Electrode sheet and lithium ion battery containing the same

By using organic/inorganic composite porous coating on the electrode sheet of the lithium-ion battery, combining polymer adhesives and conductive materials, the safety hazards of lithium-ion batteries during mechanical damage are solved, and the safety and electrochemical performance of the battery is improved. , especially in low temperatures and cycle performance.

CN114050225BActive Publication Date: 2024-11-22AMPREUS WUXI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202111145021.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-28
Publication Date
2024-11-22
Estimated Expiration
2041-09-28

AI Technical Summary

Technical Problem

Lithium-ion batteries are prone to fire and explosion during mechanical damage, mainly due to heat discharge caused by internal short circuits. It is difficult for the prior art to improve safety performance and electrochemical performance at the same time.

Method used

Using organic/inorganic composite porous coating, including polymer adhesive, conductive materials and specific inorganic particles, it is used between the electrode active material layer and the current collector or on the electrode active material layer to improve the safety and electrochemical performance of the electrode sheet. .

Benefits of technology

Through the combination of polymer adhesives and conductive materials, a PTC-like effect is achieved, preventing coating dissolution and uneven extrusion, improving lithium ion conductivity and battery performance, enhancing electrolyte wetting, improving battery safety and electricity Chemical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0003456498170000041
    Figure GDA0003456498170000041
  • Figure GDA0003456498170000051
    Figure GDA0003456498170000051
  • Figure GDA0003456498170000052
    Figure GDA0003456498170000052
Patent Text Reader

Abstract

The present invention relates to an electrode sheet and a lithium ion battery containing the electrode sheet, comprising a current collector, an electrode active material layer, and an organic / inorganic composite porous coating between the current collector and the electrode active material layer and / or an organic / inorganic composite porous coating on the electrode active material layer; the organic / inorganic composite porous coating comprises a polymer adhesive, a conductive material and inorganic particles; the inorganic particles are selected from at least one of the following particles: a. a first type of inorganic particles with a dielectric constant ≥ 5; b. a second type of inorganic particles composed of an inorganic solid electrolyte. The present invention provides an electrode sheet and a lithium ion battery containing the electrode sheet, which can improve the safety performance of the lithium ion battery and also enhance the electrochemical performance of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium ion batteries, and in particular to an electrode sheet and a lithium ion battery containing the electrode sheet. Background Art

[0002] Lithium-ion secondary batteries have become the most widely used secondary batteries due to their advantages such as high voltage, high energy density, and long cycle life. However, lithium-ion batteries are prone to fire and explosion under some special conditions, such as mechanical damage such as extrusion, heavy impact or puncture, which leads to serious safety hazards. Therefore, their application development is greatly limited in some fields.

[0003] According to a large number of research results, the biggest cause of these safety hazards is the internal short circuit of the battery. When an internal short circuit occurs, the lithium-ion battery will release a large amount of heat in a very short time, which can lead to fire and explosion. There are many modes of internal short circuit in the battery, among which the short circuit between the positive electrode collector and the negative electrode is the fastest and most dangerous mode of heat transfer.

[0004] In order to avoid short circuits in the battery, some people use the characteristics of PTC to improve the safety performance of lithium-ion batteries. Some people add PTC to the electrode active materials. Although this method has a safety effect, it will affect the electrochemical performance of the battery. There are also people who apply PTC directly to the current collector, but when applying the electrode active material slurry, the solvent of the slurry will dissolve the PTC coating, and the PTC material is easily squeezed to the edge during the rolling process, resulting in the failure to achieve the desired effect of improving safety performance. At the same time, some people add certain inorganic fillers to the slurry similar to the PTC component and coat it on the current collector to achieve the desired safety performance, but because the added inorganic filler has a low ionic conductivity, it may affect the performance of the battery cell. Summary of the invention

[0005] The object of the present invention is to provide an electrode plate and a lithium ion battery containing the electrode plate in view of the above-mentioned problems, which can improve both the safety performance and the electrochemical performance of the lithium ion battery.

