A polyhedral CsPbBr3@CsPbX3 core-shell perovskite heterojunction and preparation method thereof
The polyhedral CsPbBr3@CsPbX3 core-shell perovskite heterojunction addresses surface defects and non-radiative recombination issues through a novel synthesis method, enhancing stability and luminescence for optoelectronic applications.
Patent Information
- Application Number
- CN202110932395.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-08-13
AI Technical Summary
Existing methods for preparing perovskite core-shell heterostructures suffer from surface defects and non-radiative recombination, limiting their application in optoelectronic devices due to poor stability and luminescence performance.
A polyhedral CsPbBr3@CsPbX3 core-shell perovskite heterojunction is prepared using a dual-temperature zone tube furnace with a small quartz tube to reduce heating area and transport precursors in a laminar flow, resulting in a densely packed, smooth-surfaced heterojunction with low defect density.
The method enhances the stability and luminescence performance of perovskite materials by reducing defects and ion diffusion, allowing for adjustable band gap width and improved environmental stability, suitable for optoelectronic devices.
Smart Images

Figure CN113838980B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of perovskite photoelectric materials, and specifically relates to a polyhedron CsPbBr 3 @CsPbX 3 Core-shell perovskite heterojunction and method for preparing the same. Background Art
[0002] In recent years, halide perovskites have become ideal candidates for optoelectronic devices such as photodetectors, light-emitting diodes, lasers, and photovoltaic cells due to their excellent properties such as adjustable band gap, high light absorption coefficient, high defect tolerance, high quantum yield, and high carrier mobility. Despite their great advantages, poor stability is still the main drawback that limits the practical application and future commercialization of halide perovskites. By coating perovskite single crystals with a dense shell to form a core-shell structure, not only can the stability of halide perovskites in harsh environments be improved, but more importantly, it may also improve luminescence performance, reduce surface defects, inhibit non-radiative recombination, and enhance carrier transport.
[0003] The soft ionic bond properties and low lattice energy of halide perovskite nanocrystals lead to the formation of surface defects, which makes the vacancy formation energy of halide low, resulting in the instability of the material, but also conducive to the formation of heterojunction. The core-shell structure is also a special heterostructure. The appropriate shell can effectively serve as a physical environmental barrier, inhibit the interaction between crystals, reduce the existence of surface trap states, achieve adjustable band gap width, improve luminescence performance, and improve the relative stability of the material under the environment.
[0004] In previously reported literature, perovskite core-shell heterostructures were prepared by liquid phase method. The wrapping effect of surfactants caused the prepared core-shell heterojunction to be damaged to a certain extent. The crystal surface defects are large and non-radiative recombination is serious, which seriously affects the application of perovskite core-shell structures in the field of optoelectronic devices. Therefore, it is urgent to find a simple method to prepare a perovskite core-shell heterostructure with complete structure and few defects. Summary of the invention
[0005] The object of the present invention is to provide a polyhedral CsPbBr 3 @CsPbX 3 Core-shell perovskite heterojunction and preparation method thereof; the preparation method is simple, and the obtained CsPbBr 3 @CsPbX 3 The core-shell structure has a smooth surface and the shell CsPbX 3 The package is dense and the defect density is low.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] Providing a polyhedral CsPbBr 3 @CsPbX 3 Core-shell perovskite heterojunction, polyhedral CsPbBr 3 CsPbX 3 is a shell, wherein X is Cl or I. The polyhedron CsPbBr 3 @CsPbX 3 The core-shell mineral heterojunction is tightly packed and has a smooth surface.
[0008] According to the above scheme, the core polyhedron CsPbBr 3 The particle size is 3-5 μm, and the shell is CsPbX 3 The thickness is 0.5~1μm.
[0009] According to the above scheme, the polyhedron CsPbBr 3 CsPbBr is a regular tetrahedron 3 or cubic CsPbBr 3 .
