A temperature-responsive nano foam stabilizer and a preparation method thereof, and a temperature-sensitive foaming agent and a preparation method thereof

By using temperature-responsive nanofoam stabilizers and temperature-sensitive foaming agents in oil and gas development, the problem of difficult to balance foaming and stability of foam fluids is solved, and the intelligent response of foam under temperature changes is achieved, improving the improvement of foaming The oil and gas recovery rate and application range are achieved, and meet economic and environmental protection requirements.

CN113912780BActive Publication Date: 2024-11-15CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202010643324.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-07
Publication Date
2024-11-15
Estimated Expiration
2040-07-07

AI Technical Summary

Technical Problem

The foaming properties and stability of existing foam fluids are difficult to balance in oil and gas development, and traditional methods to enhance foam stability are expensive or have formation damage. Nano foam stabilizers lack intelligent responsiveness, limiting the application range of foam fluids.

Method used

The nanofoam stabilizer preparation method is adopted to obtain nanofoam stabilizer by polymerizing diethylacrylamide and styrene in the presence of protective gas and organic solvents, and combined with dodecyl betaine and coconut The temperature-sensitive foaming agent is prepared by oleoylpropylsulfobetaine and other ingredients, so that it can reversibly foam and defoam when the temperature changes.

Benefits of technology

It realizes the intelligent responsiveness of the foam, improves the efficiency and utilization rate of the foam, and expands the application scope in the field of oil and gas development. At the same time, it has a wide range of raw materials, is cheap, is environmentally friendly, is low in toxicity and is low in irritation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005079705170000131
    Figure GDA0005079705170000131
  • Figure GDA0005079705170000141
    Figure GDA0005079705170000141
  • Figure GDA0005079705170000142
    Figure GDA0005079705170000142
Patent Text Reader

Abstract

The invention discloses a temperature-responsive nano foam stabilizer and a preparation method thereof and a temperature-sensitive foaming agent and a preparation method thereof. The preparation method comprises: in the presence of a protective gas and an organic solvent, diethyl acrylamide, styrene and an initiator are subjected to a polymerization reaction to obtain the nano foam stabilizer. The temperature-responsive nano foam stabilizer PDEA PS latex particles developed by the invention gradually change the PDEA on the surface from a highly hydrated state to a dehydrated state as the temperature gradually increases. Therefore, when the temperature rises, the steric hindrance and repulsion caused by the hydration of the particle surface will be greatly reduced, and a flocculated state can be formed to be adsorbed on the gas / liquid interface of the bubble to form a solidified film, thereby slowing down the aggregation and disproportionation between the bubbles and enhancing the foam stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oilfield chemistry, and more specifically, relates to a temperature-responsive nano foam stabilizer and a preparation method thereof, and a temperature-sensitive foaming agent and a preparation method thereof. Background Art

[0002] Foam fluid has the advantages of adjustable density, good compressibility, high viscosity, low friction resistance, small liquid dosage, small damage to reservoirs, and strong solid particle carrying capacity. It is widely used in various process links of the petroleum industry, such as acidizing, fracturing, plugging removal, sand flushing, well washing, water cone, adjustment and displacement, reservoir transformation, etc. The foaming ability and stability of foam are the two most important properties of foam in practical applications. Since foam is a thermodynamic metastable system, it will gradually decay over time. Good foaming ability and high foam stability have always been a contradiction, often increasing and decreasing, and it is difficult to achieve a balance. In oil and gas development, for example, foam drainage and gas production in water-producing gas wells, the foam needs to be stable in the drainage stage, and the subsequent produced fluid needs to be defoamed before entering the separator for processing. At present, the main way to break the foam is chemical defoaming, but the addition of defoaming agents will prevent the foam from being further recycled, thereby increasing the development cost. Therefore, if the foam is endowed with intelligent responsiveness, so that it can reversibly foam and defoam when receiving physical (temperature, light radiation, electromagnetic field, etc.) or chemical (pH value, ionic strength, etc.) stimulation signals input from the external environment, or the foam performance can change accordingly with changes in environmental conditions, it will inevitably improve the efficiency and utilization rate of the foam and expand the scope of application of foam in the field of oil and gas development.

