Substrate for electronic device and method for manufacturing the same

By bonding multiple low-resistivity single-crystal silicon substrates on a silicon substrate to form a bonding substrate with a thickness greater than 2000μm, the problem of nitride semiconductor wafer warping is solved, enabling the manufacture of high-voltage electronic devices and enhancing the strength and hardness of the substrate.

CN113994032BActive Publication Date: 2024-11-12SHIN ETSU HANDOTAI CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202080044129.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-11
Filing Date
2020-04-30
Publication Date
2024-11-12
Estimated Expiration
2040-04-30

AI Technical Summary

Technical Problem

Existing technologies for manufacturing nitride semiconductor wafers using silicon substrates are prone to warping and plastic deformation due to differences in lattice constants and coefficients of thermal expansion. The warping problem is particularly pronounced when a thick epitaxial layer is deposited, making it difficult to meet the requirements of high-voltage electronic devices.

Method used

Multiple low-resistivity single-crystal silicon substrates are manufactured using the CZ method, with a thickness greater than 2000 μm, and bonded by SiO2 film to form a high-strength bonding substrate to alleviate stress and suppress warping, suitable for growing nitride semiconductor films on it.

Benefits of technology

It significantly suppresses warping caused by nitride semiconductor films, making it suitable for high-voltage electronic devices. It also improves the strength and hardness of the substrate, making it suitable for high-voltage products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113994032B_ABST
    Figure CN113994032B_ABST
Patent Text Reader

Abstract

The present invention is a substrate for electronic devices, which is a substrate in which a nitride semiconductor film is formed on a bonding substrate of single crystal silicon, characterized in that the bonding substrate is a substrate formed by bonding multiple single crystal silicon substrates, and has a thickness greater than 2000 μm, and the multiple single crystal silicon substrates are substrates manufactured by a CZ method, and have a resistivity of 0.1 Ωcm or less. Thus, a substrate for electronic devices in which warping is suppressed and a substrate for electronic devices in which a nitride semiconductor film is formed on a silicon substrate and can be used for high-voltage products and a manufacturing method thereof are provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a substrate for electronic devices and a method for manufacturing the same. Background Art

[0002] Nitride semiconductors such as GaN and AlN can be used to manufacture high electron mobility transistors (HEMTs) or high withstand voltage electronic devices using a two-dimensional electron gas.

[0003] It is difficult to make a nitride wafer in which these nitride semiconductors are grown on a substrate, and a sapphire substrate or a SiC substrate is used as the substrate. However, in order to suppress the large diameter or the cost of the substrate, epitaxial growth on a silicon substrate based on vapor phase growth is used. In the production of epitaxial growth films on silicon substrates based on vapor phase growth, a large-diameter substrate can be used compared to a sapphire substrate or a SiC substrate, so the device has high productivity and is advantageous in terms of heat dissipation. However, the stress caused by the difference in lattice constant or thermal expansion coefficient is likely to cause an increase in warpage or plastic deformation, thereby performing stress reduction based on growth conditions or a relaxation layer.

[0004] In order to improve the high withstand voltage characteristics of high withstand voltage electronic devices, it is necessary to deposit the epitaxial layer thicker. Therefore, if the epitaxial layer is deposited thicker, the silicon substrate as the substrate will cause warping on the wafer due to the difference in thermal expansion coefficient between the epitaxial layer and the substrate.

[0005] Patent Document 1 discloses an epitaxial substrate for electronic devices in which a high-resistance substrate and a low-resistance substrate are bonded to control the warpage shape as an epitaxial layer of AlN / Si (1000 Ωcm or more) / Si (100 Ωcm or less). In addition, Patent Document 2 discloses an epitaxial substrate for electronic devices in which a low-resistance CZ substrate and a high-resistance FZ substrate are bonded to suppress the warpage as an epitaxial layer of AlN / Si (CZ low resistance) / Si (FZ high resistance).

