Formation method and formed lithium ion battery

By increasing the charging cut-off voltage to above 4.0V during the synthesis stage of the lithium-ion battery, the problem of oxygen release during the charging process of Li5FeO4 material is solved, and the stability and safety of the battery are improved.

CN113809419BActive Publication Date: 2024-11-22ENVISION DYNAMICS TECH (JIANGSU) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111074900.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-14
Publication Date
2024-11-22
Estimated Expiration
2041-09-14

AI Technical Summary

Technical Problem

The Li5FeO4 material in lithium-ion batteries releases oxygen during the first charging process, resulting in the destruction of the CEI film between the positive electrode and the electrolyte, affecting the stability and safety of the battery.

Method used

By increasing the charging cut-off voltage of the lithium-ion battery to above 4.0V during the synthesis stage, the oxidation of active O2- in the Li5FeO4 lattice is promoted, the release of unstable oxygen elements is increased, and the release of gas during subsequent storage and circulation is reduced.

Benefits of technology

It improves the stability of lithium-ion batteries during storage and circulation, reduces gas production, and extends the battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113809419B_ABST
    Figure CN113809419B_ABST
Patent Text Reader

Abstract

The present invention provides a formation method and a lithium-ion battery after formation, wherein the formation method comprises: charging and discharging the lithium-ion battery, wherein the charging cut-off voltage is greater than or equal to 4.0V, wherein the positive electrode sheet of the lithium-ion battery contains Li5FeO4. The present invention improves the formation process, increases the voltage to above 4.0V during the formation stage, and promotes the active O in the Li5FeO4 lattice 2‑ The oxidation of Li5FeO4 increases the release of unstable oxygen elements in the Li5FeO4 lattice, thereby reducing the gas release of the battery during subsequent storage and cycling, and further improving the stability of the battery during storage and cycling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lithium ion battery production, and in particular to a formation method and a formed lithium ion battery. Background Art

[0002] With the rapid development of electric vehicles and large energy storage devices, lithium-ion batteries have been widely used in electric vehicles and large energy storage devices due to their advantages such as high voltage, large energy and light weight. The electrode material in lithium-ion batteries will affect the electrochemical performance of the battery, especially the energy density. The current common battery negative electrode material is graphite material, but its theoretical specific capacity is 372mAh / g, which can no longer meet the market demand for high energy density batteries.

[0003] Silicon-based materials have a high theoretical specific capacity and are gradually being used in high energy density power battery systems. Among them, silicon oxide composite graphite materials (C-SiO x ) has a high theoretical specific capacity (>400mAh / g) and a low reaction potential (<0.4V). However, the Li-O bond energy of its lithiation product Li2O is strong and the electrochemical reversibility is poor. The first coulomb efficiency of SiOx, which is widely studied, is only about 75%. Even if it is composited with graphite (C), its first coulomb efficiency is only about 80-85%. Both are lower than the first efficiency of 88% of the positive electrode ternary layered material and the first efficiency of 98% of the positive electrode lithium iron phosphate material. Therefore, when using C-SiO x When the negative electrode is matched with the above-mentioned positive electrode material, there will be more consumption of active Li, which will reduce the overall energy density of the battery.

[0004] The lithium ion supplement material Li5FeO4, which is currently widely studied, has a high first charge capacity (>700mAh / g) and a low first coulombic efficiency (<10%). It has a good lithium ion supplement effect and can make up for the mismatch between silicon-based negative electrode materials and positive electrode materials.

[0005] A technical solution provides a lithium-ion positive electrode material lithium replenishing additive, which includes a Li5FeO4 matrix and a coating layer located on the surface of the Li5FeO4 matrix. The double-layer coated Li5FeO4 lithium replenishing additive of this invention can play the lithium replenishing role of the Li5FeO4 material and extend the service life of the lithium-ion battery; another technical solution provides a preparation method and application of the lithium-ion battery positive electrode lithium replenishing material Li5FeO4, in which during the positive electrode slurrying process, the positive electrode lithium replenishing material Li5FeO4 is evenly mixed with the positive electrode main material, the conductive agent, the binder and the solvent, and the prepared lithium-ion battery has a high first efficiency and battery capacity; there is also a technical solution by immersing the lithium-ion battery positive electrode material in a mixed solution containing glucose, lithium salt and iron salt, mixing, drying and sintering, to obtain an in-situ lithium replenishing positive electrode material with carbon and Li5FeO4 coated on the surface, which can effectively reduce the interface resistance and improve the first coulomb efficiency and cycle performance of the lithium battery.

