A method for preparing a high temperature resistant composite gas cylinder
By modifying and optimizing the winding process of polycondensation polyimide resin, the problem of difficult to dissolve and process the polyimide resin is solved, and the preparation of high-temperature composite gas cylinders is realized to meet the high-temperature and high-pressure needs of aerospace missiles is met. , expanding the scope of application.
Patent Information
- Application Number
- CN202111404662.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-11-24
AI Technical Summary
The resin system of existing composite gas cylinders cannot meet the requirements of aviation, aerospace and missiles for high temperatures above 300°C. Polyimide resins are difficult to dissolve, difficult to process and mold, and cannot be directly applied to fiber wrapping processes.
By modifying the polycondensation polyimide resin, adding dimethylacetamide mixed solvent and heating it to fully dissolve, adding alcohol to improve dissolution characteristics, using winding process and vacuum furnace step-up heating and curing, canceling the hot pressing tank Forming process, optimize and simplify gas cylinder preparation process.
It realizes the solubleness and good processing and forming performance of polyimide resin, improves the glass transition temperature and physical and mechanical properties of the material, can be used for a long time at high temperatures above 300℃, meets the storage needs of high temperature and high pressure gas, and expands the gas Application range of bottles.
Smart Images

Figure FDA0004984442800000011 
Figure FDA0004984442800000012
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and specifically relates to a method for preparing a high-temperature resistant composite gas cylinder. Background Art
[0002] Since the application of composite gas cylinders in the 1960s, they have been widely used in existing space launch vehicles, playing an important role in improving the carrying capacity of spacecraft. At present, missiles, aircraft and aero engines have increasingly higher requirements for the high temperature resistance of gas cylinders. In the solid attitude control power system of aircraft, the research and development of composite gas cylinders for storing high temperature and high pressure gases has always been a technical difficulty. The composite layer of the composite gas cylinder is a combination of fiber and resin, which is wrapped around the outside of the metal lining. The carbon fiber itself can withstand a high temperature of 1500°C. The metal lining can be formed by high temperature resistant steel materials or titanium alloys. The process is mature, and the maximum temperature resistance of the gas cylinder is mainly affected by the resin system.
[0003] At present, the resin system commonly used in composite gas cylinders is the epoxy resin system. The maximum temperature that epoxy resin can withstand is 150℃~200℃, while the high-temperature gas cylinders used in aviation, aerospace, and missiles are required to withstand temperatures above 300℃. Therefore, epoxy resin-based composite materials can no longer meet their high temperature requirements. Polyimide resins that can replace epoxy resin-based composite materials in the existing technology can withstand temperatures above 300℃, but polyimide resins have the disadvantages of being difficult to dissolve and difficult to process, and cannot be directly applied to the fiber winding process. Summary of the invention
[0004] The present invention aims at the above-mentioned problems, makes up for the deficiencies of the prior art, and provides a method for preparing a high-temperature resistant composite material gas cylinder that can solve the problems of polyimide resin being difficult to dissolve and difficult to process and shape. The present invention solves the shortcomings of polyimide resin being insoluble and difficult to melt and difficult to process and shape by modifying the polyimide resin. The polyimide resin eliminates the complex autoclave molding process in the wet winding process, thereby achieving the purpose of optimizing and simplifying the gas cylinder preparation process.
[0005] To achieve the above purpose, the present invention adopts the following technical solution.
