A method for removing polysilicon from N-TOPCon cells
By performing corrosion-resistant treatment on the BPSG area during the preparation process of N-TOPCon batteries, the battery corrosion problem caused by phosphorus diffusion is solved and the appearance and performance of the battery are improved.
Patent Information
- Application Number
- CN202111011327.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-08-31
AI Technical Summary
During the preparation process of N-TOPCon batteries, during the removal of the wraparound polysilicon caused by phosphorus diffusion, the BPSG area on the front side of the silicon wafer was corroded by hydrofluoric acid and alkali, affecting the appearance and performance of the battery.
Before de-plating, the BPSG area is treated to resist corrosion, and its density is improved through secondary annealing or BPSG is replaced with BSG to enhance its acid and alkali resistance, thereby preventing corrosion during the de-plating process.
It effectively prevents the BPSG area on the front side of the silicon wafer from being corroded during dewinding plating, improves the appearance of the battery, and increases the short-circuit current, open-circuit voltage, fill factor and battery efficiency.
Smart Images

Figure CN113948608B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of N-TOPCon cells, and in particular to a method for removing plated polysilicon of an N-TOPCon cell. Background Art
[0002] N-type tunneling oxide passivated contact (N-TOPCon) cells refer to a type of cell that is passivated by tunneling oxide and doped polysilicon. Its passivation mechanism is: ultra-thin silicon oxide directly contacts the silicon substrate, neutralizes the dangling bonds on the silicon surface, and performs excellent chemical passivation: the heavily doped polysilicon layer causes band bending on the surface of the silicon substrate due to the difference in Fermi energy level with the silicon substrate, which can more effectively block the passage of minority carriers without affecting the transmission of majority carriers, thereby achieving selective collection of carriers. Compared with traditional PERC cells, N-TOPCon cells have a full-area passivated back surface, and there is no direct contact between metal and silicon, which is conducive to improving the short-circuit voltage of the battery, comprehensively collecting carriers, reducing life sensitivity, and helping to improve the fill factor, which has a positive role in promoting industrial upgrading.
[0003] In the preparation process of N-TOPCon cells, intrinsic amorphous silicon is usually deposited first, and then the amorphous silicon is phosphorus-doped and annealed to form doped polysilicon. In this process, since the industry currently generally uses the APCVD / LPCVD method to deposit intrinsic amorphous silicon, there is often a certain width of wrapped amorphous silicon on the front, which is converted into polysilicon after phosphorus-doped annealing. Since the polysilicon layer has a high absorption coefficient, once it appears on the front of the battery, it will affect the absorption of sunlight on the front of the battery. At the same time, the conductivity of polysilicon will cause serious leakage at the edge of the battery. Therefore, de-wrapping treatment is required in the preparation process of N-TOPCon cells.
[0004] At present, the method of removing the plated polysilicon is usually alkaline solution treatment. For example, patent CN202010667851.7 discloses a method and application for removing the plated polysilicon of TOPCon cells, in which the method of removing the plated polysilicon is: after the amorphous silicon layer is crystallized into a phosphorus-doped polysilicon layer by phosphorus diffusion annealing, the PSG on the surface of the plated polysilicon layer located on the front and side of the silicon substrate is removed by hydrofluoric acid water bleaching, and then the plated polysilicon layer located on the front and side of the silicon substrate is removed by alkaline solution etching. Although this method can remove the polysilicon that has been plated and prevent it from affecting the performance of the battery, it also has the following problems: during the phosphorus deposition process after the amorphous silicon is deposited, the phosphorus diffusion plating width on the front side of the silicon wafer is often greater than the plating width of the amorphous silicon, thereby forming a P-BSG-rich region of a certain width in the contact area between the amorphous silicon and the borosilicate glass (BSG), namely the borophosphosilicate glass (BPSG) region. The BPSG region will be severely corroded by hydrofluoric acid and alkaline solution during the de-plating process, affecting the appearance of the battery and adversely affecting the battery performance (including short-circuit current, open-circuit voltage, fill factor and battery efficiency). Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for removing the polysilicon wrapped around the N-TOPCon cell. The method can prevent the BPSG area on the front side of the silicon wafer from being corroded during the de-wrapping process by adding a BPSG corrosion resistance treatment step before de-wrapping, thereby obtaining a better cell appearance and enabling the cell to have better performance.
