Low-temperature NOx adsorbent with enhanced hydrothermal stability

Through the combination of palladium ion exchange zeolite and alkaline earth metal and rare earth metal oxides, a catalyst that efficiently adsorbs NOx at low temperatures and releases NOx at high temperatures has been developed, solving the problem of low NOx capture efficiency at low temperatures in the existing technology. Improved overall efficiency of emissions treatment.

CN113811674BActive Publication Date: 2024-10-25BASF MOBILE EMISSIONS CATALYSTS LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080034277.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-09
Filing Date
2020-05-07
Publication Date
2024-10-25
Estimated Expiration
2040-05-07

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively capture and store nitrogen oxides (NOx) in diesel engine emissions under low temperature conditions, especially during the cold start period, and traditional catalysts are insufficiently active at low temperatures, affecting emissions treatment efficiency.

Method used

Palladium ion-exchanged zeolite is used as the low-temperature NOx adsorbent (LT-NA). By combining it with alkaline earth metal and rare earth metal oxides, the NOx adsorption and desorption performance of the zeolite is improved, forming an efficient adsorption at low temperature and high temperature. Catalyst composition that releases NOx.

Benefits of technology

It significantly improves the NOx adsorption efficiency under low temperature conditions and effectively releases NOx under high temperatures, enhancing the activity of the catalyst and meeting the increasingly stringent emission regulations, especially NOx treatment during the cold start period.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113811674B_ABST
    Figure CN113811674B_ABST
Patent Text Reader

Abstract

The present disclosure relates to low temperature NO x A catalyst composition for treating exhaust gas, a catalyst product for treating exhaust gas, and an emission treatment system, each of which comprises the LT-NA catalyst composition. A method for reducing NO in an exhaust gas stream using the catalyst product is further provided. x Specifically, the LT-NA composition comprises a zeolite, the zeolite contains a first metal component and a second metal component, the first metal component comprises palladium, and the second metal component is an alkaline earth metal component, an oxide of an alkaline earth metal component, a rare earth metal component, an oxide of a rare earth metal component, or a combination thereof. The LT-NA composition exhibits a low temperature NO x The adsorption capacity is improved and the hydrothermal stability is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-reference to related applications

[0002] This application claims the full benefit of priority to U.S. Provisional Application No. 62 / 845,359, filed on May 9, 2019. Technical Field

[0003] The present invention relates to a method suitable for treating an exhaust gas stream of a lean-burn internal combustion engine to reduce nitrogen oxides (NO x ) compositions, articles, systems and methods for preventing and controlling emissions. Background Art

[0004] Environmental regulations for internal combustion engine emissions are becoming increasingly stringent throughout the world. The operation of lean-burn engines, such as diesel engines, provides users with excellent fuel economy due to their operation at high air / fuel ratios under lean fuel conditions. However, diesel engines also emit emissions containing particulate matter (PM), unburned hydrocarbons (HC), carbon monoxide (CO), and nitrogen oxides (NO x ) of exhaust gas emissions, including NO x Describes the various chemical species of nitrogen oxides, including nitrogen monoxide and nitrogen dioxide. x It is a harmful component of air pollution. Various methods have been used to treat NO x gas mixture to reduce atmospheric pollution.

[0005] A method for reducing NO from the exhaust gas of a lean-burn engine x An effective method for reducing NOx in the presence of a selective catalytic reduction (SCR) catalyst assembly under lean-burn engine operating conditions is required. x Reaction with a suitable reducing agent. The SCR process typically uses ammonia or hydrocarbons as reducing agents in the presence of atmospheric oxygen, resulting in the formation of mainly nitrogen and steam:

[0006] 4NO+4NH 3 +O 2 →4N 2 +6H 2 O(Standard SCR reaction)

[0007] 2NO 2 +4NH 3 +O 2 →3N 2 +6H 2 O(Slow SCR reaction)

[0008] NO+NO 2 +2NH 3 →2N 2 +3H 2 O(fast SCR response)

[0009] Current catalysts used in SCR processes include molecular sieves, such as zeolites, that are ion-exchanged with catalytic metals, such as iron or copper. Useful SCR catalyst assemblies are able to effectively catalyze NO at temperatures below 600°C. x Reduction of exhaust gas components, such that reduced NO can be achieved even at low load conditions typically associated with lower exhaust temperatures x level.

[0010] One major problem encountered in the treatment of automotive exhaust gas streams is the so-called "cold start" period, which is a period of time at the beginning of the treatment process when the exhaust gas stream and the exhaust gas treatment system are at low temperatures (i.e., below 150° C.). At these low temperatures, the exhaust gas treatment system typically does not exhibit sufficient performance to effectively treat hydrocarbon (HC) emissions, nitrogen oxides (NO x ) emissions and / or carbon monoxide (CO) emissions. Typically, catalytic components such as SCR catalyst components are very effective in converting NO to CO at temperatures above 200°C. x Convert to N 2 , but do not show sufficient activity in lower temperature regions (<200°C), such as those found during cold start or extended low-speed city driving. Using catalysts that function during low temperature operation (<150°C) can help meet these increasingly stringent emission regulations (e.g., Euro-7 regulations). Since >80% of cold start NO x emissions consist of NO, so this advanced NO x It is necessary for the adsorbent material to have a great efficiency for NO adsorption. Therefore, there is an urgent need to be able to capture and store this low-temperature NO x emissions and is capable of releasing the low temperature NO at higher temperatures (>200°C) when a downstream catalytic component (e.g., SCR catalyst component) becomes effective x Therefore, considerable efforts have been made to mitigate this problem.

[0011] There are several ways to make NO x Emission minimization. For example, capture systems have been developed that can store these exhaust gas emissions (i.e., HC, CO, and NO) at low temperatures when the remaining catalytic components of the treatment system have achieved sufficient catalytic activity. x Gas) and then releases the emissions at a higher temperature. One such system is the lean NO x The LNT catalyst is a well-known and commercially proven technology. The LNT catalyst contains a catalyst that traps NO under certain exhaust conditions. x NO x Adsorbent components. For example, NOx The adsorbent component may include alkaline earth metal elements, for example, alkaline earth metal oxides and carbonates, such as oxides of Mg, Ca, Sr and / or Ba. Other LNT catalysts may contain rare earth metal oxides as NO x Adsorbent components, such as oxides of Ce, La, Pr and / or Nd. The LNT catalyst further contains a platinum group metal component (PGM), such as a dispersed x Platinum on a refractory metal oxide (e.g., alumina) support that is oxidized and reduced. The LNT catalyst operates under cyclic lean (trap mode) and rich (regeneration mode) exhaust conditions. Under lean air-fuel ratio conditions, the LNT catalyst reacts with NO x Capture and store NO during reaction ("capture") x As inorganic nitrates (e.g., in NO x The adsorbent component is BaO or BaCO 3 In the case of 3 ) 2 ). Then, NO x The adsorbent component releases the captured NO x , and the PGM components convert NO to stoichiometric or transient rich-burn engine operating conditions or to lean-burn engine operating conditions where external fuel is injected into the exhaust gas to induce rich-burn conditions. x Reduction to N 2 . NO to NO 2 The conversion is effective NO x However, when the temperature is below 200°C, the reaction rate is very slow, which makes the conventional LNT catalyst unsuitable for capturing cold start NO x Emissions are inefficient. Further, a rich purge is required to regenerate the LNT catalyst, which however minimally reduces fuel economy. Therefore, the preferred solution is to have a NO x Absorption / release components.

[0012] Another type of NO x The adsorbent is mainly Pd ion-exchanged zeolite as NO x Low temperature NO adsorbent x adsorbent (LT-NA). In this case, the NOx adsorption and desorption properties depend largely on the type of zeolite. x A LT-NA with a desorption profile optimized to meet the requirements of a specific engine application is highly desirable. Summary of the invention

[0013] The present disclosure generally provides a method for producing NO under low temperature conditions.x Compositions, articles and exhaust gas treatment systems comprising such articles having enhanced adsorption. In particular, such compositions, articles and systems include those suitable for adsorbing NO at low temperatures. x and releases the trapped NO at elevated temperatures (>200°C) when the downstream catalytic component (i.e., SCR catalyst) becomes active x NO x Adsorbent. The NO x The adsorption composition provides desirable NO under various engine operating conditions. x Adsorption and desorption properties.

[0014] Surprisingly, according to the present disclosure, it has been found that doping palladium ion-exchanged zeolites with certain metal components or metal oxides produces cold start NO after hydrothermal aging. x Enhanced adsorption capacity, NO x LT-NA compositions having a higher desorption temperature range and, when combined with a diesel oxidation catalyst (DOC) composition, having enhanced carbon monoxide (CO) and hydrocarbon (HC) conversion relative to LT-NA compositions not containing such metal components.

[0015] Therefore, on the one hand, a low temperature NO x An adsorbent (LT-NA) composition comprising a zeolite having at least a first metal component and a second metal component contained therein, wherein the first metal component comprises palladium, and wherein the second metal component is selected from the group consisting of an alkaline earth metal component, an oxide of an alkaline earth metal component, a rare earth metal component, an oxide of a rare earth metal component, and combinations thereof.

[0016] In some embodiments, the second metal component is an alkaline earth metal component or an oxide of an alkaline earth metal component. In some embodiments, the alkaline earth metal component includes: magnesium, calcium, strontium, barium; oxides of magnesium, calcium, strontium, barium; or combinations thereof. In some embodiments, the second metal component is a rare earth metal component or an oxide of a rare earth metal component. In some embodiments, the rare earth metal component includes: Ce, La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu; or oxides of Ce, La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, or Lu; or combinations thereof.

[0017] In some embodiments, at least a portion of the palladium is ion exchanged in the zeolite. In some embodiments, the palladium is present in an amount of about 0.01 wt % to about 10 wt %, based on the weight of the zeolite and calculated as elemental palladium.

[0018] In some embodiments, the weight ratio of the second metal component to the first metal component, calculated as the metal of the second metal component, is from about 0.1 to about 2. In some embodiments, the second metal component is present in an amount of from about 0.1 wt % to about 10 wt %, based on the total weight of the zeolite and calculated as the metal.

[0019] In some embodiments, the zeolite is an aluminosilicate zeolite having a silica to alumina ratio (SAR) of about 5 to about 100. In some embodiments, the aluminosilicate zeolite has a SAR of about 10 to about 40.

[0020] In some embodiments, the zeolite has a framework structure type selected from the group consisting of ABW, ACO, AEI, AEL, AEN, AET, AFI, AFN, AFO, AFR, AFS, AFT, AFX, AFY, AHT, APC, APD, ASV, ATN, ATO, ATS, ATT, ATV, AVL, AWO, AWW, BCT, BEA, BEC, BIK, BOF, BOG, BOZ, BPH, BRE, BSV, CAN, CAS, CDO, CFI, CGF, CGS, CHA, CHI, CLO, CON, CZP, DAC, DDR, DFO, DFT, DON, EAB, EDI, EEI, EMT, EON, EPI, ERI, ESV, ETR, EUO, EZT, FAU, FER, GIS, GME , GON, GOO, HEU, IFR, IFY, IHW, IMF, IRN, ISV, ITE, ITG, ITH, ITW, IWR, IWS, IWV, IWW, JBW, JRY, JSR, JST, KFI, LAU, LEV, LOV , LTA, LTF, LTL, LTN, MAZ, MEI, MEL, MER, MFI, MFS, MON, MOR, MOZ, MRE, MSE, MTF, MTT, MVY, MTW, MWF, MWW, NAB, NAT, NES, NP O, NPT, NSI, OBW, OFF, OKO, OSI, OSO, OWE, PAR, PAU, PCR, PHI, PON, PUN, RHO, RON, RRO, RSN, RTE, RTH, RWR, RWY, SAF, SAO, SA S, SAT, SAV, SBE, SBS, SBT, SCO, SEW, SFE, SFF, SFG, SFH, SFN, SFO, SFS, SFW, SGF, SIV, SOF, SOS, SSF, SSY, STF, STI, STO, STT, STW, SVR, SZR, TER, THO, TON, TSC, TUN, UEI, UFI, UOS, USI, UTL, UWY, VET, VFI, VNI, VSV, WIE, WEN, YUG, ZON and mixtures or intergrowths thereof. In some embodiments, the zeolite has a framework structure type selected from the group consisting of: BEA, CHA, FER, MFI and FAU. In some embodiments, the zeolite is selected from the group consisting of: beta zeolite, chabazite, ferrierite, mordenite, ZSM-5 and zeolite Y. In some embodiments, the zeolite is ferrierite.

[0021] In some embodiments, the LT-NA composition adsorbs NO from an exhaust gas stream at a temperature of about 30°C to about 200°C. xcomponents, and by NO present in the exhaust gas stream x Total amount, based on 1:1 NO x / Pd molar ratio, the NO x The amount of the components is at least 30-100% of the theoretical amount.

[0022] In some embodiments, the LT-NA composition converts NO to x The components are released back into the exhaust gas stream and are converted into NO by adsorption onto the LT-NA composition. x The total amount of components, the NO x The amount of the component is at least 50 to about 100 weight percent.

[0023] In some embodiments, the LT-NA composition has a first NO x The LT-NA composition has a second NOx adsorption capacity value after hydrothermal aging at 750° C. for a period of 2 to 80 hours; wherein the second NO x The adsorption capacity value is equal to or greater than the first NO x In some embodiments, the second NO x The adsorption capacity is enhanced relative to a LT-NA composition comprising a zeolite that includes a first metal component and does not include a second metal component.

[0024] In another aspect, a LT-NA article for treating an exhaust stream of an internal combustion engine is provided, the catalyst article comprising a substrate having an inlet end and an outlet end defining an overall length; and a first carrier coating disposed on at least a portion of the substrate, the first carrier coating comprising a LT-NA composition as disclosed herein.

[0025] In some embodiments, the LT-NA article further comprises a second washcoat disposed on at least a portion of the substrate, the second washcoat comprising a diesel oxidation catalyst (DOC) composition. In some embodiments, the DOC composition comprises a platinum group metal (PGM) component supported on one or more refractory metal oxide support materials. In some embodiments, the PGM component comprises platinum and palladium. In some embodiments, the refractory metal oxide support material is gamma alumina or doped with about 2% to about 10% SiO 2 In some embodiments, the DOC composition further comprises a beta zeolite that is substantially free of any PGM species.