[0006] To achieve the above purpose, the technical solution provided by the present invention is:

[0007] An electrode pole piece comprises a current collector, an electrode active material layer, and an organic / inorganic composite porous coating between the current collector and the electrode active material layer and / or an organic / inorganic composite porous coating on the electrode active material layer; the organic / inorganic composite porous coating comprises a polymer adhesive, a conductive material and inorganic particles; the inorganic particles are selected from at least one of the following particles: a. first type of inorganic particles with a dielectric constant ≥5; b. second type of inorganic particles composed of inorganic solid electrolytes.

[0008] Furthermore, the first type of inorganic particles is selected from BaTiO3, Pb(Zr, Ti)O3(PZT), Pb1-xLaxZr1-yTiO3(PLZT), HfO2, Pb(Mg3Nb 2 / 3 )At least one of O3-PbTiO3 (PMT-PT), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, and TiO2.

[0009] Furthermore, the second type of inorganic particles are inorganic particles with lithium ion conductivity, that is, inorganic particles that contain lithium elements and can conduct lithium ions without storing lithium.

[0010] Furthermore, the second type of inorganic particles is selected from lithium phosphate Li3PO4; lithium titanium phosphate LixTiy(PO4)30<x<2,0<y<3; lithium aluminum titanium phosphate LixAlyTiz(PO4)3,0<x<2,0<y<1,0<z<3; (LiAlTiP) x O y Type glass 0<x<4, 0<y<13; lithium lanthanum titanate LixLayTiO3, 0<x<2, 0<y<3; lithium germanium thiophosphate LixGeyPzSw, 0<x<4, 0<y<1, 0<z<1, 0<w<5; lithium nitride LixNy, 0<x<4, 0<y<2 or at least one of the modified materials of the above materials.

[0011] Furthermore, the conductive material is selected from at least one of a conductive carbon-based material, a conductive metal material, and a conductive polymer material; wherein the conductive carbon-based material is selected from at least one of conductive carbon black, acetylene black, graphite, graphene, carbon nanotubes, and carbon nanofibers; the conductive metal material is selected from at least one of Al powder, Ni powder, and gold powder; and the conductive polymer material is selected from at least one of conductive polythiophene, conductive polypyrrole, and conductive polyaniline.

[0012] Furthermore, the polymer adhesive is selected from at least one of polyvinylidene fluoride PVDF, carboxylic acid-modified PVDF, acrylic acid-modified PVDF, polyvinylidene chloride PVDC, carboxylic acid-modified PVDC, acrylic acid-modified PVDC, PVDF copolymer, and PVDC copolymer.

[0013] There is no particular limitation on the particle size of the inorganic particles, but the average particle size D is preferably 10 nm ≤ D ≤ 6 um; the thickness H of the coating is 1 um ≤ H ≤ 15 um, preferably 2 um ≤ H ≤ 10 um.

[0014] Furthermore, in the organic / inorganic composite porous coating, the weight percentage of the inorganic particles is 15%-60%, the weight percentage of the polymer adhesive is 35-80%, and the weight percentage of the conductive material is 5%-20%.

[0015] Furthermore, the positive electrode active material is selected from one or more of lithium cobalt oxide, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, nickel-cobalt-manganese-aluminum quaternary material, lithium iron phosphate, lithium iron manganese phosphate, lithium vanadium phosphate, and lithium manganese oxide; the negative electrode active material is selected from one or more of natural graphite, artificial graphite, mesophase carbon microbeads, hard carbon, soft carbon, silicon carbon, and silicon oxygen.

[0016] The present invention also protects a lithium ion battery containing the electrode plate.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] (1) The polymer adhesive in the electrode sheet coating of the present invention has two functions: one is that it can serve as an adhesive for the coating, and the other is that it can play a role similar to PTC when combined with a conductive agent.

[0019] (2) The conductive agent in the electrode sheet coating of the present invention has two functions: one is to increase the conductivity of the coating, and the other is to play a role similar to PTC in combination with the adhesive.

