A method for detecting sulfide nucleation core

By performing preset heating and cooling treatments on the sulfide nucleation core to expose and finalize it, and combining the detection methods of field emission electron microscopy and electron probes, the problem of poor detection effect of the sulfide nucleation core in the existing technology is solved. Accurate size and composition detection is achieved and the detection rate is improved.

CN114111653BActive Publication Date: 2024-10-18SGIS SONGSHAN CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202111403982.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-24
Publication Date
2024-10-18
Estimated Expiration
2041-11-24

AI Technical Summary

Technical Problem

When the existing technology detects sulfide nucleation cores in sulfur-containing free-cutting steel, the detection rate of smaller nucleation cores is lower, and the size of the nucleation cores cannot be accurately described, resulting in poor detection results.

Method used

The sample to be tested is heated to 1150 degrees Celsius at a preset heating rate and kept for a preset time to expose the sulfide nucleation core. It is then cooled to 25 degrees Celsius at a preset cooling rate to finalize its shape, and then sized by field emission electron microscopy. Measurements and electronic probes for component detection.

Benefits of technology

The accurate detection of sulfide nucleation cores is achieved, the detection rate is increased, and the detection effect is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114111653B_ABST
    Figure CN114111653B_ABST
Patent Text Reader

Abstract

The present invention discloses a sulfide nucleation core detection method, which relates to the technical field of free-cutting steel. First, the sample to be tested is heated to 1150 degrees Celsius at a preset heating rate, and kept warm for a preset time to expose the sulfide nucleation core in the sample to be tested; then the sample to be tested is cooled to 25 degrees Celsius at a preset cooling rate to shape the sulfide nucleation core; then the sulfide nucleation core is measured in size and tested for composition. Compared with the prior art, the sulfide nucleation core detection method provided by the present invention adopts the step of heating the sample to be tested to 1150 degrees Celsius at a preset heating rate and keeping warm for a preset time to expose the sulfide nucleation core in the sample to be tested, so it can accurately detect the size and composition of the sulfide nucleation core, improve the detection rate, and have a good detection effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of free-cutting steel, and in particular to a sulfide nucleation core detection method. Background Art

[0002] At present, the performance of sulfur-containing free-cutting steel mainly depends on the formation of sulfides inside the steel. The size, shape and distribution of sulfides have a significant impact on the performance of steel. Currently, the detection of sulfide nucleation cores mainly adopts metallographic detection method, which is a cross-sectional detection method. The detection rate of sulfide nucleation cores with smaller size is low, and the size of the nucleation core cannot be accurately described, resulting in poor detection effect.

[0003] In view of this, it is particularly important to design a sulfide nucleation core detection method with good detection effect, especially in the production of free-cutting steel. Summary of the invention

[0004] The object of the present invention is to provide a sulfide nucleation core detection method, which can accurately detect the size and composition of the sulfide nucleation core, improve the detection rate, and have a good detection effect.

[0005] The present invention is achieved by adopting the following technical solutions.

[0006] A sulfide nucleation core detection method comprises: heating a sample to be tested to 1150 degrees Celsius at a preset heating rate and keeping the temperature for a preset time to expose the sulfide nucleation core in the sample to be tested; cooling the sample to be tested to 25 degrees Celsius at a preset cooling rate to shape the sulfide nucleation core; and measuring the size and detecting the composition of the sulfide nucleation core.

[0007] Optionally, the preset heating rate ranges from 20 degrees Celsius / minute to 40 degrees Celsius / minute.

[0008] Optionally, the preset duration ranges from 5 minutes to 15 minutes.

[0009] Optionally, the preset cooling rate ranges from 50 degrees Celsius / minute to 70 degrees Celsius / minute.

[0010] Optionally, the step of heating the sample to be tested to 1150 degrees Celsius at a preset heating rate and keeping it warm for a preset time to expose the sulfide nucleation core in the sample to be tested includes: placing the sample to be tested in a confocal microscope heating furnace, and continuously introducing an inert gas into the confocal microscope heating furnace; heating the sample to be tested by using the confocal microscope heating furnace; and keeping the sample to be tested warm for a preset time.

[0011] Optionally, the inert gas flow rate ranges from 10 ml / min to 20 ml / min.