[0006] The specific technical scheme of the present invention is:
[0007] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0008] (1) Boron doping is performed on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0009] (2) Remove the borosilicate glass (BSG) and diffusion junction on the back of the boron-doped silicon wafer and retain the borosilicate glass on the front;
[0010] (3) depositing a tunnel oxide layer and intrinsic amorphous silicon on the back side of the silicon wafer after removing the borosilicate glass and diffusion junction on the back side;
[0011] (4) performing phosphorus deposition on intrinsic amorphous silicon to obtain a phosphorus-deposited silicon wafer;
[0012] (5) Phosphorus doping and borophosphosilicate glass (BPSG) corrosion resistance treatment of phosphorus deposited silicon wafers;
[0013] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with hydrofluoric acid solution and alkaline solution in turn, thereby completing the removal of the plated polysilicon.
[0014] During the preparation of N-TOPCon cells, when depositing intrinsic amorphous silicon, amorphous silicon will be formed on the front of the cell. The inventors found that during the subsequent phosphorus deposition process, the phosphorus diffusion on the front of the silicon wafer is often larger than the amorphous silicon. Therefore, a BPSG area of a certain width will be formed in the contact area between the amorphous silicon and the BSG. Since BPSG has poor acid and alkali resistance, it will be corroded by hydrofluoric acid and alkali solution during the subsequent de-plating process, resulting in poor appearance of the cell.
[0015] In view of the above technical problems, the present invention performs corrosion resistance treatment on BPSG after phosphorus deposition to improve its acid and alkali resistance, and then uses hydrofluoric acid to remove PSG on the surface of the plated polysilicon, and uses alkaline solution to remove the plated polysilicon. This can prevent the BPSG area on the front side of the silicon wafer from being corroded during the de-plating process, improve the appearance of the battery, and enable the battery to have higher short-circuit current, open-circuit voltage, fill factor and battery efficiency.
[0016] Preferably, in step (5), the phosphorus doping and corrosion resistance treatment can be achieved by scheme A or scheme B, and the specific process includes the following steps:
[0017] Solution A: Perform a first anneal on the phosphorus deposited silicon wafer to complete phosphorus doping and amorphous silicon crystallization; perform a second anneal on the silicon wafer after the first anneal in a nitrogen atmosphere to reduce the concentration of phosphorus in the borophosphosilicate glass and make the regional network structure of the borophosphosilicate glass more compact;
[0018] Solution B: Remove the phosphosilicate glass on the front side of the phosphorus-deposited silicon wafer, and then perform phosphorus doping and amorphous silicon crystallization.
[0019] In scheme A, during the secondary annealing process, the mobility of phosphorus in SiO2 increases and precipitates on the surface, thereby reducing the concentration of phosphorus in BPSG, thereby improving the compactness of BPSG and making it more resistant to acid and alkali corrosion. The secondary annealing process is carried out in a nitrogen atmosphere. The purpose is that the annealing atmosphere affects the mobility of boron and phosphorus in silicon dioxide. When annealing in N2, B has poor mobility in silicon dioxide, while P has high mobility and tends to be enriched on the silicon surface.
[0020] In scheme B, after removing the PSG on the front side, phosphorus doping and amorphous silicon crystallization are performed, which can reduce the concentration of P on the front side of the silicon wafer in the BSG area, and prevent the P on the front side of the silicon wafer from eroding the BSG area and forming BPSG during the subsequent phosphorus doping process. After removing the PSG on the front side, BSG is retained on the front side, and BSG has higher acid and alkali resistance than BPSG, thus preventing it from being corroded during de-plating.
[0021] Preferably, in scheme A, the temperature of the primary annealing is 800-850°C.
[0022] Preferably, in scheme A, the temperature of the secondary annealing is 850-1000° C., and the time is 10-50 min.
[0023] If the secondary annealing temperature is too low or the time is too short, it will be difficult to improve the density of BPSG; if the secondary annealing temperature is too high or the time is too long, the P plated on the front side will penetrate the BSG deep into the silicon substrate, affecting the quality of the PN junction.
[0024] Preferably, in Scheme B, a hydrofluoric acid solution with a concentration of 0.5 to 3 wt % is used to remove the borophosphosilicate glass on the front side of the phosphorus-deposited silicon wafer.
[0025] In the process of removing PSG, if the concentration of the hydrofluoric acid solution used is too low, the PSG glass cannot be removed; if the concentration of the hydrofluoric acid solution used is too high, the BSG will be washed away and easily corroded during subsequent de-plating.