[0003] Since the foam system is a thermodynamically unstable system, seeking an efficient foam stabilizer is a key task in the research and development of foaming agents. At present, there are mainly two ways to improve the stability of foam: 1. By compounding surfactants, or simply modifying and compounding surfactants, this mainly utilizes the synergistic effect of surfactants. On the basis of minimizing surface tension, it more effectively exerts the Margangoni effect and enhances the repair function of the surface film; 2. Add some polymers. The addition of polymers can increase the viscosity of the system to reduce the drainage rate of the foam and achieve the effect of stabilizing the foam. However, the foaming agent formed by modifying and compounding surfactants has a good effect, but it is expensive; the added polymer will thermally degrade at high temperature, and the remaining organic residue will cause formation damage to a certain extent. Therefore, these ways to enhance foam stability have some shortcomings.

[0004] As a new type of science and technology that analyzes and manipulates the material world at the nanoscale, nanotechnology has been widely used in energy, food, materials, etc. In recent years, with the development of nanotechnology, nano-foam stabilization technology has gradually shown its advantages in food, mineral flotation, fire fighting, etc., but it is relatively rare in the field of foam fluid research. The nano-foam stabilizers reported so far can only simply stabilize the foam, but cannot give the foam fluid intelligent responsiveness, and cannot control the foaming and defoaming, thus limiting the scope of application of foam fluids in oil and gas development. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a temperature-responsive nano foam stabilizer and a temperature-sensitive foaming agent prepared therefrom, which utilizes temperature to control the structure and performance of the foam, thereby improving the recovery rate of oil and gas reservoirs.

[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a method for preparing a temperature-responsive nano foam stabilizer, characterized in that the preparation method comprises: in the presence of a protective gas and an organic solvent, polymerizing diethylacrylamide, styrene and an initiator to obtain the nano foam stabilizer.

[0007] Preferably, the preparation method further comprises: after the polymerization reaction is completed, centrifugal separation is performed to obtain the nano foam stabilizer.

[0008] Preferably, the centrifugal separation comprises:

[0009] (1) subjecting the product obtained from the polymerization reaction to a first centrifugation, dispersing the first centrifugation product into the organic solvent, and repeating the first centrifugation and dispersion steps multiple times;

[0010] (2) Dispersing the product treated in step (1) into water, and then performing a second centrifugation, dispersing the second centrifuged product into water again, and repeating the second centrifugation and re-dispersion steps multiple times.

[0011] Preferably, the centrifugal speed of the first centrifugation is 3500-5500 rpm, and the centrifugal time is 20-40 min;

[0012] The centrifugal speed of the second centrifugation is 8000-12000 rpm, and the centrifugal time is 20-40 min.

[0013] Preferably, the organic solvent is isopropanol;

[0014] The initiator is 2,2'-azo[2-methyl-N-(2-hydroxyethyl)propionamide];

[0015] The protective gas is nitrogen.

[0016] Preferably, the polymerization reaction temperature is 70 to 90° C., and the reaction time is 5 to 10 days;

[0017] The mass ratio of the diethylacrylamide, styrene and initiator is 4-10:5-9:0.3-1.8.

[0018] The second aspect of the present invention provides a temperature-responsive nano foam stabilizer prepared by the above preparation method.

[0019] The third aspect of the present invention provides a temperature-sensitive foaming agent, which comprises, based on the total weight of the temperature-sensitive foaming agent, 1 to 15 wt % of the temperature-responsive nano foam stabilizer, 20 to 45 wt % of dodecyl betaine, 8 to 20 wt % of cocoyl propyl sulfobetaine, 5 to 10 wt % of sodium α-olefin sulfonate, 0.1 to 1.5 wt % of sodium dodecyl sulfonate, 0.1 to 0.5 wt % of octylphenol polyoxyethylene 10 ether, 0.15 to 0.45 wt % of dodecyl dimethyl ammonium bromide, and the balance is water.

[0020] A fourth aspect of the present invention provides a method for preparing the temperature-sensitive foaming agent, the method comprising:

[0021] (1) stirring and mixing lauryl betaine and cocoyl propyl sulfobetaine to obtain a first mixed solution;

[0022] (2) stirring and mixing the first mixed solution, sodium α-olefin sulfonate and sodium dodecyl sulfonate to obtain a second mixed solution;

[0023] (3) adding water to the second mixed solution, then heating it, and finally adding octylphenol polyoxyethylene 10 ether and dodecyl dimethyl ammonium bromide and stirring and mixing them uniformly to obtain a third mixed solution;

[0024] (4) The third mixed solution and the temperature-responsive nano foam stabilizer are stirred and mixed uniformly to obtain the temperature-sensitive foaming agent.

