Film forming method and film forming device

By performing pre- and post-infrared spectroscopy measurements and data difference analysis on the substrate, the problem of poor film quality in the concave parts of plasma film formation is solved, accurate detection and quality improvement of the film state on the substrate are achieved, and the efficiency of the film formation process is improved. Control accuracy.

CN113820290BActive Publication Date: 2024-10-01TOKYO ELECTRON LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202110652858.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-06-17
Filing Date
2021-06-11
Publication Date
2024-10-01
Estimated Expiration
2041-06-11

AI Technical Summary

Technical Problem

It is difficult to detect the state of a film formed on a substrate with a pattern of recessed portions using the existing technology. Especially during the plasma film formation process, the quality of the film on the side walls and bottom of the recessed portion is likely to deteriorate, making it impossible to detect by infrared spectroscopy. The film analysis of the monitoring substrate estimates the film state of the actual substrate.

Method used

Adopt a film forming method, including a first measurement process, a film formation process and a second measurement process, measure the data difference between the substrate before film formation and after film formation through infrared spectroscopy, and extract the difference data to detect the film state on the substrate , and adjust process parameters based on the difference data to improve membrane quality.

Benefits of technology

It achieves accurate detection and quality improvement of the film formed on the pattern substrate with concave portions, ensures the uniformity and thickness distribution of the film, and improves the control accuracy of the film forming process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113820290B_ABST
    Figure CN113820290B_ABST
Patent Text Reader

Abstract

The present invention provides a film forming method and a film forming device for detecting the state of a film formed on a substrate having a pattern including a concave portion. In a first measuring process, the substrate having a pattern including a concave portion is measured by infrared spectroscopy. In the film forming process, after the first measuring process, a film is formed on the substrate. In a second measuring process, after the film forming process, the substrate is measured by infrared spectroscopy. In an extraction process, difference data between the measurement data of the first measuring process and the measurement data of the second measuring process is extracted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a film forming method and a film forming device. Background Art

[0002] Patent Document 1 discloses a technique for performing film formation by placing a film formation substrate and a monitoring substrate, analyzing a thin film formed on the monitoring substrate by infrared spectroscopy, and optimizing the film quality of the film formed on the film formation substrate based on the analysis value.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 10-56010 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] The present disclosure provides a technology for detecting a state of a film formed on a substrate having a pattern including recessed portions.

[0008] Solutions for solving problems

[0009] A film forming method according to one embodiment of the present invention includes a first measuring step, a film forming step, a second measuring step, and an extraction step. In the first measuring step, a substrate having a pattern including a concave portion formed thereon is measured by infrared spectroscopy. In the film forming step, a film is formed on the substrate after the first measuring step. In the second measuring step, the substrate is measured by infrared spectroscopy after the film forming step. In the extraction step, difference data between the measurement data of the first measuring step and the measurement data of the second measuring step is extracted.

[0010] Effects of the Invention

[0011] According to the present disclosure, it is possible to detect the state of a film formed on a substrate having a pattern including recessed portions. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a schematic cross-sectional view showing an example of a film forming apparatus according to an embodiment.

[0013] Figure 2 It is a diagram for explaining film formation using plasma according to the embodiment.

[0014] Figure 3A It is a figure explaining the analysis by TEM-EDX.

[0015] Figure 3B It is a figure explaining the analysis by TEM-EDX.

[0016] Figure 4 This is a diagram for explaining conventional FT-IR analysis.

[0017] Figure 5 It is a diagram for explaining the flow of the film forming method according to the embodiment.

[0018] Figure 6 It is a diagram for explaining difference data involved in the embodiment.

[0019] Figure 7 It is a diagram showing an example of a plasma ALD processing process according to the embodiment.

[0020] Fig. 8A It is a diagram showing an example of a substrate on which a SiN film is formed according to an embodiment.

[0021] Figure 8B This is a diagram showing an example of a silicon substrate on which a SiN film is formed according to a comparative example.

[0022] Fig. 9 This is a diagram showing an example of absorbance for each wave number of infrared light.

[0023] Fig. 10A This is a diagram showing an example of absorbance for each wave number of infrared light.

[0024] Fig. 10B This is a diagram showing an example of absorbance for each wave number of infrared light.

[0025] Fig. 10C This is a diagram showing an example of absorbance for each wave number of infrared light.

[0026] Fig.11 It is a schematic structural diagram showing another example of the film forming apparatus according to the embodiment.

[0027] Description of Reference Numerals

[0028] W: substrate; 1: chamber; 2: mounting table; 10: high-frequency power supply; 15: gas supply unit; 16: shower head; 60: control unit; 61: user interface; 62: storage unit; 80a: window; 80b: window; 81: irradiation unit; 82: detection unit; 90: pattern; 90a: recess; 91: SiN film; 95: silicon substrate; 96: SiN film; 100: film forming device; 200: film forming device; 201~204: chamber. DETAILED DESCRIPTION

[0029] Hereinafter, embodiments of the film forming method and the film forming apparatus disclosed in the present application will be described in detail with reference to the accompanying drawings. In addition, the disclosed film forming method and the film forming apparatus are not limited by the present embodiments.

[0030] In the manufacture of semiconductor devices, a film is formed on a substrate such as a semiconductor wafer on which a pattern including a concave portion is formed by a film forming device. The film forming device places the substrate in a chamber (processing container) set to a predetermined vacuum degree, supplies a film forming raw material gas into the chamber, and generates plasma in the chamber to form a film on the substrate. As film forming techniques, for example, plasma CVD (Chemical Vapor Deposition) and plasma ALD (Atomic Layer Deposition) are known.

[0031] In addition, as the pattern formed on the substrate becomes increasingly fine, the film quality of the sidewalls and bottoms of the concave parts included in the pattern is likely to deteriorate during film formation using plasma. Therefore, in addition to the actual substrate used to manufacture semiconductor devices, a film is formed on a flat monitoring substrate, and the film formed on the monitoring substrate is analyzed by infrared spectroscopy, and the state of the film formed on the actual substrate is inferred.

