Cu-WO sputtering target and oxide film

By fabricating Cu-WO sputtering targets, the problem of high resistivity in high work function oxide films during film formation was solved, enabling high-speed DC sputtering and efficient charge injection, which is suitable for transparent electrodes in organic semiconductor devices such as organic EL elements.

CN114182216BActive Publication Date: 2024-11-15JX NIPPON MINING & METALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110422866.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-15
Filing Date
2021-04-20
Publication Date
2024-11-15
Estimated Expiration
2041-04-20

AI Technical Summary

Technical Problem

In the prior art, oxide thin films with high work function, such as WO3, have high volume resistivity during film formation, making it difficult to perform high-speed DC sputtering and failing to meet the requirements of efficient charge injection in organic semiconductor devices such as organic EL elements.

Method used

Using Cu-WO sputtering targets, a sputtering target with a volume resistivity of less than 1.0 × 10³ Ω·cm is prepared by mixing tungsten, copper and oxygen. Combined with strict manufacturing processes such as wet crushing, cold isostatic pressing and atmospheric pressure sintering, high density and low resistance are ensured.

Benefits of technology

High-speed DC sputtering of oxide thin films with high work function was achieved, which improved the charge injection efficiency in organic semiconductor devices and reduced the risk of damage to powder particles and targets during the film formation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003028462570000071
    Figure BDA0003028462570000071
Patent Text Reader

Abstract

The present invention relates to a Cu-W-O sputtering target and an oxide film. A Cu-W-O sputtering target is a sputtering target comprising tungsten (W), copper (Cu), oxygen (O) and inevitable impurities, wherein the volume resistivity of the Cu-W-O sputtering target is 1.0×10 3 Ω·cm or less. An oxide thin film, which is a thin film containing tungsten (W), copper (Cu), oxygen (O) and inevitable impurities, wherein the content ratio of W and Cu satisfies 0.5≤W / (Cu+W)<1 in terms of atomic ratio. The subject of the present invention is to provide a sputtering target that can form a film with a high work function and has a low volume resistivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a Cu-WO sputtering target suitable for forming an oxide film with a high work function. Background Art

[0002] ITO (indium tin oxide) is used as a transparent electrode (anode) in light-emitting elements such as organic electroluminescent (organic EL) elements. Holes injected by applying voltage to the anode are combined with electrons in the light-emitting layer via the hole transport layer. In recent years, in order to improve the efficiency of charge injection into the hole transport layer, the use of oxides with a higher work function than ITO is being studied. For example, in Non-Patent Document 1, TiO 2 、MoO 2 、CuO、NiO、WO 3 、V 2 O 5 CrO 3 、 2 O 5 、Co 3 O 4 Oxide films with high work functions are used as oxide films in organic semiconductor devices.

[0003] As shown in Non-Patent Document 1, WO 3 Has a relatively high work function. 3 The film can be formed using a sputtering target composed of a sintered body of tungsten oxide (Patent Documents 1 and 2), but in the case of WO 3 In the case of a single phase, it is difficult to achieve a high density of the sintered body, and it is difficult to perform DC sputtering due to the high volume resistivity. 3 Add WO 2 The sintered body can be made denser and more conductive, thereby enabling DC sputtering. In addition, Patent Document 1 discloses a method of sputtering WO in an atmosphere supplied with oxygen. 3 The powder is hot pressed to increase the density of the sintered body.

[0004] Prior art literature

[0005] Patent Literature

[0006] [Patent Document 1] Japanese Patent Application Laid-Open No. 3-150357

[0007] [Patent Document 2] Japanese Patent Application Publication No. 2013-76163

[0008] [Non-patent literature]

[0009] [Non-patent document 1] Mark T Greiner and Zheng-Hong Lu, "Thin-Film metal oxides in organic semiconductor devices: their electronic structures, work functions and interfaces", NPG Asia Materials (2013) 5, e55, 19July 2013 Summary of the invention

[0010] Problems to be solved by the invention

[0011] As described above, an oxide film with a high work function is desired for a film constituting an organic semiconductor device such as an organic EL. Examples of materials having a high work function include WO 3 etc., but in the formation of WO 3 In the case of films such as , the volume resistivity of the sputtering target used in the film formation is high, so there is a problem that DC sputtering capable of high-speed film formation cannot be performed. Therefore, the present invention is proposed to solve the above-mentioned problem, and its subject is to provide a sputtering target that can form a film with a high work function and a low volume resistivity.

[0012] Means used to solve problems

[0013] The present invention is proposed to solve the above-mentioned problem. The embodiment of the present invention that can solve the problem is a Cu-WO sputtering target, which is a sputtering target containing tungsten (W), copper (Cu), oxygen (O) and inevitable impurities, wherein the volume resistivity of the Cu-WO sputtering target is 1.0×10 3 Ω·cm or less.

