A device and method for purifying capacitor-grade high-purity ammonium salt
By designing improved bipolar membrane electrodialysis devices and ammonia recovery technology with temperature-resistant materials in the capacitor industry, the problem of impurities introduction in high-purity ammonium salt purification is solved, and efficient high-purity ammonium salt purification is achieved, reducing costs and Environmental pollution improves the performance and sustainability of capacitors.
Patent Information
- Application Number
- CN202111213059.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-10-19
AI Technical Summary
The capacitor industry has extremely high requirements for the purity of high-purity ammonium salts, but the existing technology is prone to introducing foreign impurities during purification, resulting in the product not meeting the standards, increasing the cost and environmental pollution risks, and traditional bipolar membrane electrodialysis equipment cannot be used at high temperatures. Work effectively under.
A purification device including a bipolar membrane electrodialysis device, heating device, cooling crystallization and NH3 gas absorption device was designed. The water-deployed separator and hydrophobic porous deamination membrane were used to improve the water-deployed separator and hydrophobic porous deamination membrane. The high-temperature bipolar membrane electrodialysis was performed. And ammonia recovery technology achieves high purity purification of ammonium salts and avoids the introduction of foreign impurities.
Purification of high-purity ammonium salts without foreign impurities at high temperatures is achieved, ensuring the purity of the capacitor level, reducing production costs and environmental pollution, and improving the performance and sustainable development of aluminum electrolytic capacitors.
Smart Images

Figure CN114011243B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the aluminum electrolytic capacitor industry, and specifically relates to a capacitor-grade high-purity ammonium salt purification device and a capacitor-grade high-purity ammonium salt purification method. Background Art
[0002] High-purity ammonium salts are widely used in the aluminum electrolytic capacitor industry. High-purity chemicals that can be used in the capacitor industry are called capacitor grade chemicals. Their purity is often much higher than that of industrial grade and analytical grade chemicals, and impurity ions (such as Cl) that may affect the performance of capacitors are required to be - , SO 4 2- etc.) content is extremely low.
[0003] In the manufacturing process of electrode foil, the corroded foil needs to be introduced into the formation tank as the positive electrode and a high DC voltage is applied to form a dense oxide film layer on the foil surface. This operation is often called formation, which is carried out in an organic acid ammonium salt (such as ammonium adipate, ammonium azelaic acid, ammonium sebacate, ammonium benzoate, etc.) or an inorganic weak acid ammonium salt (such as ammonium pentaborate, etc.) solution. The quality of the oxide film formed by formation is crucial to improving the electrical stability of capacitor products and reducing leakage current. If there are impurities in the formation solution, the oxide film will be defective. In the assembly and manufacturing process of capacitors, ammonium salts of linear carboxylic acids (ammonium adipate, ammonium suberate, ammonium hydrogen azelaic acid, ammonium sebacate, ammonium dodecanoate, etc.), ammonium salts of branched carboxylic acids (2-n-butyl ammonium suberate, 2-n-hexyl ammonium adipate, etc.) and ammonium salts of other organic / inorganic weak acids (ammonium pentaborate, ammonium benzoate, etc.) can all be used as the main solute or additive of the working electrolyte. As the core component of aluminum electrolytic capacitors, the performance of electrolyte directly affects the quality of capacitor products, especially the service life, reliability and electrical characteristics. In addition to the excellent electrochemical properties that the electrolyte solute itself needs to have, it is also required to be extremely pure and contain no trace impurities that react with or corrode the constituent materials.
