Metal super-hydrophobic surface preparation method and laser processing equipment
The metal surface is laser scanned using laser processing equipment to form a conical micro-nano structure, which solves the problems of contamination and difficulty in cleaning during the preparation of metal superhydrophobic surfaces and achieves efficient superhydrophobic effects.
Patent Information
- Application Number
- CN202111173206.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-10-08
AI Technical Summary
When preparing metal superhydrophobic surfaces with existing technology, it is easy to cause metal to be polluted by the environment and the surface is inconvenient to clean. Especially after treatment with fluoride, the metal surface is prone to corrosion and stains and solvents are attached and difficult to clean.
Using laser processing equipment, by controlling the laser parameters and scanning path of the laser emitter, at least two sets of laser scanning processes are performed on the metal surface to form a conical micro-nano structure, thereby achieving a super-hydrophobic surface without adding chemicals such as fluoride.
It achieves the super-hydrophobic effect on the metal surface, while avoiding the problems of environmental pollution and inconvenient cleaning of the surface. It is easy to operate and does not require the use of harmful chemicals.
Smart Images

Figure CN114012271B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal material surface modification, and in particular to a metal super-hydrophobic surface preparation method and laser processing equipment. Background Art
[0002] Bionic superhydrophobic materials have become a research hotspot at home and abroad in recent years due to their potential applications in self-cleaning, microfluidic systems, biocompatibility, etc., especially from the perspective of actual application conditions in the engineering field. How to obtain excellent superhydrophobic properties on the surfaces of different types of materials is a challenging task for researchers at present.
[0003] The metal surface is inherently hydrophilic due to its high surface free energy. Almost all liquids can easily spread and wet the metal surface. Before marking the metal, the metal surface needs to be treated to reduce the surface free energy of the material on the metal surface, so as to obtain a super hydrophobic surface. The general treatment technology is to add fluoride to the metal surface, and then reduce the surface free energy of the material on the metal surface by combining laser with fluoride. This will make the metal susceptible to environmental corrosion on the one hand, and on the other hand, it will easily cause the metal surface to be uneven, stains and solvents are easy to adhere, and it is not easy to clean, affecting the user experience.
[0004] The above contents are only used to assist in understanding the technical solution of the present invention and do not constitute an admission that the above contents are prior art. Summary of the invention
[0005] The main purpose of the present invention is to provide a method for preparing a metal super-hydrophobic surface and a laser processing device, aiming to solve the problem that when preparing a metal super-hydrophobic surface by adding fluoride, the metal is easily polluted by the environment and the surface feels difficult to clean.
[0006] To achieve the above object, the present invention provides a method for preparing a metal super-hydrophobic surface, the steps of the method for preparing a metal super-hydrophobic surface comprising:
[0007] Acquiring control parameters corresponding to the metal to be processed, wherein the control parameters include laser parameters and scanning paths;
[0008] Controlling the laser emitter of the laser processing equipment to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path using the laser parameters, so as to process the metal surface of the metal to be processed into a conical micro-nano structure and thus form a super-hydrophobic surface;
[0009] The laser processing equipment includes a laser emitter and a control system, wherein the laser emitter is a picosecond laser; the control system is used to set the laser parameters and scanning path of the laser emitter, wherein the laser parameters include at least one of the focal length of the field lens, pulse width, power, frequency, scanning speed, scanning spacing, and number of scans.
[0010] Optionally, the laser parameters include: field lens focal length of F100 to F160, pulse width of 10ps to 15ps, power of 6W to 7W, frequency of 400-500KHz, scanning speed of 4500mm / s to 5500mm / s, scanning spacing of 0.001mm to 0.005mm, and number of scans of 50 to 250 times.
[0011] Optionally, the scanning path includes a first scanning path and a second scanning path, the first scanning path includes a square grid scanning path composed of at least two groups of mutually parallel first straight line scanning paths, the second scanning path includes a square grid scanning path composed of at least two groups of mutually parallel second straight line scanning paths, the first straight line width corresponding to the first straight line is greater than the second straight line width corresponding to the second straight line, the first straight line width is 0.02 mm, and the second straight line width is 0.01 mm.
[0012] Optionally, the preset angles corresponding to the at least two groups of first straight scanning paths and the at least two groups of second straight scanning paths respectively corresponding to the first scanning path and / or the second scanning path are in a range of 30 degrees to 90 degrees.
[0013] Optionally, the preset angle is 30 degrees.
[0014] Optionally, the step of controlling the laser emitter of the laser processing equipment to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path using the laser parameters includes:
[0015] Controlling the laser emitter to perform a first scan on the metal to be processed along the first scanning path using the laser parameters to obtain a cylindrical micro-nano structure distributed in a grid pattern;
[0016] After completing the first scan, the laser emitter is controlled to use the laser parameters to perform a second scan on the metal to be processed along the second scanning path to obtain a grid-shaped distributed conical micro-nano structure, thereby forming a super-hydrophobic metal surface.