[0025] Preferably, in step (1), the stirring speed is 800 to 2000 rpm, and the time is 10 to 40 min;

[0026] In step (2), the stirring and mixing temperature is 40 to 60° C., the stirring speed is 800 to 2000 rpm, and the time is 10 to 40 min;

[0027] In step (3), the heating temperature is 65-80° C., the stirring speed is 800-2000 rpm, and the time is 10-40 min;

[0028] In step (4), the stirring and mixing temperature is 40 to 60° C., the stirring speed is 800 to 2000 rpm, and the time is 10 to 40 min.

[0029] The technical solution of the present invention has the following beneficial effects:

[0030] (1) The nano foam stabilizer (PDEA-PS) of the present invention has intelligent temperature responsiveness. At 25°C, the polystyrene latex particles (PDEA-PS) carrying polydiethylacrylamide (PDEA) on the surface are in a highly hydrated state. There are steric hindrances and huge repulsive effects between the latex particles. Therefore, at this temperature, the latex particles can only be evenly dispersed in water. The foam prepared therefrom exhibits serious aggregation and disproportionation over time, leading to foam rupture. As the temperature rises, the hydration of PDEA gradually weakens, so the repulsive force between the PDEA-PS latex particles decreases, presenting a flocculated state, and can form a dense solidified film at the gas / liquid interface of the bubbles, reducing the diffusion of gas between the bubbles, thereby playing a role in stabilizing the foam. When the temperature drops again, as PDEA is hydrated again, the PDEA-PS latex particles cannot present a flocculated state and adsorb on the gas / liquid interface to form a dense solidified film, so the stability of the foam decreases accordingly.

[0031] (2) The thermosensitive foaming agent of the present invention imparts intelligent responsiveness to the foam, enabling it to reversibly foam and defoam upon receiving temperature stimulation, thereby improving the efficiency and utilization rate of the foam. The foam can be used to improve tertiary recovery such as foam flooding and foam drainage and gas recovery, thereby expanding the application scope of the foam in the field of oil and gas development.

[0032] (3) The raw materials for preparing the temperature-responsive nano foam stabilizer and the temperature-sensitive foaming agent prepared therefrom are widely available and inexpensive, and are environmentally friendly, low in toxicity and irritation, and can be applied on a large scale on site.

[0033] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0034] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0035] The first aspect of the present invention provides a method for preparing a temperature-responsive nano foam stabilizer, the method comprising: subjecting diethylacrylamide, styrene and an initiator to a polymerization reaction in the presence of a protective gas and an organic solvent to obtain the nano foam stabilizer.

[0036] The temperature-responsive nano foam stabilizer PDEA-PS latex particles developed by the present invention gradually changes the polydiethylacrylamide (PDEA) on its surface from a highly hydrated state to a dehydrated state as the temperature gradually increases. Therefore, when the temperature rises, the steric hindrance and repulsion caused by the hydration of the particle surface will be greatly reduced, and a flocculated state can be formed to be adsorbed on the gas / liquid interface of the bubbles to form a solidified film, thereby slowing down the aggregation and disproportionation between the bubbles and enhancing the foam stability.

[0037] In the present invention, diethylacrylamide (DEAA) is used as a reactant to make the prepared nano foam stabilizer have a colloidal particle structure, and can also be used as a macromolecular initiator to cooperate with the initiator to initiate the polymerization reaction.

[0038] According to the present invention, preferably, the preparation method further comprises: after the polymerization reaction is completed, centrifugal separation is performed to obtain the nano foam stabilizer.

[0039] According to the present invention, preferably, the centrifugal separation comprises:

[0040] (1) subjecting the product obtained from the polymerization reaction to a first centrifugation, dispersing the first centrifugation product into the organic solvent, and repeating the first centrifugation and dispersion steps multiple times;

[0041] (2) Dispersing the product treated in step (1) into water, and then performing a second centrifugation, dispersing the second centrifuged product into water again, and repeating the second centrifugation and re-dispersion steps multiple times.

[0042] According to the present invention, preferably, the centrifugal speed of the first centrifugation is 3500-5500 rpm, and the centrifugal time is 20-40 min;

[0043] The centrifugal speed of the second centrifugation is 8000-12000 rpm, and the centrifugal time is 20-40 min.

[0044] According to the present invention, preferably, the organic solvent is isopropanol;

[0045] The initiator is 2,2'-azo[2-methyl-N-(2-hydroxyethyl)propionamide];

[0046] The protective gas is nitrogen.

[0047] According to the present invention, preferably, the polymerization reaction temperature is 70 to 90° C., and the reaction time is 5 to 10 days;

[0048] The mass ratio of the diethylacrylamide, styrene and initiator is 4-10:5-9:0.3-1.8.