[0010] Provide a polyhedron CsPbBr 3 @CsPbX 3 The method for preparing a core-shell perovskite heterojunction comprises the following steps:
[0011] A quartz tube 2 is placed inside the quartz tube 1 of the dual-temperature zone tube furnace to deposit polyhedral CsPbBr on the substrate. 3 The mixed powders of cesium halide and lead halide are placed at the two ends of the quartz tube 2, wherein the polyhedron CsPbBr 3 The mixed powder of cesium halide and lead halide is located at the center of the thermocouple in the upstream zone of the double-temperature zone tube furnace. The temperature of the upstream zone of the double-temperature tube furnace is set at 540-700°C, and the temperature of the downstream zone is set at 270-330°C. The polyhedron CsPbBr is prepared by reaction in an inert gas atmosphere. 3 @CsPbX 3 Core-shell heterojunction, where X is Cl or I.
[0012] According to the above scheme, the outer diameter ratio of quartz tube 1 and quartz tube 2 is 4:(1-3).
[0013] According to the above scheme, cesium halide and lead halide are mixed in equimolar amounts.
[0014] According to the above scheme, the polyhedron CsPbBr 3 The molar ratio of cesium halide to cesium halide is 1:0.5-2.
[0015] According to the above scheme, the inert gas flow rate is controlled to be 80-150 sccm.
[0016] According to the above scheme, the reaction time is 10 to 30 minutes.
[0017] According to the above scheme, the substrate is SiO 2 / Si substrate.
[0018] According to the above scheme, the polyhedron CsPbBr 3 CsPbBr is a regular tetrahedron 3 or cubic CsPbBr 3 .
[0019] According to the above scheme, the regular tetrahedron CsPbBr 3 Prepared as:
[0020] CsBr and PbBr 2 After mixing, the mixture is fully ground and then placed in the center of the thermocouple in the upstream zone of the quartz tube 1 in the dual-temperature tube furnace. The substrate is placed in the quartz tube 3 and then placed in the center of the thermocouple in the downstream zone of the quartz tube 1. The temperature of the upstream zone of the dual-temperature tube furnace is set to 580-650°C, and the temperature of the downstream zone is set to 300-380°C. The reaction is carried out in an inert gas atmosphere to prepare the tetrahedral CsPbBr 3 .
[0021] Preferably, the inert gas flow rate is controlled to be 50-300 sccm.
[0022] Preferably, the reaction time is 10 to 30 minutes.
[0023] Preferably, CsBr and PbBr 2 Mix equimolar quantities.
[0024] Preferably, the outer diameter ratio of the quartz tube 1 to the quartz tube 3 is 4:(1-3).
[0025] Preferably, the substrate is SiO 2 / Si substrate.
[0026] Preferably, the specific steps are: setting the temperature of the upstream zone of the dual-temperature tube furnace to 580-650°C, the temperature of the downstream zone to 300-380°C, and accurately controlling the inert gas flow rate to 50-300sccm through a flow meter; keeping the argon gas flowing during the reaction process, and after the temperature control program is completed, closing the flow meter and the argon bottle decompression valve, and taking out the sample in time to obtain a uniformly sized tetrahedral CsPbBr 3 .
[0027] According to the above scheme, the cubic CsPbBr 3 Prepared as:
[0028] CsBr and PbBr 2After mixing, the mixture was fully ground and then placed at the center of the thermocouple in the upstream zone of the dual-temperature tubular furnace. The substrate was placed at the center of the thermocouple in the downstream zone. The temperature of the upstream zone of the dual-temperature tubular furnace was set to 580-670°C and the temperature of the downstream zone was set to 320-360°C. The cubic CsPbBr was prepared by reaction in an inert gas atmosphere. 3 .
[0029] Preferably, the inert gas flow rate is controlled to be 30-200 sccm.
[0030] Preferably, the reaction time is 10 to 30 minutes.
[0031] Preferably, CsBr and PbBr 2 Mix equimolar quantities.
[0032] Preferably, the substrate is SiO 2 / Si substrate.
[0033] Preferably, the specific steps are: setting the temperature of the upstream zone of the dual-temperature tube furnace to 580-670°C, the temperature of the downstream zone to 320-360°C, and controlling the inert gas flow rate to 30-200 sccm by a flow meter; keeping the argon gas flowing during the reaction process, and after the temperature control program is completed, closing the flow meter and the argon bottle decompression valve, and taking out the sample in time, so as to obtain uniform-sized cubic CsPbBr 3 .
