyl (meth)acrylate; (meth)acrylate monoesters of polyols such as glycerol and trimethylolpropane; and N-methylol (meth)acrylamide.
[0049] Polyacrylic acid polyols may contain monomer components other than those mentioned above. Other monomer components include unsaturated monocarboxylic acids such as (meth)acrylic acid; unsaturated dicarboxylic acids such as maleic acid and their anhydrides and diesters; unsaturated nitriles such as (meth)acrylonitrile; unsaturated amides such as (meth)acrylamide and N-hydroxymethyl (meth)acrylamide; vinyl esters such as vinyl acetate and vinyl propionate; vinyl ethers such as methyl vinyl ether; α-olefins such as ethylene and propylene; halogenated α,β-unsaturated aliphatic monomers such as vinyl chloride and vinylidene chloride; α,β-unsaturated aromatic monomers such as styrene and α-methylstyrene, etc.
[0050] Polyester polyols can be obtained by reacting polybasic acids and polyols. Examples of polybasic acids include aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, 1,4-naphthalene dicarboxylic acid, 2,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, biphenyl dicarboxylic acid, and tetrahydrophthalic acid; aliphatic dicarboxylic acids such as oxalic acid, succinic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, dodecanedicarboxylic acid, octadecane dicarboxylic acid, tartaric acid, alkyl succinic acid, linolenic acid, maleic acid, fumaric acid, mesaconic acid, citraconic acid, and itaconic acid; alicyclic dicarboxylic acids such as hexahydrophthalic acid, tetrahydrophthalic acid, 1,3-cyclohexane dicarboxylic acid, and 1,4-cyclohexane dicarboxylic acid; or reactive derivatives thereof such as anhydrides, alkyl esters, and acid halides.
[0051] Examples of the polyol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, neopentyl glycol, pentylene glycol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, 1-methyl-1,3-butylene glycol, 2-methyl-1,3-butylene glycol, 1-methyl-1,4-pentanediol, 2-methyl-1,4-pentanediol, 1,2-dimethyl-neopentyl glycol, 2,3-dimethyl-neopentyl glycol, Pentanediol, 1-methyl-1,5-pentanediol, 2-methyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,2-dimethylbutanediol, 1,3-dimethylbutanediol, 2,3-dimethylbutanediol, 1,4-dimethylbutanediol, diethylene glycol, triethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, 1,4-cyclohexanedimethanol, 1,4-cyclohexanediol, bisphenol A, bisphenol F, hydrogenated bisphenol A, hydrogenated bisphenol F, etc.
[0052] The polyether polyol can be obtained by ring-opening polymerization of an alkylene oxide and then adding the alkylene oxide to a polyol. Examples of the polyol include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, glycerol, trimethylolpropane, etc. Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, styrene oxide, tetrahydrofuran, etc.
[0053] Examples of the polyisocyanate include tetramethylene diisocyanate, dodecamethylene diisocyanate, 1,4-butane diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2-methylpentane-1,5-diisocyanate, 3-methylpentane-1,5-diisocyanate and other aliphatic diisocyanates; isophorone diisocyanate, hydrogenated xylylene diisocyanate, 4,4'-cyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexylene diisocyanate, Alicyclic diisocyanates such as hexane; aromatic diisocyanates such as toluene diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, xylene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate; aromatic aliphatic diisocyanates such as dialkyl diphenylmethane diisocyanate, tetraalkyl diphenylmethane diisocyanate, α,α,α,α-tetramethylxylene diisocyanate, etc.
[0054] The carbamate resin constituting the easy-slip layer 15 preferably has a carboxyl group. The carbamate resin can be introduced into a cross-linked structure by having a carboxyl group. The carbamate resin having a carboxyl group can be obtained, for example, by reacting a chain extender having a free carboxyl group with a polyol and a polyisocyanate resin. Examples of the chain extender having a free carboxyl group include dihydroxycarboxylic acids and dihydroxysuccinic acid. Examples of the dihydroxycarboxylic acid include dialkyl alkanoic acids such as dimethylol alkanoic acid (e.g., dimethylol acetic acid, dimethylol butyric acid, dimethylol propionic acid, dimethylol butyric acid, and dimethylol valeric acid).
[0055] The method for producing the carbamate resin is not particularly limited, and may be any one of a one-step method in which the monomer components are reacted at once and a multi-stage method in which the monomer components are reacted in stages. When a chain extender having a free carboxyl group is used to introduce a carboxyl group into the carbamate resin, a multi-stage method is preferred. When producing the carbamate resin, a carbamate reaction catalyst may be used as needed.
[0056] The number average molecular weight of the urethane resin is preferably 5,000 to 600,000, more preferably 10,000 to 400,000. The acid value of the urethane resin is preferably 10 to 50, more preferably 20 to 45.
[0057] The carbamate resin may have a cross-linked structure. By introducing a cross-linked structure into the carbamate resin, there is a tendency that the adhesion of the slippery layer 15 to the film substrate 11 and the hardness of the slippery layer 15 are improved. As a cross-linking agent, a cross-linking agent that can react with the cross-linking functional group of the carbamate resin can be used without particular restriction. When the carbamate resin has a carboxyl group, a cross-linking agent comprising an amino group, an oxazoline group, an epoxy group, a carbodiimide group, etc. can be used. Among these, a cross-linking agent having an oxazoline group is preferably used. Oxazoline groups have a small reactivity with carboxyl groups at room temperature, and therefore have a long pot life when mixed with the carbamate resin, and can flexibly cope with the lead time (lead time) of the process.
[0058] The crosslinking agent may be a low molecular weight compound or a polymer. From the viewpoint of high solubility in the aqueous composition and excellent compatibility with the urethane resin, the crosslinking agent is preferably an acrylic polymer, and particularly preferably an acrylic polymer having an oxazoline group.
[0059] The amount of the cross-linking agent used is preferably 1 to 30 parts by weight, more preferably 3 to 20 parts by weight, based on 100 parts by weight of the urethane resin.
[0060] (particle)
[0061] By making the slippery layer 15 contain microparticles and forming fine concavo-convex shapes on the surface of the slippery layer, the slipperiness of the optical film 1 is improved and adhesion can be suppressed. From the viewpoint of forming concavo-convex shapes that help improve slipperiness, the particle size (average primary particle size) of the microparticles is preferably 10 nm or more, more preferably 15 nm or more, and further preferably 20 nm or more. The average primary particle size of the microparticles is preferably smaller than the thickness of the slippery layer. By making the particle size of the microparticles smaller than the thickness of the slippery layer, the microparticles can be suppressed from falling off the slippery layer. The particle size of the microparticles is preferably 250 nm or less, more preferably 200 nm or less. In addition, by making the average primary particle size of the microparticles smaller than the wavelength of visible light, visible light scattering at the interface between the binder resin and the microparticles can be suppressed. From the viewpoint of improving transparency, the particle size of the microparticles is preferably 100 nm or less, more preferably 80 nm or less, further preferably 60 nm or less, and particularly preferably 50 nm or less.