[0004] In the capacitor industry, trace impurities in bulk ammonium salt products produced by industrial methods often exceed the standard and cannot be used. This forces the capacitor industry to purchase small quantities of specially customized products, and the supply chain security is often not guaranteed and the cost remains high. On the other hand, in the process of electrode foil production, it is inevitable that trace impurities will be brought from the upstream into the high-purity ammonium salt solution being used, which will cause its purity index to fail to meet the standard and can only be completely replaced; this will not only further increase the company's raw material costs, but also cause potential environmental pollution risks. Due to the capacitor industry's stringent requirements on the purity of chemical raw materials, the company's production costs are high, the utilization rate of chemical materials is low, and pollutant emissions increase, which is not conducive to the sustainable and healthy development of the industry. Therefore, it is very necessary to develop a purification production method for capacitor-grade high-purity ammonium salts for the aluminum electrolytic capacitor industry.
[0005] Most of the ammonium salt solutes used in the capacitor industry, including the ammonium salts of linear carboxylic acids listed above, the ammonium salts of branched carboxylic acids, and the ammonium salts of other organic / inorganic weak acids, have a common characteristic, that is, their solubility in water is closely related to temperature, as shown in Table 1. For example, adipic acid is soluble in water at 60 o The solubility at 10 °C is as high as 148 g / L. o The solubility at 40 °C is only 9.9 g / L. Taking advantage of the fact that the solubility decreases sharply with decreasing temperature, these chemicals can be purified by cooling and recrystallizing. Chinese patents CN101219946B and CN103588632B respectively provide a method for recovering adipic acid from ammonium adipate waste liquid. The core technology of the method is to add inorganic strong acid (such as HCl, H2O2) to the concentrated ammonium adipate solution at high temperature. 2 SO 4 or HNO 3 ) to convert it into a concentrated adipic acid solution, and then cool it down to obtain a relatively pure adipic acid solid product. However, since a large amount of inorganic acid needs to be added to the system during this process, a large amount of foreign ions (such as Cl - 、SO 4 2- or NO 3 - ), a small part of these foreign ions will inevitably be adsorbed / entrained into the final solid product, making its purity completely unable to meet the capacitance level requirements.
[0006] Table 1 Solubility of common organic acids / inorganic acids in water in the capacitor industry at different temperatures.
[0007]
[0008] Electrodialysis bipolar membrane (EDBM) is an emerging electrochemical membrane separation method that can directly convert salt solutions into corresponding acid and alkaline solution products without introducing any foreign substances. However, the application of bipolar membrane technology to the conversion of ammonium salt solutes in the capacitor industry still faces huge challenges. Therefore, it is necessary to design a purification device and method that can achieve capacitor-grade high-purity ammonium salts. Summary of the invention
[0009] The purpose of the invention is to provide a device and method for purifying capacitor-grade high-purity ammonium salt.
[0010] The capacitor-grade high-purity ammonium salt purification device proposed in the present invention comprises a bipolar membrane electrodialyzer 1, a heating device 2, a cooling crystallization and solid-liquid separation device 3 and an NH 3Gas absorption device 4; wherein the heating device 2 is connected to the inlet of the bipolar membrane electrodialyzer acid chamber through a pipeline, and the outlet of the bipolar membrane electrodialyzer acid chamber is connected to the inlet of the cooling crystallization and solid-liquid separation device 3, NH 3 The deammoniation side inlet of the gas absorption device 4 is connected to the outlet of the alkali chamber of the bipolar membrane electrodialyzer 1, NH 3 The outlet of the deammoniation side in the gas absorption device 4 is connected to the inlet of the alkali chamber of the bipolar membrane electrodialyzer 1 .
[0011] In the present invention, the bipolar membrane electrodialyzer adopts a bipolar membrane plus a cation exchange membrane two-compartment membrane stack configuration, which is composed of alternating stacking of bipolar membranes and cation exchange membranes. Water distribution partitions are arranged between adjacent membranes, and the materials used are one or more of epoxy resin, polytetrafluoroethylene, glass fiber reinforced polypropylene or polyethylene terephthalate.
[0012] Due to the thermal stability limitations of membrane materials and their supporting water-distributing baffles, conventional electrodialysis equipment can generally only operate within the normal temperature range (5-35°C). However, in order to obtain a high-concentration acid solution to achieve a high solid recovery rate in the subsequent cooling and recrystallization process, the above-mentioned conversion of ammonium salts to acid and base must be carried out at high temperatures (50-95°C), and conventional bipolar membrane electrodialysis equipment cannot meet the above requirements.