[0006] However, in the Li5FeO4 material, the oxidation energy level of some lattice oxygen is around 4.2V relative to lithium potential. Therefore, oxygen will be released during the first charging process. The released oxygen will react with the electrolyte and destroy the stable CEI film between the positive electrode and the electrolyte, thereby deteriorating the stability of the battery and even causing safety problems.

[0007] Therefore, how to solve the above problems and prepare lithium-ion batteries with better performance has become an urgent problem to be solved. Summary of the invention

[0008] In view of the shortcomings of the prior art, the present invention aims to provide a formation method and a lithium-ion battery after formation. The present invention improves the formation process, increases the voltage to above 4.0V during the formation stage, and promotes the active O in the Li5FeO4 lattice. 2- The oxidation of Li5FeO4 increases the release of unstable oxygen elements in the Li5FeO4 lattice, thereby reducing the gas release of the battery during subsequent storage and cycling, and further improving the stability of the battery during storage and cycling.

[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a formation method, the formation method comprising:

[0011] The lithium-ion battery is charged and discharged, and the charging cut-off voltage is greater than or equal to 4.0V, wherein the positive electrode sheet of the lithium-ion battery contains Li5FeO4.

[0012] Li5FeO4 is a commonly used lithium supplement material for lithium-ion batteries. It has a high initial charge capacity (>700mAh / g) and a low initial coulombic efficiency (<10%), and has a good lithium ion supplement effect. However, the oxidation energy level of some lattice oxygen in Li5FeO4 is around 4.2V relative to lithium potential. Therefore, oxygen will be released during the first charge process. The released oxygen will react with the electrolyte, destroying the stable CEI film between the positive electrode and the electrolyte, thereby deteriorating the stability of the battery and even causing safety problems.

[0013] The present invention improves the chemical formation process and increases the voltage to above 4.0V during the chemical formation stage, thereby promoting the active O in the Li5FeO4 lattice to form a 2- The oxidation of Li5FeO4 increases the release of unstable oxygen elements in the Li5FeO4 lattice, thereby reducing the gas release of the battery during subsequent storage and cycling, and further improving the stability of the battery during storage and cycling.

[0014] In the formation method of the present invention, the charge cut-off voltage is greater than or equal to 4.0V, for example, it can be 4.0V, 4.05V, 4.1V, 4.2V, 4.3V, 4.4V or 4.5V.

[0015] Preferably, the charging cut-off voltage is 4.0-4.5V, preferably 4.2-4.3V.

[0016] Preferably, during the charge and discharge process, the number of charge and discharge is 1 to 5 times, for example, 1 time, 2 times, 3 times, 4 times or 5 times, preferably 2 to 3 times.

[0017] Preferably, the charging current during the charging and discharging process is 0-1A and does not include 0, for example, it can be 0.01A, 0.02A, 0.05A, 0.1A, 0.2A, 0.5A, 0.8A or 1A, etc., preferably 0.01-0.2A.

[0018] Preferably, the charging includes: first charging with a current of 0.01 to 0.2 A, and then increasing the current to charge until the voltage reaches a cut-off voltage, and the cut-off voltage is greater than or equal to 4.0V.

[0019] Preferably, the current is increased to 0.1-1A, for example, 0.1A, 0.2A, 0.5A, 0.8A or 1A.

[0020] When the current density is appropriate, it is beneficial to improve the uniformity of SEI film formation in the negative electrode. In the present invention, a two-step charging mode is preferably adopted, in which a smaller current in the range of 0 to 0.2A is selected in the first step of charging to make the negative electrode of the battery better and more stable, and a larger current in the range of 0 to 1A is selected in the second step of charging to improve work efficiency.