[0026] Preferably, in scheme B, the temperature of phosphorus doping and amorphous silicon crystallization is 800-1000° C., and the time is 5-60 min.
[0027] Preferably, in step (4), the phosphorus deposition temperature is 750-850° C., the time is 20-50 min, and the phosphorus source flow rate is 1000-4000 sccm.
[0028] Preferably, in step (6), the concentration of the hydrofluoric acid solution is 3 to 10 wt %.
[0029] Preferably, in step (6), the alkali solution is a NaOH solution, a KOH solution or a tetramethylammonium hydroxide (TMAH) solution, and the concentration is 3 to 15 wt%.
[0030] Preferably, in step (2), a chain single-sided etching method is used to remove the borosilicate glass and the diffusion junction on the back side of the boron-doped silicon wafer.
[0031] Compared with the prior art, the present invention has the following advantages: the present invention improves the corrosion resistance of BPSG on the front side of the silicon wafer by improving the compactness of BPSG through secondary annealing (Scheme A) or replacing BPSG with BSG (Scheme B), can prevent it from being corroded by hydrofluoric acid and alkali solution during the de-plating process, improves the appearance of the battery, and enables the N-TOPCon battery to have higher short-circuit current, open-circuit voltage, fill factor and battery efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a front photo of the silicon wafer obtained in Example 1;
[0033] Figure 2 This is a front photo of the silicon wafer obtained in Comparative Example 1. DETAILED DESCRIPTION
[0034] The present invention will be further described below in conjunction with the embodiments.
[0035] Overall embodiment
[0036] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0037] (1) Boron doping is performed on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0038] (2) removing the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer and retaining the borosilicate glass on the front;
[0039] (3) depositing a tunnel oxide layer and intrinsic amorphous silicon on the back side of the silicon wafer after removing the borosilicate glass and diffusion junction on the back side;
[0040] (4) depositing phosphorus on the intrinsic amorphous silicon at a temperature of 750 to 850° C. and a phosphorus source flow rate of 1000 to 4000 sccm for 20 to 50 minutes to obtain a phosphorus deposited silicon wafer;
[0041] (5) Phosphorus doping and corrosion resistance treatment:
[0042] Solution A: The phosphorus-deposited silicon wafer is subjected to a primary annealing at 800-850°C to complete phosphorus doping and amorphous silicon crystallization; the silicon wafer after the primary annealing is subjected to a secondary annealing at 850-1000°C for 10-50 minutes in a nitrogen atmosphere to reduce the concentration of phosphorus in the borophosphosilicate glass and make the regional network structure of the borophosphosilicate glass more compact;
[0043] Solution B: using a hydrofluoric acid solution with a concentration of 0.5-3wt% to remove the phosphosilicate glass on the front side of the phosphorus-deposited silicon wafer, and then performing phosphorus doping and amorphous silicon crystallization at 800-1000°C for 5-60 minutes;
[0044] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with 3-10wt% hydrofluoric acid solution and 3-15wt% alkaline solution in sequence, wherein the alkaline solution is NaOH solution, KOH solution or TMAH solution, thereby completing the removal of the plated polysilicon.
[0045] Example 1
[0046] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0047] (1) Boron is doped by diffusion on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0048] (2) Using a chain single-sided etching method to remove the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer, and retain the borosilicate glass on the front;
[0049] (3) using LPCVD equipment to deposit a tunnel oxide layer and intrinsic amorphous silicon on the back side of the etched silicon wafer;
[0050] (4) performing phosphorus deposition on the intrinsic amorphous silicon at a temperature of 750° C. and a phosphorus source flow rate of 1000 sccm for 50 minutes to obtain a phosphorus deposited silicon wafer;
[0051] (5) annealing the phosphorus deposited silicon wafer at 800° C. to complete phosphorus doping and amorphous silicon crystallization; annealing the silicon wafer after the primary annealing at 850° C. for 50 min in a nitrogen atmosphere to reduce the concentration of phosphorus in the borophosphosilicate glass and make the regional network structure of the borophosphosilicate glass more compact;
[0052] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with a 3 wt % hydrofluoric acid solution and a 15 wt % TMAH solution in turn, thus completing the removal of the coated polysilicon. Figure 1 shown.