[0014] Effects of the Invention

[0015] According to the present invention, there are excellent effects that a sputtering target is a sputtering target capable of forming a film having a high work function, and since the volume resistivity is low, DC sputtering is possible, thereby enabling high-speed film formation. DETAILED DESCRIPTION

[0016] As mentioned above, WO 3 Has a high work function, but in WO 3 In the case of a single phase, it is difficult to produce a sputtering target with a low volume resistivity that can be used for DC sputtering. In addition, when using other oxide materials with high work functions (for example, CuO single phase), the volume resistivity is also high and DC sputtering is difficult. In view of such problems, the present inventors have conducted in-depth research and obtained the following insights: by producing CuO and WO 3The present invention is completed by using a mixed system of a sputtering target with low volume resistivity that can be DC sputtered while maintaining a high work function.

[0017] The sputtering target (referred to as a Cu-WO sputtering target) according to an embodiment of the present invention contains tungsten (W), copper (Cu), oxygen (O), and inevitable impurities, and has a volume resistivity of 1.0×10 3 Ω·cm or less. If the volume resistivity of the sputtering target is 1.0×10 3 Ω·cm or less, DC sputtering can be performed, thereby enabling high-speed film formation. The preferred volume resistivity is 1.0×10 2 This makes it possible to achieve more stable high-speed film formation by DC sputtering.

[0018] The sputtering target of the present embodiment contains W, Cu, O and inevitable impurities, and the content ratio of W and Cu is preferably W / (Cu+W)≥0.5 in terms of atomic ratio. When W / (Cu+W)<0.5, the volume resistivity may become high, and the desired high work function may not be obtained. Preferably, W / (Cu+W)≥0.7, more preferably W / (Cu+W)≥0.8, and further preferably W / (Cu+W)≥0.9. In addition, when WO 3 In the case of a single phase, as described above, the volume resistivity of the sputtering target is high, so it is set to W / (Cu+W) < 1. It should be noted that the unavoidable impurities are impurities mixed in the raw materials, manufacturing process, etc., and may be contained in an amount that does not particularly affect the properties such as the work function. As long as it is 0.1 wt % or less, it can be said that there is no particular problem.

[0019] The relative density of the sputtering target of this embodiment is preferably 95% or more. The preferred relative density is 98% or more. Such a high-density sputtering target can prevent cracks and breakages during sputtering, and can reduce particles during film formation. In addition, the relative density of the sputtering target is also related to the volume resistivity. When the relative density value becomes lower, the volume resistivity tends to become higher. Therefore, in order to reduce the volume resistivity, in addition to the content ratio of W and Cu in the sputtering target, it is also necessary to increase the relative density by strictly adjusting the manufacturing method and manufacturing conditions of the sputtering target.

[0020] The work function of the sputtering target of one embodiment of the present invention is 4.3 eV or more. By using such a sputtering target with a high work function, a film with a high work function can be produced. Moreover, such a film with a high work function can, for example, improve the efficiency of charge injection into the hole transport layer in organic semiconductor devices such as organic EL and organic solar cells, and can be expected to improve the luminous efficiency or conversion efficiency.

[0021] The following is a description of a method for producing a sputtering target according to the present embodiment. However, the following production conditions and the like are not limited to the disclosed ranges, and it is obvious that some omissions and changes may be made.

[0022] Prepare tungsten oxide (WO 3 ) powder and copper oxide (CuO) powder are used as raw material powders, and these raw material powders are weighed to achieve the desired composition ratio. As copper oxide, in addition to CuO, Cu 2 O, etc. Next, wet pulverization is performed using zirconium oxide beads with a ball diameter of 0.5 mm to 3.0 mm. Then, pulverization is performed until the median particle size reaches 0.1 μm to 5.0 μm, and then granulation is performed. Next, the obtained granulated powder is pressed and molded. The pressing and molding is preferably performed at 300 kgf / cm 2 ~400kgf / cm 2 Then, cold isostatic pressing (CIP) is performed. The cold isostatic pressing is preferably performed at 1000 kgf / cm 2 ~2000kgf / cm 2 The obtained molded body is then subjected to normal pressure sintering for 10 to 20 hours in an oxygen gas flow. At this time, the sintering temperature is preferably set to be greater than or equal to 900°C and less than 950°C. When the sintering temperature is less than 900°C, a high-density sintered body cannot be obtained. On the other hand, when the sintering temperature is greater than or equal to 950°C, the WO 3 CuWO composite oxide with CuO 4 It is not preferred because it reacts with the sintered component of aluminum oxide and melts. Then, the obtained sintered body is cut, ground, etc. to form a target shape, thereby making a sputtering target. It should be noted that when hot pressing sintering is used, CuO is sometimes reduced to Cu due to the sintered component of carbon, which intensifies the consumption of components.

[0023] In the present specification, various physical properties of a sputtering target and the like are analyzed using the following measuring methods.

[0024] (Sputtering target and film composition)

[0025] Device: SPS3500DD manufactured by SII

[0026] Method: ICP-OES (high frequency inductively coupled plasma optical emission spectroscopy)

[0027] (Membrane composition)

[0028] Device: JXA-8500F manufactured by JEOL

[0029] Method: EPMA (Electron Probe Microanalyzer)

[0030] Accelerating voltage: 5keV~10keV

[0031] Irradiation current: 2.0×10 -7 A~2.0×10 -8 A

[0032] Probe diameter: 10 μm

[0033] Five points of smooth film-formed portions where dust or the like was not attached and the substrate surface was not visible were selected for point analysis, and their average composition was calculated.