[0026] In some embodiments, the first washcoat and the second washcoat are present in a layered configuration, wherein the first washcoat is disposed directly on the substrate and the second washcoat is disposed on at least a portion of the first washcoat. In some embodiments, the first washcoat and the second washcoat are present in a layered configuration, wherein the second washcoat is disposed directly on the substrate and the first washcoat is disposed on at least a portion of the second washcoat. In some embodiments, the first washcoat and the second washcoat are combined and disposed on the substrate in a single homogenous layer. In some embodiments, the first washcoat and the second washcoat are present in a zoned configuration, wherein the first washcoat is disposed on the catalyst substrate from the inlet end to a length of about 10% to about 70% of the total length; and wherein the second washcoat is disposed on the catalyst substrate from the outlet end to a length of about 30% to about 90% of the total length.

[0027] In some embodiments, the substrate comprises a honeycomb substrate in the form of a wall flow filter or a flow-through substrate.

[0028] In another aspect, an exhaust gas treatment system is provided, comprising the LT-NA article as disclosed herein disposed downstream of and in fluid communication with an internal combustion engine.

[0029] In some embodiments, the exhaust gas treatment system further includes one or more of a lean NOx trap (LNT), a selective catalytic reduction (SCR) catalyst, an ammonia or ammonia precursor injection assembly, a catalyzed soot filter (CSF), or an ammonia oxidation (AMOx) catalyst.

[0030] In another aspect, a method for reducing NO in an exhaust gas stream from an internal combustion engine is provided. x A method for treating an exhaust gas stream with the LT-NA article as disclosed herein or the exhaust gas treatment system as disclosed herein. In some embodiments, the contacting comprises contacting the exhaust gas stream with the LT-NA article continuously, the exhaust gas stream having an initial temperature of about 150° C. or less and the exhaust gas stream gradually increasing in temperature during additional engine operation; adsorbing and storing the NO from the exhaust gas stream; x , until the exhaust gas stream reaches a predetermined temperature, wherein the NO x releasing into the exhaust gas stream exiting the LT-NA article; and continuously contacting the exhaust gas stream exiting the LT-NA article with at least one downstream catalytic material to remove NO as the exhaust gas stream temperature increases and heating each such downstream catalytic material to an operating temperature between about 200° C. and about 450° C.x Component.

[0031] In another aspect, a method for regulating NO in a LT-NA composition is provided. x Adsorption / desorption curves and NO of LT-NA compositions x The method comprises a method of one or both of the desorption temperature ranges, the LT-NA composition comprising a zeolite, the zeolite comprising a first metal component and a second metal component, wherein the first metal component comprises palladium, and the second metal component is selected from the group consisting of an alkaline earth metal component, an oxide of an alkaline earth metal component, a rare earth metal component, an oxide of a rare earth metal component, and combinations thereof, the method comprising selecting the second metal component and its loading. In some embodiments, NO x The desorption temperature ranges from about 150°C, about 175°C, about 200°C, about 225°C, or about 250°C to about 275°C, about 300°C, about 325°C, about 350°C, or about 400°C.

[0032] By reading the following detailed description and the accompanying drawings briefly described below, these and other features, aspects and advantages of the present disclosure will become apparent. The present invention includes any combination of two, three, four or more of the above-described embodiments, and any combination of two, three, four or more features or elements set forth in the present disclosure, regardless of whether these features or elements are clearly combined in the specific embodiment description herein. The present disclosure is intended to be understood as a whole, so that unless the context clearly indicates otherwise, in any one of the various aspects and embodiments of the present invention, any separable features or elements of the present invention should be considered as combinable. Other aspects and advantages of the present invention will become apparent from the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to provide an understanding of embodiments of the present invention, reference is made to the accompanying drawings, in which the reference numerals refer to components of exemplary embodiments of the present invention. The accompanying drawings are exemplary only and should not be construed as limiting the present invention. The disclosure described herein is shown in the accompanying drawings by way of example and not limitation. For simplicity and clarity of illustration, the features illustrated in the drawings do not have to be drawn to scale. For example, for clarity, the size of some features may be enlarged relative to other features. Further, where deemed appropriate, reference numerals have been repeated in the accompanying drawings to indicate corresponding or similar elements.

[0034] Figure 1A is a perspective view of a honeycomb-type substrate that may include a catalyst (i.e., low temperature NOx adsorbent) washcoat composition according to the present disclosure;

[0035] Figure 1B is relative to Figure 1A Zoom in and follow the Figure 1A A partial cross-sectional view taken through a plane of an end surface of a substrate of FIG. 1 , the figure showing an enlarged view of the plurality of gas flow channels shown in FIG. 1 in an embodiment in which the substrate is a flow-through substrate;

[0036] Figure 2 is relative to Figure 1A A cross-sectional view of an enlarged portion of the Figure 1A The honeycomb-type substrate in represents a wall-flow filter;

[0037] Figure 3A is a cross-sectional view of one embodiment of a zoned catalytic article of the present disclosure;

[0038] Figure 3B is a cross-sectional view of an embodiment of a layered catalytic article of the present disclosure;

[0039] Figure 3C is a cross-sectional view of another embodiment of a layered catalytic article of the present disclosure;

[0040] Figure 4 is a schematic depiction of an embodiment of an exhaust gas treatment system including a LT-NA article of the present disclosure in combination with additional emission treatment system components;

[0041] Figure 5 It is NO for the embodiments of the present disclosure x Plots of adsorption and desorption versus time and temperature;

[0042] Figure 6 It is a NO that demonstrates the embodiments of the present disclosure. x Bar graph of desorption capacity;

[0043] Figure 7 It is NO for the embodiments of the present disclosure x Plots of adsorption and desorption versus time and temperature;

[0044] Figure 8 is a diagram showing the NO during FTP cold start conditions for embodiments of the present disclosure. x Bar graph of adsorption efficiency;

[0045] Fig. 9 is a plot of total hydrocarbon conversion versus time and temperature for embodiments of the present disclosure;

[0046] Fig.10 is a CO-DRIFTS spectrum for an embodiment of the present disclosure; and

[0047] Fig.11 The effect of La concentration on the FER of zeolite is shown, where the effect of La concentration on NO xThe best effect of adsorption capacity is achieved at about 1.4% La; higher La concentrations make the desorption of NO during 1200-1600 seconds higher. x The amount increased slightly. DETAILED DESCRIPTION

[0048] The present disclosure generally provides a method for adsorbing and subsequently thermally releasing NO. x Compositions, articles and exhaust gas treatment systems including such articles. In particular, such articles and systems include a composition suitable for adsorbing NO at low temperatures. x (LT-NA) and thermally releases the captured NO at elevated temperatures x NO x This is particularly important, for example, when the LT-NA article is placed upstream of a selective catalytic reduction (SCR) catalyst assembly that converts NO to CO at temperatures greater than 200°C. x Convert to N 2 It is very effective at low temperatures, but does not show sufficient activity in lower temperature regions (<200°C), such as during cold start and before urea can be injected into the exhaust gas.

[0049] The present invention will now be described more fully below. However, the present invention may be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein; on the contrary, these embodiments are provided to make this disclosure thorough and complete, and will fully convey the scope of the present invention to those skilled in the art.

[0050] definition

[0051] The article "a / an" refers to one (a kind) or more than one (a kind) (e.g., at least one (a kind)) grammatical object in this article. Any range listed herein includes end values. The term "about" used throughout the article is used to describe and illustrate small fluctuations. For example, "about" can mean that a numerical value can be modified by ± 5%, ± 4%, ± 3%, ± 2%, ± 1%, ± 0.5%, ± 0.4%, ± 0.3%, ± 0.2%, ± 0.1% or ± 0.05%. Whether or not it is clearly stated, all numerical values ​​are modified by the term "about". The numerical values ​​modified by the term "about" include specific identification values. For example, "about 5.0" includes 5.0.

[0052] The term "reduced" means a decrease in amount caused by any means.

[0053] The term "associated" means, for example, "equipped with," "connected to," or "in communication with," such as "electrically connected to," or "in fluid communication with," or otherwise connected in a manner that performs a function. The term "associated" may mean directly associated or indirectly associated, such as through one or more other articles or elements.

[0054] "Average particle size" is synonymous with D50, meaning that half of the particle population has a particle size above this point and half below this point. Particle size refers to primary particles. Particle size can be measured by laser scattering techniques, with dispersions or dry powders, for example, according to ASTM method D4464. The D90 particle size distribution indicates that 90% of the particles (by number) have a Feret diameter below a certain size as measured by scanning electron microscopy (SEM) or transmission electron microscopy (TEM) for submicron particles; and a certain size for particles (micrometers) containing a carrier as measured by a particle size analyzer.

[0055] The term "catalyst" refers to a material that promotes a chemical reaction. A catalyst comprises a "catalytically active species" and a "support" that carries or loads the active species. For example, a zeolite can be a support for active catalytic species such as platinum group metals (PGMs) or alkali metals. Similarly, refractory metal oxide particles can be a support for platinum group metal catalytic species. Catalytically active species are also referred to as "promoters" because they promote chemical reactions. For example, the PGM-containing zeolite of the present invention can be referred to as a PGM-promoted zeolite. "Promoted zeolite" refers to a zeolite to which a catalytically active species is intentionally added.

[0056] The term "catalytic article" or "catalyst article" in this disclosure means an article comprising a substrate having a catalyst coating composition.

[0057] As used herein, "crystal size" means an edge of a crystal face, preferably the length of the longest edge, provided that the crystal is not needle-shaped. Direct measurements of crystal size can be performed using microscopy methods such as SEM and TEM. For example, the measurement performed by SEM involves examining the morphology of the material at a high magnification (typically 1000x to 10,000x). The SEM method can be performed by distributing a representative portion of the zeolite powder on a suitable base so that individual particles are reasonably evenly distributed in the visual field at 1000x to 10,000x magnification. From this population, statistically significant samples (e.g., 50-200) of random individual crystals are inspected, and the longest dimension of the individual crystals parallel to the horizontal line of the straight edge is measured and recorded. Particles that are apparently large polycrystalline aggregates are not included in the measurement results. Based on these measurement results, the arithmetic mean of the sample crystal size is calculated.

[0058] "CSF" refers to a catalyzed soot filter, which is a wall-flow monolith. A wall-flow filter consists of alternating inlet and outlet channels, where the inlet channels are plugged at the outlet end and the outlet channels are plugged at the inlet end. The soot-laden exhaust gas stream entering the inlet channels is forced through the filter walls before exiting the outlet channels. In addition to soot filtration and regeneration, the CSF may carry an oxidation catalyst to oxidize CO and HC to CO 2 and H 2 O, or oxidize NO to NO 2 , thereby accelerating downstream SCR catalysis or promoting oxidation of soot particles at lower temperatures. The SCR catalyst composition can also be directly coated on a wall-flow filter called SCRoF.

[0059] As used herein, the phrase "catalyst system" refers to a combination of two or more catalysts or articles, such as a low temperature NO x A combination of an adsorbent (LT-NA) and a second catalyst which may be a DOC, LNT or SCR catalyst preparation. The catalyst system may alternatively be in the form of a washcoat, where the two catalysts are mixed together or coated in separate layers.

[0060] The term "configured" as used in the specification and claims is intended to be an open term like the terms "including" or "containing". The term "configured" does not mean to exclude other possible articles or elements. The term "configured" can be equivalent to "suitable for".

[0061] "DOC" refers to a diesel oxidation catalyst, which converts hydrocarbons and carbon monoxide in the exhaust gas of a diesel engine. Typically, a DOC includes one or more platinum group metals, such as palladium and / or platinum; a support material, such as alumina; a zeolite for HC storage; and optionally a promoter and / or stabilizer.

[0062] Typically, the term "effective" means, for example, about 35% to 100% effective, such as about 40%, about 45%, about 50% or about 55% to about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, about 90% or about 95% by weight or mole with respect to a defined catalytic activity or storage / release activity.

[0063] The term "exhaust stream" or "exhaust gas stream" refers to any combination of flowing gases that may contain solid or liquid particulate matter. The gas stream includes a gaseous component and is, for example, the exhaust gas of a lean burn engine, which may contain certain non-gaseous components such as liquid droplets, solid particles, etc. The exhaust gas stream of an internal combustion engine generally further includes combustion products (CO 2 and H 2 O), incomplete combustion products (carbon monoxide (CO) and hydrocarbons (HC)), nitrogen oxides (NO x), combustibles and / or carbonaceous particulate matter (soot), and unreacted oxygen and nitrogen. As used herein, the terms "upstream" and "downstream" refer to the relative directions of flow of the engine exhaust gas stream from the engine toward the exhaust pipe, wherein the engine is in an upstream position and the exhaust pipe and any pollutant reduction products such as filters and catalysts are located downstream of the engine. The inlet end of the substrate is synonymous with the "upstream" end or "front" end. The outlet end is synonymous with the "downstream" end or "rear" end. The upstream zone is upstream of the downstream zone. The upstream zone can be closer to the engine or manifold, while the downstream zone can be farther away from the engine or manifold.

[0064] A "high surface area refractory metal oxide support" specifically refers to a support having pores larger than High surface area refractory metal oxide supports, such as alumina support materials also known as "gamma alumina" or "activated alumina", typically exhibit fresh material BET surface areas in excess of 60 square meters per gram ("m 2 / g”), usually up to about 200m 2 / g or more. This activated alumina may also be a mixture of γ and δ phases of alumina, but may also contain a large amount of η, κ and θ alumina phases.

[0065] As used herein, "impregnated" or "impregnation" refers to the penetration of the catalytic material into the porous structure of the support material.

[0066] The term "fluidly connected" is used to designate articles that are located on the same exhaust line, i.e., a common exhaust flow passes through the articles that are fluidly connected to each other. The articles that are fluidly connected may be adjacent to each other in the exhaust line. Alternatively, the articles that are fluidly connected may be separated by one or more articles also referred to as "washcoat monoliths".

[0067] The term "functional article" in the present invention means an article comprising a substrate having disposed thereon a functional coating composition, specifically a catalyst and / or adsorbent coating composition.

[0068] As used herein, "impregnated" or "impregnation" refers to the penetration of the catalytic material into the porous structure of the support material.

[0069] “LNT” refers to Lean NO x The trap contains a filter suitable for adsorbing NO during lean combustion conditions. x The catalysts are platinum group metals, rare earth metal oxides and alkaline earth metal capture materials (e.g., BaO or MgO). Under enrichment conditions, NO is released. x and converts it to nitrogen.