[0034] The conventional atmospheric pressure chemical vapor deposition (APCVD) method usually directly places the precursor and substrate in the upstream and downstream of the quartz tube of the double temperature zone tube furnace, but this will cause the local heating area to be too large, and the precursor gas source is transported to the substrate surface in the form of turbulence. When used in the present invention, the core part CsPbBr 3 The present invention reduces the heating area of the deposition part by inserting a small quartz tube into the quartz tube of the dual-temperature zone tubular furnace, and the precursor is transported downstream in a laminar flow to form CsPbBr 3 @CsPbX 3 The core-shell mineral heterojunction is densely packed, with a smooth surface and low defect density.
[0035] The beneficial effects of the present invention are as follows:
[0036] 1. The present invention provides a polyhedron CsPbBr 3 @CsPbX 3 Core-shell perovskite heterojunction, polyhedral CsPbBr 3 CsPbX 3It is a shell layer and is densely wrapped, the heterojunction surface is smooth, the defect degree is low, and the environmental stability is good (anti-oxidation and anti-moisture), which can realize the absorption and band gap width adjustment in the blue-green band region.
[0037] 2. The present invention uses polyhedral CsPbBr 3 The single crystal is used as the core and a layer of CsPbX is coated by atmospheric pressure chemical vapor deposition. 3 Perovskite, successful synthesis of polyhedral CsPbBr 3 @CsPbX 3 Core-shell perovskite heterojunction; in the process of atmospheric pressure chemical vapor deposition, a small quartz tube is placed inside the quartz tube of a dual-temperature zone tubular furnace to reduce the heating area of the deposition part, and the precursor is transported downstream in a laminar flow manner. The prepared core-shell heterojunction has dense wrapping, smooth surface and low defect density; at the same time, by controlling the downstream temperature, the degree of ion diffusion is reduced, which effectively improves the stability of the heterojunction.
[0038] 3. The preparation method of the present invention is simple, has good repeatability, does not generate gas-liquid intermediates, has high reaction efficiency, and can be produced on a large scale commercially. Compared with the liquid phase method for preparing perovskite core-shell structure, this method greatly reduces the interface defects of perovskite heterojunction and reduces the non-radiative recombination of carriers and holes. It has good application prospects in the field of optoelectronic devices and provides a material basis for studying the optical and electrical properties of perovskite core-shell heterostructures. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a process flow chart in an embodiment of the present invention.
[0040] Figure 2 The tetrahedron CsPbBr prepared in Example 1 of the present invention 3 Single crystal (Figures (1) and (2)) and tetrahedral CsPbBr 3 @CsPbCl 3 SEM images of core-shell heterojunction (Figures (3) and (4)).
[0041] Figure 3 The tetrahedron CsPbBr prepared in Example 1 of the present invention 3 @CsPbCl 3 SEM of core-shell heterojunction after high-temperature platinum etching.
[0042] Figure 4 The tetragonal CsPbBr prepared in Example 1 of the present invention 3 Single crystal (Figures (1) and (2)) and cubic CsPbBr 3 @CsPbCl 3 SEM image of the core-shell heterojunction (3).
[0043] Figure 5 The tetrahedron CsPbBr prepared in Example 1 of the present invention 3 @CsPbCl 3 EDS image of core-shell heterojunction.
[0044] Figure 6 The cubic CsPbBr prepared in Example 1 of the present invention 3 @CsPbCl 3 EDS image of core-shell heterojunction.
[0045] Figure 7 The tetrahedron CsPbBr prepared in Example 2 of the present invention 3 @CsPbCl 3 EDS image of core-shell heterojunction.
[0046] Figure 8 The cubic CsPbBr prepared in Example 2 of the present invention 3 @CsPbCl 3 EDS image of core-shell heterojunction.
[0047] Fig. 9 The tetrahedron CsPbBr prepared in Example 3 of the present invention 3 @CsPbCl 3 EDS image of core-shell heterojunction.
[0048] Fig.10 The cubic CsPbBr prepared in Example 3 of the present invention 3 @CsPbCl 3 EDS image of core-shell heterojunction.
[0049] Fig.11 The tetrahedron CsPbBr prepared in Example 4 of the present invention 3 @CsPbI 3 EDS image of core-shell heterojunction.
[0050] Fig.12 The cubic CsPbBr prepared in Example 4 of the present invention 3 @CsPbI 3 EDS image of core-shell heterojunction.