[0013] The present invention adopts a new design of bipolar membrane electrodialysis membrane stack suitable for high temperature operation environment, so that its operating temperature can be increased from 5 to 35 o C is expanded to a wider temperature range of 5‒90℃. In bipolar membrane electrodialysis systems, with the continuous advancement of the ion membrane industry, it is no longer the ion exchange membrane material that restricts the upper limit of the system's operating temperature, but the water distribution baffle. Conventional baffle materials, including PE, PP, EVA and other materials, tend to soften and lose their mechanical strength in an environment ≥40℃ due to their low glass transition temperature, causing overall deformation of the membrane stack and failure of the flow channel. The present invention redesigns and customizes the water distribution baffle using materials with better temperature resistance, including epoxy resin, polytetrafluoroethylene (PTFE), glass fiber reinforced polypropylene (FRPP) or polyethylene terephthalate (PET), etc., and its stable operating temperature can be widened to 100℃.
[0014] In the present invention, NH 3 The gas absorption device 4 comprises an ammonia removal tower 5 and an ammonia absorption tower 6 .
[0015] In the present invention, NH 3 The gas absorption device 4 comprises an ammonia removal membrane assembly 7 , in which a hydrophobic porous ammonia removal membrane 8 is installed.
[0016] In the present invention, the hydrophobic porous ammonia removal membrane 8 uses a polytetrafluoroethylene hollow fiber degassing membrane.
[0017] In the process of bipolar membrane acid and alkali production, the product acid solution and the alkali solution are in contact with each other through the ion membrane material in the membrane stack. The non-ideal selectivity and defects of the membrane will cause some impurity ions in the initial raw materials to leak / migrate into the product alkali solution (ammonia water). In the previous work (patent application number 202110641428.4), it was found that anionic impurities (such as Cl - 、NO 3 - 、SO 4 2- ) ratio is 4‒8%, resulting in alkali products failing to meet the quality requirements of the capacitor industry.
[0018] To address the problem of some impurity ions in the initial raw materials leaking / migrating into the product alkaline solution (ammonia water) (such as Figure 2 As shown in the figure, the present invention proposes a new idea of recovering ammonia in the form of ammonia gas. By taking advantage of the fact that high-concentration ammonia solution is easy to volatilize (high vapor pressure) at high temperature, high-purity NH 3 Ammonia is recovered in the form of gas, which completely eliminates the problem of impurity ion leakage. The leakage rate of various impurity ions that are difficult to volatilize is basically 0 (<0.1%).
[0019] Another object of the present invention is to provide a method for purifying a capacitor-grade high-purity ammonium salt, comprising the following steps:
[0020] (1) Heat the ammonium salt solution to be treated to 50-95°C;
[0021] (2) introducing the ammonium salt solution obtained in step (1) into the acid chamber of a bipolar membrane electrodialyzer, treating it with a bipolar membrane electrodialyzer, maintaining the temperature of the acid chamber and the alkaline chamber of the bipolar membrane electrodialyzer between 50 and 95° C., and treating to obtain an acid solution and an alkaline solution; wherein the material used for the water distribution baffle of the bipolar membrane electrodialyzer is one or more of epoxy resin, polytetrafluoroethylene, glass fiber reinforced polypropylene or polyethylene terephthalate;
[0022] (3) cooling the acid solution obtained in step (2) and crystallizing it to obtain solid acid crystals;
[0023] (4) The alkaline solution obtained in step (2) is introduced into NH 3 After the gas absorption device is deammonified, it is input into the alkaline chamber of the bipolar membrane electrodialyzer;
[0024] (5) The solid acid crystals obtained in step (3) are mixed with pure water to prepare an acidic solution for NH 3 NH in the absorption unit 3 Absorb liquid flow.