[0062] The particles of the slippery layer 15 may be either inorganic particles or organic particles. From the perspective of excellent dispersibility and uniformity of particle size, inorganic particles are preferred as particles. As inorganic particles, inorganic oxides such as titanium dioxide, aluminum oxide, and zirconium oxide; calcium carbonate, talc, clay, calcined kaolin, calcined calcium silicate, hydrated calcium silicate, aluminum silicate, magnesium silicate, and calcium phosphate can be cited. Among these, inorganic oxides are preferred. As organic particles, silicone resins, fluorine resins, and acrylic resins can be cited. In order to suppress light scattering caused by particles, it is preferred that the difference in refractive index between the binder resin (generally having a refractive index of about 1.5) and the particles is small. From the perspective of having a small refractive index difference with the binder resin and excellent dispersibility, silica particles are preferred as particles of the slippery layer 15.
[0063] When the slippery layer 15 is formed from an aqueous composition, it is preferred to use fine particles with high water dispersibility. An aqueous dispersion of fine particles may also be mixed into the composition. In order to improve the dispersibility of the fine particles, it is preferred to add an alkaline component such as amine or ammonia to make the slippery layer-forming composition weakly alkaline.
[0064] As water-dispersible silica particles, colloidal silica is preferably used. As colloidal silica, commercially available products such as Quartron.PL series manufactured by Fuso Chemical Industry Co., Ltd., SnowTex series manufactured by Nissan Chemical Industry Co., Ltd., AERODISP series and AEROSIL series manufactured by NIPPON AEROSIL Co., Ltd., and SEAHOSTAR KE series manufactured by Nippon Shokubai Co., Ltd. can be used.
[0065] From the viewpoint of improving the sliding property of the optical film 1 by forming the concavo-convex on the surface of the easy-slip layer 15, the content of the fine particles in the easy-slip layer 15 is preferably 3% by weight or more, and more preferably 5% by weight or more. In particular, when the thickness of the easy-slip layer 15 is small (for example, when it is less than 280 nm), it is preferable to increase the content of fine particles and increase the amount of fine particles per unit area (number density), so as to form the concavo-convex uniformly in the surface of the easy-slip layer 15. The content of fine particles in the easy-slip layer 15 is preferably 8% by weight or more, more preferably 10% by weight or more, and further preferably 12% by weight or more. When the content of fine particles in the easy-slip layer 15 is too large, the optical properties may be reduced due to the increase in light scattering at the interface between the binder resin and the fine particles. In addition, as the content of fine particles increases, the relative content of the binder resin decreases, so that the adhesion of the easy-slip layer may be reduced. Therefore, the content of fine particles in the easy-slip layer 15 is preferably 50% by weight or less, more preferably 40% by weight or less, and further preferably 30% by weight or less.
[0066] (Residual alkali content)
[0067] When alkaline components such as amines and ammonia are used to improve the dispersibility of the particles, alkaline components inevitably remain in the slippery layer. When the optical film 1 is used as a polarizer protective film, the residual alkaline components of the slippery layer 15 are dissolved into water or the like, or the alkaline components that penetrate the film substrate 11 may sometimes deteriorate the polarizer, resulting in optical defects such as reduced polarization degree of the polarizing plate and stripe-shaped unevenness.
[0068] From the viewpoint of improving the moisture durability of the polarizing plate, the residual alkali content of the easy-slip layer 15 is preferably 75 ppm or less, more preferably 70 ppm or less, further preferably 60 ppm or less, and particularly preferably 55 ppm or less. From the viewpoint of improving the moisture durability of the polarizing plate, the smaller the residual alkali content in the easy-slip layer 15, the more preferred.
[0069] On the other hand, if the residual alkali content of the easy-slip layer 15 is too small, the dispersibility of the particles is impaired, and sometimes poor appearance such as white turbidity due to the aggregation of the particles occurs. In addition, due to the aggregation of the particles caused by the reduction in dispersibility and the detachment from the easy-slip layer, appropriate unevenness is not formed on the surface of the easy-slip layer, and the sliding property of the optical film tends to be reduced. Therefore, the residual alkali content of the easy-slip layer 15 is preferably 5 ppm or more, more preferably 10 ppm or more, and even more preferably 20 ppm or more.
[0070] Specific examples of residual alkaline components in the slippery layer include amines and ammonia. Preferably, the total content of amines and ammonia in the slippery layer is within the above range. The amount of alkali in the slippery layer can be quantified by liquid chromatography, ion chromatography, etc. according to the type of alkaline component. The alkaline component can be quantified by an analytical method combining chromatography and mass spectrometry (MS) (e.g., LC / MS). When the slippery layer contains multiple alkaline components, the total of each component is taken as the alkaline component content (residual amount) of the slippery layer.
[0071] <Formation of Slippery Layer>
[0072] The method for forming the easy-slip layer 15 on the surface of the film substrate 11 is not particularly limited. The easy-slip layer 15 is preferably formed by applying an easy-slip layer-forming composition (coating liquid) containing a binder resin and fine particles onto the film substrate 11 and heating it.
[0073] (Composition for forming an easy-slip layer)
[0074] The composition for forming the easy-slip layer is preferably an aqueous composition using water as a solvent (and a dispersion medium for the fine particles). The concentration of the solid content (non-volatile content) in the composition for forming the easy-slip layer is preferably 1 to 30% by weight, more preferably 2 to 20% by weight, and even more preferably 3 to 15% by weight.
[0075] The aqueous composition for forming a slippery layer contains water as a solvent (and a dispersion medium), a binder resin or a precursor thereof, and fine particles. The composition for forming a slippery layer preferably further contains an alkaline component. As mentioned above, the alkaline component has the effect of promoting the dispersion of fine particles. Therefore, although fine particles with a small particle size tend to aggregate easily, the composition for forming a slippery layer can improve the dispersibility of fine particles by containing alkaline components such as ammonia and amines, and can obtain an optical film with excellent appearance and sliding properties.
[0076] On the other hand, when the alkali contained in the composition for forming the easy-slip layer remains in the easy-slip layer, it will become a cause of reducing the moisture and heat resistance of the polarizing plate. In particular, even a small amount of strong alkali such as caustic soda will cause the polarizer to deteriorate. Therefore, as the alkaline component contained in the composition for forming the easy-slip layer, a weak alkaline component such as ammonia and amine is preferred. From the viewpoint of helping to improve the dispersibility of the particles and preventing the polarizer from deteriorating, the pH of the composition for forming the easy-slip layer (coating liquid) is preferably about 7.5 to 9.