[0053] Example 2
[0054] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0055] (1) Boron is doped by diffusion on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0056] (2) Using a chain single-sided etching method to remove the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer, and retain the borosilicate glass on the front;
[0057] (3) using LPCVD equipment to deposit a tunnel oxide layer and intrinsic amorphous silicon on the back side of the etched silicon wafer;
[0058] (4) performing phosphorus deposition on intrinsic amorphous silicon at a temperature of 800° C. and a phosphorus source flow rate of 2500 sccm for 35 minutes to obtain a phosphorus-deposited silicon wafer;
[0059] (5) annealing the phosphorus-deposited silicon wafer at 800° C. to complete phosphorus doping and amorphous silicon crystallization; annealing the silicon wafer after the primary annealing at 930° C. for 30 min in a nitrogen atmosphere to reduce the concentration of phosphorus in the borophosphosilicate glass and make the regional network structure of the borophosphosilicate glass more compact;
[0060] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with 10 wt % hydrofluoric acid solution and 3 wt % NaOH solution in turn, thereby completing the removal of the plated polysilicon.
[0061] Example 3
[0062] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0063] (1) Boron is doped by diffusion on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0064] (2) Using a chain single-sided etching method to remove the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer, and retain the borosilicate glass on the front;
[0065] (3) using LPCVD equipment to deposit a tunnel oxide layer and intrinsic amorphous silicon on the back side of the etched silicon wafer;
[0066] (4) depositing phosphorus on the intrinsic amorphous silicon at a temperature of 850° C. and a phosphorus source flow rate of 4000 sccm for 20 minutes, so as to form a P-rich layer on the surface of the amorphous silicon to obtain a phosphorus-deposited silicon wafer;
[0067] (5) annealing the phosphorus deposited silicon wafer at 850° C. to complete phosphorus doping and amorphous silicon crystallization; annealing the silicon wafer after the primary annealing at 1000° C. for 10 min in a nitrogen atmosphere to reduce the concentration of phosphorus in the borophosphosilicate glass and make the regional network structure of the borophosphosilicate glass more compact;
[0068] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with 7wt% hydrofluoric acid solution and 5wt% KOH solution in turn, thereby completing the removal of the plated polysilicon.
[0069] Example 4
[0070] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0071] (1) Boron is doped by diffusion on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0072] (2) Using a chain single-sided etching method to remove the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer, and retain the borosilicate glass on the front;
[0073] (3) using LPCVD equipment to deposit a tunnel oxide layer and intrinsic amorphous silicon on the back side of the etched silicon wafer;
[0074] (4) depositing phosphorus on the intrinsic amorphous silicon at a temperature of 750° C. and a phosphorus source flow rate of 1000 sccm for 50 minutes, so as to form a P-rich layer on the surface of the amorphous silicon, thereby obtaining a phosphorus-deposited silicon wafer;
[0075] (5) using a 0.5 wt % hydrofluoric acid solution to remove the phosphosilicate glass on the front side of the phosphorus-deposited silicon wafer, and then placing the silicon wafer in a high-temperature furnace to perform phosphorus doping and amorphous silicon crystallization at 800° C. for 60 min;
[0076] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with 3 wt % hydrofluoric acid solution and 15 wt % TMAH solution in turn, thereby completing the removal of the plated polysilicon.
[0077] Example 5
[0078] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0079] (1) Boron is doped by diffusion on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0080] (2) Using a chain single-sided etching method to remove the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer, and retain the borosilicate glass on the front;
[0081] (3) using LPCVD equipment to deposit a tunnel oxide layer and intrinsic amorphous silicon on the back side of the etched silicon wafer;
[0082] (4) depositing phosphorus on the intrinsic amorphous silicon at a temperature of 800° C. and a phosphorus source flow rate of 2500 sccm for 35 minutes, so as to form a P-rich layer on the surface of the amorphous silicon to obtain a phosphorus-deposited silicon wafer;
[0083] (5) using a 1.5 wt % hydrofluoric acid solution to remove the phosphosilicate glass on the front side of the phosphorus-deposited silicon wafer, and then placing the silicon wafer in a high-temperature furnace to perform phosphorus doping and amorphous silicon crystallization at 1000° C. for 5 min;
[0084] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with 10 wt % hydrofluoric acid solution and 3 wt % NaOH solution in turn, thereby completing the removal of the plated polysilicon.