[0012] Optionally, before the step of heating the sample to be tested to 1150 degrees Celsius at a preset heating rate and keeping it warm for a preset time to expose the sulfide nucleation core in the sample to be tested, the sulfide nucleation core detection method also includes: cutting a cylindrical sample to be tested from the product; grinding the sample to be tested; and polishing the sample to be tested.

[0013] Optionally, the step of grinding the sample to be tested includes: grinding the surface of the sample to be tested using sandpapers of 100 mesh, 200 mesh, 400 mesh, 800 mesh, 1000 mesh and 1200 mesh in sequence, wherein the grinding directions of two adjacent sandpapers are perpendicular.

[0014] Optionally, the step of polishing the sample to be tested includes: polishing the surface of the sample to be tested with 3 micron and 1 micron polycrystalline diamond suspensions in sequence; dry polishing the sample to be tested with a flannel cloth sprayed with alcohol; rinsing the sample to be tested with clean water; dripping alcohol on the sample to be tested and blowing it dry with hot air.

[0015] Optionally, the steps of measuring the size and detecting the composition of the sulfide nucleation core include: measuring the size of the sulfide nucleation core using a field emission electron microscope; and detecting the composition of the sulfide nucleation core using an electron probe.

[0016] The sulfide nucleation core detection method provided by the present invention has the following beneficial effects:

[0017] The sulfide nucleation core detection method provided by the present invention first heats the sample to be tested to 1150 degrees Celsius at a preset heating rate and keeps it warm for a preset time to expose the sulfide nucleation core in the sample to be tested; then cools the sample to be tested to 25 degrees Celsius at a preset cooling rate to shape the sulfide nucleation core; then measures the size and detects the composition of the sulfide nucleation core. Compared with the prior art, the sulfide nucleation core detection method provided by the present invention can accurately detect the size and composition of the sulfide nucleation core, improve the detection rate, and have a good detection effect because it adopts the steps of heating the sample to be tested to 1150 degrees Celsius at a preset heating rate and keeping it warm for a preset time to expose the sulfide nucleation core in the sample to be tested. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0019] Figure 1A flowchart of a sulfide nucleation core detection method provided by an embodiment of the present invention;

[0020] Figure 2 The sulfide nucleation core detection method provided in the embodiment of the present invention is a sulfide nucleation core image obtained by detecting the sulfide nucleation core under the conditions of a heating temperature of 1100 degrees Celsius and a preset time of 20 minutes;

[0021] Figure 3 The sulfide nucleation core detection method provided in the embodiment of the present invention is a sulfide nucleation core image obtained by detecting the sulfide nucleation core under the conditions of a heating temperature of 1150 degrees Celsius and a preset time of 10 minutes;

[0022] Figure 4 The sulfide nucleation core detection method provided in the embodiment of the present invention is a sulfide nucleation core image obtained by detecting the sulfide nucleation core under the conditions of a heating temperature of 1150 degrees Celsius and a preset time of 20 minutes;

[0023] Figure 5 The sulfide nucleation core detection method provided in the embodiment of the present invention detects a sulfide nucleation core image under the conditions of a heating temperature of 1250 degrees Celsius and a preset time of 20 minutes. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0025] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0027] In the description of the present invention, it should be noted that the terms "inside", "outside", "upper", "lower", "horizontal", etc. indicate the orientation or position relationship based on the orientation or position relationship shown in the drawings, or the orientation or position relationship in which the product of the invention is usually placed when in use, which is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.

[0028] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "connect", "install", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0029] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the features of the following embodiments can be combined with each other.

[0030] Please refer to Figure 1 The embodiment of the present invention provides a sulfide nucleation core detection method for detecting the size and composition of the sulfide nucleation core. The method can accurately detect the size and composition of the sulfide nucleation core, improve the detection rate, and have a good detection effect.

[0031] It should be noted that the sulfide nucleation core detection method is applied to the performance test of free-cutting steel. Free-cutting steel is a type of steel that aims to reduce machining costs, improve cutting quality, reduce cutting resistance, or improve cutting processability in automatic machine tools for machining. Its cutting performance is mainly achieved by adding appropriate amounts of free-cutting elements such as sulfur, phosphorus, lead, selenium, tellurium, calcium, bismuth, etc. to carbon steel, so that the carbon steel has excellent cutting performance. The sulfide nucleation core detection method in this embodiment is to detect the sulfide nucleation core in sulfur-containing free-cutting steel.