[0021] Preferably, during the charge and discharge process, the temperature of the lithium ion battery is 25-60°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C, etc., preferably 40-50°C.

[0022] In the present invention, the temperature of the lithium-ion battery during the charge and discharge process will affect the degree of the delithiation reaction. A suitable temperature can accelerate the reaction speed, thereby allowing the lithium supplement material to be fully converted.

[0023] As a preferred technical solution of the formation method of the present invention, the charging and discharging comprises:

[0024] The lithium-ion battery is charged at 40 to 50° C. with a constant current of 0.01 to 0.2 A for 1.5 to 3.5 h, then charged with a current of 0.1 to 1 A until the voltage reaches a cutoff voltage of 4.0 to 4.5 V; and discharged.

[0025] Preferably, after the charging and before the discharging, the charging and discharging further comprises: placing for 40 to 50 hours, for example, 40 hours, 41 hours, 42 hours, 45 hours, 48 ​​hours or 50 hours. Placing can make the reaction more complete and the interface more uniform.

[0026] Preferably, the positive electrode sheet includes Li5FeO4 and positive electrode active material.

[0027] Preferably, the mass ratio of Li5FeO4 and the positive electrode active material in the positive electrode sheet is (0.1-10):(90-99), wherein the selection range of Li5FeO4 (0.1-10) can be, for example, 0.1, 0.2, 0.5, 1, 2, 3, 5, 8 or 10, etc.; the selection range of the positive electrode active material (90-99) can be, for example, 90, 91, 92, 93, 94, 95, 98 or 91, etc.

[0028] Preferably, the positive electrode active material includes at least one of lithium iron phosphate and a ternary material.

[0029] Preferably, the lithium iron phosphate has a spherical shape.

[0030] Preferably, the lithium iron phosphate is nano lithium iron phosphate.

[0031] Preferably, the lithium iron phosphate has a spherical shape, and a particle size D50 of the lithium iron phosphate is 6 to 15 μm, for example, 6 μm, 8 μm, 10 μm, 11 μm, 12 μm, 13 μm or 15 μm.

[0032] Preferably, the lithium iron phosphate is nano lithium iron phosphate, and the particle size D50 of the lithium iron phosphate is 0.3-2.0 μm, for example, 0.3 μm, 0.5 μm, 0.6 μm, 0.8 μm, 1.0 μm, 1.2 μm, 1.5 μm or 2.0 μm, etc. It should be noted that in the present invention, nano lithium iron phosphate refers to the particle size of primary particles at the nanometer level. In fact, lithium iron phosphate may exist in the form of secondary agglomerates, so the particle size D50 of lithium iron phosphate may be at the micrometer level.

[0033] Preferably, the chemical composition of the ternary material is LiNi x Co y Mn 1-x-y O2, wherein 0.5≤x≤0.9, 0≤y≤0.20, wherein x may be, for example, 0.5, 0.6, 0.7, 0.8 or 0.9, etc.; y may be, for example, 0, 0.01, 0.05, 0.08, 0.1, 0.12, 0.15, 0.18 or 0.20, etc.

[0034] Preferably, the ternary material is in a secondary spherical shape, that is, the ternary material is a secondary particle formed from primary particles, and the secondary particle is spherical.

[0035] Preferably, the ternary material is a single crystal material.

[0036] Preferably, the ternary material is a secondary sphere, and the particle size D50 of the ternary material is 9 to 25 μm, for example, it can be 9 μm, 10 μm, 12 μm, 13 μm, 14 μm, 15 μm, 17 μm, 18 μm, 20 μm, 21 μm, 22 μm, 23 μm or 25 μm, etc.

[0037] Preferably, the ternary material is a single crystal material, and a particle size D50 of the ternary material is 2 to 6 μm, for example, 2 μm, 2.5 μm, 3 μm, 4 μm, 4.5 μm, 5 μm or 6 μm.

[0038] Preferably, the positive electrode sheet also includes a composite conductive agent and / or a binder.

[0039] Preferably, the composite conductive agent comprises conductive carbon black Super P and carbon nanotubes.