[0017] Optionally, after completing the first scan, controlling the laser emitter to use the laser parameters to perform a second scan on the metal to be processed along the second scanning path to obtain a grid-shaped cone micro-nano structure, thereby forming a super-hydrophobic metal surface, further comprising:
[0018] Get the current number of scans;
[0019] When the current number of scans is consistent with the number of scans in the laser parameters, a step is performed to control the laser emitter to perform a second scan on the metal to be processed along the second scanning path using the laser parameters.
[0020] Optionally, the laser emitter is an ultraviolet picosecond laser emitter.
[0021] In addition, to achieve the above-mentioned purpose, the present invention further provides a laser processing device, the laser processing device comprising a laser emitter and a control system, the laser emitter being a picosecond laser emitter; the control system being used to set laser parameters for the operation of the laser emitter, the laser parameters comprising at least one of scene focal length, pulse width, power, scanning speed, scanning spacing, and scanning times;
[0022] The control system is also used to control the laser emitter of the laser processing equipment to use the laser parameters to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path, so as to process the metal surface of the metal to be processed into a conical micro-nano structure and thus form a super-hydrophobic surface.
[0023] A method for preparing a metal super-hydrophobic surface and a laser processing device proposed in an embodiment of the present invention obtain control parameters corresponding to the metal to be processed after cleaning the metal surface of the metal to be processed, wherein the control parameters include laser parameters and a scanning path, wherein the laser parameters are operating parameters of the laser when the laser emitter controls the laser to emit the laser, and the scanning path is used to control the laser emission trajectory of the laser emitter emitting the laser. The present application only needs to set the laser parameters and the scanning path when the laser processing equipment is running, and then control the laser emitter of the laser processing equipment to use the laser parameters to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path, so that the metal surface of the metal to be processed can be processed into a conical micro-nano structure without the need to add additional chemicals such as fluorides. The operation is simple, and the problem that the metal is easily polluted by the environment and the surface is inconvenient to clean when the metal super-hydrophobic surface is prepared by adding fluorides is solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the structure of a laser processing device in a hardware operating environment involved in an embodiment of the present invention;
[0025] Figure 2 This is a schematic diagram of the scanning path of the present invention;
[0026] Figure 3 This is another example diagram of the scanning path of the present invention;
[0027] Figure 4 It is a schematic diagram of the cone microstructure of the present invention;
[0028] Figure 5 Schematic diagram of the process of the first embodiment of the method for preparing a metal super-hydrophobic surface according to the present invention.
[0029] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0030] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
[0031] The main solution of the embodiment of the present invention is: obtaining control parameters corresponding to the metal to be processed, the control parameters including laser parameters and scanning paths; controlling the laser emitter of the laser processing equipment to use the laser parameters to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path, so as to process the metal surface of the metal to be processed into a conical micro-nano structure and thus form a super-hydrophobic surface; the laser processing equipment includes a laser emitter and a control system, the laser emitter is a picosecond laser; the control system is used to set the laser parameters and scanning path of the laser emitter, the laser parameters including at least one of the focal length of the field lens, pulse width, power, frequency, scanning speed, scanning spacing, and number of scans.
[0032] like Figure 1 As shown, Figure 1 It is a schematic diagram of the structure of the laser processing equipment in the hardware operating environment involved in the embodiment of the present invention.
[0033] like Figure 1 As shown, a laser processing device is used to process ceramic products. The laser processing device includes a processing platform 100. The processing platform 100 has a table. The processing platform 100 is used to place the metal to be processed. The metal to be processed can be stainless steel, zirconium, or titanium. It is understood that the metal to be processed includes but is not limited to the above-mentioned types. A laser emitter 200, a control system (not shown in the figure) and a laser adjustment device 300 are installed on the table. Optionally, the laser emitter 200 can be an infrared laser emitter, an ultraviolet laser emitter, and an X-ray laser emitter. In order to ensure the efficiency of laser marking, the laser emitter 200 can be an infrared laser emitter or an ultraviolet laser emitter, that is, it can be an infrared nanosecond laser emitter, an infrared picosecond laser emitter, an ultraviolet nanosecond laser emitter, or an ultraviolet picosecond laser emitter. It is understood that in this technical solution, the laser emitter 200 can be one, or two or more.
[0034] Optionally, in an embodiment of the present application, the laser emitter 200 is an ultraviolet picosecond laser emitter.
[0035] Optionally, the laser processing equipment further includes a control system, which is used to set the laser parameters and scanning path of the laser emitter 200. The control system controls the laser emitter 200 to emit laser with the set laser parameters and controls the laser emitter to emit laser along the set scanning path using the set laser parameters.