[0006] The present invention is a method for preparing a high temperature resistant composite gas cylinder, comprising the following steps:
[0007] 1) Metal lining preparation: using steel or titanium alloy to make a seamless metal lining;
[0008] 2) Preparation of polyimide resin: Select polycondensation polyimide, add the polycondensation polyimide to a dimethylacetamide mixed solvent according to a proportion, and fully dissolve the polycondensation polyimide in the dimethylacetamide mixed solvent by heating to prepare a polyimide resin; add alcohol to the prepared polyimide resin and stir evenly. The density of the alcohol and the polyimide resin after evenly mixing is 0.896 g / mm 3 ; The Tg temperature of the prepared polyimide resin is 460°C to 480°C, where Tg is the glass transition temperature;
[0009] 3) Winding: First, the thickness of the circumferential fiber winding layer and the thickness of the spiral fiber winding layer are selected by the winding thickness calculation formula, and the longitudinal fiber winding angle is selected by the winding angle calculation formula to complete the winding of the fiber winding layer on the outside of the metal liner; then, the polyimide resin layer is wound on the outside of the fiber winding layer to form a winding composite layer on the outside of the metal liner; the polyimide resin layer is wound by brushing;
[0010] The formula for calculating winding thickness is: The formula for calculating the winding angle is: In the formula: h θ is the thickness of the hoop fiber winding layer, h α is the thickness of the spiral fiber winding layer, σ fb is the fiber tensile strength, V f is the fiber volume content, P b is the bursting pressure of the gas cylinder, P b1 is the bursting pressure of the metal liner, α is the longitudinal fiber winding angle, R is the radius of the metal liner, d is the diameter of the cylinder mouth, and D is the outer diameter of the cylinder;
[0011] 4) Curing: Use vacuum furnace vacuum heating curing to extract the gas and use a step-by-step heating method to ensure uniform curing process and reduce the void ratio of the winding composite layer.
[0012] As a preferred solution of the present invention, the mass of the polycondensation type polyimide is 40% of the mass of the prepared polyimide resin.
[0013] As another preferred embodiment of the present invention, the fibers in the winding composite layer are carbon fibers, aramid fibers or PBO high-strength fibers.
[0014] As another preferred embodiment of the present invention, the polyimide resin glue is preheated by water bath heating during the winding process, and the preheating temperature is 40°C; the polyimide resin glue heated in the water bath is poured into the glue tank, and the glue tank needs to be heated, and the heating temperature of the glue tank is set to 40°C.
[0015] As another preferred embodiment of the present invention, the polyimide resin layer is coated with a brush to increase the adhesive content of the polyimide resin during the winding process, and the polyimide resin content after winding is 22% to 28%.
[0016] Beneficial effects of the present invention:
[0017] The present invention provides a method for preparing a high-temperature resistant composite gas cylinder. Through the polyimide resin preparation process of step 2) of the present invention, the polyimide resin is modified, and the shortcomings of being difficult to dissolve and difficult to process are solved. Through the curing method of step 4) of the present invention, the polyimide resin eliminates the complex autoclave molding process in the wet winding process, thereby achieving the purpose of optimizing and simplifying the gas cylinder preparation process. DETAILED DESCRIPTION
[0018] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific implementation methods. It should be understood that the specific implementation methods described herein are only used to explain the present invention and are not used to limit the present invention.
[0019] Example 1
[0020] The present invention provides a method for preparing a high temperature resistant composite gas cylinder, comprising the following steps:
[0021] 1) Metal lining preparation: using steel or titanium alloy to make a seamless metal lining;
[0022] 2) Preparation of polyimide resin: Select polycondensation polyimide, add the polycondensation polyimide to a dimethylacetamide mixed solvent according to a proportion, the mass of the polycondensation polyimide is 40% of the mass of the prepared polyimide resin; fully dissolve the polycondensation polyimide in the dimethylacetamide mixed solvent by heating to prepare a polyimide resin; add alcohol to the prepared polyimide resin and stir evenly, the density of the alcohol and the polyimide resin after evenly mixing is 0.896 g / mm 3 ; Alcohol can improve the solubility of polyimide and reduce the precipitation of polyimide; the Tg of the prepared polyimide resin is 460℃~480℃, Tg is the glass transition temperature, which can meet the high temperature 420℃ use environment requirements of gas cylinders;