[0077] From the viewpoint of improving the dispersibility of the particles, the amount of the alkaline component contained in the easy-slip layer-forming composition is preferably 300 ppm or more, and more preferably 500 ppm or more relative to the solid content of the easy-slip layer-forming composition. On the other hand, when the content of the alkaline component is too large, it is sometimes difficult to reduce the amount of residual alkali, so the amount of the alkaline component contained in the easy-slip layer-forming composition is preferably 50,000 ppm or less, more preferably 10,000 ppm or less, and further preferably 5,000 ppm or less relative to the solid content of the easy-slip layer-forming composition. As mentioned above, specific examples of the alkaline component contained in the easy-slip layer-forming composition include amines and ammonia, and the total content of these alkaline components is preferably within the above range.
[0078] The basic component contained in the easy-slip layer-forming composition may be a substance that has a catalytic effect in addition to improving the dispersibility of the fine particles. For example, when the binder resin is a urethane resin, the easy-slip layer-forming composition may contain a tertiary amine such as triethylamine as a urethane-forming catalyst for a polyurethane precursor (polyol, isocyanate, etc.).
[0079] By applying the composition for forming an easy-slip layer on the film substrate and then heating it, the alkaline component can be volatilized and removed, thereby reducing the residual alkaline component of the easy-slip layer 15. From the viewpoint of promoting the volatilization of the alkaline component by heating, the alkaline component contained in the composition for forming an easy-slip layer preferably has a boiling point of 150°C or less. The boiling point of the alkaline component is more preferably 130°C or less, further preferably 120°C or less, and particularly preferably 110°C or less. The boiling point of the alkaline component may be 100°C or less or 90°C or less. When the composition for forming an easy-slip layer contains a plurality of alkaline components, it is preferred that the boiling point of at least one alkaline component is within the above range, and it is preferred that the boiling points of two or more alkaline components are within the above range. With respect to 100 parts by weight of the total amount of alkali contained in the easy-slip layer, it is preferred that the boiling point of 50% by weight or more of the alkaline components is within the above range. It is desirable that the boiling points of all the alkaline components contained in the composition for forming an easy-slip layer are within the above range.
[0080] The composition for forming the easy-slip layer may contain a crosslinking agent in addition to the binder resin (or its precursor), fine particles and alkaline components. The composition for forming the easy-slip layer may contain additives such as catalysts such as crosslinking accelerators, antioxidants, ultraviolet absorbers, leveling agents, anti-blocking agents, antistatic agents, dispersion stabilizers, defoamers, thickeners, dispersants, surfactants, lubricants, etc.
[0081] (Formation of a slippery layer on a film substrate)
[0082] Before applying the easy-slip layer-forming composition on the film substrate 11, the film substrate may be subjected to a surface treatment. By performing the surface treatment, the wetting tension of the film substrate can be adjusted and the adhesion between the film substrate and the easy-slip layer 15 can be improved. Examples of the surface treatment include corona treatment, plasma treatment, ozone blasting, ultraviolet irradiation, flame treatment, and chemical treatment. Among these, corona treatment or plasma treatment is preferred.
[0083] Examples of the coating method of the easy-slip layer-forming composition include rod coating, roll coating, gravure coating, rod coating, slot coating, curtain coating, and injection coating. The easy-slip layer-forming composition after coating is heated to remove the solvent and form the easy-slip layer 15. The precursor of the binder resin can be reacted and cured by heating. For example, when the easy-slip layer-forming composition contains a crosslinking agent, the crosslinking reaction can be promoted by heating.
[0084] The heating temperature when forming the easy-slip layer is, for example, about 50 to 200° C. From the viewpoint of promoting the curing reaction of the resin component in the easy-slip layer-forming composition and effectively volatilizing and removing the alkaline component contained in the easy-slip layer-forming composition, the heating temperature is preferably 100° C. or higher, more preferably 120° C. or higher, further preferably 130° C. or higher, and particularly preferably 135° C. or higher. In addition, the heating temperature is preferably higher than the boiling point of the alkaline component contained in the easy-slip layer-forming composition.
[0085] The heating temperature during the formation of the easy-slip layer is preferably a temperature higher than the glass transition temperature (Tg) of the film substrate. By heating at a high temperature, the curing reaction of the resin component in the easy-slip layer-forming composition can be promoted, and the alkaline component contained in the easy-slip layer-forming composition can be effectively volatilized and removed. The heating temperature is preferably a temperature higher than the Tg of the film substrate by 10°C or more.
[0086] It is believed that by heating at a temperature higher than the Tg of the film substrate, the volatilization removal efficiency of the alkali in the easy-slip layer-forming composition can be improved, and the easy-slip layer-forming composition becomes easy to penetrate into the surface of the film substrate, thereby improving the adhesion between the film substrate 11 and the easy-slip layer 15. From the viewpoint of improving the adhesion of the easy-slip layer, the heating temperature is preferably Tg of the film substrate + 10°C or more, more preferably Tg + 15°C or more, and even more preferably Tg + 20°C or more.
[0087] When heated at a temperature higher than Tg+10°C of the film substrate, the film substrate changes from a glass state to a rubber state, and the surface becomes easily deformed, so an interface layer in which the resin component of the film substrate and the constituent components of the easy-slip layer are mixed is easily formed at the interface between the film substrate 11 and the easy-slip layer 15. The formation of the interface layer tends to improve the adhesion between the film substrate 11 and the easy-slip layer 15.
[0088] Especially if Figure 3 As shown in the cross-sectional observation image of , when there is a region on the surface of the film substrate 11 where the fine particles of the easy-slip layer 15 are embedded and buried, an optical film having high adhesion between the film substrate 11 and the easy-slip layer 15 can be obtained. It is considered that when the film substrate is heated to a rubber state at a temperature higher than Tg, the fine particles are buried in the film substrate, and when the film substrate is subsequently restored to a glass state, the fine particles buried in the surface of the film substrate and the binder resin existing around them are fixed to the surface of the film substrate, thereby improving the adhesion between the film substrate 11 and the easy-slip layer 15.
[0089] The slippery layer may be formed in the manufacturing process of the film substrate. Alternatively, the slippery layer may be formed by heating during the formation of the film substrate. For example, when the film substrate is a stretched film, the slippery layer-forming composition is applied to the surface of the film before stretching or after longitudinal stretching, and the solvent may be dried and the resin may be cured by heating during transverse stretching or simultaneous biaxial stretching by a tenter.