[0036] Optionally, the control system sets the scanning path in such a way that after receiving a preset marking pattern input by a user, the control system of the laser processing equipment generates a scanning path based on the preset marking pattern, and then controls the laser emitter to use laser parameters to emit laser along the scanning path to the metal surface of the metal to be processed. It is understandable that the laser processing equipment also includes a galvanometer, which is used to adjust the emission angle and emission direction of the laser emitter. The specific implementation of the control system controlling the laser emitter to use laser parameters to emit laser along the scanning path to the metal surface of the metal to be processed is to control the galvanometer to adjust the emission angle and / or emission direction of the laser emitter based on the scanning path, so that the laser emitter emits laser along the scanning path to the metal surface of the metal to be processed.
[0037] Optionally, in another embodiment, after receiving a preset marking pattern input by a user, the control system determines a preset marking position on the metal surface according to the preset marking pattern, and then controls the laser emitter to emit laser at the preset marking position to form a corresponding preset marking pattern.
[0038] Optionally, in an embodiment of the present application, the laser parameters include: when the laser processing equipment performs laser scanning processing, the laser parameters of the laser emitter include: the focal length of the field lens is F100 to F160, the pulse width is 10ps to 15ps, the power is 6W to 7W, the frequency is 400-500KHz, the scanning speed is 4500mm / s to 5500mm / s, the scanning spacing is 0.001mm to 0.005mm, and the number of scans is 50 to 250 times.
[0039] Optionally, the laser parameters may also be determined according to the type of metal to be processed, and the laser parameters corresponding to different types of metals to be processed may be different or the same.
[0040] Optionally, when the metal to be processed is zirconium, the laser parameters include: the field lens focal length is F100 to F160, the pulse width is 10ps to 15ps, the power is 6.5W, the frequency is 400KHz, the scanning speed is 5000mm / s, the scanning spacing is 0.001mm to 0.005mm, and the number of scans is 250 to 500 times.
[0041] Optionally, when the metal to be processed is stainless steel or titanium, the laser parameters include: field lens focal length of F100 to F160, pulse width of 10ps to 15ps, power of 7W, frequency of 400KHz, scanning speed of 5000mm / s, scanning spacing of 0.001mm to 0.005mm, and scanning times of 250 to 500 times.
[0042] Optionally, the laser processing equipment is controlled to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path using the laser parameters, and the corresponding laser parameters of each laser scanning process may be the same or different.
[0043] Optionally, in another embodiment, the laser parameters include first laser parameters and second laser parameters, the first laser parameters include: field lens focal length of F100 to F160, pulse width of 10ps to 15ps, power of 6W to 7W, frequency of 400-500KHz, scanning speed of 4500mm / s to 5500mm / s, scanning spacing of 0.005mm, and number of scans of 50 to 250 times; the second laser parameters include: field lens focal length of F100 to F160, pulse width of 10ps to 15ps, power of 6W to 7W, frequency of 400-500KHz, scanning speed of 4500mm / s to 5500mm / s, scanning spacing of 0.001mm, and number of scans of 50 to 250 times.
[0044] It is understandable that the effect of laser preparation of metal super-hydrophobic surface is not affected by only a single parameter. The laser pulse width, power, frequency, scanning speed and filling spacing all affect the effect of laser preparation of metal super-hydrophobic surface. During the preparation process, it can be adjusted in real time according to the metal to be treated to achieve the corresponding effect.
[0045] Optionally, the laser adjustment device 300 may be a galvanometer, and the laser adjustment device 300 is used to adjust the emission direction and emission angle of the laser emitter 200. After setting the preset laser parameters for the operation of the laser emitter, the emission direction and emission angle of the laser emitter 200 are adjusted by controlling the laser adjustment device 300 so that the laser emitted by the laser emitter 200 is directed toward the metal to be processed.
[0046] Optionally, the laser adjustment device 300 also includes a galvanometer, a beam expander and a focusing mirror, the beam expander is used to expand the diameter of the laser; the galvanometer is used to deflect the laser; the focusing mirror is used to focus the laser on the metal surface of the metal to be processed. In the embodiment of the present application, the laser emitter is a picosecond laser, and the control system is used to set the laser parameters of the laser emitter 200. The laser emitted by the laser emitter 200 according to the laser parameters, the laser is sequentially expanded by the beam expander, the galvanometer 230 changes the direction of the laser beam, and the focusing mirror focuses, and then reaches the metal surface of the metal to be processed and acts on the metal surface.
[0047] Optionally, when controlling the laser emitter to emit laser to the metal surface of the metal to be processed along the scanning path based on preset laser parameters, corresponding grooves are formed at the places where the laser is irradiated. Based on the fact that the laser emitted by the laser emitter is a Gaussian laser beam, the closer to the focus, the deeper the depth. The place not irradiated by the laser is equivalent to a protrusion relative to the groove. Based on the fact that the laser emitter emits laser on the metal surface along the scanning path, protrusions and grooves are formed on the metal surface. Based on the fact that the scanning path is generated by a preset marking pattern, the grooves form the preset marking pattern on the metal surface.