[0049] The second aspect of the present invention provides a temperature-responsive nano foam stabilizer prepared by the above preparation method.

[0050] The third aspect of the present invention provides a temperature-sensitive foaming agent, which comprises, based on the total weight of the temperature-sensitive foaming agent, 1 to 15 wt % of the temperature-responsive nano foam stabilizer, 20 to 45 wt % of dodecyl betaine (BS-12), 8 to 20 wt % of cocoyl propyl sulfobetaine (ASB), 5 to 10 wt % of sodium α-olefin sulfonate (AOS), 0.1 to 1.5 wt % of sodium dodecyl sulfonate, 0.1 to 0.5 wt % of octylphenol polyoxyethylene 10 ether (TX-10), 0.15 to 0.45 wt % of dodecyl dimethyl ammonium bromide, and the balance is water.

[0051] In the present invention, the preparation scheme of the temperature-sensitive foaming agent of the present invention is as follows: (1) in terms of foaming property, an anionic surfactant with a sulfonic acid group having strong foaming performance, significantly reducing surface tension, and being resistant to high temperatures is introduced, and at the same time, a zwitterionic surfactant that can form a good synergistic effect with the anionic surfactant is introduced to enhance the foaming property; (2) in terms of foam stability, a temperature-responsive nano foam stabilizer (PDEA-PS nanospheres) prepared by the above method is introduced as a nano foam stabilizer.

[0052] The foaming performance and foam stabilizing performance of the temperature-sensitive foaming agent developed by the present invention are significantly increased when the temperature is increased from 25°C to 80°C. As the temperature decreases again, the foaming performance and foam stabilizing performance will decrease again, and the foam will automatically burst. Therefore, the structure and stability of the foam can be adjusted by temperature.

[0053] The temperature-sensitive foaming agent of the present invention can be used in the fields of foam flooding for improving the recovery rate of oil and gas reservoirs and foam drainage and gas production, and can achieve a high foaming effect and foam stabilizing effect at formation temperature. When the foam fluid reaches the ground, the foam will automatically burst as the temperature decreases, which can save the step of adding defoaming agents in traditional processes, improve the efficiency of foam fluids, and expand the application scope of foam in the field of oil and gas development.

[0054] A fourth aspect of the present invention provides a method for preparing the temperature-sensitive foaming agent, the method comprising:

[0055] (1) stirring and mixing lauryl betaine and cocoyl propyl sulfobetaine to obtain a first mixed solution;

[0056] (2) stirring and mixing the first mixed solution, sodium α-olefin sulfonate and sodium dodecyl sulfonate to obtain a second mixed solution;

[0057] (3) adding water to the second mixed solution, then heating it, and finally adding octylphenol polyoxyethylene 10 ether and dodecyl dimethyl ammonium bromide and stirring and mixing them uniformly to obtain a third mixed solution;

[0058] (4) The third mixed solution and the temperature-responsive nano foam stabilizer are stirred and mixed uniformly to obtain the temperature-sensitive foaming agent.

[0059] According to the present invention, preferably, in step (1), the stirring speed is 800 to 2000 rpm, and the time is 10 to 40 min;

[0060] In step (2), the stirring and mixing temperature is 40 to 60° C., the stirring speed is 800 to 2000 rpm, and the time is 10 to 40 min;

[0061] In step (3), the heating temperature is 65-80° C., the stirring speed is 800-2000 rpm, and the time is 10-40 min;

[0062] In step (4), the stirring and mixing temperature is 40 to 60° C., the stirring speed is 800 to 2000 rpm, and the time is 10 to 40 min.

[0063] The present invention is further described below by examples:

[0064] The diethylacrylamide used in the following examples was purchased from Sigma-Aldrich Company; octylphenol polyoxyethylene 10 ether was purchased from Haian Petrochemical Company with a brand name of OP-10.

[0065] Example 1

[0066] The preparation method of the temperature-responsive nano foam stabilizer of this embodiment is as follows:

[0067] a. Pour 250 mL of isopropanol into a 500 mL single-mouth round-bottom flask, then add 4.45 g of DEAA (diethylacrylamide), 0.323 g of VA-086 (2,2'-azo[2-methyl-N-(2-hydroxyethyl)propionamide]), and 5.5 g of styrene to the isopropanol in sequence, and stir vigorously at room temperature (25°C) until all are dissolved;

[0068] b. The mixture obtained in step a was deoxygenated by nitrogen purging, placed in an oil bath at 70°C under nitrogen protection, and reacted at a low speed of 400 rpm for 10 days;

[0069] c. Centrifuge the product obtained in step b at 4000 rpm for 40 min, and disperse the centrifuged product into isopropanol. Repeat the centrifugation and dispersion process 3 times to remove unreacted substances and reaction by-products.