[0006] However, in electronic device substrates used for high-voltage electronic devices, it is desired to further suppress the warpage of the wafer when the epitaxial layer is deposited thickly.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: International Publication No. 2011 / 016219

[0010] Patent Document 2: Japanese Patent Publication No. 2014-192226 Summary of the invention

[0011] 1. Technical issues to be resolved

[0012] The present invention is made to solve the above-mentioned problems, and its object is to provide an electronic device substrate and a manufacturing method thereof which can suppress warping in an electronic device substrate in which a nitride semiconductor film is formed on a silicon substrate and can also be used for high-voltage products.

[0013] (II) Technical solution

[0014] In order to achieve the above object, the present invention provides a substrate for electronic devices, which is a substrate having a nitride semiconductor film formed on a single crystal silicon bonding substrate, characterized in that:

[0015] The bonding substrate is a substrate formed by bonding a plurality of single crystal silicon substrates, and has a thickness greater than 2000 μm.

[0016] The plurality of single crystal silicon substrates are substrates manufactured by a CZ method and have a resistivity of 0.1 Ωcm or less.

[0017] In the electronic device substrate of the present invention, the strength of the bonded substrate is greatly increased by setting the plurality of single crystal silicon substrates to substrates manufactured by the CZ method with a resistivity of 0.1 Ωcm or less, and further making the thickness of the bonded substrate greater than 2000 μm, so that the warping of the electronic device substrate caused by the formed nitride semiconductor film can be suppressed. Therefore, the electronic device substrate is particularly suitable as a substrate for high withstand voltage products.

[0018] At this time, the oxygen concentration of the plurality of single crystal silicon substrates is preferably 3.0×10 17 ~1×10 18 atoms / cm 3 (ASTM'79).

[0019] Such a substrate can prevent slip from occurring in the single crystal silicon substrate.

[0020] Furthermore, the bonding substrate is preferably a substrate formed by bonding a plurality of CZ single crystal silicon substrates via a SiO 2 film.

[0021] With such a substrate, stress generated by the nitride semiconductor film can be relaxed, and a thicker nitride semiconductor film can be formed.

[0022] In addition, the present invention provides a method for manufacturing a substrate for an electronic device, which is used to form a nitride semiconductor film on a bonding substrate of single crystal silicon, and is characterized by comprising the following steps:

[0023] bonding a plurality of single crystal silicon substrates to form a bonded substrate having a thickness greater than 2000 μm; and

[0024] epitaxially growing a nitride semiconductor film on the bonding substrate,

[0025] As the plurality of single crystal silicon substrates, substrates having a resistivity of 0.1 Ωcm or less manufactured by a CZ method are used.

[0026] According to the method for manufacturing an electronic device substrate of the present invention, a plurality of CZ single crystal silicon substrates having a resistivity of 0.1 Ωcm or less are used, and the thickness of the bonding substrate is made greater than 2000 μm, so that a bonding substrate with high strength can be manufactured, and thus warping of the electronic device substrate when forming a nitride semiconductor film can be suppressed. Therefore, the method is particularly suitable as a method for manufacturing an electronic device substrate for a high withstand voltage product.

[0027] In addition, it is preferred to use an oxygen concentration of 3.0×10 17 ~1×10 18 atoms / cm 3 (ASTM'79) substrates are used as the plurality of single crystal silicon substrates.

[0028] Such a method can prevent the occurrence of slip in the single crystal silicon substrate.

[0029] Furthermore, in the step of forming the bonding substrate, it is preferable to bond a plurality of CZ single crystal silicon substrates via a SiO 2 film.

[0030] Such a method can alleviate the stress applied during nitride growth and form a thicker nitride semiconductor film.

[0031] (III) Beneficial effects

[0032] According to the electronic device substrate and the manufacturing method thereof of the present invention, the strength of the bonding substrate is greatly increased by setting the plurality of single crystal silicon substrates to substrates manufactured by the CZ method with a resistivity of 0.1 Ωcm or less, and further making the thickness of the bonding substrate greater than 2000 μm, so that the warping of the electronic device substrate caused by the formed nitride semiconductor film can be suppressed. Therefore, it is particularly suitable as an electronic device substrate for high withstand voltage products. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 (a) is a conceptual diagram showing the electronic device substrate of the present invention in the case where an adhesive layer is provided between a plurality of single crystal silicon substrates. Figure 1 (b) is a conceptual diagram showing the electronic device substrate of the present invention in the case of not having an adhesive layer. DETAILED DESCRIPTION

[0034] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.