[0032] However, the states of the films formed on the actual substrate and the monitoring substrate are different, and even if the film formed on the monitoring substrate is analyzed by infrared spectroscopy, the state of the film formed on the actual substrate cannot be obtained.

[0033] Therefore, a technology for detecting the state of a film formed on a substrate having a pattern including recessed portions is desired.

[0034] [Implementation Method]

[0035] [Structure of film forming apparatus]

[0036] Next, an embodiment will be described. First, a film forming apparatus 100 according to an embodiment will be described. Figure 1 1 is a schematic cross-sectional view showing an example of a schematic structure of a film forming apparatus 100 according to an embodiment. In one embodiment, the film forming apparatus 100 is an apparatus for forming a film on a substrate W. Figure 1 The film forming apparatus 100 shown is airtightly configured and includes a chamber 1 electrically grounded. The chamber 1 is cylindrical and made of, for example, aluminum or nickel with an anodic oxide film formed on the surface. A stage 2 is provided in the chamber 1 .

[0037] The stage 2 is formed of a metal such as aluminum or nickel. A substrate W such as a semiconductor wafer is placed on the upper surface of the stage 2. The stage 2 supports the placed substrate W horizontally. The lower surface of the stage 2 is electrically connected to a support member 4 formed of a conductive material. The stage 2 is supported by the support member 4. The support member 4 is supported on the bottom surface of the chamber 1. The lower end of the support member 4 is electrically connected to the bottom surface of the chamber 1 and is grounded via the chamber 1. The lower end of the support member 4 is electrically connected to the bottom surface of the chamber 1 via a circuit adjusted to reduce the impedance between the stage 2 and the ground potential.

[0038] The stage 2 has a built-in heater 5, and the substrate W placed on the stage 2 can be heated to a predetermined temperature by the heater 5. A flow path (not shown) for circulating a refrigerant can be formed inside the stage 2, and a refrigerant whose temperature is controlled by a cooling device provided outside the chamber 1 is circulated and supplied into the flow path. The stage 2 can control the substrate W to a predetermined temperature by heating with the heater 5 and cooling with the refrigerant supplied from the cooling device. In addition, the temperature of the stage 2 can be controlled only by the refrigerant supplied from the cooling device without installing the heater 5.

[0039] In addition, an electrode may be embedded in the mounting table 2. The mounting table 2 can absorb the substrate W mounted on the upper surface of the mounting table 2 by utilizing the electrostatic force generated by the DC voltage supplied to the electrode. In addition, the mounting table 2 is provided with lift pins (not shown) for transferring the substrate W to and from a transport mechanism (not shown) provided outside the chamber 1.

[0040] A shower head 16 formed in a substantially disk shape is provided above the mounting table 2 and on the inner side surface of the chamber 1. The shower head 16 is supported on the upper portion of the mounting table 2 via an insulating member 45 such as ceramic. Thus, the chamber 1 is electrically insulated from the shower head 16. The shower head 16 is formed of, for example, a conductive metal such as nickel.

[0041] The shower head 16 includes a top plate member 16a and a shower plate 16b. The top plate member 16a is provided so as to seal the chamber 1 from the upper side thereof. The shower plate 16b is provided below the top plate member 16a so as to face the mounting table 2. A gas diffusion space 16c is formed in the top plate member 16a. A large number of gas ejection holes 16d opening toward the gas diffusion space 16c are dispersedly formed in the top plate member 16a and the shower plate 16b.

[0042] The top plate member 16a is provided with a gas introduction port 16e for introducing various gases into the gas diffusion space 16c. The gas introduction port 16e is connected to the gas supply path 15a. The gas supply path 15a is connected to the gas supply unit 15.

[0043] The gas supply unit 15 has gas supply lines connected to gas supply sources of various gases used for film formation. Each gas supply line is appropriately branched in a manner corresponding to the film formation process, and a control device for controlling the flow rate of the gas, such as a valve such as an on-off valve, and a flow controller such as a mass flow controller, is provided on each gas supply line. The gas supply unit 15 can control the flow rate of various gases by controlling the control devices such as the on-off valve and the flow controller provided on each gas supply line.

[0044] The gas supply unit 15 supplies various gases for film formation to the gas supply path 15a. For example, the gas supply unit 15 supplies the raw material gas for film formation to the gas supply path 15a. In addition, the gas supply unit 15 supplies the purge gas and the reaction gas that reacts with the raw material gas to the gas supply path 15a. The gas supplied to the gas supply path 15a diffuses in the gas diffusion space 16c and is ejected from each gas ejection hole 16d.

[0045] The space surrounded by the lower surface of the shower head 16b and the upper surface of the mounting table 2 constitutes a processing space for performing film forming processing. In addition, the shower head 16b and the mounting table 2 grounded via the support member 4 and the chamber 1 constitute a pair of electrode plates for forming a capacitively coupled plasma (CCP) in the processing space. The shower head 16 is connected to the high-frequency power supply 10 via the matcher 11, and high-frequency power (RF power) is supplied from the high-frequency power supply 10 to the gas supplied to the processing space 40 via the shower head 16, thereby forming the above-mentioned CCP. In addition, it is also possible that the high-frequency power supply 10 is connected to the mounting table 2 instead of being connected to the shower head 16, and the shower head 16 is grounded. In the present embodiment, the parts that implement film formation, such as the shower head 16, the gas supply unit 15, and the high-frequency power supply 10, correspond to the film forming unit of the present disclosure.

[0046] An exhaust port 71 is formed at the bottom of the chamber 1 and is connected to an exhaust device 73 via an exhaust pipe 72. The exhaust device 73 includes a vacuum pump and a pressure regulating valve, and the pressure in the chamber 1 can be reduced to a predetermined vacuum level by operating the vacuum pump and the pressure regulating valve.