[0020] (3) The inorganic particles in the electrode sheet coating of the present invention have four functions. One is to prevent the NMP in the slurry from directly dissolving the adhesive in the coating. The second is to prevent the conductive agent and the adhesive from being squeezed unevenly when the electrode sheet is rolled, causing the loss of their safety function. The third is to improve the lithium ion conductivity, improve the battery's rate, low-temperature discharge and cycle and other electrochemical properties. The fourth is to improve the wettability of the electrolyte, thereby improving the battery's rate, low-temperature discharge and cycle and other electrochemical properties. DETAILED DESCRIPTION

[0021] The above contents of the present invention are further described in detail below in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following embodiments, and all technologies realized based on the above contents of the present invention belong to the scope of the present invention.

[0022] Example

[0023] An electrode plate and a method for preparing a lithium-ion battery containing the electrode plate:

[0024] The preparation steps of the coating are as follows: a certain proportion of polymer adhesive, conductive material, inorganic particles and NMP solvent are stirred evenly and then coated on the current collector (positive current collector or negative current collector), and the coating is obtained after drying. The main materials used in the coating of each specific embodiment are as follows: polymer adhesive: PVDF, conductive material: SP; inorganic particles: lithium iron phosphate, lithium aluminum titanium phosphate, aluminum oxide; the above materials are common and commonly used materials in the lithium battery industry.

[0025] The preparation steps of the electrode positive plate:

[0026] Coated positive electrode sheet: Use 96% NCM, 2% SP and 2% PVDF, use NMP as solvent, stir evenly and apply it on the above-mentioned coated positive electrode collector, dry it at 90°C, roll it, cut it, and then dry it at 110°C under vacuum conditions for 4h, weld the pole ears, and make a lithium-ion secondary battery positive electrode sheet that meets the requirements.

[0027] Conventional positive electrode sheet 1#: The preparation method is the same as described above, except that the surface of the current collector aluminum foil is completely uncoated.

[0028] The preparation steps of the electrode negative plate:

[0029] Negative electrode sheet with coating: add the main material graphite, conductive agent SP, thickener CMC and adhesive SBR into solvent deionized water in a mass ratio of 96.8:1:1:1.2 and mix evenly to make negative electrode slurry, then apply the negative electrode slurry on the negative electrode collector with coating, dry it at 85℃, roll it and cut it. Then dry it at 130℃ under vacuum for 6h, weld the pole ear, and make the negative electrode sheet of lithium ion battery that meets the requirements.

[0030] Conventional negative electrode sheet 1#: The preparation method is the same as described above, except that the surface of the current collector copper foil is completely uncoated.

[0031] Electrolyte preparation steps: In a glove box filled with argon, ethylene carbonate, propylene carbonate and propyl propionate are mixed in a mass ratio of 2:1:3, and then lithium hexafluorophosphate with a concentration of 1 mol / L is slowly added to the mixed solution and stirred evenly to obtain the lithium ion battery electrolyte of the embodiment.

[0032] The preparation steps of the battery are as follows: the positive electrode sheet, the negative electrode sheet and the polyethylene separator with a thickness of 12 μm are stacked and wound in sequence into a square core, and the core is loaded into a polymer soft-pack battery shell (made of aluminum-plastic film), and then vacuum-baked and injected with the above-prepared electrolyte. After packaging, the polymer soft-pack lithium-ion battery is obtained after standing, forming, degassing, aging and capacity separation.

[0033] Electrochemical performance test:

[0034] 1) 0.7C cycle performance test: At 25°C, charge the formed battery to 4.35V at 0.7C constant current and constant voltage, with a cut-off current of 0.02C, and then leave it for 10 minutes, and then discharge it to 3.0V at 0.7C constant current. The charge and discharge cycle is stopped when the capacity decays to less than 80% of the initial discharge capacity;

[0035] 2) Needle penetration test: At 25℃, discharge the divided lithium-ion battery at 0.2C to 3.0V, leave it for 10 minutes, then charge it at 0.5C constant current and constant voltage to 4.35V, and cut off at 0.02C. A high-temperature resistant steel needle is inserted into the battery at a speed of 25±5mm / s from a direction perpendicular to the battery plate. The penetration position should be close to the geometric center of the pierced surface. The steel needle stays in the battery to observe whether the battery catches fire or explodes.