[0090] In the case of stretching the film substrate after applying the composition for forming the easy-slip layer, from the viewpoint of suppressing the occurrence of cracks in the easy-slip layer, the stretching ratio is preferably 5 times or less, more preferably 4 times or less, further preferably 3 times or less, and particularly preferably 2.5 times or less. The lower limit of the stretching ratio is not particularly limited, but from the viewpoint of improving the film strength, the stretching ratio is preferably 1.3 times or more, more preferably 1.5 times or more. In the case of the film substrate being an acrylic film, from the viewpoint of improving the film strength, it is preferably stretched in the conveying direction (MD) and the width direction (TD) at the above-mentioned stretching ratios, respectively.
[0091] When biaxial stretching of the film substrate is performed, the biaxial stretching may be sequential biaxial stretching or simultaneous biaxial stretching. In addition, oblique stretching may be performed. When sequential biaxial stretching is performed, as described above, after the film is stretched in one direction (MD) by roller stretching, the easy-slip layer-forming composition is coated on the film, and the easy-slip layer-forming composition is heated during the stretching by the tenter.
[0092] As described above as the heating temperature of the easy-slip layer, the stretching temperature is preferably a temperature higher than the Tg of the film substrate, preferably Tg+10°C or higher, more preferably Tg+15°C or higher, and further preferably Tg+20°C or higher. It is particularly preferred that the film is stretched in at least one direction at the above temperature after the easy-slip layer-forming composition is applied. When the film substrate is stretched in a rubber state at a temperature higher than the Tg of the film substrate, a region where the microparticles in the easy-slip layer-forming composition are buried on the surface of the film substrate is easily formed, and there is a tendency that the adhesion between the film substrate 11 and the easy-slip layer 15 is improved. As a reason why microparticles are easily buried in the film substrate by stretching at a high temperature, it can be cited that when the film substrate is stretched in a rubber state, the easy-slip layer-forming composition is easy to wet and spread when the film substrate is deformed, and the microparticles are easily embedded in the concave parts of the surface unevenness formed when the film substrate is deformed. In addition, it is considered that if the film substrate is cooled while releasing the stress after stretching, the particles embedded in the surface of the film substrate are fixed when the film substrate shrinks, so that the region where the microparticles are buried in the film substrate is easily formed.
[0093] The thickness of the slippery layer 15 can be adjusted by adjusting the solid content concentration and coating thickness of the slippery layer-forming composition. When the film substrate is stretched after coating the slippery layer-forming composition, the thickness of the slippery layer 15 can also be adjusted by the stretching ratio.
[0094] The thickness of the slippery layer 15 is not particularly limited, but from the viewpoint of promoting the removal of alkaline components by heating, it is preferably 280 nm or less, more preferably 250 nm or less, and further preferably 230 nm or less. When the optical film 1 is used as a polarizer protective film, the smaller the thickness of the slippery layer 15, the higher the humidification durability of the polarizer.
[0095] When the composition for forming the slippery layer is heated and dried, if the alkaline component is removed excessively, the dispersibility of the particles in the binder resin decreases, and the particles are easily aggregated and the particles are easily detached from the surface of the slippery layer. When the particles are aggregated and detached, the slipperiness of the optical film decreases, and scratches during transportation and adhesion during winding are easily generated. Therefore, the thickness of the slippery layer 15 is preferably 40 nm or more, more preferably 50 nm or more, further preferably 80 nm or more, and particularly preferably 100 nm or more. The thickness of the slippery layer can be 110 nm or more, 120 nm or more, 130 nm or more, 140 nm or more, or 150 nm or more.
[0096] [Polarizing plate]
[0097] The polarizing plate may have a transparent protective film on only one side of the polarizer, or Figure 2A and Figure 2B As shown in FIG. 1 , a polarizer 5 is provided with transparent protective films on both sides. By laminating the above optical film on one side of the polarizer as a polarizer protective film, a polarizing plate having a transparent protective film only on one side of the polarizer can be formed. For a polarizing plate having polarizer protective films on both sides of the polarizer, the above optical film may be laminating on at least one side of the polarizer. The polarizing plate may also have the above optical film laminating on both sides of the polarizer. The polarizer 5 and the optical film 1 are laminating with the aid of an adhesive layer 6.
[0098] <Polarizer>
[0099] As the polarizer 5, a polyvinyl alcohol (PVA) polarizer can be used, in which a polyvinyl alcohol film such as polyvinyl alcohol or partially formalized polyvinyl alcohol is adsorbed with a dichroic substance such as iodine or a dichroic dye and oriented in one direction. For example, a PVA polarizer can be obtained by dyeing a polyvinyl alcohol film with iodine and stretching it.
[0100] In the manufacturing process of the polarizer 5, water washing, swelling, cross-linking and other treatments may be performed as needed. Stretching may be performed before or after iodine dyeing, or while dyeing. Stretching may be performed by stretching in the air (dry stretching), or in water or in an aqueous solution containing boric acid, potassium iodide, etc. (wet stretching), or these may be used in combination. The film thickness of the polarizer 5 is not particularly limited, but is generally about 1 to 50 μm.
[0101] As the polarizer 5, a thin PVA-based polarizer with a thickness of less than 10 μm can also be used. As a thin polarizer, for example, thin polarizers described in Japanese Patent Publication No. 51-069644, Japanese Patent Publication No. 2000-338329, WO2010 / 100917, Japanese Patent No. 4691205, Japanese Patent No. 4751481, etc. can be cited. These thin polarizers can be obtained by a method including the following steps: a step of stretching a PVA-based resin layer and a stretching resin substrate in a laminate state, and a step of iodine dyeing. In this method, even if the PVA-based resin layer is thin, it can be stretched without causing undesirable conditions such as breakage due to stretching because it is supported by the stretching resin substrate.
[0102] <Adhesive>
[0103] As long as the adhesive layer 6 for bonding the polarizer 5 and the optical film 1 is optically transparent, there is no particular limitation on the material thereof, and examples thereof include epoxy resins, silicone resins, acrylic resins, polyurethanes, polyamides, polyethers, polyvinyl alcohol, and the like. The thickness of the adhesive layer 6 is, for example, about 0.01 to 20 μm, and can be appropriately set according to the type of adherend, the material of the adhesive, and the like. In the case of using a curing adhesive that exhibits adhesiveness through a cross-linking reaction after coating, the thickness of the adhesive layer 6 is preferably 0.01 to 5 μm, and more preferably 0.03 to 3 μm.
[0104] As the adhesive, various adhesives can be used, such as water-based adhesives, solvent-based adhesives, hot melt adhesives, active energy ray-curable adhesives, etc. Among these, water-based adhesives or active energy ray-curable adhesives are preferred because they can reduce the thickness of the adhesive layer.