[0025] In the present invention, in step (2), the operation of the bipolar membrane electrodialyzer is stopped when the conductivity of the acid chamber is between 2.5 and 5 mS / cm.
[0026] In the present invention, NH 3 The gas absorption device uses an ammonia removal tower and an ammonia absorption tower.
[0027] In the present invention, NH 3 The gas absorption device uses a polytetrafluoroethylene hollow fiber degassing membrane to deammonify the alkali chamber solution.
[0028] The purification method of the present invention has a brief processing flow as follows: Figure 3 As shown:
[0029] (1) Use bipolar membrane electrodialysis technology to convert the ammonium salt solution containing impurities into the corresponding acid solution and alkali (ammonia) solution. The characteristics of this step are: (i) The conversion is carried out at high temperature (50-90°C) to ensure that the acid with low solubility at room temperature can be completely dissolved at this time; (ii) The bipolar membrane electrodialysis stack adopts a bipolar membrane + cationic membrane two-compartment configuration, and most of the anionic impurities in the original feed solution (such as Cl - 、NO 3 - 、SO 4 2- etc.) stay in the acid chamber liquid flow; (iii) the initial solution for receiving the alkali (ammonia water) can be pure water, a feed solution of the original ammonium salt, or a mixture thereof;
[0030] (2) Cooling the acid chamber liquid product (high-temperature, high-concentration acid solution) causes the acid solute therein to precipitate in the form of crystals, and obtaining a pure recovered acid solid product through solid-liquid separation;
[0031] (3) Ammonia water easily evaporates at high temperature to produce NH 3 Gas characteristics, NH 3 The pure alkali in the product solution of the alkali chamber is recovered in the form of gas. 3 Gas absorption can be achieved by re-preparing the recovered acid solid into an acid solution to absorb NH 3 Gas. The preferred gas absorption method is a gas absorption tower or a hydrophobic and permeable deammoniation membrane adsorption method. Remove part / all of the NH 3 The alkaline chamber solution can be recycled and reused as the alkaline chamber feed solution for bipolar membrane electrodialysis.
[0032] The beneficial effects of the present invention are:
[0033] The device proposed in the present invention has a bipolar membrane electrodialysis membrane stack that is newly designed to be suitable for high temperature operating environments, so that its operating temperature can be increased from 5 to 35 oC to expand the temperature range to 5-90 o C. The water distribution baffles were redesigned and customized using materials with better temperature resistance, including epoxy resin, PTFE, FRPP (glass fiber reinforced PP), PET, etc., so that its stable operating temperature can be extended to 100 o C. At the same time, the present invention proposes a new idea of recovering ammonia in the form of ammonia gas. By taking advantage of the fact that high-concentration ammonia solution is easy to volatilize (high vapor pressure) at high temperature, high-purity NH 3 Ammonia is recovered in the form of gas, which completely eliminates the problem of impurity ion leakage. The leakage rate of various impurity ions that are difficult to volatilize is basically 0 (<0.1%).
[0034] The method proposed by the present invention converts the original ammonium salt into the corresponding acid and ammonia solution by inputting electric energy; then, a pure acid solid product is obtained by cooling and recrystallizing, and a pure ammonia product is obtained by volatilizing and recovering ammonia water. The combination of the two obtains a capacitor-grade high-purity ammonium salt solute, which can be applied to the aluminum electrolytic capacitor industry. In the present invention: (1) the entire purification process does not require the addition of any additional substances to the system, eliminating the possibility of introducing additional impurities; (2) the acid radical ion component in the final ammonium salt product is purified by recrystallization, and the ammonium ion component is purified by gas-liquid separation. This is equivalent to selectively separating the acid radical ions and ammonium ions from the original ammonium salt raw material, avoiding the removal of all other possible impurity ions, and can achieve the preparation of capacitor-grade high-purity ammonium salt solute in one step. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a schematic diagram of the internal structure of the bipolar membrane electrodialyzer of the purification device of the present invention, wherein a is the basic repeating unit of the membrane stack structure, b is the cation membrane, c is the bipolar membrane, and d is the water distribution partition.
