A combined screw of a twin-screw extruder and a process for producing low-odor polyolefin
By designing a specific combined screw structure and process flow in a twin-screw extruder, the problem of poor vacuum devolatility is solved, and the production of low-odor polyolefins is achieved, which simplifies the process flow and reduces costs.
Patent Information
- Application Number
- CN202111418831.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-11-26
AI Technical Summary
The existing twin-screw extruders have poor results in vacuum devolatility, especially for high-melt finger substances, which are difficult to effectively remove volatiles, affecting the odor and quality of the product.
A combined screw structure is designed, including a reflux element, a kneading element and a conveying element. Through the arrangement and combination of threaded elements, the exhaust time of the melt is extended, and the volatiles discharge effect of the exhaust port is increased. The vacuum exhaust port and The combination of natural exhaust ports, combined with appropriate temperature and speed control, adjust the feed and vacuum degree to achieve the production of low-odor polyolefins.
It achieves simple and easy extension of the exhaust time of the melt, enhances the volatile discharge effect of the exhaust port, reduces the product odor and volatile content, and does not require new exhaust ports or equipment, and is low in cost.
Smart Images

Figure CN113977908B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of screw extruders, in particular to a combined screw of a twin-screw extruder and a process for producing low-odor polyolefin. Background Art
[0002] Chinese patent CN201520053U discloses a combined screw for a twin-screw extruder, the upstream side of which includes a conveying part, a mixing and compression part and an extrusion part in sequence, the conveying part is provided with a feeding position corresponding to the feeding port of the external extruder, the extrusion part is provided with an exhaust position corresponding to the exhaust port of the external extruder, and a distance between the feeding position and the exhaust position is provided with a plurality of screw elements and kneading elements arranged in a certain order according to the discharge direction. The patent increases the compression ratio of the compression section by adding some screw elements with long lead and short pitch, which is beneficial to the negative pressure extraction of volatiles. The method of adding some screw elements with long lead and short pitch has a certain effect on increasing the compression ratio of the compression section, but the effect of removing volatiles from the vacuum devolatilization port located in the extrusion section is not ideal, especially for high melt index (MFI>300) materials prepared by peroxide degradation method, because they have good fluidity and contain a lot of volatiles, and the requirements for vacuum devolatilization effect are higher. Summary of the invention
[0003] In view of this, the object of the present invention is to provide a simple, low-cost twin-screw extruder combined screw and a process for producing low-odor polyolefins, which prolongs the exhaust time of the melt and enhances the effect of exhausting volatiles from the exhaust port.
[0004] The present invention is implemented by the following scheme: a combined screw of a twin-screw extruder, comprising a barrel and a screw located in the barrel, wherein a main material port is provided at the rear end of the barrel, a vacuum exhaust port is provided near the front end of the barrel, and a natural exhaust port is provided behind the vacuum exhaust port; a reverse flow element is provided at the rear position of the screw near the vacuum exhaust port, a kneading element B is provided at the rear position of the screw near the natural exhaust port, and a plurality of continuous kneading elements A and a plurality of continuous conveying elements are sequentially provided on the screw from front to back between the reverse flow element and the kneading element B.
[0005] Furthermore, the reverse flow element has one thread layer, a length of 10 mm, a helix angle of 67°, and a thread direction opposite to that of the conveying element.
[0006] Furthermore, the lengths of the kneading element A and the kneading element B are both 30 mm, and the kneading element A and the kneading element B are both provided with three layers of spiral plates, the planes where the spiral plates are located are perpendicular to the axis of the screw, each layer of spiral plates is 10 mm thick, and the circumferential angles between two adjacent layers of spiral plates are staggered at 0°, 30°, 60° or 90°.
[0007] Furthermore, the length of the conveying element is 90 mm, the helix angle is 71°, the number of thread layers is 5, and the width of each layer is 18 mm, or the number of thread layers is 9, and the width of each layer is 10 mm.
[0008] Furthermore, the aspect ratio of the screw is 44.
[0009] Furthermore, the distance between the vacuum exhaust port and the natural exhaust port is 4 to 8 times the screw diameter.