[0047] A window 80a and a window 80b are provided on the side wall of the chamber 1 and face each other across the stage 2. The windows 80a and 80b are sealed by embedding a member that is transparent to infrared light, such as quartz. An irradiation unit 81 that irradiates infrared light is provided on the outside of the window 80a. A detection unit 82 that can detect infrared light is provided on the outside of the window 80b. The positions of the window 80a and the irradiation unit 81 are adjusted so that the infrared light irradiated from the irradiation unit 81 can be irradiated onto the substrate W via the window 80a. In addition, the positions of the window 80b and the detection unit 82 are adjusted so that the infrared light reflected by the substrate W is incident on the detection unit 82 via the window 80b. In addition, a loading and unloading port (not shown) for loading and unloading the substrate W is provided on a side wall of the chamber 1 that is different from the side wall on which the windows 80a and 80b are provided. A gate valve for opening and closing the loading and unloading port is provided at the loading and unloading port.

[0048] The irradiation unit 81 is configured so that the irradiated infrared light reaches a predetermined area near the center of the substrate W through the window 80a. For example, the irradiation unit 81 irradiates the infrared light to an area ranging from about 1 mm to 10 mm of the substrate W. The detection unit 82 is configured so that the infrared light reflected by the predetermined area of ​​the substrate W enters the detection unit 82 through the window 80b.

[0049] The film forming apparatus 100 according to the present embodiment obtains absorbance for each wave number of infrared light reflected by the substrate W by infrared spectroscopy (IR), thereby detecting the state of the film formed on the substrate W. Specifically, the film forming apparatus 100 obtains absorbance for each wave number of infrared light reflected by the substrate W by Fourier transform infrared spectroscopy (FT-IR), thereby detecting substances included in the film formed on the substrate W.

[0050] The irradiation unit 81 is equipped with a light source, a mirror, a lens and other optical elements that emit infrared light, and the irradiation unit 81 can irradiate infrared light after interference. For example, the middle part of the optical path of the infrared light generated by the light source until it is emitted to the outside is separated into two optical paths by a semi-transparent and semi-reflective mirror, and the optical path difference is changed by changing the length of one optical path relative to the length of the other optical path, so that the two optical paths interfere with each other, and the irradiation unit 81 irradiates infrared light of various interference waves with different optical path differences. In addition, a plurality of light sources can be provided in the irradiation unit 81, and the infrared light of each light source can be controlled by an optical element so as to irradiate infrared light of various interference waves with different optical path differences.

[0051] The detection unit 82 detects the signal intensity of infrared light of various interference waves reflected by the substrate W. In the present embodiment, the irradiation unit 81, the detection unit 82 and other parts that perform infrared spectroscopy measurements correspond to the measurement unit of the present disclosure.

[0052] The operation of the film forming apparatus 100 configured as described above is centrally controlled by the control unit 60. The control unit 60 is connected to a user interface 61 and a storage unit 62.

[0053] The user interface 61 includes an operation unit such as a keyboard for a process manager to input commands to manage the film forming apparatus 100, and a display unit such as a display that visually displays the operating status of the film forming apparatus 100. The user interface 61 accepts various operations. For example, the user interface 61 accepts a predetermined operation to instruct the start of plasma processing.

[0054] The storage unit 62 stores data such as programs (software), processing conditions, and process parameters for realizing various processes performed by the film forming apparatus 100 under the control of the control unit 60. In addition, the programs and data can be used in a state where they are stored in a computer-readable computer recording medium (such as a hard disk, a CD, a floppy disk, a semiconductor memory, etc.). Alternatively, the programs and data can be used online by being transmitted from another device at any time, for example, via a dedicated line.

[0055] The control unit 60 is, for example, a computer including a processor, a memory, etc. The control unit 60 reads programs and data from the storage unit 62 based on instructions from the user interface 61 and controls each unit of the film forming apparatus 100 to execute the film forming method described below.

[0056] The control unit 60 is connected to the irradiation unit 81 and the detection unit 82 via an interface (not shown) for inputting and outputting data, and inputs and outputs various information. The control unit 60 controls the irradiation unit 81 and the detection unit 82. For example, the irradiation unit 81 irradiates various interference waves with different optical path differences based on the control information from the control unit 60. In addition, information on the signal intensity of infrared light detected by the detection unit 82 is input to the control unit 60.

[0057] In addition, as semiconductor devices become increasingly miniaturized, patterns formed on substrates W also have complex nano-scale shapes. In film formation using plasma, the film quality of the sidewalls and bottoms of recesses included in the nano-scale fine pattern is likely to deteriorate. Figure 2 FIG. 2 is a diagram for explaining film formation using plasma according to an embodiment of the present invention. Figure 2, a substrate W is shown. A pattern 90 including a concave portion 90a at a nanoscale is formed on the substrate W. In the film formation using plasma, it is difficult for ions and radicals to reach the sidewalls and bottom of the concave portion 90a, and the film quality of the sidewalls and bottom of the concave portion 90a is likely to deteriorate. In order to improve the film quality, it is necessary to analyze the composition of the film on the sidewalls and bottom of the concave portion 90a.

[0058] Examples of techniques for analyzing the formed film include energy dispersive X-ray spectroscopy such as TEM-EDX and infrared spectroscopy such as Fourier transform infrared spectroscopy (FT-IR).

[0059] Figure 3A and Figure 3B This is a diagram illustrating the analysis performed using TEM-EDX. Figure 3A FIG. 2 schematically shows a state where a SiN film 91 is formed on a pattern 90 having a recess 90a by plasma ALD. The SiN film 91 at the bottom 90b (Bottom) of the recess 90a, the side wall 90c (Side), and the upper surface 90d (Top) of the pattern 90 are analyzed by TEM-EDX. Figure 3B 1 shows an example of the analysis results obtained by analyzing the bottom 90b (Bottom), the side wall 90c (Side), and the upper surface 90d (Top) of the SiN film 91 by TEM-EDX. The element composition of the SiN film 91 can be known by TEM-EDX.

