A precision machining process for the inner hole of a cast iron part

By configuring tightening mandrels and CBN inserts on CNC lathes and using constant-line speed cutting technology, the problems of low clamping accuracy and unstable shape and position tolerance in the inner hole processing of cast iron step are solved, and efficient cast iron step is achieved Precise processing of inner holes ensures product quality and production efficiency.

CN113857513BActive Publication Date: 2024-12-06HEBEI HUABEI DIESEL ENGINE
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202111151541.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-29
Publication Date
2024-12-06
Estimated Expiration
2041-09-29

AI Technical Summary

Technical Problem

In the prior art, the machining method of cast iron parts is low in clamping accuracy, the shape and position tolerance of the inner hole is unstable, the boring roughness of cemented carbide tool is difficult to ensure, and the cutting line speed cannot be improved, resulting in the roughness of the inner hole of the machining parts and The shape and position tolerance is unstable, and excessive products are sometimes generated.

Method used

The CNC lathe is equipped with a tightening mandrel, a CBN blade is selected, and a constant-line speed cutting is used to set technical parameters. Through the coordination of positioning blocks, wedge-shaped vertebrae, a swell and a pulling bolt, the inner holes of the step are processed from the outside to the inside to ensure that The clamping force is uniform and the cutting speed is constant.

Benefits of technology

It effectively ensures the roughness and shape tolerance of the inner holes of the cast iron step, improves the stability and production efficiency of product quality, and solves the problem of precision machining of the inner holes of the cast iron step.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113857513B_ABST
    Figure CN113857513B_ABST
Patent Text Reader

Abstract

The invention discloses a precision machining process for the inner hole of the step of a cast iron part, which belongs to the field of mechanical machining technology. A CNC lathe is used, a tensioning mandrel is configured, a CBN blade is selected, constant linear speed cutting is adopted, technical parameters are set, and the inner hole of the step is roughed and finely bored from the inside to the outside. The application can effectively ensure the roughness and form and position tolerance of the inner hole of the step of the cast iron part, the product quality is stable, the production efficiency is high, and the machining problem that the roughness and form and position tolerance of the inner hole of the step of the cast iron part are not easy to ensure is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of mechanical processing technology, and specifically relates to a precision processing method for a stepped inner hole of a cast iron part. Background Art

[0002] Shell parts with stepped inner holes are widely used in various industrial product parts. To meet the needs of use, the surface roughness and shape and position tolerances of parts with stepped inner holes are required to be high to meet the assembly and sealing requirements. The inner hole of this type of parts has steps and a small diameter of about φ50mm, and there is a 20° cone transition at the connection between the two stepped holes. The inner hole cannot be ground, and it is not easy to use a machining center for boring. The precision machining of the stepped inner hole is the technical difficulty of machining this type of parts. In the prior art, the processing method of this type of parts is to use a CNC lathe, equipped with soft three-jaws and carbide tools, to rough and fine turn the inner hole. However, this method has low clamping accuracy, unstable shape and position tolerances of the inner hole, and it is difficult to ensure the roughness of the inner hole when boring with a carbide tool, and the cutting line speed cannot be increased; at the same time, the cutting edge of the tool is severely worn and has low durability. The roughness and shape and position tolerances of the inner hole of the processed parts are unstable, and out-of-range products are sometimes produced.

[0003] Therefore, there is an urgent need for a precision machining process for the inner hole of the step of cast iron parts, which can ensure the requirements of inner hole roughness and form and position tolerance and solve the problem of precision machining of the inner hole of the step of cast iron parts. Summary of the invention

[0004] The invention provides a precision machining process method for a step inner hole of a cast iron part, which can effectively ensure the roughness and shape and position tolerance of the step inner hole of the cast iron part, and has stable product quality and high production efficiency.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0006] The invention discloses a precision machining process for the inner hole of a cast iron part, which uses a numerically controlled lathe, is equipped with a tensioning mandrel, selects CBN blades, adopts constant linear speed cutting, sets technical parameters, and sequentially roughs and fines bores the inner hole of the step from the outside to the inside.

[0007] A further improvement of the technical solution of the present invention is that the tensioning core shaft includes a positioning block, a wedge-shaped vertebral body, an expansion sleeve and a pull bolt, the top of the pull bolt is provided with a cap, the pull bolt passes through the wedge-shaped vertebral body and covers the end face of the expansion sleeve, the expansion sleeve is sleeved on the outside of the wedge-shaped vertebral body and the inner angle of the expansion sleeve matches the angle of the outer side of the wedge-shaped vertebral body.

[0008] A further improvement of the technical solution of the present invention is that: the positioning block is fixed to the outer side of the wedge-shaped vertebral body and the lower end of the expansion sleeve, and the pull bolt can move relative to the positioning block.