[0036] 3) Heavy object impact test: At 25℃, discharge the divided lithium-ion battery at 0.2C to 3.0V, leave it for 10 minutes, and then charge it at 0.5C constant current and constant voltage to 4.35V, with a cut-off of 0.02C. Place the battery on the platform surface, place a metal rod with a diameter of 15.8±0.2mm horizontally on the upper surface of the geometric center of the battery, and use a weight of 9.1kg±0.1kg to hit the battery surface with the metal rod in a free fall state from a height of 610mm±25mm, and observe for 6 hours to see if there is any fire or explosion.

[0037] 4) PTC effect test: At 25°C, the divided lithium-ion battery was first discharged at 0.2C to 3.0V, and after 10 minutes, it was charged to 4.35V at 0.5C constant current and constant voltage, and then cut off at 0.02C. The AC internal resistance of the battery was tested, and then the battery was placed at a constant temperature of 130°C for 1 hour, the AC resistance was tested, and the AC resistance growth rate was calculated.

[0038] 5) Rate discharge performance test: At 25°C, the divided lithium-ion battery was first discharged at 0.2C to 3.0V, left for 10 minutes, and then charged at 0.5C constant current and constant voltage to 4.35V, with a cut-off of 0.02C. Then, it was discharged at different rates of 0.2C / 0.5C / 1C / 1.5C / 2C to 3.0V.

[0039] 6) High and low temperature discharge performance: At 25℃, the divided lithium-ion battery was first discharged at 0.2C to 3.0V, left for 10 minutes, and then charged to 4.35V at 0.5C constant current and constant voltage, and then cut off at 0.02C. Then, it was discharged at 0.2C to 3.0V at different temperatures of 25℃ / 55℃ / 0℃ / -10℃ / -20℃.

[0040] Performance Test Results

[0041] In the embodiment, the specific materials and amounts listed in Table 1-1 are used to prepare the corresponding coating, positive electrode sheet, negative electrode sheet and battery according to the method and steps described in the "Preparation Method", and then tested according to the method specified in the "Battery Performance Test". To ensure the accuracy of the data, 5 batteries of each type are prepared (10 batteries for needle puncture and heavy object impact are prepared) and tested independently, and the final test results are averaged. The test results are shown in Tables 1-2, 1-3 and 1-4:

[0042] Table 1-1 Pole components

[0043]

[0044]

[0045] Table 1-2 Lithium-ion battery performance test results of Example 1-5 (verifying the influence of coating)

[0046]

[0047] Comparing Examples 1 and 2, 1 and 3 / 4 / 5, it can be seen that the coating can improve the safety performance of the battery cell against needle puncture and heavy object impact, whether on the positive electrode or the negative electrode, and the addition of LATP can greatly improve the low-temperature discharge and cycle performance of the battery cell. By adding inorganic particles, the AC internal resistance growth rate of the battery cell at high temperature can be significantly increased, thereby improving the passing rate of the battery cell through needle puncture and heavy object impact.

[0048] Table 1-3 Performance test results of lithium-ion batteries in Examples 1 and 6-9 (verifying the influence of different material coatings)

[0049]

[0050]

[0051] By comparing Examples 1 and 6-7, it can be seen that different types of inorganic particles in the coating are helpful to improve the safety performance of battery cells under needle puncture and heavy object impact. Among them, the coating with the addition of alumina particles improves the growth rate of the AC internal resistance of the battery cell at high temperature most significantly, but has the greatest impact on the performance of the battery cell; the addition of LATP particles greatly improves the electrical properties, especially the low-temperature discharge and cycle performance; and at the same time. Adding a small amount of alumina to LATP can play a synergistic role, not only increasing the growth rate of the AC internal resistance compared to LATP, but also improving the electrical performance. This may be because the dielectric constant of alumina is 9-10, which can increase the dissociation degree of lithium salts in the electrolyte, thereby improving the ionic conductivity of the electrolyte. At the same time, due to its porous characteristics, it will also increase the liquid absorption of the electrode sheet, and the high ionic conductivity and porous structure of LATP itself greatly improve the apparent performance of the battery.

