Conductive coated wire, conductive woven fabric, filter and sunshade system with electrostatic adsorption function of PM2.5 particles

By using conductive braided fabric with conductive cladding wire in the sunshade window system, the PM2.5 particles are adsorbed using the electrostatic adsorption principle, the problem of failure to effectively block PM2.5 in the prior art is solved, and efficient air purification and conduction are achieved , flame retardant performance.

CN113767194BActive Publication Date: 2024-11-22NINGBO XIANFENG NEW MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180002377.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-06
Publication Date
2024-11-22
Estimated Expiration
2041-08-06

AI Technical Summary

Technical Problem

The existing sunshade window system fails to effectively block and adsorb PM2.5 particles, making it difficult to improve indoor air quality.

Method used

Using conductive clad wire, a conductive braided fabric is formed by coating the fiber layer with conductive polyvinyl chloride layer and an electrostatic vacuum cleaner layer, and the electrostatic adsorption effect is enhanced by the DC power supply.

Benefits of technology

It realizes the long-term electrostatic adsorption effect of conductive braided fabrics, effectively reduces indoor PM2.5 particles, improves air quality, and has conductive, flame retardant and weather resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113767194B_ABST
    Figure CN113767194B_ABST
Patent Text Reader

Abstract

The present invention relates to a conductive coated wire, conductive woven fabric, filter screen and sunshade system with the function of electrostatically absorbing PM2.5 particles. The conductive coated wire includes a fiber layer, a conductive polyvinyl chloride layer and an electrostatic dust absorber layer from the inside to the outside, and the electrostatic dust absorber layer is formed by applying an electrostatic dust absorber solution to the surface of the conductive polyvinyl chloride layer and heating and curing. The electrostatic dust absorber solution includes the following components by weight: 8 to 12 parts of electrostatic dust absorber, 10 to 15 parts of vinyl chloride-vinyl acetate copolymer resin, 0.1 to 0.2 parts of dispersant, and 50-70 parts of butyl acetate. The conductive coated wire can be made into a conductive woven fabric and used in a filter screen and a sunshade system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and daily necessities, and relates to a conductive coated wire, a conductive woven fabric, a filter screen and a sunshade system with the function of electrostatically absorbing PM2.5 particles. Background Art

[0002] Particles are divided into total suspended particulate matter (0-100μm) and inhalable particulate matter (0-19μm) according to their aerodynamic diameter and the location of their deposition in the human respiratory system. PM2.5 is a general term for particles with an aerodynamic equivalent diameter of less than or equal to 2.5 microns. It is a type of inhalable particulate matter that can remain in the atmosphere for a long time, has a long transport distance, a small particle size, and a large specific surface area. It is very easy to accumulate toxic substances in the air, such as various acidic oxides, toxic heavy metals, bacteria, molds, germs, volatile organic compounds (VOCs), polycyclic aromatic hydrocarbons (PHAs), etc. And because its aerodynamic diameter is ≤2.5μm, it can not only enter the nasal cavity and throat, but also enter the alveolar deposition or human blood circulation, causing various diseases.

[0003] The harm of PM2.5 is multifaceted and multi-faceted and cannot be ignored. Today, PM2.5 is a hot topic in the study of inhalable particulate matter. As early as 1997, the US Environmental Protection Agency (EPA) had already recognized the harm of PM 2.5 and issued the air quality standard for PM 2.5.

[0004] As my country included PM2.5 in the "national standard" in 2012 and issued a number of regulations to control air pollution, people have gradually become more aware of PM2.5, and PM2.5 in the living environment has become a topic of concern to residents.

[0005] Windows are the main channels for external gases and dust particles to enter the room. When the air quality is poor and the weather such as haze and smog has not been significantly improved, if the sunshade window system can reduce or block the entry of dust particles that are harmful to the human body, it will be the most direct and effective measure for people indoors to stay away from PM2.5. This sunshade system that can not only ensure sunshade, ventilation, and air permeability, but also block and adsorb PM2.5 particles is an important direction for the development of sunshade windows in the future. At present, traditional sunshade window systems mainly focus on the wind resistance, sunshade, appearance, heat insulation, etc. of sunshade windows, and there are few reports on sunshade systems with electrostatic adsorption of PM2.5 particles. Summary of the invention

[0006] The purpose of the present invention is to address the above-mentioned problems existing in the prior art and to propose a conductive coated wire with the function of electrostatically adsorbing PM2.5 particles. The conductive woven fabric woven with the conductive coated wire not only has the properties of sunshade, ventilation and air permeability, but also has the characteristics of adsorbing PM2.5 and other particles.

[0007] The purpose of the present invention can be achieved by the following technical scheme: a conductive coated wire with the function of electrostatically adsorbing PM2.5 particles, the conductive coated wire comprises a fiber layer, a conductive polyvinyl chloride layer and an electrostatic dust absorber layer from the inside to the outside, the electrostatic dust absorber layer is formed by coating an electrostatic dust absorber solution on the surface of the conductive polyvinyl chloride layer and then heating and curing, and the electrostatic dust absorber solution comprises the following components by weight: 8 to 12 parts of electrostatic dust absorber, 10 to 15 parts of vinyl chloride-vinyl acetate copolymer resin, 0.1 to 0.2 parts of dispersant, and 50-70 parts of butyl acetate.

[0008] In the above-mentioned conductive coated wire, the diameter of the conductive coated wire is 0.20 mm to 0.35 mm.

[0009] In the above-mentioned conductive coated wire, the fiber is one or more of polyester fiber, glass fiber, acrylic fiber, polypropylene fiber, aramid fiber, spandex fiber, and polyethylene fiber, the fiber specification is 100-300D long fiber, and the single fiber breaking strength is greater than 10N.

[0010] In the above-mentioned conductive coated wire, the electrostatic dust absorber is a mixture of calcium sulfide, ferrosoferric oxide, zinc stannate and magnesium hydroxide.