[0070] As used herein, the term "molecular sieve" such as zeolites and other zeolite framework materials (e.g., isomorphously substituted materials) refers to materials that can support catalytic PGMs or other catalytic metals in particulate form. Molecular sieves are materials based on an extensive three-dimensional network of oxygen ions that generally contain tetrahedral sites and have a substantially uniform pore distribution, wherein the average pore size is no greater than 10 angstroms. It can be mainly based on (SiO 4 ) / AlO 4 Molecular sieves are distinguished by the geometry of the interstices formed by the rigid network of tetrahedra. The entrance to the interstices is formed by 6, 8, 10 or 12 ring atoms relative to the atoms forming the entrance opening. Molecular sieves are crystalline materials with fairly uniform pore sizes, ranging from about 3 to 100 mm in diameter, depending on the type of molecular sieve and the type and amount of cations contained in the molecular sieve lattice. Molecular sieves include small pore, medium pore and large pore molecular sieves or a combination thereof. The pore size is defined by the maximum ring size.

[0071] As used herein, the term "nitrogen oxide" or "NO x " indicates nitrogen oxides, such as NO, NO 2 or N 2 O.

[0072] The terms "on" and "over" with respect to coatings may be used synonymously. The term "directly on" means in direct contact. In certain embodiments, the disclosed articles are referred to as including one coating "on" a second coating, and such language is intended to encompass embodiments with intervening layers where direct contact between the coatings is not required (i.e., "on" is not equivalent to "directly on").

[0073] As used herein, the term "selective catalytic reduction" (SCR) refers to the reduction of nitrogen oxides to dinitrogen (N 2 ) catalytic process.

[0074] "Substantially free" means "little or no" or "not intentionally added", and also only trace and / or unintentional amounts. For example, in certain embodiments, "substantially free" means less than 2 wt% (weight %), less than 1.5 wt%, less than 1.0 wt%, less than 0.5 wt%, 0.25 wt%, or less than 0.01 wt%, based on the weight of the indicated total composition.

[0075] As used herein, the term "substrate" refers to a monolithic material to which a catalyst composition (that is, a catalytic coating) is usually coated in the form of a carrier coating. In one or more embodiments, the substrate is a flow-through monolith and a monolithic wall-flow filter. For example, a flow-through substrate and a wall-flow substrate are also taught in International Application Publication No. WO2016 / 070090, which is incorporated herein by reference. The carrier coating is formed by preparing a slurry of a catalyst containing a specific solid content (e.g., 30-90% by weight) in a liquid, and then applying the slurry to a substrate and drying to provide a carrier coating layer. Reference to "monolithic substrate" refers to a monolithic structure that is uniform and continuous from inlet to outlet. The carrier coating is formed by preparing a slurry of particles containing a certain solid content (e.g., 20% by weight-90% by weight) in a liquid vehicle, and then applying the slurry to a substrate and drying to provide a carrier coating layer.

[0076] As used herein, the term "support" refers to any high surface area material, typically a metal oxide material, to which the catalytic noble metal is applied.

[0077] As used herein, the term "carrier coating" in the art generally means a thin adherent coating of a catalytic material or other material applied to a substrate material such as a honeycomb substrate, the thin adherent coating being porous enough to allow the treated gas flow to pass through. The carrier coating containing the metal-promoted molecular sieve of the present invention may optionally include a binder selected from silica, alumina, titania, zirconium oxide, ceria or a combination thereof. The loading amount of the binder is about 0.1 wt.% to 10 wt.% by weight of the carrier coating. As used herein and as described in Heck, Ronald and Farrauto, Robert, Catalytic Air Pollution Control, New York: Wiley-Interscience, 2002, pages 18-19, the carrier coating layer comprises a layer of material of different composition disposed on a monolithic substrate or an underlying carrier coating layer. The substrate may contain one or more carrier coating layers, and each carrier coating layer may be different in some way (e.g., may be different in its physical properties, such as particle size or microcrystalline phase) and / or may be different in chemical catalytic function.

[0078] If not otherwise indicated, "weight percent (wt%)" is based on the entire composition excluding any volatiles, that is, based on dry solids content. Unless otherwise indicated, all parts and percentages are by weight.

[0079] As used herein, the term "zeolite" refers to a specific example of a molecular sieve, further comprising silicon atoms and aluminum atoms. In general, a zeolite is defined as having TOs shared by corners.4 Aluminosilicates with an open 3-dimensional framework structure of tetrahedra, where T is Al or Si, or optionally P. The cations that balance the charge of the anionic framework are loosely associated with the framework oxygens, and the remaining pore volume is filled with water molecules. Non-framework cations are usually exchangeable, and the water molecules are removable.

[0080] The aluminosilicate zeolite structure does not contain phosphorus or other metals isomorphously substituted in the framework. That is, "aluminosilicate zeolite" does not include aluminum phosphate materials such as SAPO, AlPO and MeA1PO, while the broader term "zeolite" includes aluminosilicates and aluminophosphates. For the purposes of this disclosure, SAPO, AlPO and MeA1PO materials are considered to be non-zeolitic molecular sieves.

[0081] The zeolite of the present invention may independently include SiO2 connected by common oxygen atoms to form a three-dimensional network. 4 / AlO 4 Tetrahedral. The silica to alumina ("SAR") molar ratio of the zeolites of the present invention can vary widely, but is generally 2 or greater. For example, the zeolites of the present invention can have a SAR of from about 5 to about 1,000.

[0082] Zeolite comprises secondary building units (SBU) and composite building units (CBU), and appears in many different framework structures. Secondary building units contain up to 16 tetrahedral atoms and are achiral. Composite building units do not need to be achiral, nor are they necessarily used to build the entire framework. For example, a group of zeolites has a single 4-ring (S4R) composite building unit in its framework structure. In the 4 rings, "4" represents the position of tetrahedral silicon and aluminum atoms, and oxygen atoms are located between tetrahedral atoms. Other composite building units include, for example, single 6-ring (S6R) units, double 4-ring (D4R) units, and double 6-ring (D6R) units. The D4R unit is produced by connecting two S4R units. The D6R unit is produced by connecting two S6R units. In the D6R unit, there are twelve tetrahedral atoms.

[0083] Generally, any framework type of zeolite can be used, such as framework types ABW, ACO, AEI, AEL, AEN, AET, AFI, AFN, AFO, AFR, AFS, AFT, AFX, AFY, AHT, APC, APD, ASV, ATN, ATO, ATS, ATT, ATV, AVL, AWO, AWW, BCT, BEA, BEC, BIK, BOG, BPH, BRE, CAN, CAS, SCO, CFI, SGF, CGS, CHA, CHI, CLO, CON, CZP, DAC, DDR, DFO, DFT, DON, EAB, EDI, EEI, EMT, EON, EPI, ERI, ESV, ETR, EUO, FAU, FER, GIS, GME, GON, GOO, HEU, IFR, IFY, IHW, IRN, ISV, ITE, ITH, ITW, IWR, IWW , JBW, KFI, LAU, LEV, LOV, LTA, LTL, LTN, MAZ, MEI, MEL, MER, MFI, MFS, MON, MOR, MOZ, MTF, MTT, MTW, MWF, MWW, NAB, NAT, NES, NPO, NPT, NSI, OBW, OFF, OSI, OSO, OWE, PAR, PAU, PHI, PON, RHO, RON, RRO, R SN, RTE, RTH, RWR, RWY, SAO, SAS, SAT, SAV, SBE, SBS, SBT, SFE, SFF, SFG, SFH, SFN, SFO, SFW, SOS, SS Y, STF, STI, STT, TER, THO, TON, TSC, UEI, UFI, USI, UTL, VET, VFI, VNI, VSV, WIE, WEN, YUG, ZON, or combinations thereof.

[0084] Zeolites are crystalline materials with fairly uniform pore sizes ranging from about 3 to 10 angstroms in diameter, depending on the type of zeolite and the type and amount of cations contained in the zeolite lattice. The pore size is defined by the ring size. As used herein, the term "small pore" refers to a pore opening that is less than about 5 angstroms, such as about 3.8 angstroms or so.

[0085] Small pore zeolites contain channels defined by up to eight tetrahedral atoms. The phrase "8-ring" zeolite refers to a zeolite having 8-ring pore openings and double six-ring secondary building blocks and having a cage-like structure resulting from the double six-ring building blocks connected by 4 rings.

[0086] Exemplary small pore zeolites include framework types ACO, AEI, AEN, AFN, AFT, AFX, ANA, APC, APD, ATT, CDO, CHA, DDR, DFT, EAB, EDI, EPI, ERI, GIS, GOO, IHW, ITE, ITW, LEV, KFI, MER, MON, NSI, OWE, PAU, PHI, RHO, RTH, SAT, SAV, SIV, THO, TSC, UEI, UFI, VNI, YUG, ZON, and mixtures or intergenes thereof.

[0087] Medium pore zeolites contain channels defined by ten-membered rings. Exemplary medium pore zeolites include framework types AEL, AFO, AHT, BOF, BOZ, CGF, CGS, CHI, DAC, EUO, FER, HEU, IMF, ITH, ITR, JRY, JSR, JST, LAU, LOV, MEL, MFI, MFS, MRE, MTT, MVY, MWW, NAB, NAT, NES, OBW, PAR, PCR, PON, PUN, RRO, RSN, SFF, SFG, STF, STI, STT, STW, SVR, SZR, TER, TON, TUN, UOS, VSV, WEI, WEN, and mixtures or inter-organisms thereof.

[0088] Large pore zeolites contain channels defined by twelve-membered rings. Exemplary large pore zeolites include framework types AFI, AFR, AFS, AFY, ASV, ATO, ATS, BEA, BEC, BOG, BPH, BSV, CAN, CON, CZP, DFO, EMT, EON, EZT, FAU, GME, GON, IFR, ISV, ITG, IWR, IWS, IWV, IWW, JSR, LTF, LTL, MAZ, MEI, MOR, MOZ, MSE, MTW, NPO, OFF, OKO, OSI, RON, RWY, SAF, SAO, SBE, SBS, SBT, SEW, SFE, SFO, SFS, SFV, SOF, SOS, STO, SSF, SSY, USI, UWY, VET, and mixtures or intergenes thereof.

[0089] Unless otherwise indicated, all parts and percentages are by weight. If not otherwise indicated, "weight percent (wt %)" is based on the entire composition excluding any volatiles, that is, based on dry solid content.

[0090] Unless otherwise specified herein or clearly contradicted by context, all methods described herein may be performed in any suitable order. Unless otherwise stated, the use of any and all examples or exemplary language (e.g., "such as") provided herein is intended only to better illustrate the materials and methods and is not intended to limit the scope. The language in the specification should not be interpreted as indicating that any unclaimed element is necessary for the practice of the materials and methods of the present disclosure.

[0091] All U.S. patent applications, pre-grant publications, and patents mentioned herein are hereby incorporated by reference in their entirety.

[0092] Low temperature NOx adsorbent (LT-NA) composition

[0093] The present disclosure provides a LT-NA composition comprising a zeolite having at least a first metal component and a second metal component contained therein, wherein the first metal component comprises palladium, and wherein the second metal component is selected from the group consisting of an alkaline earth metal component, an oxide of an alkaline earth metal component, a rare earth metal component, an oxide of a rare earth metal component, and combinations thereof. Individual components of the LT-NA composition are further described below.

[0094] Zeolite

[0095] As mentioned above, the LT-NA composition of the present invention includes a zeolite having at least a first metal component and a second metal component contained therein. As described herein above, the term "zeolite" refers to a specific example of a molecular sieve, further comprising silicon atoms and aluminum atoms. According to one or more embodiments, the zeolite can be based on a framework topology by which the structure is identified. Generally, any framework type of zeolite can be used, such as ABW, ACO, AEI, AEL, AEN, AET, AFI, AFN, AFO, AFR, AFS, AFT, AFX, AFY, AHT, APC, APD, AST, ASV, ATN, ATO, ATS, ATT, ATV, AVL, AWO, AWW, BCT, BEA, BEC, BIK, BOF, BOG, BOZ, BPH, BRE, BSV, CAN, CAS, CDO, CFI, CGF, CGS, CHA, CHI, CLO, CON, CZP, DAC, DDR, DFO, DFT, DON, EAB, EDI, EEI, EMT, EON, EPI, ERI, ESV, ETR, EUO, EZT, FAU, FER, GIS, GME, GON, GOO ,HEU,IFR,IFY,IHW,IMF,IRN,ISV,ITE,ITG,ITH,ITW,IWR,IWS,IWV,IWW,JBW,JRY,JSR,JST,KFI,LAU,LEV,LOV,LTA,LT F, LTL, LTN, MAZ, MEI, MEL, MER, MFI, MFS, MON, MOR, MOZ, MRE, MSE, MTF, MTT, MVY, MTW, MWF, MWW, NAB, NAT, NES,, NPO, NPT, NSI, OBW, OFF, OKO, OSI, OSO, OWE, PAR, PAU, PCR, PHI, PON, PUN, RHO, RON, RRO, RSN, RTE, RTH, RWR, RWY, SAF, SAO, SAS, SAT , SAV, SBE, SBS, SBT, SCO, SEW, SFE, SFF, SFG, SFH, SFN, SFO, SFS, SFW, SGF, SIV, SOF, SOS, SSF, SSY, STF, STI, STO, STT, STW, SVR, SZR, TER, THO, TON, TSC, TUN, UEI, UFI, UOS, USI, UTL, UWY, VET, VFI, VNI, VSV, WIE, WEN, YUG, ZON and mixtures or inter-organisms thereof. In some embodiments, the zeolite has a framework structure type selected from the group consisting of BEA, CHA, FER, MFI and FAU.

[0096] In some embodiments, the zeolite has a two-dimensional pore system. In some embodiments, the zeolite having the two-dimensional pore system may have a framework type such as, but not limited to, FER, CSV, DAC, HEU, MFS, MWW, NES, RRO, SFG, STI, STT, or TER. The synthesis of zeolites having a FER structure and a discussion of pore geometry are disclosed in, for example, Weitkamp et al., Chem. Eng. Technol. 25, (2002), 3, 273-275; Pinar et al., Proceedings of the 5th Serbian-Croatian-Slovenian Zeolite Symposium. th Serbian-Croatian-Slovenian Symposium on Zeolites, 32-35; and Parikh et al., Indian Journal of Chemical Technology, Sept. 18, 2011, 335-342, each of which is incorporated herein by reference in its entirety.