[0048] Optionally, the scanning path includes a first scanning path and a second scanning path, the first scanning path includes a square grid scanning path composed of at least two groups of mutually parallel first straight scanning paths, the second scanning path includes a square grid scanning path composed of at least two groups of mutually parallel second straight scanning paths, the first straight line width corresponding to the first straight scanning path is greater than the second straight line width corresponding to the second straight scanning path, optionally, the first straight line width is 0.02mm, and the second straight line width is 0.01mm. Figure 2 As shown, the scanning path includes a first scanning path and a second scanning path, the first scanning path includes a square grid scanning path composed of two groups of mutually parallel first straight line scanning paths, the second scanning path includes a square grid scanning path composed of two groups of mutually parallel second straight line scanning paths, the first straight line width of the first scanning path is 0.05mm, the second straight line width is 0.01mm, and the preset angle corresponding to the two groups of first straight line scanning paths in the first scanning path is 90 degrees. It can be understood that the preset angle corresponding to the two groups of second straight line scanning paths in the second scanning path is the same as the preset angle corresponding to the two groups of first straight line scanning paths in the first scanning path, both of which are 90 degrees.
[0049] Optionally, in the embodiment of the present application, the preset angles corresponding to at least two groups of first straight scanning paths and at least two groups of second straight scanning paths respectively corresponding to the first scanning path and / or the second scanning path are 30 degrees to 90 degrees. Figure 3 As shown, Figure 3 The first scanning path corresponding to three groups of first straight scanning paths corresponding to the first scanning path has a preset angle of 30 degrees. Figure 3 The method includes three sets of mutually parallel first straight line scanning paths, namely, a first straight line scanning path A, a first straight line scanning path B, and a first straight line scanning path C. The first straight line scanning path A is horizontal, the angle between the first straight line scanning path B and the first straight line scanning path is +30 degrees, and the angle between the first straight line scanning path C and the first straight line scanning path is -30 degrees.
[0050] Optionally, the preset angle may be 30 degrees, 45 degrees, 60 degrees, or 90 degrees.
[0051] Optionally, in an embodiment of the present application, the preset angle is 30 degrees.
[0052] Optionally, after determining the first scanning path and the second scanning path, the control system is also used to control the laser emitter of the laser processing equipment to use the laser parameters to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path, so as to process the metal surface of the metal to be processed into a conical micro-nano structure and then form a super-hydrophobic surface. Specifically, the laser emitter 200 is controlled to perform a first scan on the metal to be processed from top to bottom and from left to right along the first scanning path. It can be understood that after the first scan, based on the square grid scanning path composed of at least two groups of mutually parallel first straight line scanning paths, the metal surface of the metal to be processed forms a grid-shaped cylindrical micro-nano structure.
[0053] Optionally, after completing the first scan, the laser emitter 200 is controlled to scan the metal to be processed for a second time along the second scanning path. When the metal to be processed is scanned for the second time, the laser continues to extend downward in the first groove obtained by the first scan to form a second groove similar to the first groove. The second straight line width of the second straight line scanning path corresponding to the second scanning path is smaller than the first straight line width, and the surface area of the second groove is smaller than the first groove. Then, the first groove and the second groove form a groove on the metal surface of the metal to be processed. It can be understood that conical protrusions are formed next to the groove, that is, a grid-shaped distributed conical micro-nano structure, thereby forming a super-hydrophobic metal surface. Figure 4As shown, Figure 4 A schematic diagram of the cone-shaped micro-nano structure on the metal surface of stainless steel is shown.
[0054] It can be understood that the conical micro-nano structure presents abundant nano-scale particles and burr-like nano-scale structures, thereby changing the wettability of the metal surface of the metal to be treated to obtain a metal super-hydrophobic surface, and the maximum contact angle of the metal super-hydrophobic surface can reach 165 degrees.
[0055] In an embodiment of the present application, a laser processing device is proposed, which includes a laser emitter 200 and a control system. The control system sets the laser parameters and scanning path of the laser emitter 200, and then controls the laser emitter 200 to use the laser parameters to perform at least two groups of laser scanning processes along the scanning path, so as to first prepare the metal surface of the metal to be processed into a cylindrical micro-nano structure with a grid distribution, and then transform the metal surface based on the cylindrical micro-nano structure into a conical micro-nano structure through a second scanning path with a small straight line width, thereby forming a super-hydrophobic metal surface. The present application only needs to set the laser parameters and scanning path when the laser processing equipment is running, and then control the laser processing equipment to use the laser parameters to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path to process the metal surface of the metal to be processed into a conical micro-nano structure, without the need to add additional chemicals such as fluorides, and the operation is simple, and it solves the problem that when preparing a super-hydrophobic surface of a metal by adding fluorides, it is easy to cause the metal to be polluted by the environment and the surface has a tactile feel that is inconvenient to clean.