[0011] Preferably, in the electrostatic dust collector, calcium sulfide, ferroferric oxide, zinc stannate, and magnesium hydroxide account for 15-30%, 15-30%, 15-30%, and 15-30% of the total mass of the mixture, respectively, by mass percentage. The best effect is achieved when the mass of calcium sulfide, ferroferric oxide, zinc stannate, and magnesium hydroxide are the same. Therefore, it is further preferred that the mass ratio of calcium sulfide, ferroferric oxide, zinc stannate, and magnesium hydroxide in the electrostatic dust collector is 25%.

[0012] The inorganic electrostatic dust absorber used in the present invention has poor compatibility with the polymer resin material itself, and is difficult to have good compatibility with the conductive polyvinyl chloride composite material layer in the coated wire. The present invention introduces a vinyl chloride-vinyl acetate copolymer resin into the electrostatic dust absorber solution, which has a good compatibility coupling effect with the electrostatic dust absorber (calcium sulfide, ferroferric oxide, zinc stannate, magnesium hydroxide) used in the present invention, and also has good compatibility with the conductive polyvinyl chloride composite material layer, so that the electrostatic dust absorber coating can be well integrated with the intermediate conductive polyvinyl chloride composite material layer, solving the problem that the electrostatic dust absorber coating has poor compatibility with the conductive coated wire of the polymer resin substrate and the electrostatic effect gradually weakens over time, so that the conductive coated wire of the present invention has a long-term electrostatic adsorption effect.

[0013] In the above-mentioned conductive coated wire, the dispersant can be selected from BYK-110, BYK-111, and BYK-161. The dispersant can make the electrostatic dust absorber more evenly dispersed in the matrix resin, so as to form a uniform and smooth coating on the surface of the coated wire.

[0014] In the above-mentioned conductive coated wire, the conductive polyvinyl chloride material includes the following components by weight: 70 parts of polyvinyl chloride resin (PVC), 25-35 parts of chlorinated polyethylene, 3-5 parts of stabilizer, 25-35 parts of plasticizer, 5-8 parts of flame retardant, 6-10 parts of conductive filler, 10-15 parts of modified resin, 0.2-0.4 parts of lubricant, and 0.6-1 parts of other additives.

[0015] Preferably, the conductive filler is a mixture of silver-plated nanographite flakes, nickel-coated copper powder, and single-arm carbon nanotubes in a mass ratio of 1: (0.2-0.6): (0.05-0.1). Further preferably, the conductive filler is a mixture of silver-plated nanographite flakes, nickel-coated copper powder, and single-arm carbon nanotubes in a mass ratio of 1: (0.2-0.4): (0.05-0.08). Further preferably, the mass ratio of silver-plated nanographite flakes, nickel-coated copper powder, and single-arm carbon nanotubes in the conductive filler is 1: 0.3: 0.07. Silver-plated nanographite flakes are used as the main conductive filler in the conductive polyvinyl chloride material. The specific gravity of graphite is small, and a smaller amount of addition can be used under the same volume. Its own chemical stability is also relatively high; nickel-coated copper powder not only has good conductive properties but also has excellent electromagnetic shielding performance. It has good conductive properties in combination with silver-plated nanographite flakes in the present invention. Single-arm carbon nanotubes are a supplement to the conductivity of silver-plated nanographite sheets, and have ultra-high conductivity and good mechanical and mechanical properties. When forming a composite material, since the crystal structure of silver-plated nanographite sheets, nickel-coated copper powder and single-arm carbon nanotubes is different from that of the matrix resin, silver-plated nanographite sheets, nickel-coated copper powder and single-arm carbon nanotubes as conductive particles can only stay embedded in the relatively loose grain boundaries in the matrix. When the conductive particles embedded in the grain boundaries are in contact with each other or the gap is very small, the potential barrier of the conductive filler particles is continuously reduced, and an electric percolation network is formed, and a part of the conductive channel with strong conductivity will be formed in the high resistance phase, thereby realizing the conductive function. As the main conductive particle, the silver-plated nanographite sheet is a nano-scale sheet structure at the microscopic level, which is conducive to its formation of a conductive path in the polymer, and can greatly reduce the conductive percolation threshold of the composite material system, thereby realizing the low conductive filler addition and obtaining the characteristics of high conductivity. The silver-plated nanographite microsheets are used as the main conductive particles, and different conductive particles are in ohmic contact. There is no potential barrier on the contact surface, which reduces the resistance encountered by electrons during migration, thereby increasing the migration rate of electrons in the composite material, that is, improving the conductive properties of the composite material. However, when the weight of the conductive filler in the PVC composite material of the present invention reaches about 10 parts, the conductivity of the composite material reaches a certain value and no longer changes significantly with the increase in the amount of the conductive filler, so the amount of the conductive filler is controlled to 6 to 10 parts. The addition of silver-plated nanographite microsheets and single-arm carbon nanotubes can not only improve the conductivity of the composite material, but also play a reinforcing role, so that the mechanical properties of the composite material are improved.

[0016] Preferably, the nickel content of the nickel-clad copper powder is 10 to 35% by mass. More preferably, the nickel content of the nickel-clad copper powder is 15 to 30% by mass.

[0017] The modified resin can be one or more of ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer resin. When the modified resin is a mixture of ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer resin, the mass ratio of ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer resin is 1: (0.5-1.6). Ethylene-vinyl acetate copolymer resin is copolymerized by ethylene and vinyl acetate; vinyl chloride-vinyl acetate copolymer resin is a polymer obtained by copolymerizing vinyl chloride (VC) and vinyl acetate (VAC) monomers. Both copolymer resins have polar and non-polar groups and have good compatibility with polyvinyl chloride resin. The vinyl acetate polar groups contained therein can have a chemical coupling effect with the conductive filler and inorganic additives such as antimony trioxide of the present invention, thereby playing a compatibility role on the matrix PVC resin and various inorganic additives, which can improve the flexibility, toughness and processing flowability of the composite material, and make the composite material system more uniform and reasonable. In addition, the vinyl acetate groups in ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer have good self-adhesive properties, so that the polyvinyl chloride composite material of the present invention has good thermal bonding properties. After being made into a coated wire woven fabric and subjected to heat setting treatment, the flatness and firmness of the structure can be improved.