[0060] exist Figure 3B The ratios of N (nitrogen), O (oxygen), and Si (silicon) at the bottom 90b (Bottom), the side wall 90c (Side), and the top surface 90d (Top) are shown. The ratio of N at the top surface 90d is higher than the ratio of N at the bottom 90b and the side wall 90c. In addition, the ratio of O gradually increases in the order of the top surface 90d, the side wall 90c, and the bottom 90b. In addition, the ratio of Si at the top surface 90d is lower than the ratio of Si at the bottom 90b and the side wall 90c. According to the results, it can be seen that different elemental compositions are observed at the bottom 90b, the side wall 90c, and the top surface 90d, so a more detailed analysis is required. However, although TEM-EDX can detect elements, it cannot detect chemical bonds. For example, it is unknown to which of O and Si N is bonded. In addition, in the analysis performed using TEM-EDX, light atoms such as H (hydrogen) cannot be detected.

[0061] Figure 4: is a diagram for explaining the conventional FT-IR analysis. Conventionally, in addition to forming a film on the actual substrate W used to manufacture semiconductor devices, the FT-IR analysis also forms a film on a flat monitoring substrate, irradiates the monitoring substrate with infrared light, analyzes the light that passes through the monitoring substrate or is reflected by the monitoring substrate, and infers the state of the film formed on the actual substrate W. Figure 4 FIG. 2 schematically shows a state where a SiN film 96 is formed on a flat silicon substrate 95 for monitoring by plasma ALD. Figure 4 In the process, infrared light is irradiated to the silicon substrate 95, and the light transmitted through the silicon substrate 95 is detected by a detector and FT-IR analysis is performed. Information on chemical bonds is obtained in the FT-IR analysis. In addition, in the FTIR analysis, the vibration of hydrogen atoms can be observed, and light atoms such as hydrogen can be detected. For example, in the SiN film 96, infrared light is absorbed and the molecules vibrate, so chemical bonds such as SiN, SiO, SiH, and NH can be detected by FT-IR analysis.

[0062] However, the states of the films formed on the actual substrate W used to manufacture semiconductor devices and the monitoring silicon substrate 95 are different. Even if the SiN film 96 formed on the silicon substrate 95 is analyzed by infrared spectroscopy, the state of the SiN film 91 formed on the substrate W cannot be determined.

[0063] Therefore, in the film forming apparatus 100 according to the embodiment, the control unit 60 controls each unit to perform the following film forming method process, and analyzes the composition of the film formed on the substrate W.

[0064] Figure 5 1 is a diagram for explaining the flow of the film forming method involved in the embodiment. First, a substrate having a pattern including a concave portion formed thereon before film formation is measured by infrared spectroscopy (step S10). For example, a substrate W as a film forming object having a pattern 90 including a concave portion 90a formed on its surface is placed on the mounting table 2. In the film forming apparatus 100, the control unit 60 controls the irradiation unit 81 to irradiate infrared light from the irradiation unit 81 to the substrate W before film formation, and the detection unit 82 detects the infrared light reflected by the substrate W, and FT-IR analysis is performed in the control unit 60.

[0065] Next, a film is formed on the substrate using plasma such as plasma CVD or plasma ALD (step S11). For example, the control unit 60 controls the gas supply unit 15 and the high frequency power supply 10 to form a SiN film 91 on the surface of the substrate W by plasma ALD.

[0066] Next, the substrate after film formation is measured by infrared spectroscopy (step S12). For example, in the film forming apparatus 100, the control unit 60 controls the irradiation unit 81 after film formation so that infrared light is irradiated from the irradiation unit 81 to the substrate W, and the detection unit 82 detects the infrared light reflected by the substrate W, and FT-IR analysis is performed in the control unit 60.

[0067] Next, the control unit 60 extracts difference data between the measurement data measured in step S10 and the measurement data measured in step S12 (step S13). For example, the control unit 60 extracts difference data between the measurement data after film formation and the measurement data before film formation. Figure 6 FIG. 2 is a diagram for explaining difference data according to an embodiment of the present invention. Figure 6 In FIG. 1 , as “before film formation”, a substrate W having a pattern 90 including a concave portion 90a formed thereon is shown. In addition, as “after film formation”, a substrate W having a SiN film 91 formed on the pattern 90 is shown. By extracting the difference between the measurement data after film formation and the measurement data before film formation, the signal of the SiN film 91 can be extracted as the difference data.

[0068] Next, the state of the film formed on the substrate W is displayed based on the extracted difference data (step S14 ). For example, the control unit 60 detects chemical bonds included in the SiN film 91 based on the difference data, and displays the detected chemical bonds on the user interface 61 .

[0069] In addition, the film formation process parameters are controlled based on the extracted difference data (step S15). For example, the control unit 60 detects chemical bonds included in the SiN film 91 based on the difference data, and controls the process parameters according to the detected chemical bonds.

[0070] Here, an example of a specific detection result is described. According to the film forming method according to the embodiment, a SiN film 91 is formed by plasma ALD on a substrate W having a pattern 90 including a concave portion 90 a formed thereon. Figure 7 1 is a diagram showing an example of a plasma ALD process according to an embodiment of the present invention. In plasma ALD, first, DCS (DiChloroSilane: SiH2Cl2) gas is supplied to adsorb the precursor onto the substrate W, and then the DCS gas is purged. Next, H2 gas is supplied while 13 MHz high frequency power is supplied to generate plasma for modification. Next, NH3 gas is supplied while 13 MHz high frequency power is supplied to generate plasma for nitridation. Plasma ALD forms a SiN film of a desired thickness by repeating each of these steps.

[0071] Fig. 8A1 is a diagram showing an example of a substrate W on which a SiN film 91 is formed according to an embodiment. In the substrate W, a pattern 90 including a concave portion 90a is formed on single crystal silicon (c-Si). The aspect ratio of the depth to the diameter of the concave portion 90a of the pattern 90 is set to 8. The SiN film 91 is formed on the pattern 90 of the substrate W.