[0051] Fig.13 The tetrahedron CsPbBr prepared in Example 1 of the present invention 3 , cube CsPbBr 3 , tetrahedral CsPbBr 3 @CsPbCl 3 Core-shell heterojunction, cubic CsPbBr 3 @CsPbCl 3Steady-state photoluminescence spectrum of the core-shell heterojunction. DETAILED DESCRIPTION
[0052] The present invention is further explained below through specific examples.
[0053] Example 1
[0054] A polyhedron (tetrahedron, cube) CsPbBr 3 @CsPbCl 3 The preparation method of the core-shell heterojunction comprises the following specific steps:
[0055] (1) Preparation of precursors: Use an electronic balance to weigh 0.074 g of CsBr and 0.126 g of PbBr. 2 The powder was ground thoroughly in a mortar, and 0.100 g of the ground powder was weighed and placed in combustion boat No. 1 for later use. 0.056 g of CsCl and 0.093 g of PbCl were weighed. 2 The powder was ground thoroughly in a mortar, and 0.100 g of the ground powder was weighed and placed in the No. 2 combustion boat for later use. Alternatively, 0.065 g of CsI and 0.115 g of PbI were weighed. 2 The powder was ground thoroughly in a mortar, and 0.100 g of the ground powder was weighed and placed in a No. 3 combustion boat for later use.
[0056] (2)SiO 2 Preparation of Si substrate: Use a diamond pen to cut a 4-inch SiO 2 / Si substrate (purchased from Hefei Kejing) was cut into 1cm×1cm substrates. 2 / Si substrates were placed in acetone, ethanol, and ultrapure water for 15 min, and the SiO 2 The Si substrate was blown dry with ultrapure argon (purity 99.999%) and placed on a porcelain boat for later use.
[0057] (3) Preparation of uniformly sized tetrahedral CsPbBr 3 Single crystal: The No. 1 combustion boat mixed powder obtained in step 1 is placed in the center of the upstream thermocouple in the quartz tube of the dual-temperature zone tubular furnace (the outer diameter of the quartz tube is 80 mm). 2The Si substrate was inserted into a small quartz tube (outer diameter 50 mm, length 12 cm) and placed in the center of the thermocouple in the downstream zone of the dual-temperature tubular furnace quartz tube. The upstream zone temperature of the dual-temperature tubular furnace was accurately set to 610°C, and the downstream zone temperature was 350°C. The argon flow rate was accurately controlled to 100 sccm by the flow meter. The argon was kept flowing during the reaction process. After the temperature control program was completed (reaction time was 20 min), the flow meter and the argon bottle decompression valve were closed, and the sample was taken out in time. This method can obtain uniform-sized regular tetrahedron CsPbBr 3 , the reaction flow chart is as follows Figure 1 (2).
[0058] (4) Preparation of CsPbBr with uniform size 3 Single crystal: The mixed powder obtained in step 1 is placed in the center of the upstream thermocouple in a quartz tube of a dual-temperature zone tubular furnace (the outer diameter of the quartz tube is 80 mm). 2 The Si substrate was placed at the center of the thermocouple in the downstream zone of the quartz tube of the dual-temperature tubular furnace. The temperature of the upstream zone of the dual-temperature tubular furnace was accurately set to 610°C and the temperature of the downstream zone was 350°C. The argon flow rate was accurately controlled to 100 sccm by the flow meter. The argon was kept flowing during the reaction process. After the temperature control program was completed (the reaction time was 20 min), the flow meter and the argon bottle decompression valve were closed, and the sample was taken out in time. This method can obtain uniform-sized cubic CsPbBr 3 , the reaction flow chart is as follows Figure 1 (1).