[0056] Reference Figure 5 The first embodiment of the method for preparing a metal super-hydrophobic surface of the present invention provides a method for preparing a metal super-hydrophobic surface, and the method for preparing a metal super-hydrophobic surface comprises:
[0057] Step S10, obtaining control parameters corresponding to the metal to be processed, wherein the control parameters include laser parameters and scanning paths;
[0058] Step S20, controlling the laser emitter of the laser processing equipment to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path using the laser parameters, so as to process the metal surface of the metal to be processed into a conical micro-nano structure and thus form a super-hydrophobic surface;
[0059] The laser processing equipment includes a laser emitter and a control system, wherein the laser emitter is a picosecond laser; the control system is used to set the laser parameters and scanning path of the laser emitter, wherein the laser parameters include at least one of the focal length of the field lens, pulse width, power, frequency, scanning speed, scanning spacing, and number of scans.
[0060] In an embodiment of the present application, before obtaining the control parameters of the metal to be processed, the metal surface of the metal to be processed can be cleaned first, wherein the method of cleaning the metal surface of the metal to be processed includes: ultrasonically cleaning the metal to be processed with clean water at room temperature for 10 minutes to remove residual oil stains from surface machining.
[0061] Optionally, the method of cleaning the metal surface of the metal to be treated may also include wiping the metal surface of the metal to be treated with a non-woven fabric, or wiping it with deionized water or alcohol to remove dust or oil on the surface.
[0062] Optionally, control parameters corresponding to the metal to be processed are obtained, and the control parameters include laser parameters and scanning paths, wherein the laser parameters can be obtained by a user adaptively inputting corresponding input data through a configuration page of the laser device, and after receiving the user's input data, the control system of the laser processing device sets the laser parameters of the laser transmitter during operation according to the input data.
[0063] Optionally, the method for obtaining the laser parameters can also be that the system calls the laser parameters saved last time. It can be understood that after the user currently inputs the corresponding input data, the control system sets the laser parameters according to the input data and saves the laser parameters for direct call next time.
[0064] Optionally, the laser parameters include at least one of the focal length of the field lens, pulse width, power, frequency, scanning speed, scanning spacing and the number of scans, and the laser parameters may also include the focal position. It is understood that different parameter sizes have different effects on the preparation of metal super-hydrophobic surfaces. The laser parameters include the focal length of the field lens, which can change the position of the laser imaging beam. The focal length of the field lens has a certain relationship with the working distance. The spot size of the laser beam focus is related to the selected focal length of the field lens. The smaller the focal length of the field lens, the smaller the focused spot, and the more concentrated the energy. The pulse width refers to the duration of a single laser pulse. Since the laser is mainly embodied in thermal energy, the smaller the pulse width, the shorter the duration of the laser, the higher the peak power, and the easier it is to protect the metal surface, so as to prevent the destruction of ceramic products when preparing the metal super-hydrophobic surface. Power refers to the energy size of the laser beam emitted by the laser transmitter. If the energy is too large, it is easy to damage the metal to be processed, resulting in the destruction of the cone micro-nano structure on the metal surface; if it is too small, the laser processing conditions cannot be achieved, and the metal surface does not react. It is understandable that the laser beam energy is not affected by power alone, and it is also related to laser parameters such as pulse width and frequency. The frequency refers to the number of pulses emitted by the laser emitter per second. In a unit of time, the higher the frequency, the denser the points produced. Conversely, the lower the frequency, the more transported the points produced. The scanning speed affects the working time of the laser beam. The faster the scanning speed, the shorter the time the laser pulse stays. The focal position is the distance between the focal plane and the metal to be processed. When the focal position is negatively defocused, the focal plane is below the metal to be processed. When the focal position is positively defocused, the focal plane is above the metal to be processed. Preferably, the focal position of the embodiment of the present application is negatively defocused to avoid the influence of the peak power of the laser beam on the metal to be processed, thereby realizing the use of the high energy of the laser beam to mark the metal to be processed. It can be understood that laser scanning is a line scanning method, that is, a line is composed of laser pulses, and multiple lines are superimposed in the same direction at a certain spacing to achieve the effect of laser marking. When the scanning spacing is too large, it affects the laser processing efficiency. When the scanning spacing is small, it will be missed and affect the processing effect. It can be seen that the effect of preparing metal superhydrophobic surface is not only affected by a single parameter. The laser pulse width, power, frequency, scanning speed and scanning spacing all affect the laser marking effect. During the processing, it can be adjusted in real time according to the metal to be processed to achieve the corresponding effect.