[0010] Another technical solution of the present invention:
[0011] A process for producing low-odor polyolefins, using a twin-screw extruder with the above-mentioned combined screw, comprises the following steps: (1) cleaning the material residue on the surface of the screw; (2) setting the barrel temperature to 60-280°C and the screw speed to 150-450 rpm, raising the temperature to the set temperature and keeping the temperature for at least 15 minutes; (3) adding the polypropylene raw material, the degradation agent and the antioxidant compound into the hopper and mixing them evenly; (4) appropriately raising the temperature, extruding the polypropylene melt to clean the inside of the combined screw, and after cleaning, lowering the temperature to the set temperature and keeping the temperature constant for at least 15 minutes; (5) extrusion traction, underwater cooling, and then granulation; (6) adjusting the appropriate speed and feed according to the desired deodorization degree and fluidity of the target product, adjusting the extruder load and the vacuum degree of the vacuum exhaust port, observing the exhaust state of the vacuum exhaust port and the natural exhaust port, maintaining ventilation, but the molten polymer does not emerge from the exhaust port; (7) sampling and testing the product properties and starting to collect samples after stabilization.
[0012] Compared with the prior art, the present invention has the following beneficial effects: the combined screw structure of the twin-screw extruder of the present invention is simple and easy to operate, and the effect of reducing the odor and volatile matter of the product can be achieved through the arrangement and combination of the threaded elements. While the exhaust time of the melt is extended, the melt does not emerge from the exhaust port due to the back pressure of the threaded elements, the melt flow resistance and the like; the effect of the exhaust port in discharging volatiles is enhanced, and there is no need to add an exhaust port or exhaust equipment, and the cost is low.
[0013] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention will be further described in detail below through specific embodiments and related drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 is a cross-sectional view of a combined screw rod according to an embodiment of the present invention;
[0015] Figure 2 is a side view of a conveying element in an embodiment of the present invention;
[0016] Figure 3 is a cross-sectional view of a conveying element in an embodiment of the present invention;
[0017] Figure 4 is a side view of a kneading element A or a kneading element B in an embodiment of the present invention;
[0018] Figure 5 is a cross-sectional view of a kneading element A or a kneading element B in an embodiment of the present invention;
[0019] Figure 6 is a side view of a reverse flow element in an embodiment of the present invention;
[0020] Explanation of the numbers in the figure: 100 - barrel, 110 - main material port, 120 - vacuum exhaust port, 130 - natural exhaust port, 200 - screw, 210 - counterflow element, 220 - kneading element A, 230 - conveying element, 240 - kneading element B. DETAILED DESCRIPTION
[0021] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0022] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0023] like Figures 1 to 6As shown, a combined screw of a twin-screw extruder comprises a barrel 100 and a screw 200 located in the barrel, wherein a main material port 110 is provided at the rear end of the barrel, a vacuum exhaust port 120 is provided near the front end of the barrel, and a natural exhaust port 130 is provided behind the vacuum exhaust port; a reverse flow element is provided at the rear position of the screw near the vacuum exhaust port, a kneading element B is provided at the rear position of the screw near the natural exhaust port, and a plurality of continuous kneading elements A and a plurality of continuous conveying elements are sequentially provided on the screw between the reverse flow element and the kneading element B from front to back; in addition to the reverse flow element, the kneading element A, the conveying element and The other parts of the kneading element B are all conveying elements, and the conveying elements in other parts can adopt a conventional thread structure or the thread structure of the conveying element in this embodiment; the purpose of the above-mentioned element combination and position setting is to extend the exhaust time of the melt while preventing the melt from escaping from the exhaust port due to the back pressure of the threaded element, the melt flow resistance, etc.; to enhance the effect of exhausting volatiles from the exhaust port, especially for polypropylene with a high melt index (MFI>300) prepared by the peroxide degradation method; there is no need to add an exhaust port or exhaust equipment, and the effect of reducing the product odor and volatiles can be achieved only by the arrangement and combination of the threaded elements, which is simple, easy and inexpensive.