[0059] (5) Preparation of polyhedral CsPbBr 3 @CsPbX 3 (X=Cl, I) Core-shell heterojunction: A small quartz tube 2 (outer diameter 50 mm, length 60 cm) is placed inside a quartz tube 1 (outer diameter 80 mm) in a dual-temperature tube furnace to deposit a polyhedral CsPbBr 3 (Step 3 obtained regular tetrahedron CsPbBr 3 Or the cubic CsPbBr obtained in step 4 3 ) and CsCl and PbCl obtained in step 1 2 The mixed powder (combustion boat No. 2) is placed at both ends of the quartz tube 2, where the polyhedron CsPbBr 3 Placed in the downstream zone of the dual-temperature zone tube furnace, CsCl and PbCl 2The mixed powder is placed at the center of the thermocouple in the upstream zone of the dual-temperature tube furnace. The temperature of the upstream zone of the dual-temperature tube furnace is accurately set to 650°C, and the temperature of the downstream zone is 290°C. The argon flow rate is accurately controlled to 100 sccm through the flow meter; the argon gas is kept flowing during the reaction process. After the temperature control program is completed (the reaction time is 20 minutes), the flow meter and the argon bottle decompression valve are closed, and the sample is taken out in time. This method can obtain polyhedron CsPbBr with uniform size and dense packaging. 3 @CsPbCl 3 Core-shell heterojunction, reaction flow chart as shown Figure 1 (3).
[0060] Figure 2 The tetrahedron CsPbBr prepared in Example 1 of the present invention 3 Single crystal (Figures (1) and (2)) and tetrahedral CsPbBr 3 @CsPbCl 3 SEM images of core-shell heterojunction (Figures (3) and (4)); Figure 4 The tetragonal CsPbBr prepared in Example 1 of the present invention 3 Single crystal (Figures (1) and (2)) and cubic CsPbBr 3 @CsPbCl 3 SEM image of the core-shell heterojunction (3). Figure 2 and Figure 4 The results show that the core polyhedron CsPbBr 3 The particle size is 3-5 μm, and the shell is CsPbCl 3 The thickness is 0.5 to 1 μm. Regular tetrahedron and cubic CsPbBr 3 @CsPbCl 3 The surface morphologies of the core-shell heterojunctions are shown in Figure 2 (4) Figure 4 (3), we can see that the polyhedrons (tetrahedrons, cubes) form a clear core-shell encapsulation structure, and there is an obvious stratification phenomenon on the edges. Compared with the polyhedron CsPbBr before encapsulation, 3 like Figure 2 (2), 4(2), CsPbBr 3 @CsPbCl 3 The junction of the core-shell heterojunction is relatively smooth, and the CsPbBr 3 @CsPbCl 3 Core-shell structure.
[0061] Figure 3 CsPbBr 3 @CsPbCl 3 The core-shell heterojunction partially decomposes at high temperature, and CsPbBr 3 With CsPbCl3 A clear heterogeneous interface can be observed between CsPbBr 3 @CsPbCl 3 The core-shell heterojunction was successfully prepared.
[0062] like Figure 5 , 6 Single particle polyhedron (tetrahedron, cube) CsPbBr 3 @CsPbCl 3 The core-shell heterojunction was analyzed by energy dispersive spectroscopy (EDS). Figure 5 The tetrahedron CsPbBr 3 @CsPbCl 3 The Cs, Pb, Cl, and Br content of the core-shell heterojunction are 18.33%, 18.87%, 56.69%, and 6.11%, respectively; Figure 6 The cubic CsPbBr 3 @CsPbCl 3 The Cs, Pb, Cl, and Br content of the core-shell heterojunction are 17.75%, 20.71%, 56.23%, and 5.90%, respectively. The atomic content ratio of Cs, Pb, and Cl is close to 1:1:3, indicating that the tetrahedron and cubic CsPbBr 3 @CsPbCl 3 The core-shell heterojunction was successfully prepared. The Br content in the tetrahedral and cubic core-shell heterojunctions was only 6.11% and 5.90%, respectively. - In CsPbBr 3 @CsPbCl 3 The degree of ion diffusion at the core-shell heterojunction interface is small.
[0063] The steady-state photoluminescence spectrum was obtained by 375 nm laser excitation. Fig.13 , compared to the tetrahedral CsPbBr 3 , tetrahedral CsPbBr 3 @CsPbCl 3 The photoluminescence peak position of the core-shell heterojunction red-shifts from 530nm to 445nm. 3 , cube CsPbBr 3 @CsPbCl 3 The photoluminescence peak position of the core-shell heterojunction blue shifts from 520nm to 460nm. 3 @CsPbCl 3 The photoluminescence peak position of the core-shell heterojunction has a significant blue shift, indicating the formation of a densely packed CsPbBr 3 @CsPbCl 3The core-shell heterojunction realizes controllable absorption in the blue-green band region.