[0072] The control unit 60 extracts difference data between the measurement data of the FT-IR analysis after film formation and the measurement data of the FT-IR analysis before film formation. For example, the control unit 60 obtains the absorbance of infrared light for each wave number of infrared light based on the measurement data before film formation and the measurement data after film formation. Furthermore, the control unit 60 extracts the absorbance of the SiN film 91 for each wave number of infrared light as difference data by subtracting the absorbance of infrared light before film formation from the absorbance of infrared light after film formation.

[0073] Furthermore, as a comparative example, a SiN film was formed on a flat silicon substrate using plasma ALD by the film forming method according to the embodiment. Figure 8B : is a diagram showing an example of a silicon substrate 95 on which a SiN film 96 is formed according to a comparative example. The silicon substrate 95 is a silicon wafer having a flat upper surface, and a SiN film 96 is formed on the upper surface of the silicon substrate 95. Similarly, in the comparative example, the control unit 60 extracts difference data between the measurement data of the FT-IR analysis after film formation and the measurement data of the FT-IR analysis before film formation. For example, the control unit 60 calculates the absorbance of infrared light for each wave number of infrared light based on the measurement data before film formation and the measurement data after film formation. Moreover, the control unit 60 extracts the absorbance of the SiN film 96 for each wave number of infrared light as difference data by subtracting the absorbance of infrared light before film formation from the absorbance of infrared light after film formation.

[0074] Fig. 9 This is a diagram showing an example of absorbance for each wave number of infrared light. Fig. 9 The horizontal axis is the wave number of infrared light. The vertical axis is the absorbance of infrared light. Fig. 9 A waveform L1 representing the absorbance of a SiN film 91 formed on a pattern 90 of a substrate W for each wave number is shown. In addition, as a comparative example, a waveform L2 representing the absorbance of a SiN film 96 formed on a flat silicon substrate 95 for each wave number is shown. The shorter the wavelength of infrared light, the greater the wave number. In addition, the wave number of the absorbed infrared light varies depending on the substance. Therefore, FT-IR analysis can determine what kind of substance is included based on the wave number of infrared light. In addition, FT-IR analysis can determine the content of a substance based on the absorbance for each wave number. In addition, FT-IR analysis can estimate the deposition (film thickness) of the formed film based on the absorbance for each wave number.

[0075] like Fig. 8A , 8B As shown in FIG. 1 , the SiN film 91 is also formed on the sidewalls and bottom of the concave portion 90a of the pattern 90, so the volume of the SiN film 91 is larger than that of the SiN film 96 on the flat silicon substrate 95. Therefore, the absorbance of the waveform L1 of the SiN film 91 is larger than the absorbance of the waveform L2 of the SiN film 96. The waveform L1 also detects a weaker signal than the waveform L2, so the waveform L1 can also detect a trace amount of a substance.

[0076] The greater the aspect ratio of the concave portion 90a of the pattern 90 of the SiN film 91, the greater the volume of SiN on the side wall of the concave portion 90a. Therefore, the greater the aspect ratio of the concave portion 90a, the more the component of the side wall of the concave portion 90a dominates in the waveform L1. That is, the greater the aspect ratio of the concave portion 90a, the more the waveform L1 represents the state of the side wall of the concave portion 90a.

[0077] Figures 10A to 10C This is a diagram showing an example of absorbance for each wave number of infrared light. Figures 10A to 10C The horizontal axis is the wave number of infrared light. The vertical axis is the absorbance of infrared light normalized based on the area of ​​the SiN film. Figures 10A to 10C , a waveform L1 showing the absorbance of the SiN film 91 formed on the pattern 90 of the substrate W for each wave number, and a waveform L2 showing the absorbance of the SiN film 96 formed on the flat silicon substrate 95 as a comparative example for each wave number. Figures 10A to 10C In FIG. 1 , the position of the wave number of the absorbed infrared light is shown for each compound and chemical bond. As shown in waveforms L1 and L2, the state of the SiN film 91 formed on the pattern 90 and the state of the SiN film 96 formed on the silicon substrate 95 are different. For example, Fig. 10A As shown in FIG. 1 , at the position of Si-N, the absorbance of waveform L2 is greater than that of waveform L1. On the other hand, at each position of Si-N, Si-O, and NH, the absorbance of waveform L1 is greater than that of waveform L2. Therefore, the SiN film 91 formed on the pattern 90 contains Si-O and NH in addition to Si-N. In addition, as shown in FIG. Fig. 10B As shown in FIG. 1 , the absorbance at the position of NH2 in waveform L2 is small. On the other hand, the absorbance at the position of NH2 in waveform L2 is large. Therefore, the SiN film 91 formed on the pattern 90 also contains NH2. Fig. 10C As shown in FIG. 1 , the waveform L1 has a larger absorbance at the position of NH than the waveform L2. Therefore, the SiN film 91 formed on the pattern 90 contains a lot of NH. As such, the states of the SiN film 91 and the SiN film 96 formed on the substrate W with the pattern 90 formed thereon and the flat silicon substrate 95 are different. For example, Figures 10A to 10CIn the case of NH, SiO, and NH2, there are many NH, SiO, and NH2 in the SiN film 91. This causes the WER (Wet Etching Rate) to deteriorate. The reason why NH, SiO, and NH2 exist in the SiN film 91 is that ions and radicals cannot fully reach the side wall of the recess 90a, resulting in insufficient nitridation. In this way, the state of the SiN film 91, such as the substances and chemical bonds contained in the SiN film 91, can be obtained based on the difference data. For example, NH can be detected based on the difference data. x 、SiH x , SiO and other substances that affect the film quality of the SiN film 91.

[0078] The control unit 60 displays the state of the SiN film 91 formed on the substrate W based on the difference data. For example, the control unit 60 displays the following in the user interface 61: Fig. 9 , Figures 10A to 10C The waveform L1 representing the absorbance for each wave number of the SiN film 91 is shown. In addition, for example, the control unit 60 determines the substances and chemical bonds included in the SiN film 91 based on the absorbance of each substance and chemical bond at the position of the wave number of the absorbed infrared light, and displays the determined substances and chemical bonds in the user interface 61. In addition, the control unit 60 can estimate the film thickness of the formed SiN film 91 based on the absorbance for each wave number, and display the estimated film thickness in the user interface 61.