[0018] Preferably, the modified resin is a mixture of ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer resin in a mass ratio of 1:1.

[0019] The stabilizer can be any heat stabilizer for polyvinyl chloride, such as a calcium-zinc composite stabilizer.

[0020] The plasticizer can be selected from any one or more of dioctyl terephthalate, diisooctyl adipate, dioctyl sebacate, tri-n-butyl citrate, tributyl acetyl citrate, triethyl citrate, butyl epoxy stearate, and trioctyl trimellitate. A certain amount of plasticizer is added to the conductive polyvinyl chloride material, and the molecules of the plasticizer can be inserted between the PVC molecular chains, increasing the mobility of the PVC molecular chains and reducing the crystallinity of the PVC molecular chains, thereby increasing the plasticity and flexibility of the PVC. The plasticizer is used together with chlorinated high-density polyethylene to significantly improve the flow processing performance of PVC, and a coating layer can be uniformly formed on the surface of a single fiber bundle by heating, melting, and plasticizing.

[0021] The flame retardant is antimony trioxide. Antimony trioxide itself has no flame retardant effect, but it will show a synergistic effect in the presence of halides. The chlorine element in polyvinyl chloride resin and chlorinated high-density polyethylene resin will react to generate high-concentration hydrochloric acid or free chlorine, which will react with antimony trioxide to produce antimony trichloride or antimony pentachloride-type antimony chloride substances. These antimony compounds can reduce the contact between combustibles and oxygen, so that a carbon covering layer is generated. In the gaseous state, it can also capture free radicals in the combustion process, thereby achieving the purpose of high flame retardancy with a low flame retardant addition, giving the final woven fabric good flame retardant properties and mechanical properties.

[0022] The lubricant can be any lubricant, such as ethylene bis stearamide or oxidized polyethylene wax.

[0023] The present invention also provides a method for preparing a conductive coated wire with the function of electrostatically absorbing PM2.5 particles, the method comprising: weighing 8 to 12 parts of an electrostatic dust absorber, 10 to 15 parts of a vinyl chloride-vinyl acetate copolymer resin, 0.1 to 0.2 parts of a dispersant, and 50 to 70 parts of butyl acetate, adding them into a stirring device, stirring at room temperature for 1.5 to 2 hours, and preparing an electrostatic dust absorber solution. The conductive polyvinyl chloride material is coated on the fiber surface, and then the electrostatic dust absorber solution is coated on the conductive polyvinyl chloride layer and then heated and cured to obtain a conductive coated wire.

[0024] The present invention also provides a conductive woven fabric with the function of electrostatically adsorbing PM2.5 particles, wherein the conductive woven fabric is woven by the above-mentioned conductive coated wire. The conductive woven fabric has a warp and weft structure, and a rectangular or square gap is left between the warp structure and the weft structure, and the opening rate is 10% to 15%.

[0025] The present invention sets the opening rate within the above range. The gap not only makes the fabric have good air permeability, but also makes it have a certain light transmittance. A part of the light can pass through the pores on the composite material. The light transmittance can be controlled by adjusting the size of the gap in the material, thereby achieving controllable sunshade.

[0026] The present invention also provides a method for preparing the above-mentioned conductive woven fabric, which comprises first weaving the conductive coated wire, and then placing it in a hot drying room under tension for heat setting treatment to obtain a conductive woven fabric with warp and weft threads.

[0027] Preferably, during the heat setting treatment, the temperature of the hot drying room is 90°C to 135°C, the heat setting time is 4min to 8min, the warp tension is 500N to 1300N, and the weft tension is 400N to 900N. After the heat setting treatment, the intersection of the coated wires is lightly bonded, which can prevent the conductive coated wires from shifting, so that the coated wires can be firmly bonded to prevent the fabric from deforming.

[0028] The present invention also provides a filter screen with the function of electrostatically absorbing PM2.5 particles, and the filter screen is made of the above-mentioned conductive woven fabric with the function of electrostatically absorbing PM2.5 particles.

[0029] The present invention also provides a sunshade system with the function of electrostatically absorbing PM2.5 particles, and the sunshade system includes the above-mentioned filter with the function of electrostatically absorbing PM2.5 particles.

[0030] Preferably, the sunshade system includes a left filter, a right filter, and a DC power supply, and the left filter and the right filter are respectively connected to the positive and negative electrodes of the DC power supply through wires.

[0031] Further preferably, the DC power supply provides a voltage of 50V to 220V during operation.

[0032] Further preferably, the left side of the left filter screen and the right side of the right filter screen are respectively provided with automatic winding devices.

[0033] More preferably, the automatic winding device includes a rolling tube, a cloth outlet is provided on the rolling tube, a cloth rolling shaft is provided inside the rolling tube, and the left end portion of the left filter screen and the right end portion of the right filter screen are respectively connected to the cloth rolling shaft.

[0034] More preferably, the rolling curtain tube is also provided with a stepping motor, and the stepping motor is connected to the cloth rolling shaft.

[0035] More preferably, a strip-shaped insulating sheet is provided at the right end of the left filter screen and the left end of the right filter screen, and guide rails are provided at the upper and lower ends of the left filter screen and the right filter screen, respectively.

[0036] In the present invention, the left filter, the right filter and the DC power supply form an electrostatic adsorption system, and the left filter and the right filter become two electrostatic adsorption electrodes. After power is turned on, the left filter and the right filter are respectively positively charged and negatively charged in the working state. When an object without static electricity (PM2.5 and other non-charged fine particles) approaches the electrostatic woven fabric filter, due to electrostatic induction, the side of the object without static electricity close to the electrostatic object will gather charges of opposite polarity to the charges carried by the charged object (the other side generates the same number of charges of the same polarity), and because opposite charges attract each other, the "electrostatic adsorption" phenomenon will be manifested, and PM2.5 and other non-charged fine particles will be adsorbed on the filter due to electrostatic induction, so that PM2.5 and other non-charged fine particles will not enter the room.