[0040] Preferably, the binder comprises polyvinylidene fluoride.

[0041] Preferably, the sum of the mass of the composite conductive agent and the binder accounts for 1-5% of the total mass of the positive electrode sheet, for example, it may be 1%, 1.5%, 2%, 3%, 3.5%, 4% or 5%.

[0042] In a second aspect, the present invention provides a formed lithium-ion battery obtained by the formation method described in the first aspect, wherein the formed lithium-ion battery comprises a positive electrode sheet, in which the mass content of LiFeO2 is 80 to 100%, based on the sum of the masses of LiFeO2 and Li5FeO4 being 100%.

[0043] In the present invention, the mass content of LiFeO2 is 80-100%, that is, the positive electrode sheet may contain both LiFeO2 and Li5FeO4, or only LiFeO2 without Li5FeO4.

[0044] In the present invention, the positive electrode sheet of the lithium-ion battery contains a lithium supplement additive Li5FeO4, which can increase the release of lithium ions per unit mass of the positive electrode sheet, improve the capacity, and thus improve the overall energy density of the battery. The positive electrode sheet of the lithium-ion battery after formation contains a small amount of Li5FeO4, or even no Li5FeO4, because most of the Li5FeO4 or all of the Li5FeO4 is converted into LiFeO2, which can reduce the gas production in the subsequent process of the lithium-ion battery, thereby improving the overall stability of the battery.

[0045] Compared with the prior art, the present invention has the following beneficial effects:

[0046] The present invention improves the chemical formation process and increases the voltage to above 4.0V during the chemical formation stage, thereby promoting the active O in the Li5FeO4 lattice to form a 2- The oxidation of Li5FeO4 increases the release of unstable oxygen elements in the Li5FeO4 lattice, thereby reducing the gas release during subsequent storage and cycling, and further improving the stability of the battery during storage and cycling. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 The diagram shows the gas production results of Example 1 and Comparative Example 1.

[0048] Figure 2 This is a graph showing the ratio of Li5FeO4 to LiFeO2 in the positive electrode sheet in Example 1 and Comparative Example 1.

[0049] Figure 3 Graph showing the storage gas production of the lithium-ion batteries after formation in Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0050] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0051] The existing technical solution improves the electrochemical performance of lithium-ion batteries by adding lithium-supplementing material Li5FeO4 to the positive electrode material, but the lithium-ion batteries prepared therefrom will release oxygen during the first charging process. The released oxygen will react with the electrolyte and destroy the stable CEI film between the positive electrode and the electrolyte, thereby affecting the stability of the battery.

[0052] In order to solve the above technical problems, the present invention discloses a formation method and a lithium ion battery after formation.

[0053] The embodiment of the present invention provides a formation method, which comprises: charging and discharging a lithium-ion battery, wherein the charging cut-off voltage is greater than or equal to 4.0V, wherein the positive electrode sheet of the lithium-ion battery contains Li5FeO4.

[0054] The present invention improves the chemical formation process and increases the voltage to above 4.0V during the chemical formation stage, thereby promoting the active O in the Li5FeO4 lattice to form a 2- The oxidation of Li5FeO4 increases the release of unstable oxygen elements in the Li5FeO4 lattice, thereby reducing the gas release of the battery during subsequent storage and cycling, and further improving the stability of the battery during storage and cycling.

[0055] In some embodiments, the charge cut-off voltage is 4.0 to 4.5V, preferably 4.2 to 4.3V.

[0056] In some embodiments, during the charge and discharge process, the number of charge and discharge is 1 to 5 times, preferably 2 to 3 times.

[0057] In some embodiments, the charging current during the charging and discharging process is 0 to 1A and does not include 0, preferably 0.01 to 0.2A.

[0058] In some embodiments, the charging includes: first charging with a current of 0.01 to 0.2 A, and then increasing the current to charge until the voltage reaches a cut-off voltage, and the cut-off voltage is greater than or equal to 4.0V.

[0059] In some embodiments, the current is increased to 0.1-1A.