[0085] Example 6
[0086] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0087] (1) Boron is doped by diffusion on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0088] (2) Using a chain single-sided etching method to remove the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer, and retain the borosilicate glass on the front;
[0089] (3) using LPCVD equipment to deposit a tunnel oxide layer and intrinsic amorphous silicon on the back side of the etched silicon wafer;
[0090] (4) depositing phosphorus on the intrinsic amorphous silicon at a temperature of 850° C. and a phosphorus source flow rate of 4000 sccm for 20 minutes, so as to form a P-rich layer on the surface of the amorphous silicon to obtain a phosphorus-deposited silicon wafer;
[0091] (5) using a 3 wt % hydrofluoric acid solution to remove the phosphosilicate glass on the front side of the phosphorus-deposited silicon wafer, and then placing the silicon wafer in a high-temperature furnace to perform phosphorus doping and amorphous silicon crystallization at 850° C. for 30 min;
[0092] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with 7wt% hydrofluoric acid solution and 5wt% KOH solution in turn, thereby completing the removal of the plated polysilicon.
[0093] Comparative Example 1
[0094] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0095] (1) Boron is doped by diffusion on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0096] (2) Using a chain single-sided etching method to remove the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer, and retain the borosilicate glass on the front;
[0097] (3) using LPCVD equipment to deposit a tunnel oxide layer and intrinsic amorphous silicon on the back side of the etched silicon wafer;
[0098] (4) depositing phosphorus on the intrinsic amorphous silicon at a temperature of 850° C. and a phosphorus source flow rate of 4000 sccm for 20 minutes, so as to form a P-rich layer on the surface of the amorphous silicon to obtain a phosphorus-deposited silicon wafer;
[0099] (5) annealing the phosphorus deposited silicon wafer at 850° C. to complete phosphorus doping and amorphous silicon crystallization;
[0100] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with 7 wt% hydrofluoric acid solution and 5 wt% KOH solution in turn, thus completing the removal of the plated polysilicon. Figure 2 shown.
[0101] Comparative Example 2
[0102] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0103] (1) Boron is doped by diffusion on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0104] (2) Using a chain single-sided etching method to remove the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer, and retain the borosilicate glass on the front;
[0105] (3) using LPCVD equipment to deposit a tunnel oxide layer and intrinsic amorphous silicon on the back side of the etched silicon wafer;
[0106] (4) performing phosphorus deposition on the intrinsic amorphous silicon at a temperature of 750° C. and a phosphorus source flow rate of 1000 sccm for 50 minutes to obtain a phosphorus deposited silicon wafer;
[0107] (5) annealing the phosphorus deposited silicon wafer at 800° C. to complete phosphorus doping and amorphous silicon crystallization; annealing the silicon wafer after the primary annealing at 800° C. for 50 min in a nitrogen atmosphere to reduce the concentration of phosphorus in the borophosphosilicate glass and make the regional network structure of the borophosphosilicate glass more compact;
[0108] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with 3 wt % hydrofluoric acid solution and 15 wt % TMAH solution in turn, thereby completing the removal of the plated polysilicon.
[0109] Comparative Example 3
[0110] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0111] (1) Boron is doped by diffusion on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0112] (2) Using a chain single-sided etching method to remove the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer, and retain the borosilicate glass on the front;
[0113] (3) using LPCVD equipment to deposit a tunnel oxide layer and intrinsic amorphous silicon on the back side of the etched silicon wafer;
[0114] (4) depositing phosphorus on the intrinsic amorphous silicon at a temperature of 850° C. and a phosphorus source flow rate of 4000 sccm for 20 minutes, so as to form a P-rich layer on the surface of the amorphous silicon to obtain a phosphorus-deposited silicon wafer;
[0115] (5) annealing the phosphorus deposited silicon wafer at 850° C. to complete phosphorus doping and amorphous silicon crystallization; annealing the silicon wafer after the primary annealing at 1050° C. for 10 min in a nitrogen atmosphere to reduce the concentration of phosphorus in the borophosphosilicate glass and make the regional network structure of the borophosphosilicate glass more compact;
[0116] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with a 10 wt % hydrofluoric acid solution and a 3 wt % KOH solution in turn, thereby completing the removal of the plated polysilicon.