[0070] d. The product obtained in step c was dispersed in deionized water and centrifuged at 8000 rpm for 40 min, and the centrifuged product was dispersed in deionized water again. The centrifugation and re-dispersion process was repeated 3 times to obtain the target product PDEA-PS nanospheres (nano foam stabilizer).

[0071] Example 2

[0072] The preparation method of the temperature-responsive nano foam stabilizer of this embodiment is as follows:

[0073] a. Pour 250 mL of isopropanol into a 500 mL single-necked round-bottom flask, then add 5.45 g of DEAA (diethylacrylamide), 0.643 g of VA-086 (2,2'-azo[2-methyl-N-(2-hydroxyethyl)propionamide]), and 6.5 g of styrene to the isopropanol in sequence, and stir vigorously at room temperature (25°C) until all are dissolved;

[0074] b. The mixture obtained in step a was deoxygenated by nitrogen purging, placed in an oil bath at 75°C under nitrogen protection, and reacted at a low speed of 500 rpm for 9 days;

[0075] c. Centrifuge the product obtained in step b at 4500 rpm for 30 min, and disperse the centrifuged product into isopropanol. Repeat the centrifugation and dispersion process 3 times to remove unreacted substances and reaction by-products.

[0076] d. The product obtained in step c was dispersed in deionized water and centrifuged at 9000 rpm for 30 min, and the centrifuged product was dispersed in deionized water again. The centrifugation and re-dispersion process was repeated 3 times to obtain the target product PDEA-PS nanospheres (nano foam stabilizer).

[0077] Example 3

[0078] The preparation method of the temperature-responsive nano foam stabilizer of this embodiment is as follows:

[0079] a. Pour 250 mL of isopropanol into a 500 mL single-mouth round-bottom flask, then add 7.28 g of DEAA (diethylacrylamide), 1.382 g of VA-086 (2,2'-azo[2-methyl-N-(2-hydroxyethyl)propionamide]), and 7.6 g of styrene to the isopropanol in sequence, and stir vigorously at room temperature (25°C) until all are dissolved;

[0080] b. The mixture obtained in step a was deoxygenated by nitrogen purging, placed in an 80°C oil bath under nitrogen protection, and reacted at a low speed of 600 rpm for 7 days;

[0081] c. Centrifuge the product obtained in step b at 5000 rpm for 25 min, and disperse the centrifuged product into isopropanol. Repeat the centrifugation and dispersion process 3 times to remove unreacted substances and reaction by-products.

[0082] d. The product obtained in step c was dispersed in deionized water and centrifuged at 11000 rpm for 25 min, and the centrifuged product was dispersed in deionized water again. The centrifugation and re-dispersion process was repeated 3 times to obtain the target product PDEA-PS nanospheres (nano foam stabilizer).

[0083] Example 4

[0084] The preparation method of the temperature-responsive nano foam stabilizer of this embodiment is as follows:

[0085] a. Pour 250 mL of isopropanol into a 500 mL single-mouth round-bottom flask, then add 9.26 g of DEAA (diethylacrylamide), 1.66 g of VA-086 (2,2'-azo[2-methyl-N-(2-hydroxyethyl)propionamide]), and 8.8 g of styrene to the isopropanol in sequence, and stir vigorously at room temperature (25°C) until all are dissolved;

[0086] b. The mixture obtained in step a was deoxygenated by nitrogen purging, placed in an oil bath at 85°C under nitrogen protection, and reacted at a low speed of 700 rpm for 5.5 days;

[0087] c. Centrifuge the product obtained in step b at 5500 rpm for 20 min, and disperse the centrifuged product into isopropanol. Repeat the centrifugation and dispersion process 3 times to remove unreacted substances and reaction by-products.

[0088] d. The product obtained in step c was dispersed in deionized water and centrifuged at 11500 rpm for 20 min, and the centrifuged product was dispersed in deionized water again. The centrifugation and re-dispersion process was repeated 3 times to obtain the target product PDEA-PS nanospheres (nano foam stabilizer).

[0089] Example 5

[0090] The present embodiment provides a temperature-sensitive foaming agent, which is composed of the following components, based on the total weight of the temperature-sensitive foaming agent: 1wt% of a temperature-responsive nano foam stabilizer, 20wt% of dodecyl betaine, 8wt% of cocoyl propyl sulfobetaine, 5wt% of sodium α-olefin sulfonate, 0.1wt% of sodium dodecyl sulfonate, 0.1wt% of octylphenol polyoxyethylene 10 ether, 0.15wt% of dodecyl dimethyl ammonium bromide, and the balance is water.