[0023] 3) Winding: First, the thickness of the circumferential fiber winding layer and the thickness of the spiral fiber winding layer are selected respectively through the winding thickness calculation formula, and the longitudinal fiber winding angle is selected through the winding angle calculation formula to complete the winding of the fiber winding layer on the outside of the metal liner, so that the metal liner can bear a larger internal pressure load and produce a smaller deformation with the smallest mass; then, the polyimide resin layer is wound on the outside of the fiber winding layer to form a winding composite layer on the outside of the metal liner; during the winding process of the polyimide resin layer, a brushing method is used to increase the glue content of the polyimide resin, and the polyimide resin content after winding is 22% to 28%; the fibers in the winding composite layer are carbon fibers; during the winding process, the polyimide resin glue is preheated by water bath heating, and the preheating temperature is 40°C; the polyimide resin glue heated in a water bath is poured into the glue tank, the glue tank needs to be heated, and the heating temperature of the glue tank is set to 40°C;
[0024] The formula for calculating winding thickness is: The formula for calculating the winding angle is: In the formula: h θ is the thickness of the hoop fiber winding layer, h α is the thickness of the spiral fiber winding layer, σ fb is the fiber tensile strength, V f is the fiber volume content, P b is the bursting pressure of the gas cylinder, P b1 is the bursting pressure of the metal liner, α is the longitudinal fiber winding angle, R is the radius of the metal liner, d is the diameter of the cylinder mouth, and D is the outer diameter of the cylinder;
[0025] 4) Curing: Use vacuum furnace for curing. Since polyimide resin generates gas during the curing process, vacuum heating and curing are used to extract the gas. A step-by-step heating method is used to ensure uniform curing process and reduce the void ratio of the winding composite layer.
[0026] Specifically, the present invention improves the solubility of polyimide in solvent by adjusting the polyimide resin preparation process, and increases the polyimide resin content of the gas cylinder by controlling the precipitation of the polyimide resin glue during winding.
[0027] Example 2
[0028] The present invention provides a method for preparing a high temperature resistant composite gas cylinder, comprising the following steps:
[0029] 1) Metal lining preparation: using steel or titanium alloy to make a seamless metal lining;
[0030] 2) Preparation of polyimide resin: Select polycondensation polyimide, add the polycondensation polyimide to a dimethylacetamide mixed solvent according to a proportion, the mass of the polycondensation polyimide is 40% of the mass of the prepared polyimide resin; fully dissolve the polycondensation polyimide in the dimethylacetamide mixed solvent by heating to prepare a polyimide resin; add alcohol to the prepared polyimide resin and stir evenly, the density of the alcohol and the polyimide resin after evenly mixing is 0.896 g / mm 3 ; Alcohol can improve the solubility of polyimide and reduce the precipitation of polyimide; the prepared polyimide resin has a Tg of 460°C, where Tg is the glass transition temperature, which can meet the high temperature 420°C use environment requirements of gas cylinders;
[0031] 3) Winding: First, the thickness of the circumferential fiber winding layer and the thickness of the spiral fiber winding layer are selected respectively through the winding thickness calculation formula, and the longitudinal fiber winding angle is selected through the winding angle calculation formula to complete the winding of the fiber winding layer on the outside of the metal liner, so that the metal liner can bear a larger internal pressure load and produce a smaller deformation with the smallest mass; then, the polyimide resin layer is wound on the outside of the fiber winding layer to form a winding composite layer on the outside of the metal liner; during the winding process of the polyimide resin layer, a brushing method is used to increase the glue content of the polyimide resin, and the polyimide resin content after winding is 22%; the fiber in the winding composite layer is aramid; during the winding process, the polyimide resin glue is preheated by water bath heating, and the preheating temperature is 40°C; the polyimide resin glue heated in a water bath is poured into the glue tank, the glue tank needs to be heated, and the heating temperature of the glue tank is set to 40°C;
[0032] The formula for calculating winding thickness is: The formula for calculating the winding angle is: In the formula: h θ is the thickness of the hoop fiber winding layer, h α is the thickness of the spiral fiber winding layer, σ fb is the fiber tensile strength, V f is the fiber volume content, P b is the bursting pressure of the gas cylinder, P b1 is the bursting pressure of the metal liner, α is the longitudinal fiber winding angle, R is the radius of the metal liner, d is the diameter of the cylinder mouth, and D is the outer diameter of the cylinder;
[0033] 5) Curing: Use vacuum furnace for curing. Since polyimide resin generates gas during the curing process, vacuum heating and curing are adopted to extract the gas. A step-by-step heating method is used to ensure uniform curing process and reduce the void ratio of the winding composite layer.