[0117] Comparative Example 4
[0118] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0119] (1) Boron is doped by diffusion on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0120] (2) Using a chain single-sided etching method to remove the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer, and retain the borosilicate glass on the front;
[0121] (3) using LPCVD equipment to deposit a tunnel oxide layer and intrinsic amorphous silicon on the back side of the etched silicon wafer;
[0122] (4) depositing phosphorus on the intrinsic amorphous silicon at a temperature of 750° C. and a phosphorus source flow rate of 1000 sccm for 50 minutes, so as to form a P-rich layer on the surface of the amorphous silicon, thereby obtaining a phosphorus-deposited silicon wafer;
[0123] (5) using a hydrofluoric acid solution with a concentration of 0.1 wt% to remove the phosphosilicate glass on the front side of the phosphorus-deposited silicon wafer, and then placing the silicon wafer in a high-temperature furnace for phosphorus doping and amorphous silicon crystallization at 800° C. for 60 min;
[0124] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with 3 wt % hydrofluoric acid solution and 15 wt % TMAH solution in turn, thereby completing the removal of the plated polysilicon.
[0125] Comparative Example 5
[0126] A method for removing the polysilicon of an N-TOPCon cell comprises the following steps:
[0127] (1) Boron is doped by diffusion on the surface of the N-type silicon wafer after texturing to form a PN junction;
[0128] (2) Using a chain single-sided etching method to remove the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer, and retain the borosilicate glass on the front;
[0129] (3) using LPCVD equipment to deposit a tunnel oxide layer and intrinsic amorphous silicon on the back side of the etched silicon wafer;
[0130] (4) depositing phosphorus on the intrinsic amorphous silicon at a temperature of 850° C. and a phosphorus source flow rate of 4000 sccm for 20 minutes, so as to form a P-rich layer on the surface of the amorphous silicon to obtain a phosphorus-deposited silicon wafer;
[0131] (5) using a 4 wt % hydrofluoric acid solution to remove the phosphosilicate glass on the front side of the phosphorus-deposited silicon wafer, and then placing the silicon wafer in a high-temperature furnace to perform phosphorus doping and amorphous silicon crystallization at 1000° C. for 5 min;
[0132] (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with a 10 wt % hydrofluoric acid solution and a 3 wt % KOH solution in turn, thereby completing the removal of the plated polysilicon.
[0133] Test Case
[0134] The surfaces of the silicon wafers obtained in Examples 1 to 6 and Comparative Examples 1 to 5 were observed, and it was found that the front sides of the silicon wafers in Examples 1 to 6 and Comparative Example 3 were relatively smooth without corrosion; while the front sides of the silicon wafers in Comparative Examples 1, 2, 4 and 5 were corroded and had poor appearance.
[0135] After the removal of the plated polysilicon was completed by the methods of Examples 1 to 6 and Comparative Examples 1 to 5, a passivation layer was formed on the front and back sides of the silicon wafer by conventional methods, and screen printing and sintering were performed to produce N-TOPCon cells. The performance of the N-TOPCon cells was tested and the relative values were calculated. The results are shown in Table 1.
[0136] Table 1
[0137] Open circuit voltage Voc Short circuit current Isc Fill Factor FF Battery efficiency Eff Example 1 1.0008 1.0009 1.0073 1.0090 Example 2 1 1.0004 1.0048 1.0052 Example 3 0.9999 1.0004 1.0001 1.0004 Example 4 1.0037 1.0019 1.0098 1.0155 Example 5 1.0026 1.0018 1.0007 1.0048 Example 6 1.0001 1.0005 1.0001 1.0007 Comparative Example 1 1 1 1 1 Comparative Example 2 0.9997 0.9998 0.9995 0.9990 Comparative Example 3 0.9969 0.9988 0.9995 0.9952 Comparative Example 4 1.0002 0.9997 0.9998 0.9997 Comparative Example 5 0.9999 0.9997 0.9998 0.9994
[0138] Analyzing the data in Table 1, we can draw the following conclusions:
[0139] (1) Comparative Example 1 did not use the method of the present invention to perform corrosion resistance treatment on borophosphosilicate glass before de-coating. During the de-coating process, corrosion occurred in the BPSG area on the front of the silicon wafer; while no corrosion occurred on the front of the silicon wafer obtained in Examples 3 and 6. In addition, it can be seen from Table 1 that the N-TOPCon battery made of the silicon wafer finally obtained in Comparative Example 1 has lower open circuit voltage, short circuit current, fill factor and battery efficiency than Examples 3 and 6. This shows that the present invention can prevent the BPSG area on the front of the silicon wafer from being corroded during de-coating by adding a step of corrosion resistance treatment of BPSG before de-coating, thereby obtaining a better battery appearance and making the battery have better performance.