[0105] As the polymer component of the water-based adhesive, vinyl polymer, gelatin, vinyl latex, polyurethane, polyester, epoxy, etc. can be exemplified. Among these, vinyl polymer is preferred from the aspect of excellent adhesion to the polarizer, and polyvinyl alcohol resin is particularly preferred. Among the polyvinyl alcohol resins, polyvinyl alcohol containing acetoacetyl groups is preferred.
[0106] From the viewpoint of adhesiveness, the average degree of polymerization of the polyvinyl alcohol-based resin is preferably about 100 to 5000, and more preferably 1000 to 4000. The average degree of saponification of the polyvinyl alcohol-based resin is preferably 85 mol % or more, and more preferably 90 mol % or more.
[0107] In addition to polymers such as polyvinyl alcohol resins, aqueous adhesive compositions (solutions) may also contain crosslinking agents. As crosslinking agents, compounds having at least two functional groups reactive with the polymer constituting the adhesive in one molecule may be used. Examples of crosslinking agents for polyvinyl alcohol resins include alkylenediamines; isocyanates; epoxies; aldehydes; aminoformaldehydes such as methylol urea and methylol melamine. Among these, aminoformaldehyde is preferred. As aminoformaldehyde resins, compounds having methylol groups are preferred, and methylol melamine is particularly preferred. The amount of the crosslinking agent in the adhesive composition is preferably about 10 to 60 parts by weight, and more preferably 20 to 50 parts by weight, relative to 100 parts by weight of the polyvinyl alcohol resin.
[0108] Active energy ray curing adhesives are adhesives that can undergo free radical polymerization, cationic polymerization, or anionic polymerization by irradiation with active energy rays such as electron beams and ultraviolet rays. Among them, from the aspect of being able to cure with low energy, photoradical polymerizable adhesives, photocationic polymerizable adhesives, or hybrid adhesives that use a combination of photocationic polymerization and photoradical polymerization are preferred.
[0109] As monomers of the radical polymerizable adhesive, there can be mentioned compounds having a (meth)acryloyl group and compounds having a vinyl group. Among them, compounds having a (meth)acryloyl group are preferred. As compounds having a (meth)acryloyl group, there can be mentioned (meth)acrylic acid C 1-20 Alkyl (meth)acrylates such as chain alkyl esters, alicyclic (meth)acrylates, and polycyclic (meth)acrylates; (meth)acrylates containing hydroxyl groups; (meth)acrylates containing epoxy groups such as glycidyl (meth)acrylates, etc. The radical polymerizable adhesive may contain nitrogen-containing monomers such as hydroxyethyl (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-ethoxymethyl (meth)acrylamide, (meth)acrylamide, and (meth)acryloylmorpholine. As a crosslinking component, the radical polymerizable adhesive may contain polyfunctional monomers such as tripropylene glycol diacrylate, 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, cyclic trimethylolpropane formal acrylate, dioxanediol diacrylate, and EO-modified diglycerol tetraacrylate.
[0110] As the curable component of the cationic polymerizable adhesive, compounds having an epoxy group and an oxetane group can be cited. The compound having an epoxy group is not particularly limited as long as it has at least two epoxy groups in the molecule, and various curable epoxy compounds generally known can be used. As preferred epoxy compounds, compounds having at least two epoxy groups and at least one aromatic ring in the molecule (aromatic epoxy compounds) and compounds having at least two epoxy groups in the molecule, at least one of which is formed between two adjacent carbon atoms constituting an alicyclic ring (alicyclic epoxy compounds) can be cited. By containing free radical polymerizable compounds such as compounds having a (meth)acryloyl group in the cationic polymerizable adhesive, a mixed adhesive can also be prepared.
[0111] The photocurable adhesive preferably contains a photopolymerization initiator. The photopolymerization initiator can be appropriately selected according to the type of reaction. For example, in a radical polymerizable adhesive, as a photopolymerization initiator, it is preferred to mix a photoradical generator that generates free radicals by light irradiation. In a cationic polymerizable adhesive, as a photopolymerization initiator, it is preferred to mix a photocationic polymerization initiator (photoacid generator) that generates cationic species or Lewis acids by light irradiation. In a mixed adhesive, it is preferred to mix a photocationic polymerization initiator and a photoradical generator.
[0112] The content of the polymerization initiator is generally about 0.1 to 10 parts by weight, preferably 0.5 to 3 parts by weight, relative to 100 parts by weight of the monomer. It should be noted that when a free radical polymerizable adhesive is used as an electron beam curing adhesive, a photopolymerization initiator is not necessary. In an active energy ray curing adhesive, a photosensitizer may be added as needed to increase the curing speed and sensitivity. The amount of the photosensitizer used is generally about 0.001 to 10 parts by weight, preferably 0.01 to 3 parts by weight, relative to 100 parts by weight of the monomer.
[0113] The adhesive may contain appropriate additives as required. Examples of additives include coupling agents such as silane coupling agents and titanium coupling agents, adhesion promoters such as ethylene oxide, ultraviolet absorbers, anti-degradation agents, dyes, processing aids, ion capture agents, antioxidants, tackifiers, fillers, plasticizers, leveling agents, foaming inhibitors, antistatic agents, heat stabilizers, hydrolysis stabilizers, etc.
[0114] [Production of polarizing plate]
[0115] The polarizing plate is manufactured by bonding the optical film 1 to one side (first main surface) of the polarizer 5 via the adhesive layer 6. The optical film 1 can be Figure 2A As shown, the slippery layer is bonded to the polarizer 5 by means of an adhesive layer, or as shown in FIG. Figure 2B As shown, the non-slip layer-formed surface is bonded to the polarizer 5 via an adhesive layer.
[0116] The slippery layer 15 can also function as an easy-adhesive layer. Figure 2A As shown, when the polarizer 5 is attached to the surface of the optical film 1 formed with the slippery layer 15 by means of the adhesive layer 6, the slippery layer 15 can help improve the adhesion between the polarizer and the polarizer protective film (optical film 1). Figure 2B As shown, when the non-slip layer-formed surface is bonded to the polarizer 5 via the adhesive layer, the slip layer 15 can help improve the adhesion with other films, adhesive layers, glass substrates, etc. provided on the optical film 1.
[0117] In laminating the polarizer 5 and the optical film 1, it is preferred that: after applying the adhesive composition on either or both of the polarizer 5 and the optical film 1, the polarizer 5 and the optical film 1 are laminated by a roll laminator or the like, and the adhesive is cured. As a method for applying the adhesive composition on the polarizer 5 and / or the optical film 1, a roller method, a spray method, a dipping method, etc. can be cited. Before applying the adhesive composition on the surface of the polarizer 5 and / or the optical film 1, a surface treatment such as a corona treatment, a plasma treatment, a saponification treatment, etc. can also be performed.