[0097] In some embodiments, the zeolite is an aluminosilicate zeolite. In some embodiments, the average crystal size of the aluminosilicate zeolite crystals (i.e., the average crystal size of individual crystals including twin crystals) is greater than about 0.5 μm, preferably between about 0.1 μm and about 15 μm, such as about 0.5 μm to about 5 μm, about 0.7 μm to about 1.5 μm, about 1 μm to about 5 μm, or about 1 μm to about 10 μm.

[0098] In some embodiments, the zeolite is selected from the group consisting of beta zeolite, chabazite, ferrierite, mordenite, ZSM-5, and zeolite Y. In some embodiments, the zeolite is ferrierite.

[0099] The silica to alumina ("SAR") molar ratio of the zeolites of the present invention can vary widely, but is typically 2 or greater. For example, the zeolites of the present invention may have a SAR of about 5 to about 1000. In some embodiments, the zeolites have a silica to alumina ratio (SAR) of about 2 to about 300, including about 5 to about 250; about 5 to about 200; about 5 to about 100; and about 5 to about 50. In one or more specific embodiments, the molecular sieve has a SAR molar ratio in the range of about 10 to about 200, about 10 to about 100, about 10 to about 75, about 10 to about 60, and about 10 to about 50, about 15 to 100, about 15 to about 75, about 15 to about 60, and about 15 to about 50, about 20 to about 100, about 20 to about 75, about 20 to about 60, and about 20 to about 50. In one or more embodiments, the SAR molar ratio of the molecular sieve ranges from about 1, about 2, about 5, about 8, about 10, about 15, about 20, or about 25 to about 30, about 35, about 40, about 45, about 50, about 60, about 70, about 80, about 90, about 100, about 150, about 200, about 260, about 300, about 400, about 500, about 750, or about 1000. In some embodiments, the zeolite is an aluminosilicate zeolite having a SAR of about 5 to about 100. In some embodiments, the aluminosilicate zeolite has a SAR of about 10 to about 40. In some embodiments, the silica and alumina (SiO 2 :Al 2 O 3 ) is about 2 to about 50. In some embodiments, SiO 2 With Al 2 O 3 The molar ratio is about 25.

[0100] Without wishing to be bound by theory, high zeolite sodium content may negatively affect hydrothermal stability. Therefore, low sodium and alkali metal content in the zeolite is generally preferred. In certain embodiments, the alkali content of the zeolite is less than 3 wt%, more preferably less than 1 wt%, and even more preferably less than 0.1 wt%, based on the total weight of the calcined zeolite (reported as alkali metal oxides on a non-volatile basis). In some embodiments, low alkali content zeolites can be prepared by exchanging the sodium (Na) form of the zeolite for alumina (NH 4 ) form. 4 The ion exchange into the zeolite can be carried out at room temperature or at a temperature up to about 80° C. over a period of about 1 to 24 hours. In some embodiments, preferably, the produced zeolite material can be dried at about 100 to 120° C. to obtain NH 4 In some embodiments, NH 4The exchanged zeolite is calcined at a temperature of at least about 450°C to obtain the H-exchanged zeolite.

[0101] First metal component

[0102] As mentioned above, the disclosed LT-NA composition includes a zeolite having at least a first metal component and a second metal component contained therein, wherein the first metal component includes palladium. As used herein, the term "first metal component" refers to a first metal or an ion or compound of the first metal, such as an oxide. In some embodiments, the first metal includes palladium. As used herein, the term "comprising palladium" means that the metal component includes, contains or is palladium, including palladium in a zero-valent state (i.e., palladium metal), palladium ions or compounds thereof. The disclosed LT-NA composition can be described as comprising a zeolite that "includes" palladium (or as comprising palladium "associated" with the zeolite). In such examples, "comprising" (or "associated with") should be understood to mean palladium located in the ion exchange sites of the zeolite, on the surface of the zeolite, or both in the ion exchange sites of the zeolite and on the surface of the zeolite.

[0103] The concentration of the first metal component can vary, but will generally be from about 0.01 wt % to about 10 wt % relative to the weight of the zeolite. Palladium can be present in the zeolite, for example, from about 0.1 wt %, about 0.2 wt %, about 0.5 wt %, about 0.7 wt %, about 0.9 wt % or about 1.0 wt % to about 1.5 wt %, about 2.0 wt %, about 2.5 wt %, about 3.0 wt %, about 3.5 wt %, about 4.0 wt %, about 4.5 wt % or about 5.0 wt % by the total weight of the zeolite. The weight of palladium is measured and reported as metal.

[0104] Second metal component

[0105] As mentioned above, the disclosed LT-NA composition includes a zeolite having at least a first metal component and a second metal component contained therein. The second metal component is selected from the group consisting of an alkaline earth metal component, an oxide of an alkaline earth metal component, a rare earth metal component, an oxide of a rare earth metal component, and combinations thereof.

[0106] In some embodiments, the second metal component is present as a metal ion, which may be present, for example, within at least a portion of the ion exchange sites of a zeolite. In some embodiments, the second metal component is present as a metal oxide.

[0107] The quantity of the second metal component can vary. For example, by the total weight of the zeolite (i.e., the weight of the zeolite containing the first metal component, the second metal component and any additionally added components), the LT-NA composition of the present invention generally contains about 0.1 wt % to about 10 wt % or about 0.5 wt % to about 5 wt % of the second metal component. In some embodiments, by the total weight of the zeolite, the total amount of the second metal component is less than 10 wt %, less than 9 wt %, less than 8 wt %, less than 7 wt %, less than 6 wt %, less than 5 wt %, less than 4 wt %, less than 3 wt %, less than 2 wt %, less than 1 wt % or less than 0.5 wt %. In some embodiments, by the total weight of the zeolite, the second metal component is present in an amount of about 0.5 wt %. In some embodiments, by the total weight of the zeolite, the second metal component is present in an amount of about 0.5 wt %, about 1 wt %, about 2 wt %, about 3 wt %, about 4 wt % or about 5 wt %.

[0108] In some embodiments, the weight ratio of the second metal component to the first metal component is from about 0.1 to about 2, calculated as metal oxide and metal, respectively.

[0109] Alkaline earth metal components

[0110] In some embodiments, the second metal component of the LT-NA composition as disclosed herein is an alkaline earth metal component. As used herein, the term "alkaline earth metal component" refers to alkaline earth metal compounds, complexes, etc., which may decompose or otherwise convert into forms such as corresponding alkaline earth metal oxides when calcined or using a catalyst. In some embodiments, at least a portion of the alkaline earth metal component is present as an ion of an alkaline earth metal in the ion exchange site of the zeolite. In some embodiments, at least a portion of the alkaline earth metal component exists as an alkaline earth metal oxide, disposed on or in the zeolite. As used herein, the term "alkaline earth metal" refers to Group II metals, such as magnesium, calcium, strontium, and barium. In some embodiments, the alkaline earth metal component includes barium, calcium, magnesium, strontium, or a mixture thereof. In some embodiments, the alkaline earth metal component is barium. In some embodiments, the alkaline earth metal component is strontium.

[0111] The alkaline earth metal component also includes oxides of alkaline earth metals.

[0112] Rare earth metal components

[0113] In some embodiments, the second metal component of the LT-NA composition as disclosed herein is a rare earth metal component. The term "rare earth metal component" refers to rare earth metal compounds, complexes, etc., which may decompose or otherwise convert into forms such as corresponding rare earth metal oxides when calcined or using a catalyst. In some embodiments, at least a portion of the rare earth metal component is present as ions of rare earth metals in the ion exchange sites of the zeolite. In some embodiments, at least a portion of the rare earth metal component exists as a rare earth metal oxide, disposed on or in the zeolite. Depending on the valence of the specific transition metal, these oxides can contain various oxidation states of rare earth metals, such as monoxides, dioxides, trioxides, tetraoxides, etc. As used herein, the term "rare earth metal" refers to lanthanide metals as defined in the periodic table. Lanthanide metals include cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium. Particularly suitable rare earth metals include one or more of lanthanum, cerium, neodymium, yttrium, praseodymium and mixtures thereof. In some embodiments, the rare earth metal component includes Y, Ce, La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu or a combination thereof. In some embodiments, the rare earth metal component is lanthanum.

[0114] Although the foregoing description provides several suitable ranges or amounts for the metal components of the LT-NA composition, it should be noted that each disclosed range or amount for one of these components can be combined with the disclosed ranges or amounts of other components to form new ranges or sub-ranges. Such embodiments are also expressly contemplated by the present invention.

[0115] The rare earth metal component also includes oxides of rare earth metals.

[0116] Diesel Oxidation Catalyst (DOC) Composition

[0117] Typically, DOC compositions include one or more platinum group metal (PGM) components dispersed on a support, such as a refractory metal oxide support. Various such DOC compositions are known to be useful for treating the exhaust gas of diesel engines to convert hydrocarbon (HC) and carbon monoxide (CO) gaseous pollutants into carbon dioxide and water by catalyzing the oxidation of these pollutants.

[0118] The term "PGM component" refers to any component containing a PGM (e.g., Ru, Rh, Os, Ir, Pd, Pt and / or Au). Reference to a "PGM component" allows the PGM to exist in any valence state. For example, the PGM may be in the form of a zero-valent metal, or the PGM may be in the form of an oxide. The terms "platinum (Pt) component," "rhodium (Rh) component," "palladium (Pd) component," "iridium (Ir) component," "ruthenium (Ru) component," and the like refer to corresponding platinum group metal compounds, complexes, and the like, which decompose or otherwise convert into a catalytically active form, typically a metal or metal oxide, when calcined or using a catalyst. In some embodiments, the PGM component comprises palladium, platinum, rhodium, rhenium, ruthenium, iridium, or a combination thereof. In some embodiments, the PGM component comprises palladium, platinum, or a mixture thereof. In some embodiments, the PGM component is a metal or an oxide thereof (e.g., including but not limited to platinum or an oxide thereof).

[0119] The PGM component may be present in an amount ranging from about 0.01 to about 20% on a metal basis, based on the weight of the DOC composition. The DOC composition may include, for example, about 0.1 wt.%, about 0.5 wt.%, about 1.0 wt.%, about 1.5 wt.%, or about 2.0 wt.% to about 3 wt.%, about 5 wt.%, about 7 wt.%, about 9 wt.%, about 10 wt.%, about 12 wt.%, about 15 wt.%, about 16 wt.%, about 17 wt.%, about 18 wt.%, about 19 wt.%, or about 20 wt.% of the PGM component, based on the weight of the dry DOC composition. In specific embodiments, the PGM of the DOC composition disclosed herein includes both a platinum component and a palladium component. In some embodiments, the Pt / Pd ratio of the PGM component is from about 10:1 to about 1:10. In some embodiments, the Pt / Pd weight ratio is about 2 / 1.

[0120] Typically, both the platinum component and the palladium component of the disclosed DOC composition are supported on a support material (wherein the support material on which the platinum component and the palladium component are supported may be the same or different). The support material may be a zeolite or a non-zeolite. Reference to a "non-zeolite-support" or "non-zeolitic support" in a catalyst layer refers to a material that is not a zeolite and that receives a noble metal, stabilizer, promoter, binder, etc. by association, dispersion, impregnation or other suitable method. Examples of such non-zeolite supports include, but are not limited to, high surface area refractory metal oxides.

[0121] The support material on which the catalytically active platinum component and the second palladium component are deposited includes, for example, refractory metal oxides that exhibit chemical and physical stability at high temperatures such as those associated with gasoline or diesel engine exhaust. Exemplary refractory metal oxides include alumina, silica, zirconia, titania, ceria, praseodymium, tin oxide, and the like, as well as physical mixtures or chemical combinations thereof, including atomically doped combinations and including high surface area or active compounds, such as activated alumina. Combinations of metal oxides such as silica-alumina, ceria-zirconia, praseodymium oxide-ceria, alumina-zirconia, alumina-ceria-zirconia, lanthanum oxide-alumina, lanthanum oxide-zirconia-alumina, barium oxide-alumina, barium oxide-lanthanum oxide-alumina, barium oxide-lanthanum oxide-neodymium oxide-alumina, and alumina-ceria are included. Exemplary aluminas include macroporous boehmite, gamma-alumina, and delta / theta alumina. Useful commercial aluminas for use as starting materials in the exemplary methods include activated aluminas such as high bulk density gamma-alumina, low or medium bulk density macroporous gamma-alumina, and low bulk density macroporous boehmite and gamma-alumina.

[0122] High surface area metal oxide supports, such as alumina support materials also known as "gamma alumina" or "activated alumina", typically exhibit BET surface areas in excess of 60 m 2 / g, usually up to about 200m 2 / g or more. Exemplary refractory metal oxides include those with a specific surface area of ​​about 50 m 2 / g to about 300m 2 / g of high surface area gamma-alumina. Such activated aluminas are usually a mixture of gamma and delta phases of alumina, but may also contain significant amounts of eta, kappa and theta alumina phases. "BET surface area" has its usual meaning: it refers to the surface area of ​​the alumina measured by N 2 The Brunauer, Emmett, Teller method for determining surface area by adsorption. It is desirable that the specific surface area of ​​activated alumina be about 60 m 2 / g to about 350m 2 / g, for example, about 90m 2 / g to about 250m 2 / g.

[0123] In certain embodiments, the metal oxide support that can be used in the DOC catalyst composition disclosed herein is a Si-doped alumina material (including but not limited to 1-10% SiO 2 -Al 2 O 3 ) and other doped aluminum oxide materials, such as Si doped titanium dioxide materials (including but not limited to 1-10% SiO 2 -TiO2 ) or Si-doped ZrO 2 (including but not limited to 5-30% SiO 2 -ZrO 2 ) and other doped zirconia materials.

[0124] Thus, the refractory metal oxide support or refractory mixed metal oxide in the DOC catalyst composition is typically selected from the group consisting of alumina, zirconia, silica, titania, ceria such as bulk ceria, manganese oxide, zirconia-alumina, ceria-zirconia, ceria-alumina, lanthanum oxide-alumina, barium oxide-alumina, silica, silica-alumina, and combinations thereof.

[0125] The DOC catalyst composition may include any of the refractory metal oxides described above and in any amount. For example, the refractory metal oxide support in the catalyst composition may include from about 15 wt.%, about 20 wt.%, about 25 wt.%, about 30 wt.%, or about 35 wt.% to about 50 wt.%, about 55 wt.%, about 60 wt.%, about 65 wt.%, or about 70 wt.%, based on the total dry weight of the DOC catalyst composition. The DOC catalyst composition may, for example, include from about 10 to about 99 wt.% alumina, from about 15 to about 95 wt.% alumina, or from about 20 to about 85 wt.% alumina.