[0079] In addition, the control unit 60 detects chemical bonds contained in the SiN film 91 based on the difference data, and controls the process parameters according to the detected chemical bonds. Figures 10A to 10C In the case where the SiN film 91 is insufficiently nitrided, the control unit 60 controls the process parameters of the film formation to promote nitridation. For example, the control unit 60 controls the process parameters to increase the flow rate of the NH3 gas supplied by the nitridation process and to lengthen the nitridation time. Thus, the film forming apparatus 100 can promote nitridation in the subsequent film formation, thereby improving the film quality of the SiN film 91 formed on the pattern 90.

[0080] In addition, in this embodiment, the case where FT-IR analysis is performed before and after the formation of SiN film 91 is described as an example, but the present invention is not limited to this. FT-IR analysis may be performed before and after a specific step of plasma ALD to obtain measurement data respectively, and to extract difference data in a specific step. For example, Figure 7FT-IR analysis is performed before and after the adsorption process, modification process, and nitridation process of the precursor of the plasma ALD shown in the figure to obtain measurement data and extract difference data. In addition, FT-IR analysis can also be performed in each process all the time to monitor the difference between the data before each process and the real-time data in real time. Thus, the state of the adsorption process, modification process, and nitridation process can be detected in real time based on the difference data of the adsorption process, modification process, and nitridation process. For example, the adsorption degree of the precursor in the adsorption process can be detected, and it can be detected in real time whether the desired amount of precursor is adsorbed. In addition, the degree of modification can be detected in the modification process, and it can be detected in real time whether the desired modification is performed. In addition, the degree of nitridation can be detected in the nitridation process, and it can be detected in real time whether the desired plasma nitridation is performed. The control unit 60 controls the process parameters based on the difference data. For example, in the adsorption process, modification process, and nitridation process, the state of adsorption, modification, and nitridation is detected based on the difference data. When the adsorption, modification, and nitridation are insufficient, the control unit 60 controls the process parameters to implement the insufficient process. Thus, it is possible to suppress the deficiency of adsorption, modification, and nitridation, and improve the film quality of the SiN film 91 formed. In addition, in the case where a long treatment time is unnecessarily performed, the process time can be shortened and the productivity can be improved. Figure 7 Before or after each plasma ALD process, FT-IR analysis is performed to obtain measurement data, and difference data from the measurement data of the previous process is extracted to obtain difference data of each process. Thus, the status of each process can be detected in real time based on the difference data of each process.

[0081] As described above, the film forming method according to the embodiment includes a first measuring process (step S10), a film forming process (step S11), a second measuring process (step S12), and an extraction process (step S13). In the first measuring process, a substrate W having a pattern 90 including a concave portion 90a formed thereon is measured by infrared spectroscopy. In the film forming process, after the first measuring process, a film is formed on the substrate W. The film forming process may include a modification process. In addition, the film forming process may also be a modification process. In the second measuring process, after the film forming process, the substrate W is measured by infrared spectroscopy. In the extraction process, the difference data between the measurement data of the first measuring process and the measurement data of the second measuring process is extracted. Thus, the film forming method according to the embodiment can detect the state of a film formed on a substrate W having a pattern 90 including a concave portion 90a formed thereon.

[0082] In addition, in the extraction process, the absorbance of infrared light is calculated for each wave number of infrared light based on the measurement data before film formation obtained by the first measurement process and the measurement data after film formation obtained by the second measurement process. In the extraction process, for each wave number, the absorbance of infrared light of the film for each wave number is extracted as difference data by subtracting the absorbance of infrared light before film formation from the absorbance of infrared light after film formation. Thus, the film forming method involved in the embodiment can detect the state of the film formed on the substrate W based on the absorbance of infrared light for each wave number extracted as difference data.

[0083] In addition, the film forming method according to the embodiment further includes a display step (step S14) in which the state of the film formed on the substrate W by the film forming step is displayed based on the difference data extracted by the extraction step. Thus, the film forming method according to the embodiment can indicate the state of the film actually formed on the substrate W to the process manager.

[0084] In addition, the film forming method according to the embodiment further includes a control step (step S15), in which the process parameters of the film forming step are controlled based on the difference data extracted by the extraction step. Thus, the film forming method according to the embodiment can adjust the process parameters according to the state of the film actually formed on the substrate W, and can improve the film quality of the film formed on the substrate W in the subsequent film formation.

[0085] The above embodiments are described, but it should be understood that the embodiments disclosed herein are illustrative in all respects and are not restrictive. In fact, the above embodiments can be implemented in a variety of ways. In addition, the above embodiments can be omitted, replaced, and changed in various ways without departing from the claims and their subject matter.

[0086] For example, in the above-mentioned embodiment, the case where the state of the film near the center of the substrate W is detected by reflecting infrared light near the center of the substrate W is described, but it is not limited to this. For example, an optical element such as a mirror or a lens that reflects infrared light may be set in the chamber 1, and the state of the film at multiple locations of the substrate W may be detected by detecting infrared light irradiated from the optical element to multiple locations such as the center and the periphery of the substrate W and reflected by each location. For example, before and after film formation, FT-IR analysis is performed at multiple locations within the surface of the substrate W to obtain measurement data. The control unit 60 extracts the difference data between the measurement data after film formation and the measurement data before film formation for each of the multiple locations. The control unit 60 controls the process parameters based on the extracted difference data of the multiple locations. For example, when the SiN film 91 at any location is insufficiently nitrided, the control unit 60 controls the process parameters of the film formation to promote nitridation. The control unit 60 can estimate the film thickness at multiple locations of the substrate W based on the difference data of the multiple locations and detect the distribution of the film thickness. Furthermore, the control unit 60 can control the process parameters to make the distribution of the film thickness uniform and to achieve a predetermined film quality. For example, when the distribution of the film thickness of the SiN film 91 is uneven and the SiN film 91 at any position is insufficiently nitrided, the control unit 60 controls the process parameters of the film formation to make the SiN film 91 uniform and to promote nitridation.