[0032] The sulfide nucleation core detection method comprises the following steps:

[0033] Step S110: cutting a cylindrical sample to be tested from the product.

[0034] In this embodiment, the product is sulfur-containing free-cutting steel, the steel grade is 1215MS, the sampling position is one quarter of the free-cutting steel billet, and the manganese-sulfur ratio is 3.55 to ensure that the melting point of the sample to be tested is moderate. Specifically, a representative position is selected for sampling by wire cutting, and the defective areas need to be avoided during the sampling process. The sample to be tested is prepared into a cylindrical billet with a diameter of 7.5 mm and a height of 3 mm.

[0035] Step S120: grinding the sample to be tested.

[0036] It should be noted that in step S120, the surface of the sample to be tested is grinded in sequence using sandpapers of 100 mesh, 200 mesh, 400 mesh, 800 mesh, 1000 mesh and 1200 mesh, wherein the grinding directions of two adjacent sandpapers are perpendicular to each other, so as to enhance the grinding effect and improve the smoothness of the surface of the sample to be tested.

[0037] Step S130: polishing the sample to be tested.

[0038] Specifically, step S130 includes four steps, namely:

[0039] Step S131: polishing the surface of the sample to be tested using 3 micron and 1 micron polycrystalline diamond suspensions in sequence.

[0040] It is worth noting that for polycrystalline diamond suspension, the size and irregularity of the particles are very important. The more cutting edges there are, the faster the grinding speed is, and the better the polishing effect is. In this embodiment, the sample to be tested is first polished with a 3-micron polycrystalline diamond suspension, and then polished with a 1-micron polycrystalline diamond suspension to enhance the polishing effect and further improve the smoothness of the surface of the sample to be tested.

[0041] Step S132: dry-polish the sample to be tested using a flannel cloth sprayed with alcohol.

[0042] It should be noted that, in step S132, alcohol is sprayed on the flannel, and the surface of the sample to be tested is wiped with the flannel to remove the diamond suspension adhering to the surface of the sample to be tested, thereby improving the cleanliness of the sample to be tested.

[0043] Step S133: Rinse the sample to be tested with clean water.

[0044] Step S134: sprinkle alcohol on the sample to be tested and blow it dry with hot air.

[0045] Step S140: heating the sample to be tested to 1150 degrees Celsius at a preset heating rate and keeping the temperature for a preset time to expose the sulfide nucleation core in the sample to be tested.

[0046] Specifically, step S140 includes three steps, namely:

[0047] Step S141: placing the sample to be tested into a confocal microscope heating furnace, and continuously introducing an inert gas into the confocal microscope heating furnace.

[0048] It should be noted that in step S141, the polished sample to be tested is first loaded into a corundum crucible, and the corundum crucible containing the sample to be tested is placed in a confocal microscope heating furnace. The confocal microscope heating furnace is then evacuated and replenished with inert gas for at least three cycles to ensure that the confocal microscope heating furnace is a high-purity inert gas environment to prevent the sample to be tested from being oxidized during the subsequent heating process.

[0049] Further, the inert gas flow rate ranges from 10 ml / min to 20 ml / min. In the present embodiment, the inert gas is argon, and the inert gas flow rate is 15 ml / min, but it is not limited thereto. In other embodiments, the inert gas may be neon or helium, and the inert gas flow rate may be 10 ml / min or 20 ml / min. The type of the inert gas and the flow rate are not specifically limited.

[0050] Step S142: using a confocal microscope heating furnace to heat the sample to be tested.

[0051] It should be noted that, in step S142, the sample to be tested is quickly heated using the principle of laser focusing, so that the sample to be tested is heated to 1150 degrees Celsius at a preset heating rate.

[0052] Further, the preset temperature rise rate ranges from 20 degrees Celsius / minute to 40 degrees Celsius / minute. In this embodiment, the preset temperature rise rate is 30 degrees Celsius / minute, but it is not limited thereto. In other embodiments, the preset temperature rise rate may be 20 degrees Celsius / minute or 40 degrees Celsius / minute, and the preset temperature rise rate is not specifically limited.

[0053] Step S143: keeping the sample to be tested warm for a preset time period.