[0035] In electronic devices manufactured by epitaxially growing nitride semiconductors on silicon substrates, the present inventors conducted in-depth research on electronic device substrates and methods for manufacturing the same for suppressing warping caused by differences in thermal expansion coefficients, and found that by using a substrate having a thickness greater than 2000 μm and bonded with multiple CZ single crystal silicons of low resistivity, warping can be significantly suppressed, thereby completing the present invention.

[0036] [Substrates for electronic devices]

[0037] That is, the present invention is a substrate for electronic devices in which a nitride semiconductor film is formed on a single crystal silicon bonding substrate, characterized in that

[0038] The bonding substrate is a substrate formed by bonding a plurality of single crystal silicon substrates, and has a thickness greater than 2000 μm.

[0039] The plurality of single crystal silicon substrates are substrates manufactured by a CZ method and have a resistivity of 0.1 Ωcm or less.

[0040] The electronic device substrate of the present invention is a substrate in which a nitride semiconductor film is formed on a bonding substrate of single crystal silicon. In the present invention, the bonding substrate is a substrate formed by bonding a plurality of single crystal silicon substrates produced by the CZ method.

[0041] Figure 1 A conceptual diagram showing the electronic device substrate of the present invention.

[0042] like Figure 1 As shown in (a) and (b) of the present invention, the electronic device substrate 10 is composed of a bonding substrate 6 in which a single crystal silicon substrate 1 and a single crystal silicon substrate 2 (a plurality of single crystal silicon substrates) are bonded, and a nitride semiconductor film (device layer) 5 composed of nitride. The bonding method between the plurality of single crystal silicon substrates is not particularly limited, and an adhesive layer may be provided. Figure 1 (a) shows a structure having an adhesive layer 3 between a single crystal silicon substrate 1 and a single crystal silicon substrate 2. The adhesive layer is not particularly limited, and may be, for example, an oxide film (SiO2). Figure 1 (b) represents a structure in which there is no bonding layer 3 between the single crystal silicon substrate 1 and the single crystal silicon substrate 2. For example, by thinning the oxide film before bonding so that only the oxygen of the oxide film diffuses due to the bonding heat treatment after bonding, a structure in which there is no oxide film at the bonding interface can be achieved. In this way, if the bonding of the single crystal silicon substrates is performed through the oxide film, the stress applied during the growth of the nitride can be alleviated. In addition, the number of single crystal silicon substrates to be bonded is not limited to 2, but may be 3 or more. Referring to Figure 1 , the following description will be given by taking as an example a case where the bonding substrate is a substrate obtained by bonding two single crystal silicon substrates.

[0043] In the present invention, the single crystal silicon substrate 1 and the single crystal silicon substrate 2 are single crystal silicon substrates manufactured by the CZ method (hereinafter, sometimes referred to as CZ single crystal substrates), the resistivity is set to be less than 0.1Ωcm, and the thickness of the bonded substrate after bonding is set to be greater than 2000μm. By making the CZ single crystal substrate with a resistivity of less than 0.1Ωcm, the rigidity of the single crystal silicon substrate is improved, and the strength of the bonded substrate is increased, so that the warping of the electronic device substrate when the nitride semiconductor film is formed can be suppressed.

[0044] In addition, in the present invention, the oxygen concentration is preferably 3.0×10 17 ~1×10 18 atoms / cm 3 (ASTM'79). In general, CZ single crystals, unlike FZ single crystals, contain oxygen, which improves the strength and hardness of the substrate. On the other hand, by setting the oxygen concentration to 3.0×10 17 ~1×10 18 atoms / cm 3 (ASTM'79), which can prevent slip in the CZ single crystal substrate.