[0024] In this embodiment, the number of thread layers of the reverse flow element 210 is 1, the length is 10 mm, the helix angle is 67°, and the thread direction is opposite to the thread direction of the conveying element; the fluid conveyed to the front end of the vacuum exhaust port is affected by the reverse flow element, and part of it enters the vacuum exhaust section, and the other part flows back. On the one hand, this reduces the fluid flow and pressure in the vacuum exhaust section, so that the vacuum exhaust port can maintain a high negative pressure and improve the exhaust capacity of the vacuum exhaust port; on the other hand, the partial melt backflow will increase the residence time and mixing degree of the melt near the natural exhaust port and the vacuum exhaust port, which is conducive to the escape of volatile gases mixed in the melt from the exhaust port.
[0025] In this embodiment, the lengths of the kneading element A220 and the kneading element B240 are both 30 mm, and the kneading element A and the kneading element B are both provided with three layers of spiral sheets, the spiral sheets are elliptical, the plane where the spiral sheets are located is perpendicular to the axis of the screw, each layer of spiral sheets is 10 mm thick, and the circumferential angles between two adjacent layers of spiral sheets are staggered to 0°, 30°, 60° or 90°, preferably staggered by 60°. The kneading element A after the counterflow element has two functions: one is to establish back pressure to avoid sucking the melt near the vacuum exhaust port due to negative pressure at the vacuum exhaust port, which not only affects the efficiency of the natural exhaust port, but also increases the risk of material overflow at the vacuum exhaust port; the second is to strengthen the mixing effect of the reverse flow melt blocked by the counterflow element, which is beneficial to improve the degassing effect and reduce the odor of the product. The main function of the kneading element B after the natural exhaust port is to increase the residence time and mixing degree of the melt near the natural exhaust port.
[0026] In this embodiment, the conveying element 230 has a length of 90 mm, a helix angle of 71°, 5 thread layers, and each layer has a width of 18 mm, or 9 thread layers, and each layer has a width of 10 mm.
[0027] In this embodiment, the aspect ratio of the screw is 44.
[0028] In this embodiment, the barrel consists of 12 sections. Counting from front to back, the first section has an extrusion die head, and the vacuum exhaust port, natural exhaust port and main material port are located in the 3rd section, the 6th section and the 12th section respectively.
[0029] In this embodiment, the distance between the vacuum exhaust port and the natural exhaust port is 4 to 8 times the screw diameter.
[0030] A process for producing low-odor polyolefins, using a twin-screw extruder with the above-mentioned combined screw, comprises the following steps: (1) cleaning the material residue on the surface of the screw to ensure the bite of the twin screws and the compatibility of the barrel and the screw; (2) setting the barrel temperature to 60-280°C and the screw speed to 150-450rpm, raising the temperature to the set temperature and keeping it warm for at least 15 minutes; (3) adding polypropylene raw material, degradation agent and antioxidant compound into the hopper and mixing them evenly; (4) appropriately raising the temperature, extruding the polypropylene melt to clean the inside of the combined screw, and after cleaning, lowering the temperature to the set temperature and keeping it constant for at least 15 minutes; (5) extrusion traction, underwater cooling, and then granulation; (6) adjusting the appropriate speed and feeding according to the required deodorization degree and fluidity of the target product, adjusting the extruder load and the vacuum degree of the vacuum exhaust port, observing the exhaust state of the vacuum exhaust port and the natural exhaust port, maintaining ventilation, but the molten polymer does not emerge from the exhaust port; (7) sampling and testing the product properties and starting to collect samples after stability.
[0031] In the above step (3), the degradation agents are 101, 301, and DTBP; the antioxidant compound is a combination of one or more of 3114, 1010, 168, 626, 616, hydrotalcite, calcium stearate, zinc oxide, and magnesium stearate.
[0032] Table 1: Comparison of technical effects of the present invention and the prior art:
[0033] Comparative Example Embodiments of the present invention Melt mass flow rate (g / 10min) 34.9 35.0 Volatile matter (%) 0.1% 0.051% Bubble situation Some particles have a lot of bubbles No bubbles Residence time (s) 100~120 160~200 Screw speed (rpm) 300 300 Melt temperature (℃) 185-188 185-188 Odor level 3.5 3.0 Threaded element combination Conveyor elements with conventional threads Combination screw rod according to the embodiment of the present invention
[0034] The method of the present invention is simple, does not require additional exhaust ports or exhaust equipment, and can achieve the effect of reducing product odor and volatile matter only through the arrangement and combination of threaded elements. It is simple, easy to implement and has low cost.