[0087] In addition, in the above-mentioned embodiment, the case where the process parameters of the film formation are controlled according to the difference data of one substrate W is described as an example, but it is not limited to this. The process parameters of the film formation process can also be controlled according to the difference data of multiple substrates W based on the comparison of the difference data between the substrates W. For example, when the film forming device 100 forms a film on multiple substrates W, the state of the formed film sometimes changes with the change of time. The control unit 60 changes the process parameters of the film formation process based on the comparison of the difference data between the substrates W so that the change of the state of the film is suppressed. For example, in the case where the SiN film 91 is insufficiently nitrided, the control unit 60 controls the process parameters of the film formation to promote nitridation. In this way, the change of the state of the film formed on the multiple substrates W can be suppressed.

[0088] In addition, in the above-mentioned embodiment, the case where the process parameters of film formation are controlled based on the difference data of one substrate W is described as an example, but it is not limited to this. The condition of the film forming device 100 changes over time, and even if the film formation is performed under the same film forming conditions (process), the state of the film formed may change. Therefore, the film forming device 100 regularly forms a film under the same film forming conditions every few days or at a specified time, and performs FT-IR analysis before and after the film formation, and diagnoses the condition of the film forming device 100 based on the results of the FT-IR analysis. For example, the film forming device 100 regularly forms a film on the substrate W under the same film forming conditions. The control unit 60 diagnoses the condition of the film forming device 100 based on the difference data of multiple substrates W on which the film is formed under the same film forming conditions, based on the comparison of the difference data between the substrates W. As a result, the film forming device 100 can detect changes in the condition based on changes in the state of the film formed under the same film forming conditions.

[0089] In the above embodiment, the film forming apparatus of the present disclosure is described as a single chamber type film forming apparatus 100 having one chamber, but the present invention is not limited thereto. The film forming apparatus of the present disclosure may be a multi-chamber type film forming apparatus having multiple chambers.

[0090] Fig.11 2 is a schematic structural diagram showing another example of the film forming apparatus 200 according to the embodiment. Fig.11 As shown, the film forming apparatus 200 is a multi-chamber type film forming apparatus having four chambers 201 to 204. In the film forming apparatus 200, plasma ALD is performed in each of the four chambers 201 to 204.

[0091] The chambers 201 to 204 are connected to four walls of a vacuum transfer chamber 301 having a heptagonal shape when viewed from above, respectively, via gate valves G. The vacuum transfer chamber 301 is evacuated by a vacuum pump to maintain a predetermined vacuum degree. The three load lock vacuum chambers 302 are connected to the remaining three walls of the vacuum transfer chamber 301 via gate valves G1. An atmospheric transfer chamber 303 is provided on the side opposite to the vacuum transfer chamber 301 across the load lock vacuum chamber 302. The three load lock vacuum chambers 302 are connected to the atmospheric transfer chamber 303 via gate valves G2. When a substrate W is transferred between the atmospheric transfer chamber 303 and the vacuum transfer chamber 301, the pressure of the load lock vacuum chamber 302 is controlled to be either atmospheric pressure or vacuum.

[0092] Three carrier mounting ports 305 are provided on the wall portion of the atmospheric transfer chamber 303 on the opposite side to the wall portion on which the load lock chamber 302 is installed. The carrier mounting ports 305 are used to mount a carrier (FOUP, etc.) C for accommodating the substrate W. In addition, an alignment chamber 304 is provided on the side wall of the atmospheric transfer chamber 303 for aligning the substrate W. A downward flow of clean air is formed in the atmospheric transfer chamber 303.

[0093] A transfer mechanism 306 is provided in the vacuum transfer chamber 301. The transfer mechanism 306 transfers the substrate W to the chambers 201 to 204 and the load lock chamber 302. The transfer mechanism 306 includes two transfer arms 307a and 307b that are independently movable.

[0094] A transfer mechanism 308 is provided in the atmospheric transfer chamber 303 . The transfer mechanism 308 transfers the substrate W to the carrier C, the load lock chamber 302 , and the alignment chamber 304 .

[0095] The film forming apparatus 200 includes a control unit 310 . The operation of the film forming apparatus 200 is centrally controlled by the control unit 310 .

[0096] In the film forming apparatus 200 configured as above, a measuring section for measuring the substrate W by infrared spectroscopy may be provided in addition to the chambers 201 to 204. For example, in the film forming apparatus 200, the measuring section for measuring the substrate W by infrared spectroscopy is provided in the vacuum conveying chamber 301 or any load lock vacuum chamber 302. For example, in the measuring section, an irradiation section for irradiating infrared light and a detection section for detecting infrared light are arranged in the vertical direction. When the film forming apparatus 200 performs FT-IR analysis, the substrate W is arranged in the measuring section by the conveying mechanism 306. In the measuring section, infrared light is irradiated from the irradiation section to the substrate W, and the infrared light that has passed through the substrate W is detected by the detection section.

[0097] The control unit 310 measures the substrate W before film formation through the measuring unit. The control unit 310 forms a film on the substrate W through any of the chambers 201 to 204. The control unit 310 measures the substrate W after film formation through the measuring unit. The control unit 310 extracts difference data between the measurement data obtained by the measuring unit before film formation and the measurement data obtained by the measuring unit after film formation. Thus, the film forming apparatus 200 can also detect the state of the film formed on the substrate W on which the pattern including the concave portion is formed.