[0126] In some embodiments, the LT-NA compositions disclosed herein adsorb NO from an exhaust gas stream at a temperature of about 30°C to about 200°C, such as about 30°C, about 40°C, about 50°C, about 75°C, or about 100°C to about 125°C, about 150°C, about 175°C, or about 200°C. x Component.

[0127] In some embodiments, the LT-NA compositions disclosed herein adsorb NO from an exhaust gas stream. x Components, according to NO present in the exhaust gas stream x Based on the total amount of NOx / Pd at a 1:1 molar ratio, the NO x The amount of the component is at least 30-100% of the ideal amount, for example, about 30%, about 35%, about 40%, about 45%, about 50%, about 55%, about 60%, about 70%, about 75%, about 80%, about 85%, about 90%, about 95%, about 96%, about 97%, about 98%, about 99% or about 100% of the ideal amount.

[0128] In some embodiments, the LT-NA compositions disclosed herein convert NO to NH4O at a temperature of about 170°C to about 300°C, such as about 170°C, about 180°C, about 190°C, about 200°C, or about 225°C to about 250°C, about 275°C, or about 300°C. x The components are released back into the exhaust gas stream.

[0129] In some embodiments, the LT-NA compositions disclosed herein convert NO x The components are released back into the exhaust gas stream as NO adsorbed onto the LT-NA composition. x The total amount of components, the NO x The amount of the component is at least 55 to about 100 weight %, for example about 55 weight %, about 60 weight %, about 65 weight %, about 70 weight %, about 75 weight %, about 80 weight %, about 85 weight %, about 90 weight %, about 95 weight % or about 100 weight %.

[0130] In some embodiments, the catalyst composition is fresh. In other embodiments, the catalyst composition has been aged. "Aged" means that the composition or an article comprising such a composition has been exposed to elevated temperatures for an extended period of time, which simulates the conditions to which the composition will be exposed during use in a vehicle exhaust treatment system. Such aging may be referred to as "hydrothermal aging."

[0131] In some embodiments, a LT-NA composition as disclosed herein has a first NO x The adsorption capacity value of NO is 0.0447 W / m and the LT-NA composition has a second NO adsorption capacity value after hydrothermal aging at 750°C for a period of 2-80 hours. x adsorption capacity value; wherein the second NO x The adsorption capacity value is equal to or greater than the first NO x The comparison of the first adsorption capacity and the second adsorption capacity provides an indication of stability under vehicle application conditions. In some embodiments, the LT-NA compositions disclosed herein have an enhanced NOx adsorption capacity (i.e., the second adsorption capacity is greater than the first adsorption capacity) after such hydrothermal aging. Surprisingly, it has been found that in some embodiments, the second NOx adsorption capacity of the LT-NA compositions disclosed herein is greater than the first adsorption capacity. x The adsorption capacity is enhanced relative to LT-NA compositions comprising a zeolite comprising a first metal component and not comprising a second metal component. Without wishing to be bound by any theory or principle, it is believed that the presence of the second metal component serves to stabilize and promote the activity of the zeolite containing the first metal component.

[0132] Preparation of catalytic composition

[0133] In some embodiments, the disclosed LT-NA catalyst and DOC composition can be prepared by incipient wetness impregnation. Incipient wetness impregnation technique, also known as capillary impregnation or dry impregnation, is commonly used to synthesize heterogeneous materials, i.e., catalysts. Typically, a metal precursor is dissolved in an aqueous or organic solution, and then a metal-containing solution is added to a catalyst support (e.g., a zeolite or refractory metal oxide) having a pore volume that is the same as the volume of the added solution. Capillary action draws the solution into the pores of the support. The added solution exceeds the volume of the support pores, causing the transport of the solution to be converted from a capillary action process to a much slower diffusion process. The catalyst can then be dried and calcined to remove the volatile components in the solution, thereby depositing the metal on the surface of the catalyst support. The maximum loading is limited by the solubility of the precursor in the solution. The concentration distribution of the impregnated material depends on the mass transfer conditions in the pores during impregnation and drying. Those skilled in the art will recognize other methods for loading the metal component into the support of the composition of the present invention, such as adsorption, ion exchange, precipitation, etc.

[0134] For example, in the preparation of the components of the LT-NA catalyst composition, palladium can be impregnated onto the zeolite.Palladium salts that can be used to introduce palladium to the zeolite include, but are not limited to, nitrates.

[0135] In some embodiments, the first metal component, the second metal component, or both are ion exchanged in the zeolite. Ion exchange is a process that is commonly used to exchange ions residing in a porous support with external metal ions of interest. The zeolite framework contains open spaces in the form of channels and cages, which are usually occupied by water molecules and cations outside the framework that can be replaced. Aluminum atoms attract excess negative charges, which are compensated by these cations. The interior of the pore system is represented by a catalytically active surface. The more aluminum and the less silicon a zeolite contains, the denser the negative charge in its lattice and the greater the polarity of its inner surface.

[0136] Because there are 2-valent or 3-valent cations as tetrahedral centers in the zeolite framework, zeolite receives negative charge in the form of so-called anionic sites, and the corresponding cationic position is located near the so-called anionic sites. Negative charge is compensated by combining cations, such as metal cations, into the pores of zeolite materials. The cations of the charge of the balancing anionic framework are loosely associated with the framework oxygen, and the remaining pore volume is filled with water molecules. Non-framework cations are usually exchangeable, and water molecules are removable. These spaces and channels are the characteristics of every kind of zeolite. The term "exchange site" refers to a site that can be used for cations and is occupied by metal cations (e.g., palladium) that are mainly intentionally added to zeolite through ion exchange.

[0137] For example, with sodium ions or NH 4 +The zeolite prepared with palladium ions can be exchanged with, for example, palladium ions to form a palladium ion exchanged zeolite. This is achieved by preparing a slurry of the zeolite in a solution containing palladium ions. During this process, heat can optionally be applied. The palladium ions can now diffuse into the pores of the zeolite and interact with the resident ions, i.e., Na + or NH 4 + The exchange is performed to form a palladium ion exchanged zeolite. "Palladium ion exchange" means that at least a portion of the ion exchange sites are occupied by palladium ions. Specifically, it is preferred that more than 50% of the exchangeable sites are exchanged with palladium, and preferably more than 70% of the exchangeable sites are exchanged with palladium.

[0138] Similarly, for the preparation of DOC compositions as disclosed herein, typically, an aqueous solution of a soluble compound or complex of a platinum group metal (PGM) is used to impregnate a support material (e.g., a zeolite or a refractory metal oxide). Non-limiting examples of suitable compounds include palladium nitrate, palladium tetraamine nitrate, platinum tetraamine acetate, and platinum nitrate. During the calcination step, or at least during the initial stage of using the complex, such compounds are converted to a catalytically active form of the metal or its compound. A suitable method for preparing a DOC catalyst composition is to prepare a mixture of a solution of a desired PGM compound (e.g., a platinum compound and / or a palladium compound) and at least one support such as a finely divided high surface area refractory metal oxide support such as gamma alumina, the at least one support being dry enough to absorb substantially all of the solution to form a wet solid that is subsequently combined with water to form a coatable slurry. In one or more embodiments, the slurry is acidic, for example, with a pH of about 2 to less than about 7. The pH of the slurry can be reduced by adding an appropriate amount of an inorganic acid or an organic acid to the slurry. When the compatibility of the acidic material and the raw material is considered, a combination of the two can be used. The inorganic acid includes, but is not limited to, nitric acid. Organic acids include but are not limited to acetic acid, propionic acid, oxalic acid, malonic acid, succinic acid, glutamic acid, adipic acid, maleic acid, fumaric acid, phthalic acid, tartaric acid, citric acid, and the like.

[0139] Catalytic products

[0140] In one or more embodiments, the LT-NA composition of the present invention is disposed (coated) on a substrate to form a catalytic article (i.e., a catalytic component or catalytic article). Such an article is part of an exhaust gas treatment system (e.g., a catalyst article, including but not limited to an article comprising the LT-NA composition disclosed herein). As used herein, the terms "catalyst article", "catalytic article", "catalyst component", "catalytic component", "article" and "component" are used interchangeably without regard to any specific catalytic activity. For example, an LT-NA article may be referred to as a catalytic article, however, without wishing to be bound by any particular theory of operation, it should be recognized that such an article has an adsorption function rather than a catalytic function. Similarly, "composition" and "catalyst composition" are used interchangeably herein without regard to any specific catalytic activity.

[0141] In one aspect of the present disclosure, a catalyst article for treating an exhaust gas stream of an internal combustion engine is provided, the catalyst article comprising: a substrate having an inlet end and an outlet end defining an overall length; and a first washcoat disposed on at least a portion of the substrate, the first washcoat comprising a LT-NA composition as disclosed herein. In some embodiments, the catalyst article as disclosed herein further comprises a second washcoat disposed on at least a portion of the substrate in a layered or zoned configuration, the second washcoat comprising a diesel oxidation catalyst (DOC) composition.

[0142] To produce a catalytic article, a substrate is coated with a catalytic composition as disclosed herein (i.e., LT-NA and / or DOC). The coating is a "catalytic coating composition" or a "catalytic coating". The terms "catalyst composition" and "catalytic coating composition" are synonymous.

[0143] Coating composition

[0144] Coating compositions including LT-NA and / or DOC compositions as disclosed herein may use a binder such as ZrO derived from a suitable precursor such as zirconyl acetate or any other suitable zirconium precursor such as zirconyl nitrate. 2 The coating may be prepared by using a binder. Zirconium acetate binders provide a coating that remains uniform and intact after heat aging, such as when the catalyst is exposed to an elevated temperature of at least about 600°C, such as about 800°C, and a water vapor environment that is about 5% or more higher. Other potentially suitable binders include, but are not limited to, alumina and silica. Alumina binders include aluminum oxide, aluminum hydroxide, and aluminum oxyhydroxide. Colloidal forms of aluminum salts and aluminum oxide may also be used. Silica binders include various forms of SiO 2, comprising silicates and colloidal silica. The binder composition may comprise any combination of zirconium oxide, alumina and silica. Other exemplary binders include boehmite, gamma-alumina or delta / theta alumina and silica sol. When present, the binder is typically used in an amount of about 1 wt.% to 5 wt.% of the total carrier coating loading. Alternatively, the binder may be zirconium oxide-based or silica oxide-based, such as zirconium acetate, zirconium oxide sol or silica sol. When present, the alumina binder is typically used in an amount of about 0.05 g / in 3 To about 1g / in 3 .

[0145] Substrate

[0146] Useful substrates are 3-dimensional, having a length, diameter, and volume similar to a cylinder. The shape does not have to conform to a cylinder. The length is the axial length defined by the inlet and outlet ends.

[0147] According to one or more embodiments, the substrate for the disclosed composition can be composed of any material commonly used to prepare automotive catalysts, and will generally include a metal or ceramic honeycomb structure. The substrate generally provides a plurality of wall surfaces on which the washcoat composition is applied and adhered, thereby serving as a substrate for the catalyst composition.

[0148] The ceramic substrate can be made of any suitable refractory material, such as cordierite, cordierite-α-alumina, aluminum titanate, silicon titanate, silicon carbide, silicon nitride, zircon mullite, spodumene, alumina-silica-magnesia, zirconium silicate, sillimanite, magnesium silicate, zircon, petalite, α-alumina, aluminosilicate, etc.

[0149] The substrate may also be metallic, including one or more metals or metal alloys. The metal substrate may include any metal substrate, such as a metal substrate having openings or "punch-outs" in the channel wall. The metal substrate may be used in various shapes, such as pellets, corrugated sheets, or integral foams. Specific examples of metal substrates include heat-resistant base metal alloys, especially those in which iron is a basic or major component. Such alloys may contain one or more of nickel, chromium, and aluminum, and in each case, the total amount of these metals may advantageously include at least about 15 wt% (weight percent) of the alloy, such as about 10 to about 25 wt% chromium, about 1 to about 8 wt% aluminum, and about 0 to about 20 wt% nickel, based on the weight of the substrate. Examples of metal substrates include substrates having straight channels; substrates having blades protruding along the axial channel to interrupt the gas flow and open the gas flow between the channels; and substrates having blades and holes to enhance gas transport between the channels, thereby allowing radial gas transport through the monolith. Specifically, in certain embodiments, the metal substrate is advantageously used in a close-coupled position, thereby allowing rapid heating of the substrate and, correspondingly, the catalyst composition (eg, LT-CO oxidation catalyst composition) coated therein.

[0150] Any suitable substrate for the catalytic articles disclosed herein may be employed, such as a monolithic substrate of the type having thin parallel gas flow passages extending therethrough from the inlet or outlet face of the substrate such that the passages are open to the fluid flowing therethrough (a "flow-through substrate"). Another suitable substrate is of the type having a plurality of thin substantially parallel gas flow passages extending along the longitudinal axis of the substrate, wherein typically each passage is blocked at one end of the body of the substrate, while alternate passages are blocked at the opposite end face (a "wall-flow filter"). Flow-through and wall-flow substrates are also taught, for example, in International Application Publication No. WO2016 / 070090, which is incorporated herein by reference in its entirety.

[0151] In some embodiments, the catalyst substrate comprises a honeycomb substrate in the form of a wall flow filter or a flow-through substrate. In some embodiments, the substrate is a wall flow filter. Flow-through substrates and wall flow filters are discussed further below.

[0152] Flow-through substrate

[0153] In some embodiments, the substrate is a flow-through substrate (e.g., a monolithic substrate, including a flow-through honeycomb monolithic substrate). The flow-through substrate has thin parallel gas flow passages extending from the inlet end to the outlet end of the substrate, such that the channels are open to fluid flow. The channels, which are substantially straight paths from their fluid inlet to their fluid outlet, are defined by walls on which a catalytic coating is disposed, such that the gas flowing through the channels contacts the catalytic material. The flow channels of the flow-through substrate are thin-walled passages that can be of any suitable cross-sectional shape and size, such as trapezoidal, rectangular, square, sinusoidal, hexagonal, elliptical, circular, etc. As described above, the flow-through substrate can be ceramic or metallic.

[0154] For example, the volume of the flow-through substrate may be, for example, about 50 in. 3 To about 1200in 3 , the cell density (entrance opening) is from about 60 cells per square inch (cpsi) to about 500 cpsi or up to about 900 cpsi, for example about 200 to about 400 cpsi, and the wall thickness is from about 50 to about 200 microns or about 400 microns.