[0118] After the polarizer 5 and the optical film 1 are bonded together, the adhesive is cured according to the type of adhesive, thereby forming an adhesive layer 6. When a water-based adhesive is used, the adhesive is cured by heating and drying. When an active energy ray-curing adhesive is used, the adhesive is cured by irradiating active energy rays such as electron beams and ultraviolet rays. When a photocationically polymerizable adhesive is provided on the slippery layer 15, the photoactive species (cations or Lewis acids) are easily deactivated due to the residual alkaline components of the slippery layer, and polymerization inhibition sometimes occurs. Therefore, when a photocationically polymerizable adhesive or a photocationic / photoradical mixed adhesive is used as the adhesive layer 6, it is preferably as follows. Figure 2B As shown, the non-slip layer-formed surface of the optical film 1 is bonded to the polarizer 5 .
[0119] <Transparent protective film>
[0120] A transparent protective film 2 may be attached to the second main surface of the polarizer 5 via an adhesive layer 7. As the transparent protective film 2, any appropriate transparent film may be used. The thickness of the transparent protective film 2 is about 5 to 200 μm. From the viewpoints of mechanical strength, transparency, and handling properties, the thickness of the transparent protective film 2 is preferably 10 to 100 μm, and more preferably 15 to 60 μm. The thickness of the optical film 1 and the transparent protective film 2 may be the same or different.
[0121] Examples of materials for forming the transparent protective film 2 include polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate (PEN); cellulose polymers such as cellulose diacetate and cellulose triacetate; styrene polymers such as polystyrene and acrylonitrile-styrene copolymer; cyclic polyolefins such as polynorbornene; and polycarbonate.
[0122] The transparent protective film 2 may include a slippery layer (not shown). On the transparent protective film 2, a slippery layer similar to the slippery layer 15 of the optical film 1 may be provided.
[0123] As adhesive layer 7 for bonding polarizer 5 and transparent protective film 2, various adhesives such as water-based adhesives, solvent-based adhesives, hot melt adhesives, and active energy ray-curable adhesives can be used. Adhesive layer 6 and adhesive layer 7 can use the same adhesive composition.
[0124] [Use of polarizing plate]
[0125] An adhesive layer for bonding a liquid crystal unit, an organic EL unit, etc. may be provided on the polarizing plate. As the adhesive forming the adhesive layer, an adhesive based on a polymer such as an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyether, a fluorine-based polymer, a rubber-based polymer, etc. may be appropriately selected and used. In particular, an acrylic adhesive is preferred from the aspects of excellent optical transparency, moderate wettability and cohesiveness, and excellent weather resistance, heat resistance, etc.
[0126] The adhesive layer can be attached to the polarizing plate in any suitable manner, for example, by preparing an adhesive solution having a solid content concentration of about 10 to 40% by weight in which a base polymer is dissolved or dispersed in a solvent such as toluene or ethyl acetate, and attaching the adhesive layer to the polarizing plate, or by transferring the adhesive layer formed on a suitable substrate to the polarizing plate.
[0127] Adhesive layers may be provided on both sides of the polarizing plate. When adhesive layers are provided on both sides of the polarizing plate, the composition and thickness of the adhesive layers on the front and back sides may be the same or different. The thickness of the adhesive layer is generally about 5 to 500 μm.
[0128] A separator may be temporarily attached to the surface of the adhesive layer for the purpose of preventing contamination of the adhesive layer, etc. As the separator, it is preferred to use a separator obtained by coating the surface of a plastic film with a release agent such as a silicone release agent, a long-chain alkyl release agent, or a fluorine release agent.
[0129] The polarizing plate may be a laminated polarizing plate laminated with other optical layers. Examples of the optical layer include a phase difference plate, a viewing angle compensation film, and a brightness enhancement film.
[0130] An image display device can be formed by laminating a polarizing plate to the surface of an image display unit such as a liquid crystal unit and an organic EL unit. A liquid crystal display device is formed by appropriately assembling a liquid crystal unit and a polarizing plate, and components such as a lighting system as required, and installing a drive circuit, etc. In an organic EL display device, by laminating a circular polarizing plate composed of a combination of the polarizing plate of the present invention and a phase difference film (typically a 1 / 4 wavelength plate) on the surface of an organic EL unit, the re-emission of reflected light from external light caused by a metal electrode, etc., can be reduced, thereby improving visibility.
[0131] Example
[0132] The present invention will be described in more detail below with reference to Examples, but the present invention is not limited to these Examples. "%" described below means weight % unless otherwise specified.
[0133] [Preparation of Slippery Layer-Forming Composition]
[0134] A composition for forming an easy-slip layer was prepared by mixing 20.6 parts by weight of an aqueous polyurethane ("Super Flex 210R" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) containing polyester urethane and isophorone diisocyanate as resin components, triethylamine as a curing catalyst, and methyl ethyl ketone as a dispersion medium, with a solid content of 34%, 5.2 parts by weight of an aqueous solution of a polymer containing oxazoline with a solid content of 25% ("Epocros WS-700" manufactured by Nippon Shokubai Co., Ltd.), 2.8 parts by weight of 1% ammonia water, 7.5 parts by weight of a 20% aqueous dispersion of colloidal silica having an average primary particle size of 35 nm ("Quartron.PL-3" manufactured by Fuso Chemical Co., Ltd.), and 63.9 parts by weight of pure water to prepare a composition for forming an easy-slip layer. The composition is an aqueous solution containing 15.3 parts by weight of silica particles with a concentration of 9.8% relative to 100 parts by weight of the solid content. In the following examples and comparative examples, the easy-slip layer was formed using the composition.
[0135] [Example 1]
[0136] An optical film was prepared using a film manufacturing device equipped with a melt extrusion film-making device, a gravure coater, a tenter-type simultaneous biaxial stretching device, and a winding device. As an acrylic resin, pellets of the same imidized MS resin (glass transition temperature: 120°C) used in the preparation of the "transparent protective film 1A" described in the embodiment of Japanese Patent Publication No. 2017-26939 were used. The acrylic resin was melt-extruded from a T die and filmed with a thickness of 160 μm, and the above composition was applied to one side of the film with a wet thickness of about 9 μm by a gravure coater. In a heating furnace at a temperature of 140°C, the film was stretched to 2 times in the length direction (MD) and the width direction (TD) by a simultaneous biaxial stretching tenter, and an optical film with a thickness of 50 nm of an easy-slip layer on one side of an acrylic film of 40 μm was obtained.
[0137] [Examples 2 to 4 and Comparative Examples 1 and 2]
[0138] An optical film was obtained in the same manner as in Example 1 except that the coating thickness of the easy-slip layer-forming composition was changed. Table 2 shows the thickness of the easy-slip layer (after stretching).