[0037] The sunshade system of the present invention can be automatically unfolded and reeled by stepper motors in two automatic reeling devices on the left and right through a pair of guide rails arranged above and below the left and right filter screens. When the motor switch power is turned on, the left and right filter screens will automatically unfold along the guide rails, and the stepper motor will automatically shut down when the two insulating sheets touch each other.

[0038] The sunshade system of the present invention can also be used as a general curtain for sunshade and ventilation.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] 1. The conductive coated wire of the present invention has a conductive flame-retardant polyvinyl chloride composite material layer as the middle layer. The conductive woven fabrics made of the coated wire all have a conductive flame-retardant polyvinyl chloride composite material layer, so that the woven fabrics have excellent mechanical properties, good conductivity and flame retardant properties, are easy to clean, have excellent weather resistance, and have a very long service life. In addition, the surface of the conductive coated wire contains an electrostatic dust absorber coating, which uses the principle of electrostatics to effectively absorb PM2.5 dust particles in the air.

[0041] 2. The present invention introduces vinyl chloride-vinyl acetate copolymer resin into the electrostatic dust absorber solution on the surface of the coated wire, which has good compatibility coupling effect with calcium sulfide, ferroferric oxide, zinc stannate and magnesium hydroxide in the electrostatic dust absorber used in the present invention, and also has good compatibility with PVC, so that the electrostatic dust absorber coating can be well integrated with the conductive flame-retardant polyvinyl chloride composite material layer, thereby solving the problem that the electrostatic dust absorber coating has poor compatibility with the conductive coated wire of the conductive flame-retardant polyvinyl chloride composite material substrate, and the electrostatic effect gradually weakens over time, so that the woven fabric of the present invention has a long-term electrostatic adsorption effect.

[0042] 3. The woven fabric of the present invention is made of a conductive coated wire having an electrostatic dust absorber coating on its surface. The electrostatic adsorption effect of the electrostatic dust absorber coating enables the woven fabric to have a certain adsorption effect even when no electricity is applied, and can adsorb a certain amount of PM2.5 particles.

[0043] 4. The sunshade system of the present invention uses conductive woven fabric to make a filter. After being connected to a DC power supply, the woven fabric has a better electrostatic adsorption function, which can effectively adsorb PM2.5 particles and other dust around the filter, prevent outdoor dust from entering the room, reduce the amount of indoor dust while ensuring light and scenery, and improve indoor air quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is a structural schematic diagram of the sunshade system of the present invention.

[0045] Figure 1Middle: 1. Left filter; 2. Rolling tube; 3. Stepping motor; 4. Cloth outlet; 5. Guide rail; 6. DC power supply; 7. Strip insulation sheet. DETAILED DESCRIPTION

[0046] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the drawings of the specification, but the present invention is not limited to these embodiments.

[0047] Example 1

[0048] Conductive coated wire with the function of electrostatically adsorbing PM2.5 particles.

[0049] Preparation of conductive polyvinyl chloride composite material: 70 parts of polyvinyl chloride resin, 30 parts of chlorinated polyethylene, 4 parts of calcium zinc composite stabilizer, 30 parts of dioctyl terephthalate, 6 parts of flame retardant antimony trioxide, 0.3 parts of ethylene bisstearamide, 0.4 parts of antioxidant tetrakis [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester and 0.4 parts of anti-ultraviolet agent 2-hydroxy-4-n-octyloxybenzophenone were weighed in parts by weight, and added into a high-speed mixer for mixing. When the temperature rises to 110° C., 10 parts by weight were added. The conductive filler of the present invention is a mixture of 13 parts of ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer resin in an equal proportion of 1:0.3:0.07, and then 13 parts of a mixture of ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer resin are added. The mixing is continued for 3 minutes in a high-speed mixer. The mixed materials are then added to a cold mixer and cooled to 45°C for discharging. After discharging, the materials are cooled to room temperature and then added to a twin-screw extruder for melt extrusion and granulation. After granulation, conductive polyvinyl chloride composite material granules are obtained.

[0050] Preparation of electrostatic dust absorber solution: weigh 2.5 parts of calcium sulfide, 2.5 parts of ferrosoferric oxide, 2.5 parts of zinc stannate, 2.5 parts of magnesium hydroxide, 12 parts of vinyl chloride-vinyl acetate copolymer resin, 0.15 parts of dispersant BYK-110, and 60 parts of butyl acetate by weight, add them to a stirring device, stir at room temperature for 1.5 hours, and prepare an electrostatic dust absorber solution.

[0051] Preparation of conductive coated wire: melt-coat conductive polyvinyl chloride material onto the surface of polyester fiber with a specification of 220D and a single-filament breaking strength of 20±2N, then coat the conductive polyvinyl chloride layer with an electrostatic dust absorber solution and heat-cure it to obtain a conductive coated wire with a diameter of 0.30 mm, which includes a polyester fiber layer, a conductive polyvinyl chloride layer and an electrostatic dust absorber layer from the inside to the outside. The conductive coated wire has the function of electrostatically absorbing PM2.5 particles.

[0052] Example 2

[0053] The difference between this embodiment and embodiment 1 is that in this embodiment, 8 parts of conductive fillers of silver-plated nanographite microsheets, nickel-coated copper powder (nickel content of 30% by weight), and single-arm carbon nanotubes are added in a mass ratio of 1:0.3:0.07; the diameter of the prepared conductive coated wire is 0.28 mm. The rest is the same as embodiment 1.

[0054] Example 3

[0055] The difference between this embodiment and embodiment 1 is that the electrostatic dust absorber solution is prepared as follows: 3 parts of calcium sulfide, 3 parts of ferroferric oxide, 3 parts of zinc stannate, 3 parts of magnesium hydroxide, 12 parts of vinyl chloride-vinyl acetate copolymer resin, 0.15 parts of dispersant BYK-110, and 65 parts of butyl acetate are weighed by weight, added to a stirring device, and stirred at room temperature for 1.5 hours to prepare an electrostatic dust absorber solution. The rest is the same as embodiment 1.