[0036] Figure 2 This is a schematic diagram of material migration inside the bipolar membrane electrodialyzer used in the present invention.
[0037] Figure 3 This is a device diagram for purifying and producing capacitor-grade high-purity ammonium salt solute using low-grade ammonium salt solution as raw material, where 1 is a bipolar membrane electrodialyzer, 2 is a heating device, 3 is a cooling crystallization and solid-liquid separation device, 4 is NH 3 Gas absorption device.
[0038] Figure 4 It is a NH4+ tower using ammonia removal tower and ammonia absorption tower. 3 Gas absorption device design diagram. 5 is a deammoniation tower, which is used to remove NH 3 6 is an ammonia absorption tower, which uses an acid solution to absorb NH in the gas flow. 3 The gas generates a high-purity ammonium salt solution product.
[0039] Figure 5 A hydrophobic, breathable, ammonia removal membrane 3 Design drawing of gas absorption device, wherein 7 is a deammoniation membrane assembly and 8 is a hydrophobic porous deammoniation membrane made of PP or PTFE. DETAILED DESCRIPTION
[0040] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0041] The purification device of the capacitor-grade high-purity ammonium salt of the present invention is as follows Figure 3 As shown, it includes a bipolar membrane electrodialyzer 1 (EDBM), a heating device 2, a cooling crystallization and solid-liquid separation device 3 and NH 3 Gas absorption device 4; wherein the heating device 2 is connected to the inlet of the acid chamber of the bipolar membrane electrodialyzer by a pipeline, and the outlet of the acid chamber is connected to the inlet of the cooling crystallization and solid-liquid separation device, NH 3 The deamination side inlet of the gas absorption device 4 is connected to the outlet of the alkali chamber of the bipolar membrane electrodialyzer, and the deamination side outlet is connected to the inlet of the alkali chamber of the bipolar membrane electrodialyzer;
[0042] Among them, Figure 1 As shown, a bipolar membrane plus a cation exchange membrane two-compartment membrane stack configuration is adopted, which is composed of alternating stacking of bipolar membranes and cation exchange membranes. Water distribution baffles are arranged between adjacent membranes. The material used for the water distribution baffles is one or more of epoxy resin, polytetrafluoroethylene (PTFE), glass fiber reinforced polypropylene (FRPP) or polyethylene terephthalate (PET).
[0043] A method for purifying a capacitor-grade high-purity ammonium salt proposed by the present invention is as follows: Figure 3 As shown. First, the ammonium salt solution to be treated (low-grade raw materials, or waste chemical liquid from the electrode foil industry) is heated to a suitable temperature and introduced into the acid chamber of the bipolar membrane electrodialyzer 1. During the EDBM treatment process, the ammonium salt solution is converted into the corresponding acid solution and alkali (ammonia water) solution. The hot acid solution treated with EDBM can be cooled and crystallized to obtain solid acid crystals, and pure recovered acid crystals can be obtained after filter pressing or centrifugal drying; free NH 3 High concentration, can be used in NH 3 Part of the NH recovered in the gas absorption device 3 The hot solution after partial deammoniation is recycled as the feed liquid for the EDBM alkali chamber. At the same time, the recovered pure solid acid is reconstituted with pure water into a clean acid solution for NH 3 NH in the absorption unit 3 The absorption liquid stream absorbs NH 3 After the gas is extracted, clean high-purity ammonium salt can be recovered.