[0140] (2) The secondary annealing temperatures in Example 1 and Comparative Example 2 are 850°C and 800°C, respectively, and the rest of the processes are the same. Corrosion occurs on the front side of the silicon wafer obtained in Comparative Example 2; and, as can be seen from Table 1, the performance of the N-TOPCon cell made using the silicon wafer of Comparative Example 2 is lower than that of Example 1. This is because when the secondary annealing temperature is too low, it is difficult to improve the compactness of BPSG.
[0141] (3) The annealing temperatures in Example 3 and Comparative Example 3 are 1000°C and 1050°C respectively, and the rest of the processes are the same. As can be seen from Table 1, the performance of the N-TOPCon cell made using the silicon wafer of Comparative Example 3 is lower than that of Example 3. This is because when the secondary annealing temperature is too high, the P plated on the front side will penetrate the BSG deep into the silicon substrate, affecting the quality of the PN junction.
[0142] (4) The concentrations of the hydrofluoric acid solution used in step (5) of Example 4 and Comparative Example 4 are 0.5wt% and 0.1wt%, respectively, and the rest of the process is the same. Corrosion occurs on the front side of the silicon wafer obtained in Comparative Example 4; and, as can be seen from Table 1, the performance of the N-TOPCon cell made using the silicon wafer of Comparative Example 4 is lower than that of Example 4. This is because when the concentration of the hydrofluoric acid solution used after phosphorus deposition is too low, the PSG on the front side is not completely removed, resulting in the generation of BPSG in the subsequent phosphorus doping process, which causes corrosion during de-plating.
[0143] (5) The concentrations of the hydrofluoric acid solution used in step (5) of Example 6 and Comparative Example 5 are 3wt% and 4wt%, respectively, and the rest of the process is the same. As can be seen from Table 1, the performance of the N-TOPCon cell made using the silicon wafer of Comparative Example 5 is significantly lower than that of Example 6. This is because when removing the PSG on the front side, the HF concentration is too high, which will cause the BSG to be washed away and easily corroded during the subsequent de-plating.
[0144] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0145] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for removing polysilicon from an N-TOPCon cell, characterized in that: The following steps are involved: (1) Boron doping is performed on the surface of the N-type silicon wafer after texturing to form a PN junction; (2) removing the borosilicate glass and diffusion junction on the back of the boron-doped silicon wafer and retaining the borosilicate glass on the front; (3) depositing a tunnel oxide layer and intrinsic amorphous silicon on the back side of the silicon wafer after removing the borosilicate glass and diffusion junction on the back side; (4) performing phosphorus deposition on intrinsic amorphous silicon to obtain a phosphorus-deposited silicon wafer; (5) performing phosphorus doping and borophosphosilicate glass corrosion resistance treatment on the phosphorus deposited silicon wafer, the specific process includes the following steps: performing a first annealing on the phosphorus deposited silicon wafer to complete phosphorus doping and amorphous silicon crystallization; In a nitrogen atmosphere, the silicon wafer after the primary annealing is subjected to a secondary annealing to reduce the concentration of phosphorus in the borophosphosilicate glass and make the regional network structure of the borophosphosilicate glass more dense; (6) The front side of the silicon wafer after the corrosion resistance treatment is cleaned with hydrofluoric acid solution and alkaline solution in turn, thereby completing the removal of the plated polysilicon.
2. The method for removing the coated polysilicon as claimed in claim 1, wherein: In step (5), the temperature of the primary annealing is 800-850°C.
3. The method for removing the coated polysilicon as claimed in claim 1, characterized in that: In step (5), the secondary annealing is performed at a temperature of 850 to 1000° C. and for a time of 10 to 50 minutes.
4. The method for removing the coated polysilicon as claimed in claim 1, characterized in that: In step (4), the phosphorus deposition temperature is 750-850° C., the time is 20-50 min, and the phosphorus source flow rate is 1000-4000 sccm.
5. The method for removing the coated polysilicon as claimed in claim 1, characterized in that: In step (6), the concentration of the hydrofluoric acid solution is 3 to 10 wt %.
6. The method for removing the coated polysilicon as claimed in claim 1, characterized in that: In step (6), the alkali solution is a NaOH solution, a KOH solution or a tetramethylammonium hydroxide solution, and the concentration is 3 to 15 wt%.
7. The method for removing the coated polysilicon as claimed in claim 1, characterized in that: In step (2), a chain single-sided etching method is used to remove the borosilicate glass and the diffusion junction on the back side of the boron-doped silicon wafer.