[0056] Example 4

[0057] The difference between this embodiment and embodiment 1 is that in this embodiment, 10 parts by weight of a mixture of ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer resin in equal proportions are added. The rest is the same as in embodiment 1.

[0058] Example 5

[0059] Conductive coated wire with the function of electrostatically adsorbing PM2.5 particles.

[0060] Preparation of conductive polyvinyl chloride composite material: 70 parts of polyvinyl chloride resin, 30 parts of chlorinated polyethylene, 4 parts of calcium zinc composite stabilizer, 30 parts of dioctyl terephthalate, 6 parts of flame retardant antimony trioxide, 0.3 parts of ethylene bisstearamide, 0.3 parts of antioxidant tris (2,4-di-tert-butylphenyl) phosphite and 0.3 parts of anti-ultraviolet agent 2-hydroxy-4-methoxybenzophenone were weighed in parts by weight, and added into a high-speed mixer for mixing. When the temperature rises to 110°C, 8 parts of 1:0 weight ratio of 1 were added. .4:0.08 of silver-plated nano-graphite flakes, nickel-coated copper powder (nickel content of 30% by mass), and conductive fillers of single-arm carbon nanotubes, and then 13 parts of a mixture of ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer resin in equal proportions are added, and the mixing is continued in a high-speed mixer for 3 minutes, and then the mixed materials are added to a cold mixer and cooled to 45°C for discharge. After discharge, the materials are cooled to room temperature, and then added to a twin-screw extruder for melt extrusion and granulation, and the conductive flame-retardant polyvinyl chloride composite material pellets are obtained after pelletizing.

[0061] Preparation of electrostatic dust absorber solution: 2 parts of calcium sulfide, 3 parts of ferrosoferric oxide, 2.5 parts of zinc stannate, 2.5 parts of magnesium hydroxide, 13 parts of vinyl chloride-vinyl acetate copolymer resin, 0.15 parts of dispersant BYK-110, and 65 parts of butyl acetate were weighed by weight, added to a stirring device, and stirred at room temperature for 1.5 hours to prepare an electrostatic dust absorber solution.

[0062] Preparation of conductive coated wire: melt-coat conductive polyvinyl chloride material onto the surface of polyester fiber with a specification of 220D and a single-filament breaking strength of 20±2N, then coat the conductive polyvinyl chloride layer with an electrostatic dust absorber solution and heat-cure it to obtain a conductive coated wire with a diameter of 0.30 mm, which includes a polyester fiber layer, a conductive polyvinyl chloride layer and an electrostatic dust absorber layer from the inside to the outside. The conductive coated wire has the function of electrostatically absorbing PM2.5 particles.

[0063] Example 6

[0064] The difference between this embodiment and embodiment 1 is that the electrostatic dust absorber solution is prepared as follows: 1.5 parts of calcium sulfide, 3 parts of ferrosoferric oxide, 3 parts of zinc stannate, 2.5 parts of magnesium hydroxide, 13 parts of vinyl chloride-vinyl acetate copolymer resin, 0.15 parts of dispersant BYK-110, and 65 parts of butyl acetate are weighed by weight, added to a stirring device, and stirred at room temperature for 1.5 hours to prepare an electrostatic dust absorber solution. The rest is the same as embodiment 1.

[0065] Example 7

[0066] The difference between this embodiment and embodiment 1 is that the electrostatic dust absorber solution is prepared as follows: 1 part of calcium sulfide, 1 part of ferroferric oxide, 4 parts of zinc stannate, 4 parts of magnesium hydroxide, 13 parts of vinyl chloride-vinyl acetate copolymer resin, 0.15 parts of dispersant BYK-110, and 65 parts of butyl acetate are weighed by weight, added to a stirring device, and stirred at room temperature for 1.5 hours to prepare an electrostatic dust absorber solution. The rest is the same as embodiment 1.

[0067] Example 8

[0068] The difference between this embodiment and embodiment 1 is that the electrostatic dust absorber solution is prepared as follows: 4 parts of calcium sulfide, 1 part of ferroferric oxide, 4 parts of zinc stannate, 1 part of magnesium hydroxide, 13 parts of vinyl chloride-vinyl acetate copolymer resin, 0.15 parts of dispersant BYK-110, and 65 parts of butyl acetate are weighed by weight, added to a stirring device, and stirred at room temperature for 1.5 hours to prepare an electrostatic dust absorber solution. The rest is the same as embodiment 1.

[0069] Example 9

[0070] The difference between this embodiment and embodiment 1 is that the conductive filler in this embodiment is conductive carbon black in equal parts. The rest is the same as embodiment 1.

[0071] Example 10

[0072] The only difference between this embodiment and embodiment 2 is that the conductive filler in this embodiment is a mixture of 4 parts of conductive graphite, 2 parts of copper powder and 2 parts of iron powder. The rest is the same as embodiment 2.

[0073] Embodiment 11

[0074] The difference between this embodiment and embodiment 1 is that in this embodiment, 3 parts of conductive fillers of silver-plated nanographite microsheets, nickel-coated copper powder (nickel content of 30% by weight), and single-arm carbon nanotubes are added in a mass ratio of 1:0.3:0.07. The rest is the same as embodiment 1.

[0075] Example 12

[0076] The difference between this embodiment and embodiment 1 is that in this embodiment, 8 parts by weight of conductive fillers of silver-plated nanographite microsheets, nickel-coated copper powder (nickel content of 30% by weight), and single-arm carbon nanotubes are added in a mass ratio of 3:3:0.7. The rest is the same as embodiment 1.

[0077] Comparative Example 1

[0078] Preparation of conductive polyvinyl chloride material: Same as Example 1.

[0079] Preparation of conductive coated wire: Conductive polyvinyl chloride material was melt-coated on the surface of polyester fiber with a specification of 220D and a single-filament breaking strength of 20±2N to obtain a coated wire with a diameter of 0.30 mm. That is, there was no electrostatic dust absorbent layer in this comparative example.