[0045] In addition, an intermediate layer 4 may be formed between the single crystal silicon substrate 2 and the device layer 5. The intermediate layer 4 functions as a buffer layer inserted to improve the crystallinity of the device layer or control stress. The intermediate layer 4 can be made using the same equipment as the nitride semiconductor film, so it is preferably made using nitride.

[0046] A device layer 5 composed of a thin film of a nitride such as GaN, AlN, InN, AlGaN, InGaN, AlInN, etc. is formed on a single crystal silicon substrate 2. Here, when the intermediate layer 4 is formed, the device layer 5 can be formed on the intermediate layer 4. The device layer 5 can be grown by vapor phase growth such as MOVPE or sputtering. The nitride thin film can be 1 to 20 μm and can be designed according to the device.

[0047] For example, for gallium nitride, the lattice constant difference between it and Si (111) single crystal is 17%, and the thermal expansion coefficient difference is 116%, which applies stress to the film or substrate during growth at high temperature. In addition, since it is heated to more than 1000°C during growth, when stress is applied to the wafer, it does not break brittlely but exhibits ductility, and dislocations are generated to cause plastic deformation.

[0048] If it is a substrate for electronic devices of the present invention, by making the thickness of the substrate thick enough to form a CZ single crystal substrate with a resistivity of less than 0.1Ωcm, plastic deformation during growth can be prevented and warping can be reduced. From the viewpoint of warping of the substrate for electronic devices, the lower limit of the resistivity is not particularly limited and can be appropriately determined, and can be a value greater than 0Ωcm. In addition, by making the thickness of the bonding substrate greater than 2000μm, the strength of the bonding substrate is increased, so that the warping of the substrate for electronic devices caused by the formed nitride semiconductor film can be further suppressed. Therefore, it is particularly suitable as a substrate for electronic devices for high-voltage products. From the viewpoint of the strength of the bonding substrate, the upper limit of the thickness is not particularly limited and can be appropriately determined, but it is sufficient as long as it reaches 4800μm.

[0049] [Method for producing a substrate for electronic devices]

[0050] Furthermore, the present invention is a method for manufacturing a substrate for an electronic device in which a nitride semiconductor film is formed on a bonding substrate of single crystal silicon, characterized by comprising the following steps:

[0051] bonding a plurality of single crystal silicon substrates to form a bonded substrate having a thickness greater than 2000 μm; and

[0052] epitaxially growing a nitride semiconductor film on the bonding substrate,

[0053] As the plurality of single crystal silicon substrates, substrates having a resistivity of 0.1 Ωcm or less manufactured by a CZ method are used.

[0054] In the manufacturing method of the present invention, first, multiple single crystal silicon substrates are bonded to form a bonded substrate having a thickness greater than 2000 μm. Here, in the manufacturing method of the present invention, hard and strong substrates with a resistivity of 0.1 Ωcm or less manufactured by the CZ method are used as multiple single crystal silicon substrates.

[0055] In addition, as the plurality of single crystal silicon substrates, it is preferable to use an oxygen concentration of 3.0×10 17 ~1×10 18 atoms / cm 3 (ASTM'79) substrate. By using an oxygen concentration of 3.0×10 17 ~1×10 18 atoms / cm 3 (ASTM'79) substrate can prevent slip in the CZ single crystal substrate.

[0056] The method of bonding multiple single crystal silicon substrates is not particularly limited, but it is preferred to use an oxide film for bonding. In addition, by thinning the oxide film before bonding, only the oxygen in the oxide film is diffused by heat treatment after bonding, and a structure without an oxide film can be formed at the bonding interface. In this way, by bonding single crystal silicon substrates using an oxide film, the stress applied during nitride growth can be alleviated.

[0057] In addition, the thickness of each of the plurality of single crystal silicon substrates is preferably 1000 μm or more. In order to produce a bonding substrate having a thickness exceeding 2000 μm, a device-type fixture or the like is required, but by bonding two single crystal silicon substrates having a thickness exceeding 1000 μm, a bonding substrate having a thickness exceeding 2000 μm can be easily produced.