[0064] Example 2
[0065] A polyhedron (tetrahedron, cube) CsPbBr 3 @CsPbCl 3 The preparation method of the core-shell heterojunction comprises the following specific steps:
[0066] SiO 2 / Si substrate is the same as step 1 of the above embodiment 1.
[0067] The preparation of the precursor is the same as step 2 of Example 1 above.
[0068] Preparation of uniformly sized CsPbBr 3 The tetrahedral single crystal is the same as step 3 of the above embodiment 1.
[0069] Preparation of CsPbBr with uniform size 3 Step 4 of cubic single crystal embodiment 1.
[0070] (5) Preparation of polyhedral CsPbBr 3 @CsPbCl 3 Core-shell heterojunction: A small quartz tube 2 (outer diameter 50 mm, length 60 cm) is placed inside the quartz tube 1 (outer diameter 80 mm) of the dual-temperature zone tube furnace to deposit polyhedral CsPbBr on the substrate. 3 (Step 3 obtained regular tetrahedron CsPbBr 3 Or the cubic CsPbBr obtained in step 4 3 ) and CsCl and PbCl obtained in step 1 2 The mixed powders are placed at both ends of the quartz tube 2, where the polyhedron CsPbBr 3 Placed in the downstream zone of the dual-temperature zone tube furnace, CsCl and PbCl 2 The mixed powder (combustion boat No. 2) was placed at the center of the thermocouple in the upstream zone of the dual-temperature tubular furnace. The temperature of the upstream zone of the dual-temperature tubular furnace was accurately set to 650°C, and the temperature of the downstream zone was 330°C. The argon flow rate was accurately controlled to 100 sccm by the flowmeter. The argon was kept flowing during the reaction process. After the temperature control program was completed (the reaction time was 20 minutes), the flowmeter and the argon bottle decompression valve were closed, and the sample was taken out in time. This method can obtain polyhedrons of uniform size and dense packaging of CsPbBr 3 @CsPbCl 3 Core-shell heterojunction.
[0071] like Figure 7 , 8 , for single particle polyhedron (tetrahedron, cube) CsPbBr 3@CsPbCl 3 Energy dispersive spectroscopy (EDS) analysis of the core-shell heterojunction. 3 @CsPbCl 3 The Cs, Pb, Cl, and Br content of the core-shell heterojunction are 16.63%, 18.48%, 43.02%, and 21.87%, respectively. 3 @CsPbCl 3 The Cs, Pb, Cl, and Br content of the core-shell heterojunction are 19.38%, 19.91%, 35.90%, and 24.81%, respectively. The atomic ratio of Cs, Pb, Cl, and Br is close to 1:1:2:1. The Br content in the tetrahedral and cubic core-shell heterojunctions is 21.87% and 24.81%, respectively, which further indicates that Br at 330°C - In CsPbBr 3 @CsPbCl 3 The degree of ion diffusion at the core-shell heterojunction interface increases because Br - It gains energy, breaks free from the constraints of ionic bonds, and diffuses to the interface, so the upper limit temperature of the downstream should not exceed 330℃.
[0072] Example 3
[0073] A polyhedron (tetrahedron, cube) CsPbBr 3 @CsPbCl 3 The preparation method of the core-shell heterojunction comprises the following specific steps:
[0074] SiO 2 / Si substrate is the same as step 1 of the above embodiment 1.
[0075] The preparation of the precursor is the same as step 2 of Example 1 above.
[0076] Preparation of uniformly sized CsPbBr 3 The tetrahedral single crystal is the same as step 3 of the above embodiment 1.
[0077] Preparation of CsPbBr with uniform size 3 Step 4 of cubic single crystal embodiment 1.