[0091] The specific preparation method is as follows:

[0092] a. Slowly add dodecyl betaine (BS-12) and cocoyl propyl sulfobetaine (ASB) into a single-mouth round-bottom flask and stir at 2000 rpm for 10 min to obtain a first mixed solution;

[0093] b. Slowly add sodium α-olefin sulfonate (AOS) and sodium dodecyl sulfonate to the first mixed solution, heat the mixed solution to 40° C., and stir at 2000 rpm for 10 min to obtain a second mixed solution;

[0094] c. Add water to the second mixed solution, heat it to 65° C., add octylphenol polyoxyethylene 10 ether (TX-10) and dodecyl dimethyl ammonium bromide at one time, and stir at 2000 rpm for 10 min to obtain a third mixed solution;

[0095] d. Add the temperature-responsive PDEA-PS nanospheres to the third mixed solution at once, maintain the temperature at 40° C., and stir at 2000 rpm for 10 min. The resulting mixture is the temperature-sensitive foaming agent.

[0096] Example 6

[0097] The present embodiment provides a temperature-sensitive foaming agent, which is composed of the following components, based on the total weight of the temperature-sensitive foaming agent: 4wt% temperature-responsive nano foam stabilizer, 25wt% dodecyl betaine, 11wt% cocoyl propyl sulfobetaine, 6.5wt% sodium α-olefin sulfonate, 0.4wt% sodium dodecyl sulfonate, 0.2wt% octylphenol polyoxyethylene 10 ether, 0.25wt% dodecyl dimethyl ammonium bromide, and the balance is water.

[0098] The specific preparation method is as follows:

[0099] a. Slowly add dodecyl betaine (BS-12) and cocoyl propyl sulfobetaine (ASB) into a single-mouth round-bottom flask and stir at 1500 rpm for 15 min to obtain a first mixed solution;

[0100] b. Slowly add sodium α-olefin sulfonate (AOS) and sodium dodecyl sulfonate to the first mixed solution, heat the mixed solution to 45° C., and stir at 1500 rpm for 15 min to obtain a second mixed solution;

[0101] c. Add water to the second mixed solution, raise the temperature to 70° C., add octylphenol polyoxyethylene 10 ether (TX-10) and dodecyl dimethyl ammonium bromide at one time, and stir at 1500 rpm for 15 min to obtain a third mixed solution;

[0102] d. Add the temperature-responsive PDEA-PS nanospheres into the third mixed solution at once, keep the temperature at 45° C., and stir at 1500 rpm for 15 min. The resulting mixture is the temperature-sensitive foaming agent.

[0103] Example 7

[0104] The present embodiment provides a temperature-sensitive foaming agent, which is composed of the following components, based on the total weight of the temperature-sensitive foaming agent: 9wt% of a temperature-responsive nano foam stabilizer, 35wt% of dodecyl betaine, 15wt% of cocoyl propyl sulfobetaine, 8.5wt% of sodium α-olefin sulfonate, 0.9wt% of sodium dodecyl sulfonate, 0.35wt% of octylphenol polyoxyethylene 10 ether, 0.35wt% of dodecyl dimethyl ammonium bromide, and the balance is water.

[0105] The specific preparation method is as follows:

[0106] a. Slowly add dodecyl betaine (BS-12) and cocoyl propyl sulfobetaine (ASB) into a single-mouth round-bottom flask and stir at 1200 rpm for 25 min to obtain a first mixed solution;

[0107] b. Slowly add sodium α-olefin sulfonate (AOS) and sodium dodecyl sulfonate to the first mixed solution, heat the mixed solution to 50° C., and stir at 1200 rpm for 25 min to obtain a second mixed solution;

[0108] c. Add water to the second mixed solution, raise the temperature to 75° C., add octylphenol polyoxyethylene 10 ether (TX-10) and dodecyl dimethyl ammonium bromide at one time, and stir at 1200 rpm for 25 min to obtain a third mixed solution;

[0109] d. Add the temperature-responsive PDEA-PS nanospheres to the third mixed solution at once, maintain the temperature at 50° C., and stir at 1200 rpm for 25 min. The resulting mixture is the temperature-sensitive foaming agent.