[0155] Figure 1A and 1B An exemplary substrate 2 in the form of a flow-through substrate coated with a LT-NA composition as described herein is shown. Figure 1A , the exemplary substrate 2 has a cylindrical shape and a cylindrical outer surface 4, an upstream end face 6 and a corresponding downstream end face 8, the downstream end face being identical to the end face 6. The substrate 2 has a plurality of thin and parallel gas flow channels 10 formed therein. Figure 1B As shown, the flow channel 10 is formed by the wall 12 and extends through the carrier 2 from the upstream end face 6 to the downstream end face 8, and the channel 10 is unobstructed, thereby allowing a fluid, such as an airflow, to flow longitudinally through the carrier 2 through its airflow channel 10. Figure 1B As can be more easily seen in the figure, the wall 12 is sized and configured so that the airflow channel 10 has a substantially regular polygonal shape. As shown, if desired, the LT-NA composition can be applied in multiple different layers. In the illustrated embodiment, the LT-NA composition is composed of a discrete bottom layer 14 adhered to the wall 12 of the carrier member and a second discrete top layer 16 applied over the bottom layer 14. The present invention can be implemented with one or more (e.g., two, three, or four or more) layers of the LT-NA composition and is not limited to Figure 1B The two-layer embodiment shown in FIG. Additional coating configurations are disclosed below.

[0156] Wall Flow Filter Substrates

[0157] In some embodiments, the substrate is a wall flow filter, which typically has a plurality of thin, substantially parallel airflow channels extending along the longitudinal axis of the substrate. Typically, each channel is blocked at one end of the substrate body, and alternating channels are blocked at the opposite end face. Such monolithic wall flow filter substrates may contain up to about 900 or more flow channels (or "cells") per square inch of cross section, but a much smaller number may be used. For example, the substrate may have about 7 to 600 cells per square inch, more typically about 100 to 400 cells per square inch ("cpsi"). The cross section of the cells may have a cross section that is rectangular, square, circular, elliptical, triangular, hexagonal, or other polygonal shapes.

[0158] Figure 2 is a perspective view of an exemplary wall flow filter. Figure 2 , a cross-sectional view of a portion of an integral wall-flow filter substrate is shown showing alternating blocked and open channels (cells). Blocked or plugged ends 100 alternate with open channels 101, with each opposite end being open and closed, respectively. The filter has an inlet end 102 and an outlet end 103. Arrows through the porous cell walls 104 indicate exhaust gas flow entering the open cell end, diffusing through the porous cell walls 104 and exiting the open outlet cell end. The blocked ends 100 impede gas flow and promote diffusion through the cell walls. Each cell wall has an inlet side 104a and an outlet side 104b. The channels are surrounded by cell walls.

[0159] The volume of the wall flow filter article substrate may be, for example, about 50 cm 3 , about 100cm 3 , about 200cm 3 、About 300cm 3 、Approx. 400cm 3 、About 500cm 3 、About 600cm 3 、About 700cm 3 、About 800cm 3 、About 900cm 3 or about 1000cm 3 To approximately 1,500cm 3 , about 2000cm 3 、About 2500cm 3 、About 3000cm 3 、About 3500cm 3 、About 4000cm 3 、About 4500cm 3 or about 5000cm 3The wall thickness of the wall flow filter substrate is typically from about 50 microns to about 2000 microns, such as from about 50 microns to about 450 microns or from about 150 microns to about 400 microns.

[0160] The walls of the wall flow filter are porous and the wall porosity is generally at least about 50% or at least about 60% before the functional coating is placed, with an average pore size of at least about 5 microns. For example, the wall flow filter article substrate will have a porosity of ≥50%, ≥60%, ≥65% or ≥70% in some embodiments. For example, before the catalytic coating is placed, the wall flow filter article substrate has a wall porosity of about 50%, about 60%, about 65% or about 70% to about 75%, about 80% or about 85%, and an average pore size of about 5 microns, about 10 microns, about 20 microns, about 30 microns, about 40 microns or about 50 microns to about 60 microns, about 70 microns, about 80 microns, about 90 microns or about 100 microns. The terms "wall porosity" and "substrate porosity" mean the same thing and are interchangeable. Porosity is the ratio of the void volume divided by the total volume of the substrate. The pore size can be determined according to the ISO 15901-2 (static volume) procedure for nitrogen pore size analysis. The nitrogen pore size can be measured on a Micromeritics TRISTAR 3000 series instrument. The nitrogen pore size can be determined using a BJH (Barrett-Joyner-Halenda) calculation and 33 desorption points. Useful wall flow filters have a high porosity, thereby allowing a high loading of the catalyst composition during operation without generating excessive back pressure.

[0161] coating

[0162] A substrate is coated with a LT-NA and / or DOC composition as disclosed herein to form an article. The coating may include one or more thin adherent coatings disposed on at least a portion of the substrate and adhered thereto. In a certain embodiment, the article of the present invention may comprise the use of one or more layers and a combination of one or more layers. The coating composition may be present only on the inlet side of the substrate wall, only on the outlet side, on both the inlet side and the outlet side, or the wall itself may be composed entirely or in part of the coating composition. The coating may be located on the surface of the substrate wall and / or in the pores of the substrate wall, that is, "in" and / or "on" the substrate wall. Therefore, the phrase "catalytic coating disposed on a substrate" refers to any surface, such as on the wall surface and / or on the pore surface. The coating may include separate functional components, that is, a LT-NA composition and / or a DOC catalyst composition, each as described herein.

[0163] The catalyst composition can be applied generally in the form of a carrier coating containing a carrier material having catalytically active species thereon. In certain embodiments, the catalyst assembly can also be combined in a single carrier coating. The carrier coating is formed by preparing a slurry of a carrier containing a specified solid content (e.g., about 10 to about 60% by weight) in a liquid vehicle, then applying the slurry to a substrate and drying and calcining to provide a coating. If multiple coatings are applied, the substrate is dried and calcined after applying each layer and / or applying a large number of desired layers. In one or more embodiments, the catalytic material is applied to the substrate as a carrier coating. A binder can also be used as described above.

[0164] For the purpose of coating a catalyst substrate such as a honeycomb substrate, the above-mentioned catalyst composition is usually mixed independently with water to form a slurry. In addition to the catalyst particles, the slurry may optionally contain a binder (e.g., alumina, silica), a water-soluble or water-dispersible stabilizer, a promoter, an associative thickener and / or a surfactant (comprising anionic, cationic, nonionic or amphoteric surfactants). The typical pH range of the slurry is from about 3 to about 6. Acidic or alkaline species can be added to the slurry to adjust the pH accordingly. For example, in some embodiments, the pH of the slurry is adjusted by adding ammonium hydroxide or an aqueous nitric acid solution.

[0165] The slurry can be ground to enhance the mixing of particles and the formation of a homogeneous material. The grinding can be done in a ball mill, a continuous mill or other similar equipment, and the solid content of the slurry can be, for example, about 20-60 wt.%, more specifically about 20-40 wt.%. In one embodiment, the slurry after grinding is characterized by a D90 particle size of about 10 to about 40 microns, preferably about 10 to about 30 microns, and more preferably about 10 to about 15 microns.

[0166] The slurry is then coated on the catalyst substrate using any washcoat technique known in the art. In one embodiment, the catalyst substrate is dipped in the slurry one or more times or otherwise coated with the slurry. Thereafter, the coated substrate is dried at an elevated temperature (e.g., 100-150° C.) for a period of time (e.g., 10 minutes-3 hours), and then calcined by heating, for example, at 400-600° C., typically for about 10 minutes to about 3 hours. After drying and calcining, the final washcoat coating can be considered to be substantially free of solvent.

[0167] After calcination, the catalyst loading obtained by the above washcoat technique can be determined by calculating the difference between the coated and uncoated weights of the substrate. As will be apparent to one skilled in the art, the catalyst loading can be modified by altering the slurry rheology. In addition, the coating / drying / calcining process to produce the washcoat can be repeated as needed to build up the coating to the desired loading level or thickness, meaning that more than one washcoat may be applied.

[0168] The washcoat may be applied so that the various coating layers are in direct contact with the substrate. Alternatively, there may be one or more "undercoats" so that at least a portion of the catalytic or adsorbent coating layer or layers is not in direct contact with the substrate (but is in contact with the undercoat). There may also be one or more "overcoats" so that at least a portion of the coating layer or layers is not directly exposed to the gas stream or atmosphere (but is in contact with the overcoat).

[0169] Different coatings may be in direct contact with each other without an "intermediate" overlapping area. Alternatively, different coatings may not be in direct contact with a "gap" between two areas. In the case of a "primer" or "topcoat", the gap between different layers is called an "intermediate layer". A primer is a layer "below" a coating, a topcoat is a layer "above" a coating, and an intermediate layer is a layer between two coatings. Intermediate layers, primers, and topcoats may contain one or more functional compositions or may not contain a functional composition.

[0170] The catalytic coating can include more than one thin adhesion layer, which adheres to each other and the coating adheres to the substrate. The entire coating includes a separate "coating". The catalytic coating can be advantageously "partitioned", which includes a partitioned catalytic layer. This can also be described as "lateral partitioning". For example, a layer can extend from the inlet end to the outlet end, extending about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80% or about 90% of the length of the substrate. Another layer can extend from the outlet end to the inlet end, extending about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80% or about 90% of the length of the substrate. Different coatings can be adjacent to each other and do not cover each other. Alternatively, different layers can cover a portion of each other, thereby providing a third "middle" zone. The intermediate region may extend, for example, from about 5% to about 80% of the substrate length, such as about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60% or about 70% of the substrate length.

[0171] The different layers may each extend the entire length of the substrate, or may each extend a portion of the length of the substrate, and may partially or completely overlie or underlie each other. Each different layer may extend from the inlet end or the outlet end.

[0172] Different catalytic compositions may be present in each individual coating. For example, one coating may include a LT-NA composition as disclosed herein, and another coating may include a DOC composition as disclosed herein. Alternatively, in some embodiments, each LT-NA composition and DOC composition as disclosed herein may be combined and applied to the substrate as a single homogeneous layer. In other embodiments, the LT-NA composition may be present in one layer, and the DOC composition component may be divided into one or more additional layers.

[0173] Thus, discussion about different layers may correspond to any of these layers. The catalytic coating may include one, two, or three or more coatings. The one or more coatings together include the catalytic composition.

[0174] The zones of the present disclosure are defined by the relationship of the coatings. There are many possible zoning configurations for different coatings. For example, there can be upstream and downstream zones, there can be upstream, middle and downstream zones, there can be four different zones, etc. In the case where two layers are adjacent and do not overlap, there are upstream and downstream zones. In the case where the two layers overlap to a certain extent, there are upstream, downstream and middle zones. For example, in the case where the coating extends the entire length of the substrate and the different coating extends a certain length from the outlet end and covers a portion of the first coating, there are upstream and downstream zones. The catalytic coating of the present invention may include more than one identical layer.

[0175] In some embodiments, the first washcoat is disposed directly on the substrate and the second washcoat is disposed on at least a portion of the first washcoat. In some embodiments, the second washcoat is disposed directly on the substrate and the first washcoat is disposed on at least a portion of the second washcoat. In some embodiments, the first washcoat composition and the second washcoat composition are combined and disposed on the substrate in a single homogenous layer. In some embodiments, the catalyst article has a zoned configuration wherein the first washcoat is disposed on the catalyst substrate from the inlet end to a length of about 10% to about 70% of the total length; and wherein the second washcoat is disposed on the catalyst substrate from the outlet end to a length of about 30% to about 90% of the total length.

[0176] Figure 3A , 3B 3C show some possible coating configurations with two coatings. A monolithic wall flow filter substrate wall 200 is shown with coatings 201 and 202 disposed thereon. This is a simplified illustration, in the case of a porous wall flow substrate, the pores and coatings adhered to the pore walls are not shown, and the plugged ends are not shown. Figure 3AIn the embodiment, coating 201 extends about 50% of the length of the substrate from inlet to outlet; and coating 202 extends about 50% of the length of the substrate from outlet to inlet, and the coatings are adjacent to each other, thereby providing an inlet upstream region 203 and an outlet downstream region 204. Figure 3B In , coating 202 extends about 50% of the length of the substrate from the outlet, and layer 201 extends more than 50% of the length from the inlet and covers a portion of layer 202, thereby providing an upstream zone 203, an intermediate zone 205, and a downstream zone 204. Figure 3C , coatings 201 and 202 each extend the entire length of the substrate, with layer 201 covering layer 202. Figure 3C The substrate does not contain a zone coating configuration. Figure 3A , 3B and 3C can be used to demonstrate coating compositions on wall-flow substrates. Figure 3A , 3B and 3C can further be used to illustrate coating compositions on flow-through substrates, as described herein below. The configuration of such coatings is not limited.

[0177] In some embodiments, the DOC composition is in a partitioned configuration relative to the LT-NA composition layer. In some embodiments, the DOC composition may overlap with one or more layers of the LT-NA composition. In some embodiments, the LT-NA catalyst composition and the DOC composition are present on a substrate as a single homogeneous layer. In some embodiments, the LT-NA catalyst composition and the DOC composition are present as separate, discrete layers. In some embodiments, the LT-NA catalyst composition and the DOC composition are present in a partitioned configuration. In some embodiments, other catalytic compositions may be incorporated above, below, or between any LT-NA and DOC catalyst composition layers mentioned herein.

[0178] The loading of the catalytic coating (e.g., LT-NA and / or DOC) of the present invention on the substrate will depend on the properties of the substrate, such as porosity and wall thickness. Typically, the catalyst loading of a wall flow filter will be lower than the catalyst loading on a flow-through substrate. Catalytic wall flow filters are disclosed, for example, in U.S. Pat. No. 7,229,597, which is incorporated herein by reference in its entirety. The LT-NA and / or DOC catalyst composition of the present invention is typically present on the substrate at a concentration, for example, about 0.3 to 5.5 g / in 3 or about 0.4g / in 3 , about 0.5g / in 3 , about 0.6g / in 3 , about 0.7g / in 3 , about 0.8g / in 3 , about 0.9g / in3 or about 1.0g / in 3 To about 1.5g / in 3 , about 2.0g / in 3 , about 2.5g / in 3 , about 3.0g / in 3 , about 3.5g / in 3 , about 4.0g / in 3 , about 4.5g / in 3 , about 5.0g / in 3 or about 5.5g / in 3 The concentration of the catalyst composition or any other component on the substrate refers to the concentration per any one three-dimensional segment or zone, such as any cross-section of the substrate or the entire substrate.