[0078] (5) Preparation of polyhedral CsPbBr 3 @CsPbCl 3 Core-shell heterojunction: A small quartz tube 2 (outer diameter 50 mm, length 60 cm) is placed inside the quartz tube 1 (outer diameter 80 mm) of the dual-temperature zone tube furnace to deposit polyhedral CsPbBr on the substrate. 3 (Step 3 obtained regular tetrahedron CsPbBr 3Or the cubic CsPbBr obtained in step 4 3 ) and CsCl and PbCl obtained in step 1 2 The mixed powders are placed at both ends of the quartz tube 2, where the polyhedron CsPbBr 3 Placed in the downstream zone of the dual-temperature zone tube furnace, CsCl and PbCl 2 The mixed powder (combustion boat No. 2) was placed at the center of the thermocouple in the upstream zone of the dual-temperature tubular furnace. The temperature of the upstream zone of the dual-temperature tubular furnace was accurately set to 650°C, and the temperature of the downstream zone was 310°C. The argon flow rate was accurately controlled to 100 sccm by the flowmeter. The argon was kept flowing during the reaction process. After the temperature control program was completed (the reaction time was 20 minutes), the flowmeter and the argon bottle decompression valve were closed, and the sample was taken out in time. This method can obtain polyhedron CsPbBr with uniform size and dense packaging. 3 @CsPbCl 3 Core-shell heterojunction.
[0079] like Fig. 9 , 10 , for single particle polyhedron (tetrahedron, cube) CsPbBr 3 @CsPbCl 3 Energy dispersive spectroscopy (EDS) analysis of the core-shell heterojunction. 3 @CsPbCl 3 The element contents of Cs, Pb, Cl, and Br in the core-shell heterojunction are 18.00%, 16.95%, 57.77%, and 7.28%, respectively. 3 @CsPbCl 3 The element contents of Cs, Pb, Cl, and Br in the core-shell heterojunction are 18.45%, 19.44%, 50.26%, and 11.85%, respectively. The atomic content ratio of Cs, Pb, and Cl is close to 1:1:3, and the atomic content of Br in the tetrahedral and cubic core-shell heterojunctions is only 7.28% and 11.85%, respectively, which further indicates that Br at 310°C - In CsPbBr 3 @CsPbCl 3 The degree of ion diffusion at the core-shell heterojunction interface is small.
[0080] Example 4
[0081] A polyhedron (tetrahedron, cube) CsPbBr 3 @CsPbI 3 The preparation method of the core-shell heterojunction comprises the following specific steps:
[0082] SiO 2 / Si substrate is the same as step 1 of the above embodiment 1.
[0083] The preparation of the precursor is the same as step 2 of Example 1 above.
[0084] Preparation of uniformly sized CsPbBr 3 The tetrahedral single crystal is the same as step 3 of the above embodiment 1.
[0085] Preparation of CsPbBr with uniform size 3 Step 4 of cubic single crystal embodiment 1.
[0086] (5) Preparation of polyhedral CsPbBr 3 @CsPbI 3 Core-shell heterojunction: A small quartz tube 2 (outer diameter 50 mm, length 60 cm) is placed inside the quartz tube 1 (outer diameter 80 mm) of the dual-temperature zone tube furnace to deposit polyhedral CsPbBr on the substrate. 3 (Step 3 obtained regular tetrahedron CsPbBr 3 Or the cubic CsPbBr obtained in step 4 3 ) and CsI and PbI obtained in step 1 2 The mixed powders are placed at both ends of the quartz tube 2, where the polyhedron CsPbBr 3 Placed in the downstream area of the dual-temperature zone tube furnace, CsI and PbI 2 The mixed powder (combustion boat No. 3) was placed at the center of the thermocouple in the upstream zone of the dual-temperature tubular furnace. The temperature of the upstream zone of the dual-temperature tubular furnace was accurately set to 610°C, and the temperature of the downstream zone was 290°C. The argon flow rate was accurately controlled to 100 sccm by the flowmeter. During the reaction process, argon was kept flowing in. After the temperature control program was completed (the reaction time was 20 min, the flowmeter and the argon bottle decompression valve were closed, and the sample was taken out in time. This method can obtain polyhedrons of uniform size and dense packaging of CsPbBr 3 @CsPbI 3 Core-shell heterojunction.