[0065] Optionally, the laser parameters also include the number of scans, which is related to the marking depth, and different metals to be processed have different corresponding marking depths under the same number of scans. In the embodiment of the present application, the relationship between the number of scans and the type of metal to be processed and the marking depth is detected, and the details are as follows:
[0066] When the metal to be processed is zirconium, the corresponding marking depth is 0.04 mm when the number of scans is 50 times, the corresponding marking depth is 0.08 mm when the number of scans is 100 times, the corresponding marking depth is 0.1 mm when the number of scans is 150 times, the corresponding marking depth is 0.13 mm when the number of scans is 200 times, and the corresponding marking depth is 0.15 mm when the number of scans is 250 times.
[0067] When the metal to be processed is stainless steel, the corresponding marking depth is 0.03mm when the number of scans is 50 times, the corresponding marking depth is 0.05mm when the number of scans is 100 times, the corresponding marking depth is 0.08mm when the number of scans is 150 times, the corresponding marking depth is 0.11mm when the number of scans is 200 times, and the corresponding marking depth is 0.12mm when the number of scans is 250 times.
[0068] When the metal to be processed is titanium, the corresponding marking depth is 0.03mm when the number of scans is 50 times, the corresponding marking depth is 0.05mm when the number of scans is 100 times, the corresponding marking depth is 0.08mm when the number of scans is 150 times, the corresponding marking depth is 0.11mm when the number of scans is 200 times, and the corresponding marking depth is 0.12mm when the number of scans is 250 times.
[0069] It is understandable that, in actual application, the corresponding number of scans can be determined according to the type of metal to be processed and the depth required for marking.
[0070] Optionally, in an embodiment of the present application, when the laser processing equipment performs laser scanning processing, the laser parameters of the laser transmitter include: the focal length of the field lens is F100 to F160, the pulse width is 10ps to 15ps, the power is 6W to 7W, the frequency is 400-500KHz, the scanning speed is 4500mm / s to 5500mm / s, the scanning spacing is 0.001mm to 0.005mm, and the number of scans is 50 to 250 times.
[0071] Optionally, the laser parameters may also be determined according to the type of metal to be processed, and the laser parameters corresponding to different types of metals to be processed may be different or the same.
[0072] Optionally, when the metal to be processed is zirconium, the laser parameters include: the field lens focal length is F100 to F160, the pulse width is 10ps to 15ps, the power is 6.5W, the frequency is 400KHz, the scanning speed is 5000mm / s, the scanning spacing is 0.001mm to 0.005mm, and the number of scans is 250 to 500 times.
[0073] Optionally, when the metal to be processed is stainless steel or titanium, the laser parameters include: field lens focal length of F100 to F160, pulse width of 10ps to 15ps, power of 7W, frequency of 400KHz, scanning speed of 5000mm / s, scanning spacing of 0.001mm to 0.005mm, and scanning times of 250 to 500 times.
[0074] Optionally, the scanning path may be acquired by receiving a preset marking pattern input by a user, and then the control system of the laser processing equipment generates a scanning path based on the preset marking pattern.
[0075] Optionally, the scanning path includes a first scanning path and a second scanning path, the first scanning path includes a square grid scanning path composed of at least two groups of mutually parallel first straight line scanning paths, the second scanning path includes a square grid scanning path composed of at least two groups of mutually parallel second straight line scanning paths, the first straight line width corresponding to the first straight line scanning path is greater than the second straight line width corresponding to the second straight line scanning path, the first straight line width is 0.02 mm, and the second straight line width is 0.01 mm.
[0076] Optionally, the first straight line width may also be 0.05 mm, and the second straight line width may be 0.01 mm.
[0077] Optionally, the preset angles corresponding to the at least two groups of first straight scanning paths and the at least two groups of second straight scanning paths respectively corresponding to the first scanning path and / or the second scanning path are 30 degrees to 90 degrees.
[0078] Optionally, the first scanning path includes at least two groups of first straight line scanning paths, and there is an angle between the at least two groups of first straight line scanning paths. In an embodiment of the present application, while acquiring the first scanning path, the angle between the at least two groups of first straight line scanning paths in the first scanning path is determined according to the preset marking pattern, and the angle is determined as a preset angle corresponding to the at least two groups of first straight line scanning paths in the first scanning path, wherein the preset angle can be 30 degrees, 45 degrees, or 90 degrees.
[0079] Optionally, in an embodiment of the present application, the preset angle is 30 degrees.
[0080] Optionally, the preset angles corresponding to the first scanning path and the second scanning path are the same, for example, the preset angles corresponding to at least two groups of first straight scanning paths in the first scanning path are 30 degrees, and the preset angles corresponding to at least two groups of second straight scanning paths in the second scanning path are also 30 degrees.