[0044] Example 1: In the above-mentioned method for purifying capacitor-grade high-purity ammonium salt solutes, the waste ammonium adipate electrolyte from an electrode foil manufacturer is used as the inlet liquid, and its composition is ammonium adipate 100 g / L (equivalent to 0.55 mol / L), Cl - Impurities 60 mg / L, Na + Impurities 7.0 mg / L. First, the feed liquid is heated to 60℃ and introduced into the bipolar membrane EDBM acid chamber. Pure water is used as the feed liquid for the EDBM alkali chamber. A heat exchanger is used to maintain the temperature of the EDBM system acid / alkali chamber between 50-60℃. When the conductivity of the acid chamber drops from ~70mS / cm to 2.5 mS / cm, the EDBM operation is stopped. The EDBM water distribution baffle is made of FRPP material. The NH in the waste ammonium adipate feed solution was obtained through experimental analysis. 4 + The removal rate is 99%, Na + The removal rate was 98%, Cl - The removal rate was 6-8%. After the solution was cooled from 60°C to 5°C and kept warm for 2 hours, a large number of needle-shaped white crystals were obtained. After centrifugation (3000 rpm), granular white crystals were obtained. The residual Cl in the solid was analyzed. - The impurity is 8 mg / kg (removal rate> 98.5%), Na + Not detected (<1.0 mg / kg). The product solution of the alkali chamber is ammonia water (~1.1 mol / L) solution mixed with a small amount of ammonium adipate (~8 g / L), Cl - (5-6 mg / L) and Na + (~6 mg / L) impurities. The alkali chamber solution was deaminated using a PTFE hollow fiber degassing membrane. A 0.55 mol / L (equivalent to ~80 g / L) adipic acid solution was prepared using the previously recovered adipic acid crystals as the absorption liquid. The deammoniation membrane assembly operated at 60 o At temperature C, Figure 5 After the deammoniation membrane treatment, NH 3 The gas removal rate is 84%, and other impurity ions (such as Na + , Cl - When the pH of the receiving liquid flow in the degassing membrane rises from 2.0 to 7.2, a stoichiometrically pure ammonium adipate recovery solution can be obtained, with a concentration of ~100 g / L and an overall recovery rate of ~90%; residual Cl - 0.9 mg / L (removal rate> 98.5%), Na + Undetectable (<0.1 mg / L, removal rate>99.9%), meeting the capacitance purity requirements of the electrode foil industry and can be directly reused in the chemical production line.
[0045] Example 2: The deamination device in Example 1 is replaced by a deamination / ammonia absorption tower from a PTFE hollow fiber membrane. Figure 4 As shown in the figure, the water distribution baffle was replaced with PTFE material, and other operating conditions remained unchanged. The pH of the high-purity ammonium salt solution finally obtained was 7.1, its concentration was ~100 g / L, and the overall recovery rate was ~90%; the residual Cl - 1.2 mg / L (removal rate 98%), Na + 0.5 mg / L (removal rate 93%), meeting the capacitance purity requirements of the electrode foil industry.
[0046] Example 3: In order to verify the removal efficiency of other impurity ions of the present invention, other impurity elements, including Na + (added in the form of NaOH), K + (in the form of KOH), Cl - (in the form of HCl), SO 4 2- (H 2 SO 4 form), NO 3 - (HNO 3 The above impurity ion content is 100 mg / L. Since the relative amount of impurities added is very small, the ammonium adipate content of the feed liquid remains unchanged at 100 g / L. The working temperature and other operating conditions of EDBM (the material of the water distribution partition is PET) and PTFE degassing membrane are the same as those in Example 1. The final recovered ammonium adipate concentration is still ~100 g / L, and the recovery rate is ~90%; the residual Cl - The concentration was 1.4 mg / L, and the removal rate was 98.6%; the residual SO 4 2- The concentration was 2.0 mg / L, and the removal rate was 98.0%; the residual NO 3 - The concentration was 1.2 mg / L, and the removal rate was 98.8%; the residual Na + and K + None of them were detected (< 0.1mg / L), and the removal rate was >99.9%. The recycled products meet the capacitance purity requirements of the electrode foil industry and can be directly reused.