[0052] Table 1-4 Lithium ion battery performance test results of Examples 1 and 9-20 (verifying the influence of different component contents in the coating)

[0053]

[0054] By comparing Examples 1 and 9-20, it can be seen that: too high and too low content of inorganic particles in the coating cannot greatly improve the safety performance of the battery; the conductive agent in the coating has a certain help to the electrical performance of the battery. LATP can also greatly improve the electrical performance of the battery, probably because its high ionic conductivity and porous structure increase the wettability of the electrolyte, resulting in a certain improvement in electrical performance.

[0055] In summary, the present invention optimizes the inorganic particle LATP that can improve both safety performance and electrical performance, especially low-temperature discharge and cycle performance, and optimizes the content range of each component: the weight percentage of the polymer adhesive is 35-80%, the weight percentage of the conductive material is 5-20%, and the weight percentage of the inorganic particles is 15-60%.

[0056] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any technician familiar with the profession, without departing from the scope of the technical solution of the present invention, according to the technical essence of the present invention, any simple modification, equivalent replacement and improvement made to the above embodiment still falls within the protection scope of the technical solution of the present invention.

Claims

1. An electrode plate, characterized in that: It includes a current collector, an electrode active material layer, and an organic / inorganic composite porous coating between the current collector and the electrode active material layer and / or an organic / inorganic composite porous coating on the electrode active material layer; the organic / inorganic composite porous coating contains a polymer adhesive, a conductive material and inorganic particles; the inorganic particles are LATP+Al2O3, and the mass ratio of LATP to Al2O3 is 95:

5.

2. The electrode plate according to claim 1, characterized in that: The conductive material is selected from at least one of conductive carbon-based materials, conductive metal materials, and conductive polymer materials; wherein the conductive carbon-based material is selected from at least one of conductive carbon black, graphite, graphene, carbon nanotubes, and carbon nanofibers; the conductive metal material is selected from at least one of Al powder, Ni powder, and gold powder; and the conductive polymer material is selected from at least one of conductive polythiophene, conductive polypyrrole, and conductive polyaniline.

3. The electrode plate according to claim 1, characterized in that: The polymer adhesive is selected from at least one of polyvinylidene fluoride PVDF, carboxylic acid-modified PVDF, acrylic acid-modified PVDF, polyvinylidene chloride PVDC, carboxylic acid-modified PVDC, acrylic acid-modified PVDC, PVDF copolymer, and PVDC copolymer.

4. The electrode plate according to claim 1, characterized in that: The average particle size D of the inorganic particles is 10nm≤D≤6um; the thickness H of the coating is 1um≤H≤15um.

5. The electrode plate according to claim 1, characterized in that: In the organic / inorganic composite porous coating, the weight percentage of the inorganic particles is 15%-60%, the weight percentage of the polymer adhesive is 35%-80%, and the weight percentage of the conductive material is 5%-20%.

6. The electrode plate according to claim 1, characterized in that: The electrode active material layer contains positive electrode active material or negative electrode active material; the positive electrode active material is selected from one or more of lithium cobalt oxide, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, nickel-cobalt-manganese-aluminum quaternary material, lithium iron phosphate, lithium iron manganese phosphate, lithium vanadium phosphate, and lithium manganate; the negative electrode active material is selected from one or more of natural graphite, artificial graphite, mesophase carbon microbeads, hard carbon, soft carbon, silicon carbon, and silicon oxygen.

7. A lithium ion battery, characterized in that: An electrode sheet comprising any one of claims 1 to 6.

Citation Information

Patent Citations

  • Electrode pole plate, electrochemical device and safety coating layer

    CN109755463A

  • High-safety composite positive plate, preparation method thereof and applied lithium ion battery

    CN111697230A

  • Preparation method of coating-containing pole piece and lithium ion battery

    CN112151736A

  • Organic / inorganic composite porous layer-coated electrode and electrochemical device comprising the same

    CN1918727A