[0098] As described above, an example of applying the technology of the present disclosure to detect the state of the film in the film forming process is described, but it is not limited to this. The process of detecting the state of the film is not limited to the film forming process, for example, it can be any process related to the semiconductor manufacturing process of manufacturing semiconductor devices, such as an etching process, a resist process, or a plurality of processes including a combination of any processes. In addition, from the perspective of any process related to the semiconductor manufacturing process and / or a plurality of processes including a combination of any processes, by applying the technology of the present disclosure before and after any process or a plurality of processes, the technology of the present disclosure can be applied to perform diagnosis and monitoring within the process and between processes. For example, it can be applied to various triggers (particles, in-plane / inter-plane distribution, etc.) related to the productivity (operation rate, yield, etc.) of semiconductor manufacturing. In addition, as described above, the film forming device of the present disclosure discloses a single-chamber or multi-chamber type film forming device having a plurality of chambers as an example, but it is not limited to this. For example, it can also be a batch-type film forming device that can uniformly process a plurality of substrates, or it can be a semi-batch film forming device of a turntable type.

[0099] In addition, it should be considered that the embodiments disclosed this time are illustrative in all aspects and are not restrictive. In fact, the above-mentioned embodiments can be specifically implemented in a variety of ways. In addition, the above-mentioned embodiments can be omitted, replaced and changed in various ways without departing from the attached claims and their purport.

Claims

1. A film forming method comprising: a preparation step of preparing a substrate having a pattern including a concave portion formed thereon on a stage in the chamber; In a first measuring step, infrared light of interference waves with different optical path differences is irradiated from an irradiation unit provided on one of the chamber side walls facing each other across the mounting table to the pattern including the recessed portion, and infrared light of interference waves with different optical path differences reflected by the pattern including the recessed portion is detected by a detection unit provided on the other side wall of the chamber side wall, thereby measuring the bottom, side wall and upper surface of the recessed portion; a film forming step of forming a film on the pattern of the substrate after the first measuring step, wherein the film is formed along the bottom, side wall and upper surface of the concave portion; a second measuring step, after the film forming step, irradiating infrared light of interference waves with different optical path differences from the irradiation section provided on one of the chamber side walls facing each other across the stage to the film formed along the pattern including the recessed portion, and detecting the infrared light of interference waves with different optical path differences reflected by the film formed along the pattern including the recessed portion by the detection section provided on the other side wall of the chamber side wall, thereby measuring a film formed along the bottom, side wall and upper surface of the recessed portion; and The extraction step extracts difference data between the measurement data of the first measurement step and the measurement data of the second measurement step.

2. The film forming method according to claim 1, characterized in that: The extraction process also includes: calculating the absorbance of infrared light for each wave number of infrared light based on the measurement data before film formation obtained by the first measurement process and the measurement data after film formation obtained by the second measurement process, and for each wave number, extracting the absorbance of infrared light of the film for each wave number as difference data by subtracting the absorbance of infrared light before film formation from the absorbance of infrared light after film formation.

3. The film forming method according to claim 1 or 2, characterized in that: The method further includes a display step of displaying a state of a film formed on the substrate in the film forming step based on the difference data extracted in the extraction step.

4. The film forming method according to claim 1 or 2, characterized in that: The method further includes a control step of controlling a process parameter of the film forming step based on the difference data extracted in the extraction step.

5. The film forming method according to claim 4, characterized in that: In the control step, a process parameter of the film forming step is controlled based on a comparison of the difference data between the substrates according to the difference data of the plurality of substrates.

6. The film forming method according to claim 4, characterized in that: performing the first measuring step and the second measuring step at each of a plurality of locations within the surface of the substrate, In the control step, difference data between measurement data in the first measurement step and measurement data in the second measurement step is extracted for each of the plurality of locations, and process parameters are controlled based on the extracted difference data of the plurality of locations.

7. The film forming method according to claim 6, characterized in that: In the control step, the distribution of film thickness and the film quality of the film formed on the substrate are obtained based on the difference data of the plurality of locations, and the process parameters are controlled so that the distribution of film thickness is uniform and a predetermined film quality is achieved.

8. The film forming method according to claim 1 or 2, characterized in that: In the film forming step, a film is formed on the substrate periodically under the same film forming conditions. The film forming method further includes a diagnosis step of diagnosing a condition of an apparatus for performing the film forming step based on comparison of the difference data between substrates, based on the difference data of a plurality of substrates on which films have been formed under the same film forming conditions.

9. A film forming device comprising: A mounting table, which is located in the chamber and is used to mount the substrate on which the pattern including the concave portion is formed; a film forming unit for forming a film on the substrate; a measuring unit including an irradiating unit provided on one of the chamber side walls facing each other across the mounting table, and a detecting unit provided on the other of the chamber side walls; as well as A control unit that controls to execute the following processes: a preparation step of preparing a substrate having a pattern including a concave portion formed on the mounting table; A first measuring step, causing the irradiation unit to irradiate the pattern including the concave portion with infrared light of interference waves with different optical path differences, and causing the detection unit to detect the infrared light of interference waves with different optical path differences reflected by the pattern including the concave portion, thereby measuring the bottom, side wall and upper surface of the concave portion; a film forming step of causing the film forming unit to form a film on the pattern of the substrate after the first measuring step, wherein the film is formed along the bottom, side wall and upper surface of the recess; a second measuring step, after the film forming step, causing the irradiation unit to irradiate infrared light of interference waves with different optical path differences to the film formed along the pattern including the recessed portion, and causing the detection unit to detect the infrared light of interference waves with different optical path differences reflected by the film formed along the pattern including the recessed portion, thereby measuring the film formed along the bottom, side wall and upper surface of the recessed portion; and The extraction step extracts difference data between the measurement data of the first measurement step and the measurement data of the second measurement step.

Citation Information

Patent Citations

  • Thin film forming method

    JP1998056010A

  • Film forming method and processing system

    CN102077325A

  • Inhibitor plasma mediated atomic layer deposition for seamless feature fill

    CN104928654A

  • Decomposition detecting unit, concentration measuring unit, and concentration control apparatus

    CN105651729A

  • Method And Apparatus For Depositing Silicon-containing Film

    CN106282966A