[0087] like Fig.11 , 12 , for single particle polyhedron (tetrahedron, cube) CsPbBr 3 @CsPbI 3 Energy dispersive spectroscopy (EDS) analysis of the core-shell heterojunction. 3 @CsPbI 3 The element contents of Cs, Pb, I, and Br in the core-shell heterojunction are 17.95%, 21.78%, 51.08%, and 9.18%, respectively. 3 @CsPbI 3The element contents of Cs, Pb, I, and Br in the core-shell heterojunction are 16.42%, 21.8%, 48.24%, and 13.53%, respectively. The atomic content ratio of Cs, Pb, and I is close to 1:1:3, and the atomic content of Br in the tetrahedral and cubic core-shell heterojunctions is only 9.18% and 13.53%, respectively, which further indicates that Br is - In CsPbBr 3 @CsPbI 3 The degree of ion diffusion at the core-shell heterojunction interface is small.
[0088] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A method for preparing a polyhedral CsPbBr3@CsPbX3 core-shell perovskite heterojunction, characterized in that: In the core-shell perovskite heterojunction, the polyhedron CsPbBr3 is the core and CsPbX3 is the shell, wherein X is Cl or I; The preparation method comprises the following steps: A quartz tube 2 is placed inside a quartz tube 1 of a dual-temperature zone tubular furnace, wherein the outer diameter ratio of the quartz tube 1 to the quartz tube 2 is 4:(1-3), and the polyhedron CsPbBr3 deposited on the substrate and the mixed powder of cesium halide and lead halide are respectively placed at both ends of the quartz tube 2, wherein the polyhedron CsPbBr3 deposited on the substrate is located at the center of the downstream zone of the dual-temperature zone tubular furnace, and the mixed powder of cesium halide and lead halide is located at the center of the thermocouple in the upstream zone of the dual-temperature zone tubular furnace, and the temperature of the upstream zone of the dual-temperature zone tubular furnace is set to 540-700 °C. o C, the temperature in the downstream area is 270~330 o C, a polyhedral CsPbBr3@CsPbX3 core-shell heterojunction is prepared by reaction in an inert gas atmosphere, where X is Cl or I.
2. The preparation method according to claim 1, characterized in that: The particle size of the core polyhedron CsPbBr3 is 3 to 5 μm, and the thickness of the shell CsPbX3 is 0.5 to 1 μm.
3. The preparation method according to claim 1, characterized in that: Cesium halide and lead halide are mixed in equal moles; the molar ratio of the polyhedron CsPbBr3 to the cesium halide is 1:0.5-2.
4. The preparation method according to claim 1, characterized in that: The inert gas flow rate is controlled to be 80-150 sccm; the reaction time is 10-30 min.
5. The preparation method according to claim 1, characterized in that: The polyhedral CsPbBr3 is a regular tetrahedral CsPbBr3 or a cubic CsPbBr3.
6. The preparation method according to claim 5, characterized in that: When the polyhedron CsPbBr3 is a regular tetrahedron CsPbBr3, its preparation is as follows: CsBr and PbBr2 are mixed and fully ground, and then placed in the center of the upstream zone thermocouple in the quartz tube 1 of the dual-temperature zone tube furnace, the substrate is placed in the quartz tube 3 and then placed in the center of the downstream zone thermocouple in the quartz tube 1, and the temperature of the upstream zone of the dual-temperature tube furnace is set to 580-650 o C, the temperature of the downstream area is 300~380 o C, tetrahedral CsPbBr3 is prepared by reaction in an inert gas atmosphere; When the polyhedron CsPbBr3 is a cubic CsPbBr3, its preparation is as follows: CsBr and PbBr2 are mixed and fully ground, and then placed at the center of the thermocouple in the upstream zone of the dual-temperature tube furnace, and the substrate is placed at the center of the thermocouple in the downstream zone, and the temperature of the upstream zone of the dual-temperature tube furnace is set to 580-670 o C, the temperature of the downstream area is 320~360 o C, cubic CsPbBr3 is prepared by reaction in an inert gas atmosphere.
7. The preparation method according to claim 6, characterized in that: When preparing tetrahedral CsPbBr3: CsBr and PbBr2 are mixed in equal moles, the outer diameter ratio of quartz tube 1 to quartz tube 3 is 4: (1-3); the substrate is SiO2 / Si substrate; the inert gas flow rate is controlled to be 50-300 sccm; the reaction time is 10-30min; When preparing cubic CsPbBr3: CsBr and PbBr2 are mixed in equal moles, the substrate is a SiO2 / Si substrate; the inert gas flow rate is controlled to be 30-200 sccm; and the reaction time is 10-30 min.