[0139] [Examples 5, 6 and Comparative Examples 3 to 5]
[0140] The temperature in the furnace during tenter stretching (stretching temperature) was changed as shown in Table 2. An optical film was obtained in the same manner as in Example 1 except that the stretching temperature was changed.
[0141] [Production of polarizing plate]
[0142] (Production of polarizer)
[0143] A long roll of a polyvinyl alcohol (PVA) resin film ("PE4500" manufactured by Kuraray Co., Ltd.) having a thickness of 45 μm was uniaxially stretched in the longitudinal direction by a roll stretching machine so as to be 5.9 times in the longitudinal direction, and then conveyed in the order of a swelling bath, a dyeing bath, a crosslinking bath 1, a crosslinking bath 2, and a cleaning bath as shown in Table 1, and dried at 70° C. for 5 minutes to produce a polarizer having a thickness of 18 μm. The iodine concentration and the potassium iodide concentration in the dyeing bath were adjusted so that the single-piece transmittance of the polarizer was 43.4%.
[0144] [Table 1]
[0145] Aqueous solution composition Temperature(℃) Stretch ratio Swelling bath Pure water 20 2.2 dye bath Iodine: potassium iodide = 1:7 (weight ratio) 30 1.4 Crosslinking bath 1 5.0% boric acid, 3.0% potassium iodide 40 1.2 Crosslinking bath 2 4.3% boric acid, 5.0% potassium iodide 65 1.6 Cleansing Bath 2.6% Potassium iodide 20 -
[0146] (Preparation of UV-curable adhesive)
[0147] A UV curable adhesive was prepared containing 40 parts by weight of N-hydroxyethyl acrylamide and 60 parts by weight of acryloylmorpholine as curable components, and 3 parts by weight of 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone ("IRGACURE 819" manufactured by BASF CORPORATION) as a polymerization initiator.
[0148] (Lamination of polarizer and polarizer protective film)
[0149] As the polarizer protective film on one side, the optical film of each embodiment and comparative example was used, and as the polarizer protective film on the other side, a biaxially stretched cyclic polyolefin film (ZEONOR Film ZF-14 manufactured by Zeon Corporation) was used. The above-mentioned ultraviolet curing adhesive was applied to the surface of the optical film with a thickness of about 1 μm on the easy-slip layer forming surface and the surface of the ZEONOR Film, and then attached to the polarizer using a roll laminator, and irradiated with a cumulative light amount of 1000 / mJ / cm 2 The adhesive is cured by ultraviolet rays to obtain a polarizing plate having an acrylic film (optical film) on one side of the polarizer and ZEONORFilm on the other side.
[0150] [evaluate]
[0151] <Residual alkali content in the slippery layer>
[0152] The amount of triethylamine and ammonia remaining in the slippery layer was quantified. The residual amount of triethylamine was quantified by weighing the powder obtained by scraping off the slippery layer from the surface of the optical film and dissolving it in methanol, and the solution was quantified by gas chromatography-mass spectrometry (GC / MS). The residual amount of ammonia was quantified by immersing the optical film in pure water at 25°C, then heating and extracting it in a dryer at 120°C for 60 minutes, and quantifying the ammonia dissolved in the water by ion chromatography. The total amount of triethylamine and ammonia was taken as the residual alkali amount.
[0153] <Adhesion of the Slippery Layer>
[0154] An adhesive tape ("No. 31B" manufactured by Nitto Denko Corporation) was crimped onto the surface of the optical film forming the slippery layer at a linear pressure of 8 kg / m and a crimping speed of 0.3 m / min. After being stored at 50°C for 48 hours, a 180° peeling test was carried out by holding the front end of the adhesive tape and at a tensile speed of 30 m / min. The adhesion of the slippery layer was judged by the following standards.
[0155] ○: The slippery layer was not peeled off from the acrylic film, but peeled off at the interface between the adhesive tape and the slippery layer.
[0156] ×: Peeling occurred at the interface between the acrylic film and the easy-slip layer
[0157] <Visual evaluation>
[0158] The surface of the optical film was visually observed to evaluate the presence or absence of local turbidity (increased haze) due to aggregation of silica particles and the presence or absence of scratches on the surface on which the easy-slip layer was not formed.
[0159] ○: No aggregation of silica particles, good in-plane uniformity, no damage observed
[0160] △: Turbidity due to aggregation of silica particles was not observed, but damage with a depth of less than 1 μm was confirmed on the non-slip layer-formed surface.
[0161] ×: Turbidity due to aggregation of silica particles and damage to the non-slippery layer-formed surface were observed
[0162] <Presence or absence of interface layer>
[0163] The cross section of the optical film was observed by transmission electron microscopy (TEM) to confirm whether there was a region (interface layer) where particles in the easy-slip layer were buried in the acrylic film at the interface between the acrylic film and the easy-slip layer. The TEM observation image of Example 3 (with an interface layer) is shown in FIG. Figure 3 The TEM observation image of Comparative Example 4 (without interface layer) is shown in Figure 4 .
[0164] <Humidification durability of polarizing plate>
[0165] The polarizing plate was cut into a size of 320 mm × 240 mm, and the surface on the cyclic polyolefin film side was bonded to the glass with a 20 μm thick acrylic adhesive. The sample was placed in a constant temperature and humidity chamber at a temperature of 60°C and a relative humidity of 90% (condition 1), or a constant temperature and humidity chamber at a temperature of 85°C and a relative humidity of 85% (condition 2), and maintained for 500 hours to perform a heating / humidification durability test.
[0166] The polarization degree P0 before the durability test and the polarization degree P after the durability test were measured, and the change in polarization degree ΔP=|P-P0| was calculated. In addition, another polarizing plate was arranged on the polarizing plate after the durability test with a cross prism, and the presence of streak-like unevenness was confirmed by visual observation and evaluated according to the following criteria.
[0167] ◎: No streaks were observed in the samples after the durability tests under conditions 1 and 2.
[0168] ○: No streaks were observed in the sample after the durability test under condition 1, and slight streaks were observed in the sample after the durability test under condition 2
[0169] △: Slight streaking was observed in both samples after the durability test under conditions 1 and 2.
[0170] ×: Streak unevenness was clearly observed in both samples after the durability test under conditions 1 and 2.
[0171] Table 2 shows the production conditions of the optical films of the embodiments and comparative examples (stretching temperature and thickness of the lubricant layer after stretching), the evaluation results of the optical films (visual inspection, adhesion, presence of an interface layer), and the durability test results of the polarizing plate (presence of streaking unevenness and change in polarization degree ΔP).