[0054] It should be noted that in step S143, the sample to be tested is kept warm by using a confocal microscope heating furnace so that the warming time of the sample to be tested reaches a preset time. During the warming process, the manganese and sulfur elements in the sulfide are dissolved in the matrix, so that the sulfide nucleation core is gradually exposed.

[0055] Further, the preset duration ranges from 5 minutes to 15 minutes. In the present embodiment, the preset duration is 10 minutes, but it is not limited thereto. In other embodiments, the preset duration may be 5 minutes or 15 minutes, and the size of the preset duration is not specifically limited.

[0056] It is worth noting that the present invention uses the heating temperatures of 1100 degrees Celsius, 1150 degrees Celsius, 1200 degrees Celsius and 1250 degrees Celsius as the first variable, and the preset time lengths of 10 minutes and 20 minutes as the second variable for comparative experiments, and finds that:

[0057] Please refer to Figure 2 , under the condition that the heating temperature is 1100 degrees Celsius and the preset time is 10 minutes or 20 minutes, that is, after the sample to be tested is heated to 1100 degrees Celsius and kept warm for 10 minutes or 20 minutes, the size of the original sulfide becomes larger, no obvious solid solution occurs, and the sulfide nucleation core is not exposed;

[0058] Please refer to Figure 3 , under the condition of heating temperature of 1150 degrees Celsius and preset time of 10 minutes, that is, after the sample to be tested is heated to 1150 degrees Celsius and kept warm for 10 minutes, the size of the original sulfide becomes larger, partial solid solution occurs, and the sulfide nucleation core is exposed;

[0059] Please refer to Figure 4 , under the condition of a heating temperature of 1150 degrees Celsius and a preset time of 20 minutes, that is, the sample to be tested is heated to 1150 degrees Celsius and kept warm for 20 minutes, the size of the original sulfide increases and then gradually shrinks, manganese and sulfur elements begin to dissolve, holes are formed at the original sulfide position, and the sulfide nucleation core sinks to the bottom of the hole;

[0060] Under the conditions of a heating temperature of 1200 degrees Celsius and a preset time of 10 minutes, that is, after the sample to be tested is heated to 1200 degrees Celsius and kept warm for 10 minutes, all holes are formed at the original sulfide positions, the manganese and sulfur elements in the holes are not completely dissolved, and the sulfide nucleation cores all sink to the bottom of the holes;

[0061] Under the conditions of a heating temperature of 1200 degrees Celsius and a preset duration of 20 minutes, that is, after the sample to be tested is heated to 1200 degrees Celsius and kept warm for 20 minutes, all holes are formed at the original sulfide positions, and some large-sized sulfides are not completely dissolved, and the sulfide nucleation cores all sink to the bottom of the holes;

[0062] Please refer to Figure 5 , under the conditions of a heating temperature of 1250 degrees Celsius and a preset time of 10 minutes or 20 minutes, that is, the sample to be tested is heated to 1250 degrees Celsius and kept warm for 10 minutes or 20 minutes, holes are formed at the original sulfide positions, the edges of the matrix at the holes are passivated, some large-sized sulfides are not completely dissolved, and the sulfide nucleation cores all sink to the bottom of the holes.

[0063] From the above experimental results, it can be seen that the best solution is to perform the test under the conditions of a heating temperature of 1150 degrees Celsius and a preset time of 10 minutes. If the heating temperature is too low, the manganese and sulfur elements are not dissolved, the sulfide nucleation core is not exposed, and the sulfide nucleation core cannot be detected; if the heating temperature is too high, the manganese and sulfur elements are all dissolved, the sulfide nucleation core sinks to the bottom of the hole, and the edge of the hole is passivated, and the composition of the sulfide nucleation core cannot be detected.

[0064] Step S150: Cool the sample to be tested to 25 degrees Celsius at a preset cooling rate to allow the sulfide nucleation core to be fixed.

[0065] It is worth noting that in step S150, the sample to be tested is rapidly cooled in a high-purity inert gas environment so as to quickly cool the sample to room temperature (25 degrees Celsius) to prevent oxidation of the sample to be tested and ensure the integrity of the sulfide nucleation core.

[0066] Further, the preset cooling rate ranges from 50 degrees Celsius / minute to 70 degrees Celsius / minute. In this embodiment, the preset cooling rate is 60 degrees Celsius / minute, but it is not limited thereto. In other embodiments, the preset cooling rate may be 50 degrees Celsius / minute or 70 degrees Celsius / minute, and the preset cooling rate is not specifically limited.