[0009] A precision machining process for a step inner hole of a cast iron part, the specific steps comprising:

[0010] S1: Casting blank, rough turning of inner hole, outer circle and end face of workpiece;

[0011] S2: Configure the CBN blade on the CNC machine tool, set the parameters of the CBN blade, install the tensioning mandrel on the spindle of the CNC machine tool through the positioning block, and connect the pull bolt to the hydraulic cylinder of the CNC machine tool;

[0012] S3: Install the workpiece in step S1 on the outside of the expansion sleeve of the tensioning mandrel, the inner hole of the workpiece is a positioning hole, the matching clearance between the positioning hole of the workpiece and the tensioning mandrel is 0.10-0.20mm, and clamp the expansion sleeve;

[0013] S4: Set cutting parameters and CNC program, use constant linear speed cutting, perform rough boring and fine boring of inner holes, and first process the outermost holes of the step inner hole according to the workpiece size requirements, and then process the other holes of the step inner hole from the outside to the inside.

[0014] A further improvement of the technical solution of the present invention is that the geometric parameters of the CBN tool in step S2 are a front angle of 6°, a back angle of 7°, and a tool tip radius r of 0.4 mm.

[0015] The further improvement of the technical solution of the present invention is that the cutting parameters in step S4 are cutting depth: 0.10-0.15 mm, feed speed: 0.05-0.07 mm / r, and spindle speed: constant linear speed 150-180 mm / min.

[0016] A further improvement of the technical solution of the present invention is that when installing the tensioning mandrel in step S2, a micrometer is used for alignment, and the outer circle runout of the mandrel is less than 0.005 mm, and the end face runout is less than 0.005 mm.

[0017] A further improvement of the technical solution of the present invention is that the step of tightening the tensioning mandrel in step S2 is achieved by pulling the pull bolt.

[0018] Due to the adoption of the above technical solution, the technical progress achieved by the present invention is:

[0019] The present invention adopts this process scheme, which can effectively ensure the roughness and shape and position tolerance of the inner hole of the step of the cast iron part, and has stable product quality and high production efficiency, thus solving the processing problem that the roughness and shape and position tolerance of the inner hole of the step of the cast iron part are difficult to ensure.

[0020] The tensioning mandrel used in the processing of this application can ensure uniform clamping force of parts. The expansion sleeve is laterally translated to fit the workpiece, with uniform clamping force and high clamping precision; at the same time, it has an axial pulling effect, which solves the contradiction that the mandrel has good elasticity and high hardness and wear resistance at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1It is a cross-sectional view of the tensioning mandrel in a loosened state;

[0022] Figure 2 It is a cross-sectional view of the tensioning mandrel in a compressed state;

[0023] Figure 3 It is a processing drawing of a single pump seat of an embodiment of the present invention;

[0024] Among them, 1. positioning block, 2. wedge-shaped vertebral body, 3. expansion sleeve, 4. pull bolt, 5. workpiece. DETAILED DESCRIPTION

[0025] The process of the present invention is further described in detail below in conjunction with the embodiments:

[0026] Example 1

[0027] The single pump seat is an important part of diesel engine. It has complex structure, high precision and long processing route. The single pump seat is a component of fuel injection pump. It connects fuel injection pump and housing into one, keeps them in the correct position, and guides the fuel injection pump plunger to complete the prescribed action. Therefore, the processing quality of the single pump seat directly affects the performance, precision and life of the fuel injection pump. Figure 3 This is the processing drawing of the single pump seat. The upper end is ¢52, ¢50, and ¢48 three stepped inner holes, and the three stepped outer circles of the injector are divided into the oil inlet chamber and the oil return chamber by three sealing rings. The size accuracy of the ¢52 hole is IT7, and the position accuracy of the hole is required to be 0.05 for the runout of the ¢44 hole. The size accuracy of the ¢50 and ¢48 holes is IT8, and the runout of the hole is 0.1.

[0028] The specific steps are as follows:

[0029] S1: Casting blank, rough turning of inner hole, outer circle and end face of workpiece;

[0030] S2: Configure the CBN blade on the CNC machine tool, set the parameters of the CBN blade, and install the tensioning mandrel on the spindle of the CNC machine tool through the positioning block. The pull bolt 4 is connected to the hydraulic cylinder of the spindle of the CNC machine tool. When installing the tensioning mandrel, it is necessary to use a micrometer to align it. The outer circle runout of the mandrel is less than 0.005mm, and the end face runout is less than 0.005mm.

[0031] The geometric parameters of the CBN tool are set as 6° front angle, 7° back angle, and R0.4mm tool tip radius.