[0060] In some embodiments, during the charge and discharge process, the temperature of the lithium ion battery is 25 to 60°C, preferably 40 to 50°C.

[0061] In some embodiments, the charging and discharging comprises: charging the lithium ion battery at 40-50° C. with a current of 0.01-0.2 A for 1.5-3.5 h, then charging with a current of 0.1-1 A until the voltage reaches a cut-off voltage, the cut-off voltage being 4.0-4.5 V; and discharging.

[0062] In some embodiments, after the charging and before the discharging, the charging and discharging further comprises: placing, and the placing time is 40 to 50 hours.

[0063] In some embodiments, the positive electrode sheet includes Li5FeO4 and a positive electrode active material.

[0064] In some embodiments, the mass ratio of Li5FeO4 to the positive electrode active material in the positive electrode sheet is (0.1-10):(90-99).

[0065] In some embodiments, the positive electrode active material includes at least one of lithium iron phosphate and a ternary material.

[0066] In some embodiments, the lithium iron phosphate has a spherical shape.

[0067] In some embodiments, the lithium iron phosphate is nano lithium iron phosphate.

[0068] In some embodiments, the lithium iron phosphate has a spherical shape, and a particle size D50 of the lithium iron phosphate is 6 to 15 μm.

[0069] In some embodiments, the lithium iron phosphate is nano lithium iron phosphate, and the particle size D50 of the lithium iron phosphate is 0.3-2.0 μm.

[0070] In some embodiments, the chemical composition of the ternary material is LiNi x Co y Mn 1-x-y O2, where 0.5≤x≤0.9, 0≤y≤0.20.

[0071] In some embodiments, the ternary material is in the shape of a secondary sphere.

[0072] In some embodiments, the ternary material is a single crystal material.

[0073] In some embodiments, the ternary material is in a secondary spherical shape, and a particle size D50 of the ternary material is 9 to 25 μm.

[0074] In some embodiments, the ternary material is a single crystal material, and a particle size D50 of the ternary material is 2 to 6 μm.

[0075] In some embodiments, the positive electrode sheet further includes a composite conductive agent and / or a binder.

[0076] In some embodiments, the composite conductive agent includes conductive carbon black Super P and carbon nanotubes.

[0077] In some embodiments, the binder includes polyvinylidene fluoride.

[0078] In some embodiments, the sum of the mass of the composite conductive agent and the binder accounts for 1 to 5% of the total mass of the positive electrode sheet.

[0079] Another embodiment provides a formed lithium-ion battery obtained according to the formation method, wherein the formed lithium-ion battery includes a positive electrode sheet, in which the mass content of LiFeO2 is 80-100%, based on the sum of the masses of LiFeO2 and Li5FeO4 being 100%.

[0080] Example 1

[0081] This embodiment provides a formation method and a lithium ion battery after formation, the formation method comprising:

[0082] (1) Preparation of 1Ah soft pack battery:

[0083] First, Li5FeO4 and spherical lithium iron phosphate were mixed at a mass ratio of 3:99 by high-speed stirring to prepare a mixed active material powder. At the same time, Super P, carbon nanotubes, NMP, and polyvinylidene fluoride were dispersed and stirred at a mass ratio of 1:0.5:40:1 for 2 hours to prepare a conductive slurry, and then the mixed active material powder was mixed with the conductive slurry at a high speed to prepare a positive electrode slurry with a certain viscosity. Then, the prepared slurry was evenly coated on aluminum foil with a scraper, placed in a blast drying oven, and dried at 120°C for 20 minutes. The dried electrode sheet was rolled and cut to make a positive electrode sheet. Finally, the prepared positive electrode sheet was assembled into a 1Ah soft-pack battery, in which the negative electrode material was graphite, and the mass ratio of graphite: conductive carbon Super P: carboxymethyl cellulose CMC: styrene-butadiene rubber SBR in the negative electrode material was 96:1:1.5:1.5, and the electrolyte was a commercial lithium-ion battery electrolyte.