[0047] Example 4: A small amount of ammonium succinate and ammonium oxalate (added in pure solid form) impurities were added to the discarded ammonium adipate electrolyte of Example 1, and the concentrations were both 1000 mg / L. The material used for the water distribution baffle was PET, and the other operating conditions were the same as those of Example 1. The final recovered ammonium adipate concentration was still ~100 g / L, with a recovery rate of ~90%; the residual ammonium succinate concentration was 66 mg / L, with a removal rate of 93.4%; the residual ammonium oxalate concentration was 40 mg / L, with a removal rate of 96.0%. The recovered product meets the capacitance purity requirements of the electrode foil industry and can be directly reused.
[0048] Example 5: In order to improve the overall recovery rate of ammonium adipate, the waste ammonium adipate in Example 1 was heated to 80 o C was evaporated under reduced pressure to concentrate to ~40% of the original volume. At this time, the liquid composition became ammonium adipate 250g / L (equivalent to 1.38mol / L), Cl - Impurities 150 mg / L, Na + The impurities were 18 mg / L, and this solution was used as the feed liquid for the EDBM acid chamber. The material used for the water distribution partition was epoxy resin. Unconcentrated waste ammonium adipate feed liquid (ammonium adipate 100 g / L, Cl - The impurities were 60 mg / L) as the feed solution for the EDBM alkali chamber. The EDBM operating temperature was adjusted to 80°C, and the EDBM operation was stopped when the conductivity of ammonium adipate in the acid chamber dropped to 5 mS / cm; when the EDBM was working, the PTFE deamination membrane was operated simultaneously with the EDBM, and its operating temperature was also 80°C. The acid chamber product solution was cooled from 80°C to 5°C, and a large amount of white crystals were obtained and recovered by centrifugation. The recovered acid crystals obtained in the previous time were dissolved in hot water to obtain a 1.4 mol / L (equivalent to 200 g / L) adipic acid solution as the receiving solution in the degassing membrane. The EDBM and the deamination membrane unit were operated simultaneously, and the temperature was maintained at 80°C. The final recovered ammonium adipate concentration was 260 g / L, and the overall recovery rate was ~96%; the residual Cl - 2.1 mg / L (removal rate 98.5%), meeting the capacitance purity requirements of the electrode foil industry and can be directly reused.
[0049] Example 6: Take chemically pure ammonium pentaborate solid (where Cl - Impurity content: 70 mg / kg, Na +The impurity content is 180mg / kg) dissolved in 90℃ hot water to obtain a 280 g / L ammonium pentaborate solution, which is used as the EDBM acid chamber feed solution. The material used for the water distribution baffle is epoxy resin. Take another part of the above solution and dilute it with 90℃ pure water (the volume ratio of solution to pure water is 1:1). The diluted solution is used as the EDBM alkali chamber feed solution. EDBM treatment is stopped when the conductivity of the acid chamber feed solution no longer decreases (the conductivity is generally < 4mS / cm), and the acid chamber solution is discharged, cooled and frozen to 2℃. At this time, there is a large amount of H 3 BO 3 The crystals were precipitated, filtered using a filter press and pressed and purged with compressed air to obtain the solid boric acid containing Cl - Impurity residue 5.0 mg / kg, Na + The impurity content is 1.2 mg / kg. The PTFE deamination membrane is still used as the ammonia recovery device to recover the H 3 BO 3 Redissolve in 90℃ hot pure water as NH 3 The absorption liquid, EDBM and PTFE deamination were operated simultaneously. The pH of the high-purity ammonium salt recovery solution finally obtained was 7.0, the concentration of ammonium pentaborate was 270 g / L, the ratio of borate to ammonium ion was qualified, and the Cl in the solution was - Impurity residue 1.3 mg / L (removal rate 93%), Na + The impurity content is 0.3 mg / L (removal rate 99.4%), which meets the capacitance purity requirements of the electrode foil industry and can be directly used for formation and capacitor assembly.