[0110] Example 8

[0111] The present embodiment provides a temperature-sensitive foaming agent, which is composed of the following components, based on the total weight of the temperature-sensitive foaming agent: 14wt% of a temperature-responsive nano foam stabilizer, 45wt% of dodecyl betaine, 20wt% of cocoyl propyl sulfobetaine, 10wt% of sodium α-olefin sulfonate, 1.4wt% of sodium dodecyl sulfonate, 0.45wt% of octylphenol polyoxyethylene 10 ether, 0.45wt% of dodecyl dimethyl ammonium bromide, and the balance is water.

[0112] The specific preparation method is as follows:

[0113] a. Slowly add dodecyl betaine (BS-12) and cocoyl propyl sulfobetaine (ASB) into a single-mouth round-bottom flask and stir at 800 rpm for 40 min to obtain a first mixed solution;

[0114] b. Slowly add sodium α-olefin sulfonate (AOS) and sodium dodecyl sulfonate to the first mixed solution, heat the mixed solution to 60° C., and stir at 800 rpm for 40 min to obtain a second mixed solution;

[0115] c. Add water to the second mixed solution, heat it to 80° C., add octylphenol polyoxyethylene 10 ether (TX-10) and dodecyl dimethyl ammonium bromide at one time, and stir at 800 rpm for 40 min to obtain a third mixed solution;

[0116] d. Add the temperature-responsive PDEA-PS nanospheres into the third mixed solution at once, keep the temperature at 60° C., and stir at 800 rpm for 40 min. The resulting mixture is the temperature-sensitive foaming agent.

[0117] Test Case

[0118] In this test example, the foam performance evaluation of the foaming agent is achieved using a Roche foam tester, and the method is as follows:

[0119] Determination of foaming and foam stabilizing ability of foaming agents

[0120] 200mL of the test solution flows freely from the tube, and foam is generated after impacting 50mL of the same test solution in the tube. The foam height (initial bubble height) when 200mL of the test solution just flows and the foam height after 5 minutes are recorded, which are used to evaluate the foaming ability and foam stabilization ability of the foaming agent respectively. Each test is repeated 3 times and the average value is taken. Among them, the test solution is a test solution in which the mass concentration of the foaming agent is 0.3% by mixing the foaming agent to be tested with water.

[0121] The following describes the initial foaming height H0 and foam height H5 after 5 minutes of the temperature-sensitive foaming agents prepared in Examples 5 to 8 at different temperatures according to the above test method. At the same time, the foaming agents obtained according to the first three steps of Examples 5 to 8 (i.e., ordinary foaming agents without adding temperature-responsive PDEA-PS latex particles, respectively marked as foaming agent a, foaming agent b, foaming agent c, and foaming agent d) are tested to increase the comparison. The specific test results are shown in Tables 1 and 2.

[0122] Table 1: Foaming performance of temperature-sensitive foaming agents at different temperatures (foaming agent concentration 0.3%, mineralization degree 200000ppm)

[0123]

[0124]

[0125] Table 2: Foaming performance of common foaming agents at different temperatures (foaming agent concentration 0.3%, mineralization degree 200000ppm)

[0126]

[0127]

[0128] In summary, it can be seen from the experimental data in Table 1 and Table 2 that the initial foaming height H0 and the foam height H5 after 5 minutes of the temperature-sensitive foaming agent developed by the present invention will show a trend of gradual increase as the temperature increases, and the increase of H0 and H5 will be significantly improved when the temperature is higher than 40°C. In addition, for the temperature-sensitive foaming agents prepared in Examples 5 to 8, as the temperature increases, the decrease of H5 compared with H0 gradually decreases, and the foam stability gradually increases. This is because when the temperature gradually increases, the PDEA on the surface of the PDEA-PS latex particles gradually changes from a highly hydrated state to a dehydrated state. The higher the temperature, the higher the degree of dehydration. Therefore, when the temperature increases, its steric hindrance and repulsion will be greatly reduced, and a flocculated state can be formed to be adsorbed on the gas / liquid interface of the bubbles to form a solidified film, thereby slowing down the aggregation and disproportionation between the bubbles, thereby achieving the effect of enhancing the stability of the foam. By comparing the foam evaluation data of the common foaming agent without adding PDEA-PS latex particles, it can be seen that with the increase of temperature, its H0 and H5 do not change significantly with the increase of temperature, and its H5 has always decreased at a higher rate than H0. As the temperature decreases again, it can be seen that the foaming performance and foam stabilization performance of the temperature-sensitive foaming agent will decrease again, while the foam performance of the common foaming agent without adding the temperature-responsive nano foam stabilizer will not change with the temperature. In summary, it is proved that the temperature-responsive foam-stabilizing particles developed by the present invention have good temperature responsiveness.