[0034] Specifically, the present invention improves the solubility of polyimide in solvent by adjusting the polyimide resin preparation process, and increases the polyimide resin content of the gas cylinder by controlling the precipitation of the polyimide resin glue during winding.
[0035] Example 3
[0036] The present invention provides a method for preparing a high temperature resistant composite gas cylinder, comprising the following steps:
[0037] 1) Metal lining preparation: using steel or titanium alloy to make a seamless metal lining;
[0038] 2) Preparation of polyimide resin: Select polycondensation polyimide, add the polycondensation polyimide to a dimethylacetamide mixed solvent according to a proportion, the mass of the polycondensation polyimide is 40% of the mass of the prepared polyimide resin; fully dissolve the polycondensation polyimide in the dimethylacetamide mixed solvent by heating to prepare a polyimide resin; add alcohol to the prepared polyimide resin and stir evenly, the density of the alcohol and the polyimide resin after evenly mixing is 0.896 g / mm 3 ; Alcohol can improve the solubility of polyimide and reduce the precipitation of polyimide; the prepared polyimide resin has a Tg of 480°C, where Tg is the glass transition temperature, which can meet the high temperature 420°C use environment requirements of gas cylinders;
[0039] 3) Winding: First, the thickness of the circumferential fiber winding layer and the thickness of the spiral fiber winding layer are selected respectively through the winding thickness calculation formula, and the longitudinal fiber winding angle is selected through the winding angle calculation formula to complete the winding of the fiber winding layer on the outside of the metal liner, so that the metal liner can bear a larger internal pressure load and produce a smaller deformation with the smallest mass; then, the polyimide resin layer is wound on the outside of the fiber winding layer to form a winding composite layer on the outside of the metal liner; during the winding process of the polyimide resin layer, a brushing method is used to increase the glue content of the polyimide resin, and the polyimide resin content after winding is 28%; the fiber in the winding composite layer is PBO high-strength fiber; during the winding process, the polyimide resin glue is preheated by water bath heating, and the preheating temperature is 40°C; the polyimide resin glue heated in a water bath is poured into the glue tank, the glue tank needs to be heated, and the heating temperature of the glue tank is set to 40°C;
[0040] The formula for calculating winding thickness is: The formula for calculating the winding angle is: In the formula: h θ is the thickness of the hoop fiber winding layer, h α is the thickness of the spiral fiber winding layer, σ fb is the fiber tensile strength, V f is the fiber volume content, P bis the bursting pressure of the gas cylinder, P b1 is the bursting pressure of the metal liner, α is the longitudinal fiber winding angle, R is the radius of the metal liner, d is the diameter of the cylinder mouth, and D is the outer diameter of the cylinder;
[0041] 4) Curing: Use vacuum furnace for curing. Since polyimide resin generates gas during the curing process, vacuum heating and curing are used to extract the gas. A step-by-step heating method is used to ensure uniform curing process and reduce the void ratio of the winding composite layer.
[0042] Specifically, the present invention improves the solubility of polyimide in solvent by adjusting the polyimide resin preparation process, and increases the polyimide resin content of the gas cylinder by controlling the precipitation of the polyimide resin glue during winding.