[0080] Comparative Example 2

[0081] The difference between this example and Example 1 is that in this comparative example, the electrostatic dust collector is weighed in the following weight proportions: 1 part of calcium sulfide, 1 part of ferroferric oxide, 1 part of zinc stannate, and 1 part of magnesium hydroxide. The rest is the same as Example 1.

[0082] Comparative Example 3

[0083] The difference between this example and Example 1 is that in this comparative example, the electrostatic dust collector is weighed in the following weight proportions: 4 parts of calcium sulfide, 4 parts of ferrosoferric oxide, 4 parts of zinc stannate, and 4 parts of magnesium hydroxide. The rest is the same as Example 1.

[0084] Comparative Example 4

[0085] The difference between this embodiment and embodiment 1 is that in this embodiment, the electrostatic dust absorber is weighed in the following weight parts: 5 parts of ferrosoferric oxide and 5 parts of zinc stannate. The rest is the same as embodiment 1.

[0086] Comparative Example 5

[0087] The difference between this comparative example and Example 1 is that in this comparative example, 5 parts of a mixture of ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer resin in equal proportions are added by weight to prepare the conductive polyvinyl chloride composite material; and the electrostatic dust collector solution is prepared by weighing 2.5 parts of calcium sulfide, 2.5 parts of ferrosoferric oxide, 2.5 parts of zinc stannate, 2.5 parts of magnesium hydroxide, 0.15 parts of dispersant BYK-110, and 65 parts of butyl acetate by weight, adding them to a stirring device, stirring at room temperature for 1.5 hours, and preparing the electrostatic dust collector solution. The rest is the same as Example 1.

[0088] Comparative Example 6

[0089] The difference between this comparative example and Example 1 is that in this comparative example, the polyvinyl chloride composite material does not contain conductive filler, that is, it is a common non-conductive polyvinyl chloride material, and the rest is the same as Example 1.

[0090] Examples A1-A12

[0091] The conductive coated wires obtained in Examples 1 to 12 were twisted and woven on a loom to form a woven fabric with regular patterns and a warp and weft structure, and then the woven fabric was placed in a hot drying room under tension for heat setting treatment to obtain a conductive woven fabric with an opening rate of 10%. The heat setting warp tension was 1200N, the weft tension was 700N, the temperature of the hot drying room was 125°C, and the heat setting treatment time was 6 minutes.

[0092] Comparative Examples A1-A6

[0093] The conductive coated wires in Comparative Examples 1-6 were respectively made into conductive woven fabrics by the method in Example A1.

[0094] Examples B1-B12

[0095] like Figure 1 As shown, the sunshade system with the function of electrostatically adsorbing PM2.5 particles in the present invention includes:

[0096] DC power supply: provides 100V voltage during operation;

[0097] Left filter and right filter: The left filter and right filter are made of the conductive woven fabrics in Examples A1-A12, respectively, and the left filter and the right filter are connected to the positive electrode and the negative electrode of the DC high-voltage power supply 6 through wires;

[0098] Two sets of automatic winding devices are respectively arranged on the left side of the left filter 1 and the right side of the right filter. Each set of automatic winding devices includes a rolling tube 2, on which a cloth outlet 4 is provided. A cloth rolling shaft is provided inside the rolling tube 2. The left end of the left filter 1 and the right end of the right filter are respectively connected to the cloth rolling shaft of the corresponding automatic winding device. The rolling tube 2 is also provided with a stepping motor 3 connected to the cloth rolling shaft, which is used to drive the cloth rolling shaft to realize automatic winding and unfolding of the filter.

[0099] Two insulating guide rails 5 are respectively arranged at the upper and lower ends of the left filter 1 and the right filter; and two strip insulating sheets 7 are respectively arranged at the right end of the left filter 1 and the left end of the right filter, with a width of 5 cm and a thickness of 1 cm.

[0100] The preparation method of the above-mentioned sunshade system with the function of electrostatically adsorbing PM2.5 particles is: cut the conductive woven fabric into a left filter 1 and a right filter of appropriate size, connect the left filter 1 and the right filter to the positive and negative electrodes of the high-voltage DC power supply 6 respectively, and then fix the left filter 1 and the right filter on the corresponding automatic winding devices respectively.

[0101] Comparative Examples B1-B6

[0102] The only difference from Example B1 is that the left filter and the right filter are made of the conductive woven fabrics in Comparative Examples A1-A6, respectively, that is, the left filter and the right filter in Comparative Example B1 are made of the conductive woven fabrics in Comparative Example A1, and the left filter and the right filter in Comparative Example B2 are made of the conductive woven fabrics in Comparative Example A2.

[0103] The performances of the conductive coated wires, conductive woven fabrics, and sunshade systems with the function of electrostatically adsorbing PM2.5 particles obtained in Examples 1 to 12, Comparative Examples 1 to 6, Examples A1 to A12, Comparative Examples A1 to A6, Examples B1 to B12, and Comparative Examples B1 to B6 of the present invention are compared, and the comparison results are shown in Table 1.

[0104] Table 1:

[0105]

[0106]

[0107]

[0108] Note: Oxygen index test standard: GB / T5454-1997; Sunlight color fastness test standard: GB / T8427-2008; Conductive coated wire resistance (per 20cm): refers to the resistance of the conductive coated wire before weaving; PM2.5 adsorption efficiency a: Under the condition of no DC power supply, the ratio of PM2.5 adsorbed by the woven fabric in half an hour to the mass of the woven fabric; PM2.5 adsorption efficiency b: Under the condition of DC power supply, the ratio of PM2.5 adsorbed by the woven fabric in the sunshade system in half an hour to the mass of the woven fabric.

[0109] It can be seen from Table 1 that the resistance (per 20 cm) of the conductive coated wires prepared in Examples 1-12 of the present invention is 10 5 Ω, it has conductive properties; the conductive woven fabric has good weather resistance and good flame retardant properties, and has the function of absorbing PM2.5 particles without DC power supply; when DC power is turned on, the PM2.5 particle adsorption function of the sunshade system is more obvious.