[0129] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A method for preparing a temperature-responsive nano foam stabilizer, It is characterized in that The preparation method comprises: in the presence of protective gas and organic solvent, polymerizing diethyl acrylamide, styrene and an initiator to obtain the nano foam stabilizer; The mass ratio of diethyl acrylamide, styrene and initiator is 4-10:5-9:0.3-1.8; The organic solvent is isopropanol; The initiator is 2,2'-azo[2-methyl-N-(2-hydroxyethyl)propionamide].

2. The preparation method according to claim 1, in, The preparation method further comprises: after the polymerization reaction is completed, centrifugal separation is performed to obtain the nano foam stabilizer.

3. The preparation method according to claim 2, in, The centrifugal separation comprises: (1) subjecting the product obtained from the polymerization reaction to a first centrifugation, dispersing the first centrifugation product into the organic solvent, and repeating the first centrifugation and dispersion steps multiple times; (2) Dispersing the product treated in step (1) into water, and then performing a second centrifugation, dispersing the second centrifuged product into water again, and repeating the second centrifugation and re-dispersion steps multiple times.

4. The preparation method according to claim 3, in, The centrifugal speed of the first centrifugation is 3500-5500 rpm, and the centrifugal time is 20-40 min; The centrifugal speed of the second centrifugation is 8000-12000 rpm, and the centrifugal time is 20-40 min.

5. The preparation method according to claim 1, in, The protective gas is nitrogen.

6. The preparation method according to claim 1, in, The polymerization reaction temperature is 70-90° C., and the reaction time is 5-10 days.

7. A temperature-responsive nano foam stabilizer prepared by the preparation method according to any one of claims 1 to 6.

8. A temperature-sensitive foaming agent, It is characterized in that The temperature-sensitive foaming agent comprises, based on the total weight of the temperature-sensitive foaming agent, 1 to 15 wt % of the temperature-responsive nano foam stabilizer according to claim 7, 20 to 45 wt % of dodecyl betaine, 8 to 20 wt % of cocoyl propyl sulfobetaine, 5 to 10 wt % of sodium α-olefin sulfonate, 0.1 to 1.5 wt % of sodium dodecyl sulfonate, 0.1 to 0.5 wt % of octylphenol polyoxyethylene 10 ether, 0.15 to 0.45 wt % of dodecyl dimethyl ammonium bromide, and the balance is water.

9. The method for preparing the temperature-sensitive foaming agent according to claim 8, It is characterized in that The preparation method comprises: (1) stirring and mixing lauryl betaine and cocoyl propyl sulfobetaine to obtain a first mixed solution; (2) stirring and mixing the first mixed solution, sodium α-olefin sulfonate and sodium dodecyl sulfonate to obtain a second mixed solution; (3) adding water to the second mixed solution, then heating it, and finally adding octylphenol polyoxyethylene 10 ether and dodecyl dimethyl ammonium bromide and stirring and mixing them uniformly to obtain a third mixed solution; (4) The third mixed solution and the temperature-responsive nano foam stabilizer according to claim 7 are stirred and mixed uniformly to obtain the temperature-sensitive foaming agent.

10. The preparation method according to claim 9, in, In step (1), the stirring speed is 800 to 2000 rpm, and the time is 10 to 40 min; In step (2), the stirring and mixing temperature is 40 to 60° C., the stirring speed is 800 to 2000 rpm, and the time is 10 to 40 min; In step (3), the heating temperature is 65-80° C., the stirring speed is 800-2000 rpm, and the time is 10-40 min; In step (4), the stirring and mixing temperature is 40 to 60° C., the stirring speed is 800 to 2000 rpm, and the time is 10 to 40 min.

Citation Information

Patent Citations

  • Water-based foam stabilizer, preparation method of foam stabilizer and water-based foam system with ultrahigh stability

    CN103721625A

  • Temperature-sensitive-type intelligent nano particles used in drilling fluid and preparation method thereof

    CN105038728A

  • Preparation method of intelligent nano-foam oil-displacing agent

    CN108659807A

  • High-temperature foam stabilizer of giant surfactant and foaming liquid and preparation method and application of foaming liquid

    CN110698677A

  • Emulsion binder for formation of electrodes of nickel-hydrogen secondary batteries, and mixture ink for formation of electrodes of nickel-hydrogen secondary batteries

    JP2013110107A

Cited By

  • Dual response foam stabilizer and method of making same

    CN123026751A