[0081] Optionally, after obtaining the laser parameters and scanning path corresponding to the metal to be processed, the laser emitter is controlled to use the laser parameters to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path to process the metal surface of the metal to be processed into a conical micro-nano structure.
[0082] Among them, the specific method of controlling the laser emitter to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path is to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path according to a preset order, and the preset order is from top to bottom and from left to right.
[0083] Optionally, based on the scanning path including the first scanning path and the second scanning path, the embodiment of the present application provides a specific implementation of how to control the laser emitter to perform at least two laser scans on the metal to be processed along the scanning path. Optionally, the step S30 includes:
[0084] Controlling the laser emitter to perform a first scan on the metal to be processed along the first scanning path using the laser parameters to obtain a cylindrical micro-nano structure distributed in a grid pattern;
[0085] After completing the first scan, the laser emitter is controlled to use the laser parameters to perform a second scan on the metal to be processed along the second scanning path to obtain a grid-shaped distributed conical micro-nano structure, thereby forming a super-hydrophobic metal surface.
[0086] It can be understood that after the first scan, based on the first scanning path comprising at least two groups of mutually parallel first straight line scanning paths forming a square grid-shaped scanning path, a grid-shaped distributed cylindrical micro-nano structure is formed on the metal surface of the metal to be processed.
[0087] Optionally, after completing the first scan, the laser emitter 200 is controlled to scan the metal to be processed for a second time along the second scanning path. When the metal to be processed is scanned for the second time, the laser continues to extend downward in the first groove obtained by the first scan to form a second groove similar to the first groove. The second straight line width of the second straight line scanning path corresponding to the second scanning path is smaller than the first straight line width, and the surface area of the second groove is smaller than the first groove. Then, the first groove and the second groove form a groove in the metal to be processed. It can be understood that conical protrusions are formed next to the groove, that is, Figure 4 The grid-like distribution of cone-shaped micro-nano structures shown in the figure further forms a super-hydrophobic metal surface.
[0088] Optionally, after completing the first scan, controlling the laser emitter to use the laser parameters to perform a second scan on the metal to be processed along the second scanning path to obtain a grid-shaped cone micro-nano structure, thereby forming a super-hydrophobic metal surface, further includes:
[0089] Get the current number of scans;
[0090] When the current number of scans is consistent with the number of scans in the laser parameters, a step is performed to control the laser emitter to perform a second scan on the metal to be processed along the second scanning path using the laser parameters.
[0091] Optionally, after receiving the control parameters, the control system first controls the laser emitter to emit laser light to the metal surface along the first scanning path using the laser parameters, and simultaneously records the current number of scans when the laser emitter emits laser light to the metal surface using the laser parameters, and when the current number of scans reaches the number of scans in the laser parameters, switches the current scanning path to the second scanning path, and then controls the laser emitter to emit laser light to the metal surface along the second scanning path based on the laser parameters. For example, if the number of scans in the laser parameters is 3, the current number of scans of the laser emitter is recorded as 3, and then directly controls the laser emitter to emit laser light to the metal surface along the second scanning path using the laser parameters.
[0092] Optionally, the laser processing equipment is controlled to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path using the laser parameters, and the corresponding laser parameters of each laser scanning process may be the same or different.
[0093] Optionally, in another embodiment, the laser parameters include first laser parameters and second laser parameters, the first laser parameters include: field lens focal length of F100 to F160, pulse width of 10ps to 15ps, power of 6W to 7W, frequency of 400-500KHz, scanning speed of 4500mm / s to 5500mm / s, scanning spacing of 0.005mm, and number of scans of 50 to 250 times; the second laser parameters include: field lens focal length of F100 to F160, pulse width of 10ps to 15ps, power of 6W to 7W, frequency of 400-500KHz, scanning speed of 4500mm / s to 5500mm / s, scanning spacing of 0.001mm, and number of scans of 50 to 250 times.
[0094] Optionally, after acquiring the laser parameters and the scanning path, the control system sets the laser parameters and the scanning path of the laser emitter during operation based on the acquired laser parameters and the scanning path, and then first controls the laser emitter to emit laser toward the metal surface along the first scanning path based on the first laser parameters, and simultaneously records the current number of scans when the laser emitter emits laser toward the metal surface along the first scanning path with the first laser parameters, and when the current number of scans reaches the number of scans in the first laser parameters, switches the current scanning path to the second scanning path, and switches the current laser parameters to the second laser parameters, and then controls the laser emitter to emit laser toward the metal surface along the second scanning path based on the second laser parameters.