[0179] In some embodiments, the catalytic article comprises a loading of about 15 g / ft 3 To about 200g / ft 3 or about 60g / ft 3 To about 120g / ft 3 In some embodiments, the LT-NA article comprises about 1 g / in 3 To about 5g / in 3 or about 2g / in 3 To about 3g / in 3 In some embodiments, the catalytic article comprises a silica to alumina ratio (SAR) of about 5 to about 50 or about 10 to about 35.

[0180] In some embodiments, the catalyst articles disclosed herein exhibit enhanced oxidation of carbon monoxide (CO), hydrocarbons (HC), or both after the catalyst article is hydrothermally aged at 750° C. for a period of 80 hours, relative to oxidation of carbon monoxide (CO), hydrocarbons (HC), or both prior to hydrothermal aging.

[0181] In some embodiments, the enhanced oxidation of CO or HC is measured from the perspective of conversion efficiency. In some embodiments, the conversion efficiency is measured as a function of the light-off temperature (i.e., T 50 The light-off temperature is measured as a function of the measured light-off temperature. The light-off temperature is the temperature at which the catalyst composition is able to convert 50% of the hydrocarbons into carbon dioxide and water. Generally, for any given catalyst composition, the lower the measured light-off temperature, the more efficient the catalyst composition is in catalyzing a reaction such as hydrocarbon conversion. In some embodiments, the conversion efficiency is measured as the conversion of hydrocarbons into CO2 at a specified temperature or within a temperature range. 2 Measured as a function of percentage.

[0182] Exhaust gas treatment system

[0183] The present disclosure further provides a method for reducing NO in an exhaust gas stream from an internal combustion engine. x A horizontal exhaust gas treatment system comprising a catalytic article as disclosed herein. In another aspect of the present invention, there is provided a method for reducing NO in an exhaust gas stream from an internal combustion engine. x A method for producing a gaseous exhaust gas stream in a horizontal direction, the method comprising contacting the exhaust gas stream with a catalytic product as disclosed herein or an emission treatment system as disclosed herein. Therefore, the present invention provides an emission treatment system incorporating a catalytic product as described herein, such as an emission treatment system that generally includes an engine that produces an exhaust gas stream and one or more catalytic products positioned downstream of the engine and in fluid communication with the exhaust gas stream. The engine can be, for example, a diesel engine that operates under combustion conditions where the air exceeds the air required for stoichiometric combustion, i.e., under lean burn conditions. In other embodiments, the engine can be an engine associated with a fixed source (e.g., a generator or a pump station). In some embodiments, the emission treatment system further includes one or more additional catalytic components. The relative positions of the various catalytic components present in the emission treatment system can vary.

[0184] In the exhaust gas treatment systems and methods of the present invention, the exhaust gas flow is contained to the article or treatment system by entering the upstream end and exiting the downstream end. The inlet end of the substrate or article is synonymous with the "upstream" end or "front" end. The outlet end is synonymous with the "downstream" end or "rear" end. The treatment system is typically located downstream of the internal combustion engine and in fluid communication with the internal combustion engine.

[0185] The systems disclosed herein include LT-NA articles, which may include flow-through or wall-flow filter substrates as disclosed herein. Specifically, the systems include a filter substrate suitable for adsorbing NO at low temperatures. x and releases the captured NO at elevated temperatures x The LT-NA catalyst product of the present invention has a NO x The adsorbent component provides desirable NO under various engine operating conditions. x Adsorption and desorption properties.

[0186] Preferably, the LT-NA catalyst article is capable of absorbing NO present in the exhaust gas stream. x More importantly, however, the LT-NA catalyst article does not release NO until the exhaust gas stream and / or the exhaust gas emission system has reached a temperature high enough for other catalytic components to be active. x species. Only then, the released NO x can be effectively converted into N 2, and leaves the exhaust gas treatment system. Therefore, the LT-NA catalyst article is usually positioned to react with NO released from the LT-NA. x In some embodiments, the LT-NA catalyst article adsorbs NO present in the exhaust gas stream at low temperatures. x Species, which may have optionally been treated with at least a DOC and / or a CSF component.

[0187] In some embodiments, the LT-NA catalyst article is not located in a separate component (e.g., on a separate substrate), but can be included in the same component such as a diesel oxidation catalyst (DOC), a catalyzed soot filter (CSF), or a catalyzed selective reduction (SCR) catalyst component, wherein the catalytic composition for such components is applied to the substrate in a zoned or layered configuration. In some embodiments, the LT-NA and (DOC) are combined in a single catalyst article.

[0188] In addition to the LT-NA catalyst article, the system of the present disclosure may contain, for example, a DOC, a reductant injector, an SCR catalyst assembly, a soot filter (which may be catalyzed or uncatalyzed), and / or an ammonia oxidation catalyst (AMOx). A suitable DOC for an emission treatment system can effectively catalyze the oxidation of CO and HC to carbon dioxide (CO 2 ). Preferably, the DOC is capable of converting at least 50% of the CO or HC components present in the exhaust gas. The DOC may be positioned, for example, downstream of the LT-NA catalyst article. In some embodiments, the DOC is positioned upstream of the SCR catalyst assembly and / or the soot filter.

[0189] The exhaust gas treatment system of the present disclosure may further include an SCR catalyst assembly. The SCR catalyst assembly may be located upstream or downstream of the DOC and / or the soot filter. A suitable SCR catalyst assembly for use in an exhaust treatment system is capable of effectively catalytically reducing NO at temperatures up to 650°C. x In addition, the SCR catalyst assembly must be able to reduce NO even at low load conditions, which are typically associated with lower exhaust temperatures. x Preferably, the SCR catalyst assembly is capable of converting at least 50% of the NO x (e.g., NO) components are converted to N 2 Another desirable attribute of an SCR catalyst assembly is that it has the ability to catalyze O 2 With any excess NH 3 The reaction forms N 2 The ability of NH 3No emissions are released into the atmosphere. Useful SCR catalyst assemblies for use in emission treatment systems should also have heat resistance to withstand temperatures above 650°C. Such high temperatures may be encountered during the regeneration process of a catalyzed soot filter. Suitable SCR catalyst assemblies are described, for example, in U.S. Pat. Nos. 4,961,917 and 5,516,497, each of which is incorporated herein by reference in its entirety.

[0190] In some embodiments, the exhaust gas treatment system further includes one or more of a lean NOx trap (LNT), a selective catalytic reduction (SCR) catalyst, an ammonia or ammonia precursor injection assembly, a catalyzed soot filter (CSF), or an ammonia oxidation (AMOx) catalyst.

[0191] Certain exemplary exhaust gas treatment systems may be referenced by reference to Figure 4 For easier understanding, the figure depicts a schematic representation of a non-limiting exhaust gas treatment system 20 according to an embodiment of the present disclosure. Those skilled in the art will recognize that it may be desirable to arrange the relative position of each article in an order different from the order shown herein; the present disclosure contemplates such alternative orderings. As shown, the emission treatment system 20 can include a plurality of catalyst assemblies connected in series downstream of an engine 22, such as a lean burn gasoline engine. At least one of the catalyst assemblies will be the LT-NA catalyst of the present invention as described herein. The catalyst composition of the present invention can be combined with a number of additional catalyst materials and can be placed in a different position than the additional catalyst materials. Figure 4 Five catalyst assemblies 24, 26, 28, 30, 32 are shown in series; however, the total number of catalyst assemblies may vary, and five assemblies are merely an example. Those skilled in the art will recognize that it may be desirable to arrange the relative positions of each article in an order different from that shown herein; the present disclosure contemplates such alternative orderings.

[0192] Without limitation, Table 1 shows various exhaust gas treatment system configurations for one or more embodiments. Note that each catalyst is connected to the next catalyst by an exhaust conduit such that the engine is upstream of catalyst A, catalyst A is upstream of catalyst B, catalyst B is upstream of catalyst C, catalyst C is upstream of catalyst D, and catalyst D is upstream of catalyst E (when present). References to components AE in the table may be the same as Figure 4 Cross-references with the same name in .

[0193] References to SCR in the table refer to an SCR catalyst; any suitable SCR catalyst known in the art may be used.

[0194] References to AMOx in the table refer to an ammonia oxidation catalyst that may be disposed downstream of the catalyst of one or more embodiments of the present invention to remove any ammonia slip from the exhaust gas treatment system. In certain embodiments, the AMOx catalyst may include a PGM component. In one or more embodiments, the AMOx catalyst may include an undercoat layer having a PGM and a topcoat layer having SCR functionality.

[0195] As will be appreciated by those skilled in the art, in the configurations listed in Table 1, any one or more of assemblies A, B, C, D, or E may be disposed on a particulate filter such as a wall-flow filter, or disposed on a flow-through honeycomb substrate. In one or more embodiments, the engine exhaust system includes one or more catalyst assemblies mounted in a position near the engine (in a close coupled position, CC) and an additional catalyst assembly mounted in a position below the vehicle body (in an underfloor position, UF). In one or more embodiments, the exhaust gas treatment system may further include a urea injection assembly.

[0196] Table 1: Possible exhaust gas treatment system configurations

[0197] Component A Component B Component C Component D Component E DOC LT-NA CSF SCR Optional AMOx- LT-NA DOC CSF SCR Optional AMOx DOC LT-NA SCR CSF Optional AMOx LT-NA DOC SCR CSF Optional AMOx LT-NA / DOC CSF SCR Optional AMOx - LT-NA / DOC SCRoF Optional AMOx - - LT-NA / DOC LNT SCR Optional AMOx DOC LT-NA / DOC SCR Optional AMOx - DOC LT-NA / DOC LNT SCR Optional AMOx

[0198] Figure 4 Any of the exemplary exhaust gas treatment systems depicted may be followed by a selective ammonia oxidation catalyst (AMOx) to remove NH 2 released from the SCR catalyst assembly. 3 and selectively oxidizes it to N 2 .

[0199] Method for treating exhaust gas stream

[0200] Aspects of the present disclosure are directed to a method for treating a lean burn engine exhaust gas stream comprising contacting the exhaust gas stream with a catalytic article of the present disclosure or an emission treatment system of the present disclosure.

[0201] In some embodiments, the method includes continuously contacting the exhaust gas stream with the LT-NA catalyst article, the exhaust gas stream having an initial temperature of about 150° C. or less and the exhaust gas stream gradually increasing in temperature during further engine operation; adsorbing and storing the NO from the exhaust gas stream. x , until the exhaust gas stream reaches a predetermined temperature, wherein the NO xreleasing into the exhaust gas stream exiting the LT-NA article; and continuously contacting the exhaust gas stream exiting the LT-NA article with at least one downstream catalytic material to remove NO as the exhaust gas stream temperature increases and heating each such downstream catalytic material to an operating temperature between about 200° C. and about 450° C. x Component.

[0202] Method for adjusting the NOx adsorption / desorption curve of LT-NA

[0203] In another aspect, a method for regulating NO in a LT-NA composition is provided. x Adsorption / desorption curves and NO of LT-NA compositions x The method comprises a method of one or both of the desorption temperature ranges, the LT-NA composition comprising a zeolite, the zeolite comprising a first metal component and a second metal component, wherein the first metal component comprises palladium, and the second metal component is selected from the group consisting of an alkaline earth metal component, an oxide of an alkaline earth metal component, a rare earth metal component, an oxide of a rare earth metal component, and combinations thereof, the method comprising selecting the second metal component and its loading. In some embodiments, NO x The desorption temperature ranges from about 150°C, about 175°C, about 200°C, about 225°C, or about 250°C to about 275°C, about 300°C, about 325°C, about 350°C, or about 400°C.

[0204] The articles, systems and methods of the present invention are suitable for treating exhaust gas streams from mobile emission sources such as trucks and cars. The articles, systems and methods of the present invention are also suitable for treating exhaust gas streams from stationary sources such as power plants.

[0205] It will be apparent to those of ordinary skill in the relevant art that the compositions, methods and applications described herein may be appropriately modified and adapted without departing from the scope of any embodiment or aspect thereof. The compositions and methods provided are exemplary and are not intended to limit the scope of the claimed embodiments. All various embodiments, aspects and options disclosed herein may be combined in all variations. The scope of the compositions, formulations, methods and processes described herein includes all actual or potential combinations of the embodiments, aspects, options, examples and preferences herein. All patents and publications cited herein are incorporated herein by reference for their specific teachings as mentioned, unless other specific incorporation statements are specifically provided.

[0206] Examples

[0207] The present invention is more fully described by the following examples, which are set forth for the purpose of illustrating the present invention and should not be construed as limiting the present invention. Unless otherwise indicated, all parts and percentages are by weight, and unless otherwise indicated, all weight percentages are expressed by dry weight, meaning that water content is not included.

[0208] Preparation of monolithic catalyst products

[0209] Example 1 (reference product)

[0210] The ferrierite zeolite material (FER) was treated with diluted Pd(NO 3 ) 2 Solution incipient wetness impregnation followed by drying at 110°C / 2 hours in air followed by calcination at 550°C for 1 hour in air. A diluted zirconium acetate solution was prepared to which the calcined Pd / FER powder was added to form a slurry suspension with a solid content of approximately 50%. The slurry was milled until a final particle size D90 of 10-12 μm was achieved. The slurry was then coated onto a 400 / 4 honeycomb substrate at a solid content of 42-46%. After drying, the catalyst was calcined at 590°C for 1 hour in air. Pd loading was 80 g / ft 3 , zeolite carrier coating loading is 2.5g / in 3 , the generated ZrO 2 The loading was about 5% of the washcoat composition after calcination.

[0211] Example 2

[0212] The ferrierite zeolite material (FER) was treated with Ba(OAc) 2 The solution was impregnated with incipient wetness, followed by drying (110°C / 2 hours) and calcination (590°C / 4 hours) in air. The Ba weight percentage varied in the range of 0.45-1.5%. The resulting Ba-FER material was treated with Pd(NO 3 ) 2 The solution was further impregnated and then dried at 110°C / 2 hours in air and subsequently calcined at 550°C for 1 hour in air. A diluted zirconium acetate solution was prepared to which the calcined Pd / BEA powder was added to form a slurry suspension with a solid content of approximately 50%. The slurry was milled until the final particle size D90 reached 10-12 μm. The slurry was then coated onto a 400 / 4 honeycomb substrate at a solid content of 42-46%. After drying, the catalyst was calcined at 590°C in air for 1 hour. The Pd loading was 80 g / ft 3 , zeolite carrier coating loading is 2.5g / in 3 .