[0058] Next, a nitride semiconductor film is epitaxially grown on the bonding substrate manufactured in the above manner. Here, an intermediate layer can be formed before the growth of the nitride semiconductor film. By forming an intermediate layer during the growth of the nitride and adding an appropriate buffer layer, the stress from the film caused by the difference in thermal expansion coefficient and lattice constant can be controlled after cooling, and by thickening the substrate, plastic deformation during high-temperature growth can be prevented, thereby manufacturing a wafer with less warpage. In order to simplify the process, it is preferred to use nitride to make the intermediate layer.

[0059] According to such a manufacturing method, by using a plurality of CZ single crystal silicon substrates having a resistivity of 0.1 Ωcm or less, and further making the thickness of the bonding substrate greater than 2000 μm, a bonding substrate with high strength can be produced, thereby suppressing the warping of the electronic device substrate when the nitride semiconductor film is formed. Therefore, the method is particularly suitable as a manufacturing method for an electronic device substrate for a high withstand voltage product.

[0060] Example

[0061] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0062] (Example 1)

[0063] The resistivity is 0.007Ωcm and the oxygen concentration is 7×10 17 atoms / cm 3 Two wafers (150 mm in diameter, crystal orientation (111)) of CZ single crystal silicon substrates with a thickness of 1100 μm according to (ASTM'79).

[0064] Then, we created Figure 1The substrate for electronic devices shown in (a). The CZ single crystal silicon substrate (base wafer) 1 and the double-sided polished CZ single crystal silicon substrate (bonding wafer) 2 were thermally oxidized to form a SiO2 film with a thickness of 100nm respectively. Then, after a bonding process, a bonding heat treatment was performed at 1150°C for 2 hours. After that, as an oxide film removal, the surface oxide film was removed by immersion in 10% HF to produce a bonding substrate with a thickness of 2200μm (2 1100μm substrates + 200nm bonding layer). Then, the produced bonding substrate was epitaxially grown with 8μm thick GaN (intermediate layer: 4μm, device layer 4μm) in a MOVPE furnace. The warping of the wafer after epitaxial growth was 10μm.

[0065] (Comparative Example 1)

[0066] In Comparative Example 1, a substrate was prepared in the same manner as in Example 1 except that the thickness of the CZ single crystal silicon substrate was changed. 17 atoms / cm 3 Two wafers of 500 μm thick CZ single crystal silicon substrate (diameter 150 mm, crystal orientation (111)) of ASTM'79; and a resistivity of 0.007 Ωcm and an oxygen concentration of 7×10 17 atoms / cm 3 Two wafers (diameter 150 mm, crystal orientation (111)) of CZ single crystal silicon substrates with a thickness of 625 μm according to (ASTM'79).

[0067] The CZ single crystal silicon substrate (base wafer) is thermally oxidized (thickness 100nm), and the double-sided polished CZ single crystal silicon substrate (bonding wafer) is thermally oxidized (thickness 100nm), and after the bonding process, a bonding heat treatment is performed at 1150°C for 2 hours. After that, as an oxide film removal, the surface oxide film is removed by immersion in 10% HF to produce a bonded substrate with a thickness of 1000μm (2 500μm substrates + 200nm bonding layer) and 1250μm (2 625μm substrates + 200nm bonding layer). Then, each bonded substrate is epitaxially grown in the same MOVPE furnace to grow 8μm thick GaN (intermediate layer: 4μm, device layer 4μm). The warpage of the wafer with a substrate thickness of 1250μm is 20μm. In the wafer with a substrate thickness of 1000μm, the warpage is 50μm.

[0068] (Comparative Example 2)

[0069] In Comparative Example 2, a combined substrate was prepared by bonding a FZ single crystal silicon substrate and a CZ single crystal silicon substrate, and an epitaxial layer was grown on the combined substrate. 17 atoms / cm 3 The wafer is a 625 μm thick CZ single crystal silicon substrate (diameter 150 mm, crystal orientation (111)) with a resistivity of 0.007 Ωcm and an oxygen concentration of 7×10 17 atoms / cm 3 The wafer is a 675 μm thick CZ single crystal silicon substrate (diameter 150 mm, crystal orientation (111)) with a resistivity of 5000 Ωcm and a nitrogen concentration of 8×10 14 atoms / cm 3 The FZ single crystal silicon substrate has a thickness of 625 μm (diameter 150 mm, crystal orientation (111)); and a resistivity of 5000 Ωcm and a nitrogen concentration of 8×10 14 atoms / cm 3 The FZ single crystal silicon substrate is a 675 μm thick wafer (diameter 150 mm, crystal orientation (111)).