[0095] In an embodiment of the present application, the laser parameters and scanning path of the laser emitter are set by the control system, and then the laser emitter is controlled to use the laser parameters to perform at least two groups of laser scanning processes along the scanning path, so as to first prepare the metal surface of the metal to be processed into a cylindrical micro-nano structure with a grid distribution, and then the metal surface is transformed into a conical micro-nano structure based on the cylindrical micro-nano structure through a second scanning path with a small straight line width, thereby forming a super hydrophobic metal surface. The present application only needs to set the laser parameters and scanning path when the laser processing equipment is running, and then control the laser processing equipment to use the laser parameters to perform at least two groups of laser scanning processes on the metal to be processed along the scanning path to process the metal surface of the metal to be processed into a conical micro-nano structure, without the need to add additional chemicals such as fluorides, and the operation is simple, and the problem of easily causing the metal to be polluted by the environment and the surface being inconvenient to clean when preparing the super hydrophobic surface of the metal by adding fluorides is solved.
[0096] In addition, an embodiment of the present invention further proposes a computer-readable storage medium, on which a metal super-hydrophobic surface preparation program is stored. When the metal super-hydrophobic surface preparation program is executed by a processor, the steps of the various embodiments described above are implemented.
[0097] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or system. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or system including the element.
[0098] The serial numbers of the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.
[0099] Through the description of the above implementation methods, those skilled in the art can clearly understand that the above-mentioned embodiment methods can be implemented by means of software plus a necessary general hardware platform, and of course by hardware, but in many cases the former is a better implementation method. Based on such an understanding, the technical solution of the present invention is essentially or the part that contributes to the prior art can be embodied in the form of a software product, which is stored in a storage medium (such as ROM / RAM, magnetic disk, optical disk) as described above, and includes a number of instructions for a terminal device (which can be a mobile phone, computer, server, air conditioner, or network device, etc.) to execute the methods described in each embodiment of the present invention.
[0100] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a metal super-hydrophobic surface, characterized in that: The steps of the method for preparing a metal super-hydrophobic surface include: Acquire control parameters corresponding to the metal to be processed, the control parameters including laser parameters and a scanning path; the scanning path including a first scanning path and a second scanning path, the first scanning path including a grid-shaped scanning path composed of at least two groups of first straight scanning paths, the first straight scanning paths in each group are parallel to each other, the second scanning path including a grid-shaped scanning path composed of at least two groups of second straight scanning paths, the second straight scanning paths in each group are parallel to each other, the first straight line width corresponding to the first straight scanning path is greater than the second straight line width corresponding to the second straight scanning path, the first straight line width is 0.02 mm, and the second straight line width is 0.01 mm; Controlling the laser emitter to perform a first scan on the metal to be processed along the first scanning path using the laser parameters to obtain a cylindrical micro-nano structure distributed in a grid pattern; After completing the first scan, obtaining the current number of scans; When the current number of scans is consistent with the number of scans in the laser parameters, the laser emitter is controlled to use the laser parameters to perform a second scan on the metal to be processed along the second scanning path to obtain a grid-shaped distributed cone micro-nano structure, thereby forming a super-hydrophobic metal surface; The laser processing equipment used in the method for preparing a metal super-hydrophobic surface includes a laser emitter and a control system, wherein the laser emitter is a picosecond laser; the control system is used to set the laser parameters and scanning path of the laser emitter, and the laser parameters include at least one of the focal length of the field lens, pulse width, power, frequency, scanning speed, scanning spacing, and number of scans.
2. The method for preparing a metal super-hydrophobic surface as claimed in claim 1, wherein The laser parameters include: field lens focal length of F100 to F160, pulse width of 10ps to 15ps, power of 6W to 7W, frequency of 400-500KHz, scanning speed of 4500mm / s to 5500mm / s, scanning spacing of 0.001mm to 0.005mm, and scanning times of 50 to 250 times.
3. The method for preparing a metal super-hydrophobic surface as claimed in claim 1, wherein The preset angles corresponding to the at least two groups of first straight scanning paths and the at least two groups of second straight scanning paths respectively corresponding to the first scanning path and / or the second scanning path are in a range of 30 degrees to 90 degrees.
4. The method for preparing a metal super-hydrophobic surface as claimed in claim 3, wherein: The preset angle is 30 degrees.
5. The method for preparing a metal super-hydrophobic surface as claimed in claim 1, wherein The laser emitter is an ultraviolet picosecond laser emitter.
6. A laser processing device, characterized in that: The laser processing equipment includes a laser emitter and a control system, and the control system is used to execute the steps of the method for preparing a metal super-hydrophobic surface as described in any one of claims 1 to 5.
Citation Information
Patent Citations
Bionic metal ultra-wetting trans-scale structure design method and preparation method
CN101712102A
Method for enabling PTFE (Polytetrafluoroethylene) or FEP (Fluorinated Ethylene Propylene) surface to have super-hydrophobic and underwater high reflective properties simultaneously
CN103551734A
Cited By
Method and system for preparing low-flow-resistance corrosion-resistant oil conveying pipe from hot-rolled stainless steel
CN120206176A