[0067] Step S160: measuring the size and detecting the composition of the sulfide nucleation core.

[0068] Specifically, step S160 includes two steps, namely:

[0069] Step S161: using a field emission electron microscope to measure the size of the sulfide nucleation core.

[0070] It is worth noting that in step S161, the sample to be tested after solution treatment is placed in a scanning electron microscope to measure the size of the exposed sulfide nucleation core. The field emission electron microscope can ensure the measurement accuracy and improve the detection effect.

[0071] Step S162: using an electron probe to detect the composition of the sulfide nucleation core.

[0072] It is worth noting that in step S162, an electron probe is used to perform quantitative component detection on the sulfide nucleation core of the sample to be tested, so as to accurately detect the composition of the sulfide nucleation core.

[0073] The sulfide nucleation core detection method provided in the embodiment of the present invention first heats the sample to be tested to 1150 degrees Celsius at a preset heating rate and keeps it warm for a preset time to expose the sulfide nucleation core in the sample to be tested; then cools the sample to be tested to 25 degrees Celsius at a preset cooling rate to shape the sulfide nucleation core; then measures the size and detects the composition of the sulfide nucleation core. Compared with the prior art, the sulfide nucleation core detection method provided by the present invention can accurately detect the size and composition of the sulfide nucleation core, improve the detection rate, and have a good detection effect because it adopts the step of heating the sample to be tested to 1150 degrees Celsius at a preset heating rate and keeping it warm for a preset time to expose the sulfide nucleation core in the sample to be tested.

[0074] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for detecting sulfide nucleation cores, It is characterized in that include: Cut a cylindrical sample to be tested from the product; Grinding the sample to be tested, including: grinding the surface of the sample to be tested with sandpapers of 100 mesh, 200 mesh, 400 mesh, 800 mesh, 1000 mesh and 1200 mesh in sequence, wherein the grinding directions of two adjacent sandpapers are perpendicular; Polishing the sample to be tested; The sample to be tested is heated to 1150 degrees Celsius at a preset heating rate and kept warm for a preset time, so that the manganese element and the sulfur element in the sulfide of the sample to be tested are dissolved in the matrix, thereby exposing the sulfide nucleation core, including: placing the sample to be tested in a confocal microscope heating furnace, and continuously introducing an inert gas into the confocal microscope heating furnace; heating the sample to be tested by using the confocal microscope heating furnace; keeping the sample to be tested warm for the preset time; wherein the preset heating rate ranges from 20 degrees Celsius / minute to 40 degrees Celsius / minute, and the preset time is 10 minutes; Cooling the sample to be tested to 25 degrees Celsius at a preset cooling rate to allow the sulfide nucleation core to be fixed, wherein the preset cooling rate ranges from 50 degrees Celsius / minute to 70 degrees Celsius / minute; The size and composition of the sulfide nucleation core are measured.

2. The sulfide nucleation core detection method according to claim 1, It is characterized in that The inert gas flow rate ranges from 10 ml / min to 20 ml / min.

3. The sulfide nucleation core detection method according to claim 1, It is characterized in that The step of polishing the sample to be tested comprises: Polishing the surface of the sample to be tested using 3 micron and 1 micron polycrystalline diamond suspensions in sequence; Dry-polish the sample using a flannel sprayed with alcohol; Rinse the sample to be tested with clean water; Alcohol was dripped on the sample to be tested and blown dry with hot air.

4. The sulfide nucleation core detection method according to claim 1, It is characterized in that The steps of measuring the size and detecting the composition of the sulfide nucleation core include: Using a field emission electron microscope to measure the size of the sulfide nucleation core; The composition of the sulfide nucleation core is detected by using an electron probe.

Citation Information

Patent Citations

  • Hydrodesulphurization catalyst activity measuring method and device for implementing the method

    CN101210867A

  • Method for observing nucleation and growth of graphene on surface of metal base

    CN104568554A

  • Preparation method of sulfur-containing high-emission waste liquid glass ceramic solidifying base material

    CN104810072A

  • Method for measuring high-temperature alloy critical nucleation super-cooling degree

    CN104889348A

  • Method for observing precipitation behaviors of BN in boron-containing steel

    CN107091830A