[0084] (2) Formation of 1Ah soft pack battery:

[0085] The 1Ah soft-pack battery prepared above was placed in a constant temperature oven at 45°C, charged at a constant current of 0.02A for 3 hours, then charged to 4.2V at a current density of 0.1A, and placed at this temperature for 48 hours, and then discharged at a current of 0.1A for 5 hours to obtain a formed lithium-ion battery.

[0086] Example 2

[0087] This embodiment provides a formation method and a lithium ion battery after formation, the formation method comprising:

[0088] A 1Ah soft-pack battery was placed in a 40°C constant temperature oven and charged at a constant current of 0.01A for 3.5h. The battery was then charged to 4.1V at a current density of 0.15A and placed at this temperature for 40h to obtain a formed lithium-ion battery.

[0089] The preparation method of the above 1Ah soft-pack battery is the same as that in Example 1.

[0090] Example 3

[0091] This embodiment provides a formation method and a lithium ion battery after formation, the formation method comprising:

[0092] A 1Ah soft-pack battery was placed in a constant temperature oven at 50°C, charged at a constant current of 0.05A for 2 hours, then charged to 4.3V at a current density of 0.2A and placed at this temperature for 50 hours, then discharged at a current of 0.1A for 5 hours, and the charge and discharge cycle was repeated 3 times to obtain a formed lithium-ion battery.

[0093] The preparation method of the above 1Ah soft-pack battery is the same as that in Example 1.

[0094] Example 4

[0095] This embodiment provides a formation method and a lithium ion battery after formation, the formation method comprising:

[0096] A 1Ah soft-pack battery was placed in a 45°C constant temperature oven and charged at a constant current of 0.02A for 3 hours. The battery was then charged to 4.5V at a current density of 0.1A and placed at this temperature for 48 hours. The battery was then discharged at a current of 0.1A for 5 hours to obtain a formed lithium-ion battery.

[0097] The preparation method of the above 1Ah soft-pack battery is the same as that in Example 1.

[0098] Example 5

[0099] This embodiment provides a formation method and a lithium ion battery after formation, the formation method comprising:

[0100] A 1Ah soft-pack battery was placed in a 45°C constant temperature oven, charged to 4.2V at a current density of 0.1A, and placed at this temperature for 48 hours, and then discharged at a current of 0.1A for 5 hours to obtain a formed lithium-ion battery.

[0101] The preparation method of the above 1Ah soft-pack battery is the same as that in Example 1.

[0102] Example 6

[0103] This embodiment provides a formation method and a lithium ion battery after formation, the formation method comprising:

[0104] A 1Ah soft-pack battery was placed in a constant temperature oven at 25°C, charged at a constant current of 0.02A for 3 hours, then charged to 4.2V at a current density of 0.1A, and placed at this temperature for 48 hours, then discharged at a current of 0.1A for 5 hours to obtain a formed lithium-ion battery.

[0105] The preparation method of the above 1Ah soft-pack battery is the same as that in Example 1.

[0106] Example 7

[0107] This embodiment provides a formation method and a lithium ion battery after formation, the formation method comprising:

[0108] A 1Ah soft-pack battery was placed in a constant temperature oven at 60°C, charged at a constant current of 0.02A for 3 hours, then charged to 4.2V at a current density of 0.1A, and placed at this temperature for 48 hours, then discharged at a current of 0.1A for 5 hours to obtain a formed lithium-ion battery.

[0109] The preparation method of the above 1Ah soft-pack battery is the same as that in Example 1.

[0110] Example 8

[0111] This embodiment provides a formation method and a lithium ion battery after formation, the formation method comprising:

[0112] A 1Ah soft-pack battery was placed in a 45°C constant temperature oven and charged at a constant current of 0.02A for 3 hours. The battery was then charged to 4.2V at a current density of 0.1A and placed at this temperature for 8 hours. The battery was then discharged at a current of 0.1A for 5 hours to obtain a formed lithium-ion battery.

[0113] The preparation method of the above 1Ah soft-pack battery is the same as that in Example 1.

[0114] Comparative Example 1

[0115] This comparative example provides a formation method and a lithium-ion battery after formation, which is the same as Example 1 except that the battery is charged to 3.5V.