[0043] The glass transition temperature Tg of the polyimide resin prepared by the preparation method of the present invention is 460℃~480℃, which can meet the requirements of the high temperature 420℃ use environment; the high temperature resistant composite material gas cylinder prepared by the preparation method of the present invention can meet the high temperature environment 400℃ high pressure gas storage, greatly expand the application range of the gas cylinder, and play a significant role in promoting the military field. Through the preparation process of the polyimide resin of the present invention, the polyimide resin is modified, the disadvantage of thermoplastic materials being difficult to form and process is solved, and a resin system with excellent processing and forming properties and physical and mechanical properties is formed, which significantly improves the glass transition temperature of the polyimide resin material, so that it can be used for a long time at a high temperature of more than 300℃. The soluble polyimide resin developed by the present invention after modifying the polyimide resin can be made to have both heat resistance and good solvent by introducing a large volume of phenyl groups, which can solve the problem of high porosity of the resin and the composite material. The soluble polyimide resin prepared by the present invention after modification of the polyimide resin can improve the interlaminar shear strength and elongation at break of the polyimide resin wound product, and ensure that the gas cylinder can withstand high pressure.
[0044] It can be understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.
Claims
1. A method for preparing a high temperature resistant composite material gas cylinder, characterized in that: The steps include: 1) Metal lining preparation: using steel or titanium alloy to make a seamless metal lining; 2) Preparation of polyimide resin: Select polycondensation polyimide, add the polycondensation polyimide to a dimethylacetamide mixed solvent according to a proportion, and fully dissolve the polycondensation polyimide in the dimethylacetamide mixed solvent by heating to prepare a polyimide resin; add alcohol to the prepared polyimide resin and stir evenly. The density of the alcohol and the polyimide resin after evenly mixing is 0.896 g / mm 3 ; The Tg of the prepared polyimide resin is 460°C to 480°C, where Tg is the glass transition temperature; 3) Winding: First, the thickness of the circumferential fiber winding layer and the thickness of the spiral fiber winding layer are selected respectively by the winding thickness calculation formula, and the longitudinal fiber winding angle is selected by the winding angle calculation formula to complete the winding of the fiber winding layer on the outside of the metal lining; then, the polyimide resin layer is wound on the outside of the fiber winding layer to form a winding composite layer on the outside of the metal lining; the polyimide resin layer is wound by brushing; the polyimide resin glue is preheated by water bath heating during the winding process, and the preheating temperature is 40°C; the polyimide resin glue heated in the water bath is poured into the glue tank, the glue tank needs to be heated, and the heating temperature of the glue tank is set to 40°C; The formula for calculating winding thickness is: The formula for calculating the winding angle is: In the formula: h θ is the thickness of the hoop fiber winding layer, h α is the thickness of the spiral fiber winding layer, σ fb is the fiber tensile strength, V f is the fiber volume content, P b is the bursting pressure of the gas cylinder, P b1 is the bursting pressure of the metal liner, α is the longitudinal fiber winding angle, R is the radius of the metal liner, d is the diameter of the cylinder mouth, and D is the outer diameter of the cylinder; 4) Curing: Use vacuum furnace vacuum heating curing to extract the gas and use a step-by-step heating method to ensure uniform curing process and reduce the void ratio of the winding composite layer.
2. The method for preparing a high temperature resistant composite material gas cylinder according to claim 1, characterized in that: The mass of the polycondensation type polyimide is 40% of the mass of the prepared polyimide resin.
3. The method for preparing a high temperature resistant composite material gas cylinder according to claim 1, characterized in that: The fibers in the winding composite layer are carbon fibers, aramid fibers or PBO high-strength fibers.
4. The method for preparing a high temperature resistant composite material gas cylinder according to claim 1, characterized in that: During the winding process of the polyimide resin layer, a brushing method is adopted to increase the glue content of the polyimide resin. The content of the polyimide resin after winding is 22% to 28%.
Citation Information
Patent Citations
Manufacturing method of fishing pole made from polyimide fiber reinforced resin matrix composite
CN106113525A
Design method of high-temperature-resistant and high-pressure-resistant carbon fiber polyimide composite gas cylinder
CN112524476A
Manufacture of pressure vessel
JP2000313069A