[0213] Example 3

[0214] The ferrierite zeolite material (FER) was treated with Sr(OAc) 2 The solution was incipiently wet impregnated, followed by drying (110°C / 2 hours) and calcination (590°C / 4 hours) in air. The weight percentage of Sr based on FER was about 1%. The resulting Sr-FER material was treated with Pd(NO 3 ) 2 The solution was further impregnated and then dried at 110°C / 2 hours in air and subsequently calcined at 550°C for 1 hour in air. A diluted zirconium acetate solution was prepared to which the calcined Pd / BEA powder was added to form a slurry suspension with a solid content of approximately 50%. The slurry was milled until the final particle size D90 reached 10-12 μm. The slurry was then coated onto a 400 / 4 honeycomb substrate at a solid content of 42-46%. After drying, the catalyst was calcined at 590°C in air for 1 hour. The Pd loading was 80 g / ft 3 , zeolite carrier coating loading is 2.5g / in 3 .

[0215] Example 4

[0216] The ferrierite zeolite material (FER) was treated with La(NO 3 ) 3 The solution was incipiently wet impregnated, followed by drying (110°C / 2 hours) and calcination (590°C / 4 hours) in air. The La weight percentage based on FER was about 1.3%. The resulting La-FER material was treated with Pd(NO 3 ) 2 The solution was further impregnated and then dried at 110°C / 2 hours in air and subsequently calcined at 550°C for 1 hour in air. A diluted zirconium acetate solution was prepared to which the calcined Pd / BEA powder was added to form a slurry suspension with a solid content of approximately 50%. The slurry was milled until the final particle size D90 reached 10-12 μm. The slurry was then coated onto a 400 / 4 honeycomb substrate at a solid content of 42-46%. After drying, the catalyst was calcined at 590°C in air for 1 hour. The Pd loading was 80 g / ft 3 , zeolite carrier coating loading is 2.5g / in 3 .

[0217] Example 5 (LT-NA / DOC, reference)

[0218] The LT-NA bottom layer was prepared similarly to Example 1. For the DOC top layer, 5% SiO 2 -Al 2 O 3The material was incipiently wet impregnated with a diluted Pt amine complex solution and then added to a diluted palladium nitrate solution to form a slurry suspension. 3 The pH of the slurry suspension was adjusted to 4-5. The slurry was ground to D90 = 12-15 μm, and then beta zeolite and alumina binder material (3.5% of total carrier coating solids) were added. The slurry was then coated onto the LT-NA substrate at 25-30% solids content. After drying, the sample was calcined at 590°C in air for 1 hour. The Si-alumina loading was 0.75 g / in 3 , zeolite beta loading is 0.35 g / in 3 , PGM loading is 36g / ft 3 , and the Pt / Pd weight ratio is 1 / 2.

[0219] Example 6 (LT-NA / DOC with Ba)

[0220] The LT-NA bottom layer was prepared similarly to Example 2. The DOC layer was prepared similarly to Example 5.

[0221] Example 7 (LT-NA / DOC with Si)

[0222] The LT-NA bottom layer was prepared similarly to Example 3. The DOC layer was prepared similarly to Example 5.

[0223] Example 8 (LT-NA / DOC with La)

[0224] The LT-NA bottom layer was prepared similarly to Example 4. The DOC layer was prepared similarly to Example 5.

[0225] Example 9: Evaluation of Monolithic Catalyst Products

[0226] Both steady-state and transient tests were performed on the monolithic catalyst preparation on a diesel vehicle simulator. The gas mixture in the steady-state test consisted of a balance of N 2 100ppm NO, 250ppm C 2 H 4 , 500ppm CO, 5% H 2 O, 10% O 2 , 5% CO 2 The catalyst size was 1 x 1 x 3", and the space velocity was kept constant at 30,000 h. -1 First, the catalyst was placed in O 2 / H 2 O / CO 2 / N 2 The mixture was treated at 500°C / 5 min, and then the whole mixture was subjected to adsorption at 100°C for 10 min; the whole mixture was subjected to adsorption at O ​​with a ramp rate of 20°C / min. 2 / H2 O / CO 2 / N 2 Desorption was performed in the mixture from 100° C. to 500° C. Three adsorption-desorption tests were performed for each preparation.

[0227] For the FTP test, the feed composition was derived from a diesel engine and only NO was used for the inlet NO x Each catalyst was fed in 10% O 2 / 5% H 2 O / 5% CO 2 / N 2 The samples were pretreated in situ at 550 °C for 5 min and then subjected to three consecutive FTP cycles. x The adsorption efficiency is defined as the amount of NO adsorbed from the start to the point when the inlet temperature first reaches 200 °C. x percentage.

[0228] The adsorption-desorption curves of Examples 1-4 after hydrothermal aging (750°C / 80 hours) are Figure 5 Example 2 (+Ba) and Example 3 (+Sr) show similar NO x During desorption, Examples 2 and 3 converted the initial NO x The desorption shifts to higher temperatures and the second desorption peak at about 1400 seconds (365°C) becomes higher in intensity. Without wishing to be bound by theory, these observations suggest that Ba and Sr do not significantly affect NO x adsorption, but will convert NO x The desorption shifted to a higher temperature range. Example 4 (+La) shows that it adsorbs NO without significantly changing the desorption temperature. x Capacity and desorption of NO x Both capabilities are higher than those of Reference Example 1.

[0229] The desorbed NO of slightly aged (800°C / 2 hours, calcined in air) and hydrothermally aged (750°C / 80 hours) Examples 1-4 were analyzed in three consecutive cycles. x Compare the quantity ( Figure 6 ). Example 4 shows that after slight aging and ageing, NO x Without wishing to be bound by theory, this observation suggests that La increases the number of Pd ion exchange sites and retains these sites during aging.

[0230] Figure 7 The data show that Ba concentrations in the range of 0.5-1.5% do not affect NO xadsorption, and increasing Ba concentration makes NO x The desorption gradually shifts to higher temperatures.

[0231] NO during FTP cold start for aged LT-NA only catalysts (Examples 1-4) and LT-NA / DOC combination catalysts (Examples 5-8) x Adsorption efficiency is provided in Figure 8 In both cases, the addition of alkaline earth elements (Ba, Sr) or rare earth elements (La) confirmed the enhanced NO x Adsorption Activity. Without wishing to be bound by theory, it is believed that the addition of alkaline earth elements or rare earth elements better retains the Pd ion exchange sites after extended hydrothermal aging.

[0232] Effect of the second metal additive in LT-NA / DOC catalyst on THC conversion in FTP cycle Fig. 9 The fresh catalyst showed the same THC conversion. After aging, the catalysts of Examples 6-8 showed improved THC conversion efficiency in FTP.

[0233] Comparison of CO-DRIFTS spectra of lightly aged and aged Example 4 to Reference Example 1 is provided at Fig.10 In both cases, a higher Pd signal was detected in Example 4, and the ion exchange Pd 2+ and single Pd(0) atoms, which indicates that the addition of La promotes a higher dispersion of Pd in ​​the zeolite.

Claims

1. A low temperature NO x An adsorbent composition comprising a zeolite having at least a first metal component and a second metal component contained therein, wherein the first metal component comprises palladium, and wherein the second metal component is selected from the group consisting of an oxide of an alkaline earth metal component, an oxide of a rare earth metal component, and combinations thereof, wherein the zeolite is ferrierite.

2. The low temperature NOx adsorbent composition of claim 1, wherein the second metal component is an oxide of an alkaline earth metal component.

3. Low temperature NO according to claim 2 x The adsorbent composition wherein the alkaline earth metal component comprises: magnesium, calcium, strontium, barium; Oxides of magnesium, calcium, strontium, and barium; or a combination thereof.

4. Low temperature NO according to claim 1 x The sorbent composition wherein the second metal component is an oxide of a rare earth metal component.

5. Low temperature NO according to claim 4 x The adsorbent composition, wherein the rare earth metal component comprises: Ce, La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu; oxides of Ce, La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb or Lu; or combinations thereof.

6. Low temperature NO according to any one of claims 1 to 5 x An adsorbent composition wherein at least a portion of the palladium is ion-exchanged within the zeolite.

7. The low temperature NO according to any one of claims 1 to 6. x The adsorbent composition wherein the palladium is present in an amount of about 0.01 wt% to about 10 wt% based on the weight of the zeolite and calculated as elemental palladium.

8. Low temperature NO according to any one of claims 1 to 7. x The sorbent composition wherein the weight ratio of the second metal component to the first metal component, calculated as the metal of the second metal component, is from about 0.1 to about 2.

9. Low temperature NO according to any one of claims 1 to 8 x The adsorbent composition wherein the second metal component is present in an amount of about 0.1 wt% to about 10 wt%, based on the total weight of the zeolite and calculated as metal.

10. Low temperature NO according to any one of claims 1 to 9 x The low temperature NOx adsorbent composition adsorbs NO from an exhaust gas stream at a temperature of about 30°C to about 200°C. x components, and by NO present in the exhaust gas stream x Total amount, based on 1:1 NO x / Pd molar ratio, the NO x The amount of the components is 30-100% of the theoretical amount.

11. The low temperature NO according to claim 10 x The adsorbent composition wherein the low temperature NO x The adsorbent composition converts NO to x The components are released back into the exhaust gas stream and adsorbed onto the low temperature NO x NO on adsorbent composition x The total amount of components, the NO x The amount of the components is 50-100 wt%.

12. Low temperature NO according to any one of claims 1 to 11. x The adsorbent composition wherein the low temperature NO x The adsorbent composition has a first NO x The adsorption capacity values, and after hydrothermal aging at 750 ° C for a period of 2-80 hours, the low-temperature NO x The adsorbent composition has a second NO x adsorption capacity value; wherein the second NO x The adsorption capacity value is equal to or greater than the first NO x Adsorption capacity value.

13. The low temperature NO according to claim 12 x The adsorbent composition wherein the second NO x Adsorption capacity relative to low temperature NO containing zeolite including the first metal component and not including the second metal component x The adsorbent composition is enhanced.

14. A low temperature NOx treatment system for treating the exhaust gas stream of an internal combustion engine x Adsorbent products, the low temperature NO x Adsorbent products include: a substrate having an inlet end and an outlet end defining an overall length; as well as A first washcoat disposed on at least a portion of the substrate, the first washcoat comprising a low temperature NO according to any one of claims 1 to 13 x Adsorbent compositions.

15. The low temperature NO according to claim 14 x The adsorbent article further comprises a second washcoat disposed on at least a portion of the substrate, the second washcoat comprising a diesel oxidation catalyst composition.

16. The low temperature NO according to claim 15 x The sorbent article wherein the diesel oxidation catalyst composition comprises a platinum group metal component supported on one or more refractory metal oxide support materials.

17. The low temperature NO according to claim 16x The sorbent article wherein the platinum group metal component comprises platinum and palladium.

18. Low temperature NO according to claim 16 or 17 x The sorbent article wherein the refractory metal oxide support material is gamma alumina or alumina doped with from about 2% to about 10% SiO2.

19. Low temperature NO according to any one of claims 15 to 18. x The adsorbent article wherein the diesel oxidation catalyst composition further comprises a beta zeolite that is substantially free of any platinum group metals.

20. Low temperature NO according to any one of claims 15 to 19. x The sorbent article wherein the first washcoat and the second washcoat are present in a layered configuration wherein the first washcoat is disposed directly on the substrate and the second washcoat is disposed on at least a portion of the first washcoat.

21. Low temperature NO according to any one of claims 15 to 19. x The sorbent article wherein the first washcoat and the second washcoat are present in a layered configuration wherein the second washcoat is disposed directly on the substrate and the first washcoat is disposed on at least a portion of the second washcoat.

22. Low temperature NO according to any one of claims 15 to 19. x The sorbent article wherein the first washcoat and the second washcoat are combined and disposed on the substrate in a single homogenous layer.

23. Low temperature NO according to any one of claims 15 to 19. x The adsorbent article, the first washcoat and the second washcoat are present in a zoned configuration, wherein the first washcoat is disposed on the substrate from the inlet end to a length of about 10% to about 70% of the total length; and wherein the second washcoat is disposed on the substrate from the outlet end to a length of about 30% to about 90% of the total length.

24. Low temperature NO according to any one of claims 14 to 23. x The sorbent article wherein the substrate comprises a honeycomb substrate in the form of a wall flow filter or a flow-through substrate.

25. An exhaust gas treatment system comprising a low temperature NOx according to any one of claims 14 to 24 disposed downstream of an internal combustion engine and in fluid communication with the internal combustion engine. x Adsorbent products.

26. The exhaust gas treatment system of claim 25, further comprising one or more of a lean NOx trap, a selective catalytic reduction catalyst, an ammonia or ammonia precursor injection assembly, a catalyzed soot filter, or an ammonia oxidation catalyst.

27. A method for reducing NO in an exhaust gas stream from an internal combustion engine x A method for treating the exhaust gas stream with a low temperature NO x The sorbent article or the exhaust gas treatment system according to claim 25 or 26.

28. The method of claim 27, wherein the contacting comprises: The exhaust gas stream is mixed with the low temperature NO x The adsorbent article is continuously contacted, the exhaust gas stream having an initial temperature at or below about 150° C. and the exhaust gas stream gradually increases in temperature during further engine operation; Adsorbing and storing the NO from the exhaust gas stream x , until the exhaust gas stream reaches a predetermined temperature, wherein the NO x Release to leave the low temperature NO x in said exhaust gas stream of an adsorbent article; as well as Make the low temperature NO x The exhaust gas stream of the adsorbent article is continuously contacted with at least one downstream catalytic material to remove NO as the exhaust gas stream temperature increases and each such downstream catalytic material is heated to an operating temperature between about 200°C and about 450°C. x Component.

29. A method for regulating low temperature NO x Adsorbent composition of NO x Adsorption / desorption curves and low temperature NO x Adsorbent composition of NO x The desorption temperature range is one or two methods, the low temperature NO x The adsorbent composition comprises a zeolite comprising a first metal component and a second metal component, wherein the first metal component comprises palladium and the second metal component is selected from the group consisting of an oxide of an alkaline earth metal component, an oxide of a rare earth metal component, and combinations thereof, the method comprising selecting the second metal component and a loading thereof, wherein the zeolite is ferrierite.

30. The method of claim 29, wherein the NO x The desorption temperature ranges from about 150°C, about 175°C, about 200°C, about 225°C, or about 250°C to about 275°C, about 300°C, about 325°C, about 350°C, or about 400°C.