[0116] test:

[0117] 1. Gas production test

[0118] The initial volume V0 of the 1Ah soft-pack battery in each embodiment and comparative example was tested by the drainage method, and then the formed lithium-ion battery in each embodiment and comparative example was cooled to room temperature, and the volume V1 of the formed lithium-ion battery was tested at room temperature.

[0119] The calculation formula of the formation gas production of the battery is: formation gas production = (V1-V0) / V0×100%. The formation gas production results of each embodiment and comparative example 1 calculated according to the formula are shown in Table 1.

[0120] Table 1

[0121]

[0122] The results of the gas production in Example 1 and Comparative Example 1 are as follows: Figure 1 The experimental results show that the gas production of Example 1 is about twice that of Comparative Example 1, which indicates that increasing the charge cut-off voltage during the formation process can effectively increase the gas production of the formation. The charge cut-off voltage of Comparative Example 1 is 3.5V, which cannot achieve the effect of the present invention.

[0123] It can be seen from Table 1 that multiple charge and discharge in the formation stage can promote the formation exhaust, and the exhaust effect is best when the voltage range is 4.2-4.3V. The gas production of Example 1 is greater than that of Examples 5, 6, and 8, indicating that low current density, increased temperature, and increased standing time can effectively promote the formation exhaust. The exhaust volume of Example 1 is close to that of Example 7, indicating that when the temperature reaches 50°C, further increasing the temperature has little effect on the formation exhaust.

[0124] 2. Li5FeO4 conversion test

[0125] The positive electrode sheets of the lithium-ion batteries after formation in each embodiment and comparative example were taken out, and the proportions of Li5FeO4 and LiFeO2 in the positive electrode sheets were determined by the XRD method. Taking the sum of the masses of LiFeO2 and Li5FeO4 as 100%, the mass content of LiFeO2 is shown in Table 2.

[0126] Table 2

[0127]

[0128] The ratio of Li5FeO4 to LiFeO2 in the positive electrode sheet in Example 1 and Comparative Example 1 is Figure 2 The experimental results show that increasing the formation voltage can effectively promote the complete conversion of Li5FeO4.

[0129] It can be seen from Table 2 that multiple charge and discharge in the formation stage can promote the complete conversion of Li5FeO4, and the conversion effect is best when the voltage range is 4.2-4.3V. The conversion rate of Example 1 is greater than that of Examples 5, 6, and 8, indicating that low current density, increased temperature, and increased standing time can effectively promote the complete conversion of Li5FeO4. The exhaust volume of Example 1 is close to that of Example 7, indicating that when the temperature reaches 50°C, further increasing the temperature has little effect on the conversion of Li5FeO4.

[0130] 3. Storage gas production test

[0131] The battery air bags are cut off from the lithium-ion batteries after formation in the examples and comparative examples, and the batteries are finally sealed. At room temperature, the battery is charged to a voltage of 3.65V at a rate of 0.33C, and the initial volume V1' of the battery is recorded using the drainage method. The battery is then stored in a 60°C constant temperature oven. After 7 days, the battery is taken out of the oven, allowed to stand at room temperature, and the volume of the battery is tested and recorded as V7. The battery is then charged to a voltage of 3.65V at a rate of 0.33C, and the battery is again stored in a 60°C constant temperature oven. Every 7 days, the battery is taken out of the oven, allowed to stand at room temperature, and the volume of the battery is tested and recorded as V x , where x is the number of days the battery is stored. The volume change of the battery compared to V1' corresponds to the amount of gas generated by the battery cell during storage.

[0132] The calculation formula of battery storage gas production is: Storage gas production = (V x -V1') / V1'×100%, the storage gas production results calculated according to the formula for each embodiment and comparative example are shown in Table 3.

[0133] Table 3

[0134]

[0135] The curves of the storage gas production of the lithium ion batteries after formation in Example 1 and Comparative Example 1 as the number of days increases are as follows: Figure 3 The experimental results show that the gas production of Example 1 is about one order of magnitude lower than that of Comparative Example 1. And in terms of the increasing trend of gas production, Example 1 is obviously more gentle than Comparative Example 1. It can be clearly seen that improving the formation process can effectively increase the formation gas production of the battery, so that Li5FeO4 is more completely converted into LiFeO2, thereby reducing the storage gas production and improving the stability of the battery.