[0172] [Table 2]
[0173]
[0174] For the optical film of Comparative Example 2 having a slippery layer with a thickness of 350nm, the acrylic film has good adhesion to the slippery layer, and the appearance of the optical film is also good. However, the polarizing plate using the optical film as a polarizer protective film has a large decrease in polarization after the humidification durability test, and significant stripe-like unevenness is confirmed. In Comparative Examples 3 to 5 where the stretching temperature (heating temperature when the slippery layer is formed) is below 120°C, the decrease in polarization after the humidification durability test is large, and significant stripe-like unevenness is confirmed.
[0175] In the optical films of Examples 1 to 4, which formed a 50nm to 250nm easy-slip layer at a stretching temperature of 140°C, no white turbidity caused by the aggregation of particles was observed, showing a good appearance. It should be noted that although fine damage was observed on the non-easy-slip layer-forming surface of the optical film of Example 1, the damage was a level of damage that would not become an optical defect due to being buried by adhesives, bonding agents, etc. when attached to other components. In addition, the polarizing plate using the optical films of Examples 1 to 4 was superior in humidification durability compared to the polarizing plate using the optical film of Comparative Example 2, and the generation of streaks was suppressed.
[0176] The polarizing plate of the optical film of Comparative Example 1, in which a 30 nm thick slippery layer was formed, had good humidification durability, but was observed to be turbid due to the aggregation of silica particles and damage to the non-slippery layer-forming surface, resulting in poor appearance. The damage is believed to be caused by the silica particles falling off from the surface of the slippery layer due to the decrease in dispersibility, resulting in the decrease in the slipperiness of the optical film.
[0177] From the comparison between Examples 1 to 4 and Comparative Examples 1 and 2, it can be seen that the smaller the thickness of the easy-slip layer and the less the residual alkaline component, the more the generation of streaks after the humidity durability test is suppressed and the polarizing plate with excellent humidity durability can be obtained. On the other hand, it can be seen that when the thickness of the easy-slip layer is too small and the residual alkaline component is too small, the dispersibility of the particles is reduced, resulting in poor appearance and reduced sliding properties.
[0178] In Examples 5 and 6, in which a 200 nm thick slippery layer was formed at a stretching temperature of 160°C or 180°C, the appearance of the optical film and the humidity durability of the polarizing plate were excellent, similarly to Example 3. On the other hand, in Comparative Examples 3 to 5, in which a 200 nm thick slippery layer was formed at a stretching temperature of 80 to 120°C, the amount of residual alkali in the slippery layer was large, and similarly to Comparative Example 2, significant streaking unevenness was observed after the humidity durability test of the polarizing plate.
[0179] These results show that by reducing the residual alkali content of the easy-slip layer within a range that does not reduce the dispersibility of the fine particles, an optical film having excellent humidity durability of a polarizing plate when used as a polarizer protective film can be obtained.
[0180] Comparative Examples 3 to 5, which were stretched at low temperature, had poor adhesion between the acrylic film and the easy-slip layer compared to the other examples. In Example 3 and the like, an interface layer in which particles were buried in the acrylic film was formed at the interface between the acrylic film and the easy-slip layer (see Figure 3 ), whereas no interface layer was formed in Comparative Examples 3 to 5 (ref. Figure 4 ). From these results, it can be seen that by increasing the heating temperature after applying the easy-slip layer-forming composition, the alkaline components in the easy-slip layer-forming composition can be effectively volatilized to reduce the residual alkali amount, and in addition, the adhesion of the interface between the film substrate and the easy-slip layer can be improved.
[0181] Description of Reference Numerals
[0182] 1 Optical Film
[0183] 11 Film substrate
[0184] 15 Slippery layer
[0185] 2 Transparent film
[0186] 5 polarizers
[0187] 6, 7 Adhesive layer
[0188] 100, 101 polarizing plate
Claims
1. An optical film comprising a slippery layer on the surface of a transparent film substrate, in, The slippery layer contains a binder resin and silicon dioxide particles and has a thickness of 40 to 280 nm. The content of the silicon dioxide fine particles in the slippery layer is 10 to 50% by weight. The average primary particle size of the silicon dioxide particles is 10 to 250 nm. The total content of amine and ammonia in the easy-slip layer is 5 to 75 ppm.
2. The optical film according to claim 1, wherein: At the interface between the transparent film substrate and the easy-slip layer, there is a region where the silica fine particles are buried in the transparent film substrate.
3. The optical film according to claim 1 or 2, wherein: The transparent film substrate is an acrylic film.
4. The optical film according to claim 1 or 2, wherein: The binder resin of the easy-slip layer is a urethane resin.
5. A method for producing an optical film, which is a method for producing the optical film according to any one of claims 1 to 4, in, A lubricating layer-forming composition containing a binder resin or a precursor thereof, silica particles, one or more basic components selected from the group consisting of amines and ammonia, and a solvent is applied to the surface of a transparent film substrate. The easy-slip layer-forming composition is heated at a temperature 10° C. or higher than the glass transition temperature of the transparent film substrate to volatilize the solvent and the alkaline component.
6. The method for producing an optical film according to claim 5, wherein: The alkaline component has a function of promoting the dispersion of the silica fine particles.
7. The method for producing an optical film according to claim 5 or 6, wherein: The easy-slip layer-forming composition contains a polyurethane precursor as a precursor of the binder resin and a tertiary amine as the basic component.
8. The method for producing an optical film according to claim 5 or 6, wherein: The easy-slip layer-forming composition contains an amine having a boiling point of 150° C. or less as the alkaline component.
9. The method for producing an optical film according to claim 5 or 6, wherein: The transparent film substrate coated with the easy-slip layer-forming composition is stretched in at least one direction while heating the easy-slip layer-forming composition at a temperature 10° C. or higher than the glass transition temperature of the transparent film substrate.
10. A polarizing plate comprising: a polyvinyl alcohol-based polarizer having a first main surface and a second main surface, and a transparent film bonded to the first main surface of the polarizer via an adhesive layer, The transparent film is the optical film according to any one of claims 1 to 4.
11. The polarizing plate according to claim 10, wherein: The non-slip layer-forming surface of the optical film is bonded to the first main surface of the polarizer.
12. The polarizing plate according to claim 11, wherein The non-easy-slip layer-formed surface of the optical film is bonded to the first main surface of the polarizer via a photocationically polymerizable adhesive or a hybrid adhesive that can polymerize cationic and radically.
13. The polarizing plate according to claim 10, wherein: The surface of the optical film on which the easy-slip layer is formed is bonded to the first main surface of the polarizer.
14. The polarizing plate according to claim 13, wherein The easy-slip layer-formed surface of the optical film is bonded to the first main surface of the polarizer via a photo-radical polymerizable adhesive. 15 . An image display device comprising an image display unit and the polarizing plate according to claim 10 .