[0070] The CZ single crystal silicon substrate (base wafer) was thermally oxidized (thickness 100nm), and the double-sided polished FZ single crystal silicon substrate (bonding wafer) was thermally oxidized (thickness 100nm), and after the bonding process, a bonding heat treatment was performed at 1150°C for 2 hours. After that, as an oxide film removal, the surface oxide film was removed by immersion in 10% HF to produce a bonded substrate with a thickness of 1250μm (2 625μm substrates + 200nm bonding layer) and 1350μm (2 675μm substrates + 200nm bonding layer). Then, each bonded substrate was epitaxially grown with 8μm thick GaN (intermediate layer: 4μm, device layer 4μm) in the same MOVPE furnace. The warpage of the wafer with a substrate thickness of 1250μm is 25μm. In the wafer with a substrate thickness of 1350μm, the warpage is 15μm.

[0071] (Comparative Example 3)

[0072] In Comparative Example 3, a bonded substrate was prepared by bonding FZ single crystal silicon substrates to each other, and an epitaxial layer was grown on the bonded substrate. 14 atoms / cm 3 Two wafers (diameter 150 mm, crystal orientation (111)) with a thickness of 625 μm of FZ single crystal silicon substrate; and a resistivity of 5000 Ωcm and a nitrogen concentration of 8×1014 atoms / cm 3 Two wafers (diameter 150 mm, crystal orientation (111)) of FZ single crystal silicon substrate with a thickness of 675 μm.

[0073] The FZ single crystal silicon substrate (base wafer) 1 is thermally oxidized (thickness 100nm), and the double-sided polished FZ single crystal silicon substrate (bonding wafer) 2 is thermally oxidized (thickness 100nm), and after the bonding process, a bonding heat treatment is performed at 1150°C for 2 hours. After that, as an oxide film removal, the surface oxide film is removed by immersion in 10% HF to produce a bonded substrate with a thickness of 1250μm (2 625μm substrates + 200nm bonding layer) and 1350μm (2 675μm substrates + 200nm bonding layer). Then, each bonded substrate is epitaxially grown in the same MOVPE furnace to grow 8μm thick GaN (intermediate layer: 4μm, device layer 4μm). The warpage of the wafer with a substrate thickness of 1250μm is 30μm. In the wafer with a substrate thickness of 1350μm, the warpage is 20μm.

[0074] (Comparative Example 4)

[0075] In Comparative Example 4, the thickness of the CZ single crystal silicon substrate was made thinner than that of Comparative Example 1, and the substrate was prepared in the same manner as in Comparative Example 1. A single crystal silicon substrate having a resistivity of 0.007 Ωcm or less and an oxygen concentration of 7×10 17 atoms / cm 3 A wafer (diameter 150 mm, crystal orientation (111)) having a CZ silicon substrate of ASTM'79 and a thickness of 400 μm; and a resistivity of less than 0.007 Ωcm and an oxygen concentration of 7×10 17 atoms / cm 3 Another wafer (diameter 150 mm, crystal orientation (111)) is a CZ silicon substrate of (ASTM'79) and the thickness of the substrate is 400 μm.

[0076] The CZ single crystal silicon substrate (base wafer) 1 is thermally oxidized (thickness 50nm), and the double-sided polished CZ single crystal silicon substrate (bonding wafer) 2 is thermally oxidized (thickness 50nm), and after the bonding process, a bonding heat treatment is performed at 1150°C for 2 hours. Then, as an oxide film removal, the surface oxide film is removed by immersion in 10% HF to produce a bonded substrate with a thickness of 800μm (2 400μm substrates + 100nm bonding layer). Then, the substrate is epitaxially grown in an MOVPE furnace to form 8μm thick GaN (intermediate layer: 4μm, device layer 4μm). The warping of the wafer is 200μm.