[0136] It can be seen from Table 3 that multiple charge and discharge cycles in the formation stage can improve the storage gas production performance of the battery, and the conversion effect is best when the voltage range is 4.2-4.3V. The storage gas production of Example 1 is less than that of Examples 5, 6, and 8, indicating that low current density, increased temperature, and increased standing time can effectively improve the storage performance of the battery. The storage gas production of Example 1 is lower than that of Example 7, indicating that when the temperature reaches 50°C, further increasing the temperature will affect the storage gas production performance of the battery.

[0137] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A formation method, It is characterized in that The formation method comprises: The lithium-ion battery is charged and discharged, wherein the positive electrode sheet of the lithium-ion battery contains Li 5 FeO 4 ; The charging and discharging comprises: charging the lithium ion battery at 40-50° C. with a current of 0.01-0.05A for 1.5-3.5h, then charging with a current of 0.1-1A until the cut-off voltage is 4.2-4.3V, leaving it for 40-50h, and discharging.

2. The chemical formation method according to claim 1, It is characterized in that In the charging and discharging process, the number of charging and discharging is 1 to 5 times.

3. The chemical formation method according to claim 2, It is characterized in that During the charge and discharge process, the number of charge and discharge is 2 to 3 times.

4. The chemical formation method according to claim 1, It is characterized in that The positive electrode sheet includes Li 5 FeO 4 and positive electrode active material.

5. The chemical formation method according to claim 4, It is characterized in that The Li in the positive electrode 5 FeO 4 The mass ratio of the positive electrode active material is (0.1-10):(90-99).

6. The chemical formation method according to claim 4, It is characterized in that The positive electrode active material includes at least one of lithium iron phosphate and a ternary material.

7. The chemical formation method according to claim 6, It is characterized in that The lithium iron phosphate has a spherical shape.

8. The chemical formation method according to claim 6, It is characterized in that The lithium iron phosphate is nano lithium iron phosphate.

9. The chemical formation method according to claim 7, It is characterized in that The lithium iron phosphate has a spherical shape, and a particle size D50 of the lithium iron phosphate is 6 to 15 μm.

10. The chemical formation method according to claim 8, It is characterized in that The lithium iron phosphate is nano lithium iron phosphate, and the particle size D50 of the lithium iron phosphate is 0.3-2.0 μm.

11. The chemical formation method according to claim 6, It is characterized in that The chemical composition of the ternary material is LiNi x Co y Mn 1-x-y O 2 , where 0.5≤x≤0.9, 0≤y≤0.

20.

12. The chemical formation method according to claim 6, It is characterized in that The ternary material is in a secondary spherical shape.

13. The chemical formation method according to claim 6, It is characterized in that The ternary material is a single crystal material.

14. The chemical formation method according to claim 12, It is characterized in that The ternary material is in a secondary spherical shape, and the particle size D50 of the ternary material is 9-25 μm.

15. The chemical formation method according to claim 13, It is characterized in that The ternary material is a single crystal material, and the particle size D50 of the ternary material is 2-6 μm.

16. The chemical formation method according to claim 1, It is characterized in that The positive electrode sheet also includes a composite conductive agent and / or a binder.

17. The chemical formation method according to claim 16, It is characterized in that The composite conductive agent comprises conductive carbon black Super P and carbon nanotubes.

18. The chemical formation method according to claim 16, It is characterized in that The binder includes polyvinylidene fluoride.

19. The chemical formation method according to claim 16, It is characterized in that The sum of the mass of the composite conductive agent and the binder accounts for 1-5% of the total mass of the positive electrode sheet.

20. A lithium ion battery obtained by the formation method according to any one of claims 1 to 19, It is characterized in that The formed lithium-ion battery comprises a positive electrode sheet, in which LiFeO 2 With Li 5 FeO 4 The sum of the masses of LiFeO is 100%, 2 The mass content is 80-100%.