Claims
1. A purification device for capacitor-grade high-purity ammonium salt, characterized in that: The invention comprises a bipolar membrane electrodialyser (1), a heating device (2), a cooling crystallization and solid-liquid separation device (3) and an NH3 gas absorption device (4) connected by pipelines; wherein the heating device (2) is connected to the inlet of the acid chamber of the bipolar membrane electrodialyser through the pipeline, the outlet of the acid chamber of the bipolar membrane electrodialyser is connected to the inlet of the cooling crystallization and solid-liquid separation device (3), the inlet of the deammoniation side of the NH3 gas absorption device (4) is connected to the outlet of the alkali chamber of the bipolar membrane electrodialyser (1), and the outlet of the deammoniation side of the NH3 gas absorption device (4) is connected to the inlet of the alkali chamber of the bipolar membrane electrodialyser (1); the outlet of the cooling crystallization and solid-liquid separation device (3) is connected to the inlet of the NH3 gas absorption device (4), the NH3 gas absorption device (4) comprises a deammoniation tower (5) and an ammonia absorption tower (6), or the NH3 gas absorption device (4) comprises a deammoniation membrane assembly (7), and a hydrophobic porous deammoniation membrane (8) is installed in the deammoniation membrane assembly (7).
2. The purification device according to claim 1, characterized in that: The bipolar membrane electrodialyser (1) adopts a bipolar membrane plus a cation exchange membrane two-compartment membrane stack configuration, which is composed of bipolar membranes and cation exchange membranes stacked alternately, and water distribution baffles are arranged between adjacent membranes. The material used is one or more of epoxy resin, polytetrafluoroethylene, glass fiber reinforced polypropylene or polyethylene terephthalate.
3. The purification device according to claim 1, characterized in that: The hydrophobic porous ammonia removal membrane (8) uses a polytetrafluoroethylene hollow fiber degassing membrane.
4. A purification method according to any one of claims 1 to 3, characterized in that the capacitor-grade high-purity ammonium salt purification device The following steps are involved: (1) heating the ammonium salt solution to be treated to 50-95°C; (2) introducing the ammonium salt solution obtained in step (1) into the acid chamber of a bipolar membrane electrodialyzer, treating it with a bipolar membrane electrodialyzer, maintaining the temperature of the acid chamber and the alkaline chamber of the bipolar membrane electrodialyzer between 50° C. and 95° C., and treating to obtain an acid solution and an alkaline solution; wherein the material used for the water distribution baffle of the bipolar membrane electrodialyzer is one or more of epoxy resin, polytetrafluoroethylene, glass fiber reinforced polypropylene or polyethylene terephthalate; (3) cooling the acid solution obtained in step (2) and crystallizing it to obtain solid acid crystals; (4) the alkaline solution obtained in step (2) is input into the NH3 gas absorption device for deammoniation treatment, and then input into the alkaline chamber of the bipolar membrane electrodialyzer; (5) The solid acid crystals obtained in step (3) are mixed with pure water to prepare an acidic solution for use as the NH3 absorption liquid flow in the NH3 gas absorption device.
5. The purification method according to claim 4, characterized in that When the conductivity of the acid chamber in step (2) is between 2.5 and 5 mS / cm, the operation of the bipolar membrane electrodialyzer is stopped.
6. The purification method according to claim 4, characterized in that The NH3 gas absorption device in step (4) uses an ammonia removal tower and an ammonia absorption tower.
7. The purification method according to claim 4, characterized in that The NH3 gas absorption device in step (4) uses a polytetrafluoroethylene hollow fiber degassing membrane to deammoniate the alkali chamber solution.
Citation Information
Patent Citations
Method for recycling waste liquor of ammonium hexanedioic acid and recycling system thereof
CN101219946B
Zero-discharge treatment method for recycling and utilization of aluminum foil formation ammonium adipate wastewater
CN110759554A
Ammonium adipate waste liquid recovery method and device based on high-temperature bipolar membrane electrodialysis
CN113274882A
Bipolar electrodialyzer and purification method for amine fluid using same