[0077] (Comparative Example 5)

[0078] In Comparative Example 5, the epitaxial layer was grown without laminating the CZ single crystal silicon substrate. A substrate having a resistivity of 0.007 Ωcm or less and an oxygen concentration of 7×10 17 atoms / cm 3 The wafer is a CZ silicon substrate of ASTM'79 and has a thickness of 625 μm (diameter 150 mm, crystal orientation (111)).

[0079] Then, the substrate was epitaxially grown in a MOVPE furnace to form GaN with a thickness of 8 μm (intermediate layer: 4 μm, device layer: 4 μm). The warpage of the wafer was 300 μm.

[0080] According to the above results, as shown in Example 1, when a CZ single crystal silicon substrate with a resistivity of 0.1 Ωcm or less is bonded and the thickness of the bonded bonded substrate is greater than 2000 μm, the warpage of the wafer is minimized when a nitride semiconductor film is formed. On the other hand, it can be seen that even if a CZ single crystal silicon substrate with the same resistivity is used, the warpage of the wafer becomes larger when the thickness of the substrate is 2000 μm or less as in Comparative Examples 1, 4, and 5. In addition, from the comparison between Comparative Example 1 and Comparative Examples 2 and 3, it can be seen that even if the substrate thickness is the same, if an FZ single crystal silicon substrate softer than a CZ single crystal silicon substrate is used, the warpage of the wafer becomes larger.

[0081] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are for illustrative purposes only, and any solution having substantially the same structure and producing the same function and effect as the technical concept described in the claims of the present invention is included in the technical scope of the present invention.

Claims

1. A substrate for an electronic device, comprising a substrate having a nitride semiconductor film formed on a single crystal silicon bonding substrate, It is characterized in that The bonded substrate is a substrate formed by bonding a plurality of single crystal silicon substrates, includes the plurality of single crystal silicon substrates, and has a thickness greater than 2000 μm. The plurality of single crystal silicon substrates are substrates manufactured by a CZ method, have a resistivity of 0.1 Ωcm or less, and each has a thickness of 1000 μm or more.

2. The electronic device substrate according to claim 1, It is characterized in that The oxygen concentration of the plurality of single crystal silicon substrates according to ASTM'79 is 3.0×10 17 ~1×10 18 atoms / cm 3 .

3. The electronic device substrate according to claim 1 or 2, It is characterized in that The bonding substrate is a plurality of CZ single crystal silicon substrates connected via SiO 2 A substrate formed by film bonding.

4. A method for manufacturing a substrate for an electronic device, which is used to form a nitride semiconductor film on a bonding substrate of single crystal silicon, It is characterized in that Including the following processes: bonding a plurality of single crystal silicon substrates to form a bonded substrate having a thickness greater than 2000 μm; and epitaxially growing a nitride semiconductor film on the bonding substrate including the plurality of single crystal silicon substrates; As the plurality of single crystal silicon substrates, substrates manufactured by a CZ method having a resistivity of 0.1 Ωcm or less and each having a thickness of 1000 μm or more are used.

5. The method for producing an electronic device substrate according to claim 4, It is characterized in that The oxygen concentration based on ASTM'79 was 3.0×10 17 ~1×10 18 atoms / cm 3 as the multiple single crystal silicon substrates.

6. The method for producing a substrate for an electronic device according to claim 4 or 5, It is characterized in that In the step of forming the bonding substrate, the SiO 2 A plurality of CZ single crystal silicon substrates are film-bonded.

Citation Information

Patent Citations

  • Epitaxial substrate for electronic device

    JP2014192226A

  • Epitaxial substrate for electronic devices and manufacturing method for said epitaxial substrate

    WO2011016219A1

  • Single-crystal silicon substrate and its manufacturing method

    JP2001274166A

  • Method for manufacturing gallium nitride semiconductor substrate

    JP2007246289A

  • Nitride-semiconductor forming substrate and method of manufacturing the same

    JP2010225947A