[0110] It can be seen from the examples that as the content of the conductive filler, which plays a major role in the conductive properties, in the conductive polyvinyl chloride composite material decreases, the resistance of the prepared conductive coated wire increases, as shown in Examples 1, 2 and 11. If the polyvinyl chloride composite material does not contain the conductive filler of the present invention, the resulting composite material is not conductive, as shown in Example 1 and Comparative Example 6.

[0111] The conductive filler used in the present invention is a mixture of silver-plated nanographite flakes, nickel-coated copper powder, and single-arm carbon nanotubes. If the conductive filler of the present invention is replaced by equal parts of ordinary conductive carbon black or a mixture of conductive graphite, copper powder, and iron powder in the conductive polyvinyl chloride composite material, the conductivity of the resulting conductive material is significantly weakened, as shown in Examples 1, 2 and Examples 9, 10.

[0112] Preferably, the conductive filler is a mixture of silver-plated nano-graphite flakes, nickel-coated copper powder, and single-arm carbon nanotubes in a mass ratio of 1: (0.2-0.6): (0.05-0.1). Further preferably, the conductive filler is a mixture of silver-plated nano-graphite flakes, nickel-coated copper powder, and single-arm carbon nanotubes in a mass ratio of 1: (0.2-0.4): (0.05-0.08). Still further preferably, the mass ratio of silver-plated nano-graphite flakes, nickel-coated copper powder, and single-arm carbon nanotubes in the conductive filler is 1:0.3:0.07. In the further preferred proportions and further preferred proportions of the conductive filler, the obtained polyvinyl chloride composite material has excellent conductivity (the resistance of the conductive coated wire is 10 per 20 cm). 3 Ω), see Examples 1 to 8. If the proportion of silver-plated nanographite sheets in the conductive filler is reduced, that is, the components in the conductive filler are not within the preferred proportion, the conductivity of the obtained polyvinyl chloride composite material is reduced, see Examples 1 and 12.

[0113] After the coated wire surface of the woven fabric of the present invention is coated with an electrostatic dust absorber, the surface of the woven fabric has certain electrostatic properties, and the fabric also has adsorption properties for particles such as PM2.5 without a DC power supply, as shown in Examples A1 to A12; and within a certain addition amount range, as the content of the electrostatic dust absorber in the electrostatic dust absorber solution increases, its adsorption capacity for PM2.5 increases, as shown in Examples A1, A3 and Comparative Example A2; if the coated wire surface does not contain an electrostatic dust absorber coating, the adsorption capacity of the fabric for PM2.5 is very poor under the condition of no external DC power supply, as shown in Example A1 and Comparative Example A1; if the content of the electrostatic dust absorber in the electrostatic dust absorber layer on the coated wire surface is too high, the electrostatic adsorption effect is lost, and the adsorption capacity of the woven fabric for PM2.5 becomes poor under the condition of no external DC power supply, as shown in Example A1 and Comparative Example A3;

[0114] The electrostatic dust collector of the present invention is a mixture of calcium sulfide, ferroferric oxide, zinc stannate, and magnesium hydroxide, which is a composite whole. Preferably, calcium sulfide, ferroferric oxide, zinc stannate, and magnesium hydroxide in the electrostatic dust collector account for 15-30%, 15-30%, 15-30%, and 15-30% of the total mass of the mixture, respectively, by mass percentage. Within this preferred ratio range, the resulting woven fabric has a good adsorption capacity for PM2.5 without an external DC power supply, as shown in Examples A5 and A6. Further preferably, the mass ratio of calcium sulfide, ferroferric oxide, zinc stannate, and magnesium hydroxide in the electrostatic dust collector is 25%. Under this ratio condition, the resulting woven fabric has the best adsorption capacity for PM2.5 without an external DC power supply, as shown in Examples A1, A2, A3, and A4. If the components in the electrostatic dust collector are not within the preferred range, the adsorption capacity of the obtained woven fabric for PM2.5 is reduced under the condition of no external DC power supply, see Examples A1 to A6 and Examples A7 and A8. If the electrostatic dust collector is not a mixture of calcium sulfide, ferroferric oxide, zinc stannate, and magnesium hydroxide, the adsorption capacity of the obtained woven fabric for PM2.5 is very poor under the condition of no external DC power supply, see Examples A1 to A6 and Comparative Example A4, indicating that the electrostatic dust collector compound of the present invention has a compound synergistic effect.

[0115] Since the conductive polyvinyl chloride composite material of the present invention adopts synergistic flame retardancy and free radical flame retardancy mechanism, the composite material has good flame retardancy, and the corresponding conductive woven fabric also has good flame retardancy. If the antimony trioxide in the composite material system is not evenly dispersed or the polyvinyl chloride composite material does not contain antimony trioxide, the flame retardancy of the conductive woven fabric is reduced, see Example A1 and Comparative Examples A5 and A6

[0116] In the electrostatic dust absorber solution, the vinyl chloride-vinyl acetate copolymer resin plays a coupling and compatibility role in the electrostatic dust absorber and the PVC composite material. If there is no vinyl chloride-vinyl acetate copolymer resin in the preparation process of the electrostatic dust absorber solution, it is difficult for the electrostatic dust absorber to be compatible with the polyvinyl chloride composite material layer. Finally, the electrostatic adsorption ability of the woven fabric in the absence of an external DC power supply is significantly weakened, and the ability to adsorb PM2.5 is correspondingly weakened, see Example A1 and Comparative Example A5.

[0117] In the conductive polyvinyl chloride composite material of the present invention, the ethylene-vinyl acetate copolymer resin and the vinyl chloride-vinyl acetate copolymer resin with coupling dispersion play a positive role in the uniformity of dispersion between the inorganic metal filler and the polyvinyl chloride resin in the conductive composite material system, so that the conductive and flame retardant functions can be fully exerted. If the content of the two in the formula is reduced, the uniformity of dispersion of the inorganic metal filler in PVC is poor, and the characteristics of each functional material cannot be fully exerted. Accordingly, the resistance of the material increases, and the flame retardant performance is weakened, see Examples 1, 4 and Comparative Example 5 and Examples A1, A4 and Comparative Example A5.