[0032] like Figure 1 and Figure 2As shown, the tensioning mandrel includes a positioning block 1, a wedge-shaped vertebral body 2, an expansion sleeve 3 and a pull bolt 4. The top of the pull bolt 4 has a cap. The pull bolt 4 passes through the wedge-shaped vertebral body 2 and covers the end face of the expansion sleeve 3. The expansion sleeve 3 is sleeved on the outside of the wedge-shaped vertebral body 2, and the angle of the inside of the expansion sleeve 3 matches the angle of the outside of the wedge-shaped vertebral body 2. The positioning block 1 is fixed to the outside of the wedge-shaped vertebral body 2 and the lower end of the expansion sleeve 3. The pull bolt 4 can move relative to the positioning block 1, and the workpiece can be clamped by pulling the pull bolt 4.

[0033] S3: Install the workpiece of step S1 on the outside of the expansion sleeve of the tensioning mandrel, the inner hole of the workpiece is a positioning hole, the matching clearance between the positioning hole of the workpiece and the tensioning mandrel is 0.10-0.20mm, clamp the expansion sleeve 3, and then press the workpiece;

[0034] During this process, the clearance between the workpiece positioning hole and the tensioning mandrel is too large, and the positioning accuracy is low, which cannot guarantee the requirement of 0.05 runout between the processed inner hole and the positioning hole. If the clearance is less than 0.1mm, it is inconvenient to install the workpiece.

[0035] S4: Set cutting parameters and CNC program, use constant linear speed cutting, perform rough boring and fine boring of inner holes, first process the outermost hole of the step inner hole according to the workpiece size requirements, and then process the other holes of the step inner hole from the outside to the inside, and the fine boring cutting depth is 0.10-0.15mm. In order to ensure the roughness of each step inner hole, the linear speed of the tool cutting needs to be constant, so constant linear speed cutting is required. The linear speed of the CBN tool boring inner hole is 150-180mm / min.

[0036] The process scheme of this application can effectively ensure the roughness and form and position tolerance of the inner hole of the step of the cast iron part, with stable product quality and high production efficiency, and solves the processing problem that the roughness and form and position tolerance of the inner hole of the step of the cast iron part are difficult to ensure.

Claims

1. A precision machining process for a step inner hole of a cast iron part, characterized in that: Use a CNC lathe, configure a tensioning mandrel, select CBN blades, use constant linear speed cutting, set technical parameters, and rough and fine bore the stepped inner hole from the outside to the inside; the specific steps include: S1: Casting blank, rough turning of inner hole, outer circle and end face of workpiece; S2: arranging the CBN blade on the CNC machine tool, setting the parameters of the CBN blade, and installing the tensioning mandrel on the main shaft of the CNC machine tool through the positioning block (1), and connecting the pull bolt (4) to the hydraulic cylinder of the CNC machine tool; the tensioning mandrel comprises a positioning block (1), a wedge-shaped cone (2), an expansion sleeve (3) and a pull bolt (4), the top of the pull bolt (4) is provided with a cap, the pull bolt (4) passes through the wedge-shaped cone (2) and covers the end face of the expansion sleeve (3), the expansion sleeve (3) is sleeved on the outside of the wedge-shaped cone (2) and the angle of the inner side of the expansion sleeve (3) matches the angle of the outer side of the wedge-shaped cone (2), the positioning block (1) is fixed to the outside of the wedge-shaped cone (2) and the lower end of the expansion sleeve (3), and the pull bolt (4) can move relative to the positioning block (1); when installing the tensioning mandrel in step S2, a micrometer is used for alignment, and the outer diameter runout of the mandrel is less than 0.005 mm, and the end face runout is less than 0.005 mm; S3: The workpiece (5) of step S1 is mounted on the outside of the expansion sleeve (3) of the tensioning mandrel, the inner hole of the workpiece is a positioning hole, the clearance between the positioning hole of the workpiece and the tensioning mandrel is 0.10-0.20 mm, and the tensioning mandrel is pressed; the cutting parameters in step S4 are cutting depth: 0.10-0.15 mm, feed speed: 0.05-0.07 mm / r, and spindle speed: constant linear speed 150-180 mm / min; S4: Set cutting parameters and CNC program, use constant linear speed cutting, perform rough boring and fine boring of inner holes, and first process the outermost holes of the step inner hole according to the workpiece size requirements, and then process the other holes of the step inner hole from the outside to the inside.

2. The precision machining process for the step inner hole of a cast iron part according to claim 1, characterized in that: The geometric parameters of the CBN tool in step S2 are a rake angle of 6°, a back angle of 7°, and a tool tip radius r of 0.4 mm.

3. The precision machining process for the step inner hole of a cast iron part according to claim 1, characterized in that: The step of tightening the tensioning mandrel in step S2 is achieved by pulling the pull bolt (4).

Citation Information

Patent Citations

  • Inner-cooling indexable step drill and method for fabricating step hole

    CN101524769A

  • Expansion sleeve linkage compression mechanism

    CN103737372A

  • Machining method of precision bearing seat

    CN106826117A

  • Split-type adjustable reverse-boring cutter

    CN109128230A

  • Boring tool and one-time forming method of inner stepped hole using boring tool

    CN111036945A