[0035] Unless otherwise stated, any technical solution disclosed in the present invention disclosed above, if it discloses a numerical range, then the disclosed numerical range is a preferred numerical range, and any technician in the field should understand that the preferred numerical range is only a numerical value with a more obvious technical effect or representative value among many implementable numerical values. Since there are too many numerical values to be exhaustive, the present invention discloses some numerical values to illustrate the technical solution of the present invention, and the numerical values listed above should not constitute a limitation on the scope of protection of the present invention.
[0036] If the present invention discloses or involves components or structures that are fixedly connected to each other, then, unless otherwise stated, the fixed connection can be understood as: a detachable fixed connection (for example, connection using bolts or screws), and can also be understood as: a non-detachable fixed connection (for example, riveting, welding). Of course, the mutual fixed connection can also be replaced by an integrated structure (for example, manufactured by integrated molding using a casting process) (except when it is obviously impossible to use an integrated molding process).
[0037] In addition, unless otherwise stated, the terms used to indicate positional relationships or shapes in any of the technical solutions disclosed in the present invention include states or shapes that are approximate, similar, or close to them.
[0038] Any component provided by the present invention may be assembled from a plurality of separate components, or may be a separate component manufactured by an integral forming process.
[0039] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A process for producing low-odor polyolefins using a twin-screw extruder with a combined screw, characterized in that: The combined screw comprises a barrel and a screw located in the barrel, wherein a main material port is provided at the rear end of the barrel, a vacuum exhaust port is provided near the front end of the barrel, and a natural exhaust port is provided behind the vacuum exhaust port; a reverse flow element is provided at the rear position of the screw near the vacuum exhaust port, a kneading element B is provided at the rear position of the screw near the natural exhaust port, and a plurality of continuous kneading elements A and a plurality of continuous conveying elements are sequentially provided on the screw from front to back between the reverse flow element and the kneading element B; except for the reverse flow element, the kneading element A, the conveying element and the kneading element B, conveying elements are used in other parts of the screw; the reverse flow element The element has one thread layer, a length of 10 mm, a helix angle of 67°, and a thread direction opposite to that of the conveying element; the kneading element A and the kneading element B are both 30 mm long, and the kneading element A and the kneading element B are both provided with three layers of spiral sheets, the plane where the spiral sheets are located is perpendicular to the axis of the screw, each layer of spiral sheets is 10 mm thick, and the circumferential angle between two adjacent layers of spiral sheets is staggered to 0°, 30°, 60° or 90°; the conveying element has a length of 90 mm, a helix angle of 71°, a thread layer number of 5 layers, a width of each layer of 18 mm, or a thread layer number of 9 layers, a width of each layer of 10 mm; process for producing low-odor polyolefin The method comprises the following steps: (1) cleaning the material residue on the surface of the screw; (2) setting the barrel temperature to 60-280°C and the screw speed to 150-450 rpm, raising the temperature to the set temperature and keeping the temperature for at least 15 minutes; (3) adding the polypropylene raw material, the degradation agent and the antioxidant compound into the hopper and mixing them evenly; (4) appropriately raising the temperature and extruding the polypropylene melt to clean the inside of the combined screw, and after the cleaning is completed, lowering the temperature to the set temperature and keeping the temperature constant for at least 15 minutes; (5) extrusion traction, underwater cooling, and then granulation; (6) adjusting the appropriate speed and feed according to the required deodorization degree and fluidity of the target product, adjusting the extruder load and the vacuum degree of the vacuum exhaust port, observing the exhaust state of the vacuum exhaust port and the natural exhaust port, maintaining ventilation, but the molten polymer does not emerge from the exhaust port; (7) sampling and testing, and starting to collect samples after the product properties are stable.
2. The process for producing low-odor polyolefin according to claim 1, characterized in that: The aspect ratio of the screw is 44.
3. The process for producing low-odor polyolefin according to claim 1, characterized in that: The distance between the vacuum exhaust port and the natural exhaust port is 4 to 8 times the screw diameter.