[0118] In a sunshade system powered by a DC power supply, the positive and negative charges on the left and right woven fabrics are greatly increased by powering the DC power supply. Due to electrostatic adsorption, a large amount of PM2.5 and other fine particles can be adsorbed, as shown in Examples B1 to B6. If the conductivity of the coated wire in the woven fabric is poor, the adsorption characteristics of the sunshade system for PM2.5 will be reduced, as shown in Examples B9 to B12 and Comparative Examples B5 and B6. In addition, if the amount or ratio of the electrostatic dust absorber on the surface of the coated wire is not within the preferred range, the adsorption capacity of the woven fabric prepared by the coated wire and its sunshade system for PM2.5 will also be weakened, as shown in Examples B7, B8 and Comparative Examples B1 to B4.

[0119] The parts of the embodiments herein that are not exhaustive of the midpoint values ​​of the technical scope claimed for protection by the present invention and the new technical solutions formed by equivalent replacement of single or multiple technical features in the technical solutions of the embodiments are also within the scope claimed for protection by the present invention; at the same time, in all the listed or unlisted embodiments of the scheme of the present invention, each parameter in the same embodiment merely represents an example of its technical solution (i.e., a feasible solution), and there is no strict coordination and limitation relationship between the parameters, wherein the parameters can be replaced with each other without violating the axioms and the claims of the present invention, unless otherwise stated.

[0120] The technical means disclosed in the scheme of the present invention are not limited to the technical means disclosed in the above technical means, but also include technical schemes composed of any combination of the above technical features. The above is a specific implementation of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also regarded as the protection scope of the present invention.

Claims

1. A conductive coated wire with the function of electrostatically adsorbing PM2.5 particles, characterized in that: The conductive coated wire comprises a fiber layer, a conductive polyvinyl chloride layer and an electrostatic dust absorber layer from the inside to the outside, wherein the electrostatic dust absorber layer is formed by applying an electrostatic dust absorber solution to the conductive polyvinyl chloride layer and then heating and curing the layer, and the electrostatic dust absorber solution comprises the following components by weight: 8-12 parts of electrostatic dust absorber, 10-15 parts of vinyl chloride-vinyl acetate copolymer resin, 0.1-0.2 parts of dispersant, and 50-70 parts of butyl acetate; The electrostatic dust collector is a mixture of calcium sulfide, ferroferric oxide, zinc stannate and magnesium hydroxide; in the electrostatic dust collector, calcium sulfide, ferroferric oxide, zinc stannate and magnesium hydroxide account for 15-30%, 15-30%, 15-30% and 15-30% of the total mass of the mixture respectively by mass percentage.

2. The conductive covered wire according to claim 1, characterized in that: The diameter of the conductive coated wire is 0.20 mm to 0.35 mm.

3. The conductive covered wire according to claim 1, characterized in that: The fiber is one or more of polyester fiber, glass fiber, acrylic fiber, polypropylene fiber, aramid fiber, spandex fiber, and polyethylene fiber. The fiber specification is 100-300D long fiber, and the single fiber breaking strength is greater than 10N.

4. The conductive covered wire according to claim 1, characterized in that: The mass ratio of calcium sulfide, ferroferric oxide, zinc stannate and magnesium hydroxide in the electrostatic dust collector is 25%.

5. The conductive covered wire according to claim 1, characterized in that: The conductive polyvinyl chloride material includes the following components by weight: 70 parts of polyvinyl chloride resin, 25-35 parts of chlorinated polyethylene, 3-5 parts of stabilizer, 25-35 parts of plasticizer, 5-8 parts of flame retardant, 6-10 parts of conductive filler, 10-15 parts of modified resin, 0.2-0.4 parts of lubricant and 0.6-1 parts of other additives.

6. The conductive covered wire according to claim 5, characterized in that: The conductive filler is a mixture of silver-plated nanographite microsheets, nickel-coated copper powder and single-arm carbon nanotubes in a mass ratio of 1: (0.2-0.6): (0.05-0.1).

7. The conductive covered wire according to claim 5, characterized in that: The conductive filler is a mixture of silver-plated nanographite microsheets, nickel-coated copper powder and single-arm carbon nanotubes in a mass ratio of 1: (0.2-0.4): (0.05-0.08).

8. The conductive covered wire according to claim 5, characterized in that: The mass ratio of the silver-plated nanographite microsheets, the nickel-coated copper powder and the single-arm carbon nanotubes in the conductive filler is 1:0.3:0.

07.

9. The conductive covered wire according to claim 5, characterized in that: The modified resin is one or more of ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer resin.

10. The conductive covered wire according to claim 5, characterized in that: The modified resin is a mixture of ethylene-vinyl acetate copolymer resin and vinyl chloride-vinyl acetate copolymer resin in a mass ratio of 1: (0.5-1.6).

11. A conductive woven fabric with the function of electrostatically absorbing PM2.5 particles, characterized in that: The conductive woven fabric is woven from the conductive coated wire according to claim 1.

12. The conductive woven fabric according to claim 11, characterized in that: The conductive woven fabric has a warp and weft structure, with rectangular or square gaps between the warp structure and the weft structure, and an opening rate of 10% to 15%.

13. A filter with the function of electrostatically adsorbing PM2.5 particles, characterized in that: The filter screen is made of the conductive woven fabric according to claim 12.

14. A sunshade system with the function of electrostatically adsorbing PM2.5 particles, characterized in that: The sunshade system comprises the filter screen of claim 13.

15. The sunshade system according to claim 14, characterized in that: The sunshade system comprises a left filter, a right filter, and a DC power supply. The left filter and the right filter are respectively connected to the positive electrode and the negative electrode of the DC power supply through wires.