[0034] (Volume resistivity of sputtering target)

[0035] The volume resistivity of the sputtering target was measured at five points on the surface of the sputtering target (one point at the center and four points near the periphery), and the average value thereof was adopted. The following apparatus was used for the measurement.

[0036] Equipment: Resistivity meter Σ-5+ manufactured by NPS

[0037] Method: Constant current application method

[0038] Method: DC four-probe method

[0039] (About the relative density of sputtering target)

[0040] Relative density (%) = Archimedean density / true density × 100

[0041] Archimedean density: Small pieces are cut from the sputtering target and the density is calculated from the small pieces using the Archimedean method.

[0042] True density: The atomic ratio of Cu and W is calculated by elemental analysis. Based on the atomic ratio, the weight of Cu converted to CuO is set to a (weight %), and the weight of W converted to WO is set to 3 The converted weight is b (wt%), and CuO, WO 3 The theoretical density is set as d CuO ,d WO3 , calculate the true density (g / cm 3 )=100 / (a / d CuO +b / d WO3 ). It should be noted that the theoretical density of CuO is CuO =6.31g / cm 3 , WO 3 Theoretical density d WO3 =7.16g / cm 3 .

[0043] (About work function)

[0044] For the block (sputtering target), a sample with a length of 20 mm, a width of 10 mm, and a thickness of 5 mm to 10 mm was prepared. The measurement surface was ground using sandpaper with a mesh number of 2000. In addition, for the sputtered film, a 20 mm × 20 mm sample obtained by film formation on a Si substrate was prepared and measured under the following conditions. It should be noted that the measurement result of the work function does not depend on the size of the sample. In addition, when the measurement surface is not ground or is ground using sandpaper with a low mesh number, resulting in insufficient surface grinding, the work function may not be accurately measured and its value may be measured to be high.

[0045] Method: Photoelectron spectroscopy in air

[0046] Device: Manufactured by Riken Keiki Co., Ltd., AC-5 device

[0047] Conditions: The range of work function that can be measured: 3.4eV to 6.2eV

[0048] Light source power: 2000W

[0049] [Example]

[0050] The following is a description based on examples and comparative examples. It should be noted that this example is only an example and is not limited to this example. That is, the present invention is limited only by the claims and includes various modifications other than the examples included in the present invention.

[0051] (Example 1)

[0052] Preparation of CuO powder and WO 3 Powder, CuO:WO 3 =50:50 (mol%). Then, the powders were mixed and pulverized in a wet ball mill for 24 hours using 3.0 mm zirconia beads to obtain a mixed powder with a median particle size of 0.8 μm or less. Then, the mixed powder was pulverized at a surface pressure of 400 kgf / cm 2 The mixed powder was pressurized under the condition of 1800 kgf / cm 2 CIP was performed under the conditions of , thereby producing a molded body.

[0053] Next, the sintered body was sintered at normal pressure for 10 hours at a sintering temperature of 940° C. in an oxygen gas flow to produce a sintered body. The sintered body was then machined to be finished into the shape of a sputtering target.

[0054] The sputtering target obtained in Example 1 was evaluated and found to have a relative density of 103.3% and a volume resistivity of 1.0×10 3Ω·cm. In addition, the work function of the sputtering target was measured, and a work function as high as 4.5 eV was obtained. The above results are shown in Table 1. It should be noted that the composition analysis of the sputtering target confirmed that there was almost no change compared with the ratio when the raw materials were charged.

[0055]

[0056] (Examples 2 to 5)

[0057] Preparation of CuO powder and WO 3 The powders were weighed to give the molar ratios shown in Table 1. Then, the mixture was mixed and pulverized in a wet ball mill for 24 hours using 3.0 mm zirconia beads to obtain a mixed powder having a median particle size of 0.8 μm or less. Then, the mixture was pulverized at a surface pressure of 400 kgf / cm 2 The mixed powder was pressurized under the condition of 1800 kgf / cm 2 CIP was performed under the conditions of , thereby producing a molded body.

[0058] Next, normal pressure sintering was performed at a sintering temperature of 940° C. for 10 hours in an oxygen gas flow to produce a sintered body. Then, each sintered body was machined to be finished into a sputtering target shape.

[0059] The relative density of the sputtering targets of Examples 2 to 5 was all above 99%, and the volume resistivity was all 1.0×10 3 Ω·cm or less. In addition, the work function of the sputtering target was measured, and the result was a work function as high as 4.5 eV. It should be noted that the composition analysis of the sputtering target confirmed that there was almost no change compared with the ratio when the raw materials were put in.

[0060] (Comparative Example 1)

[0061] In Comparative Example 1, only CuO powder was used without WO 3 The Cu powder was mixed and pulverized in a wet ball mill for 24 hours using 3.0 mm zirconia beads to obtain a mixed powder having a median particle size of 0.8 μm or less. 2 The mixed powder was pressurized under the condition of 1800 kgf / cm 2 CIP was performed under the conditions of , thereby producing a molded body.

[0062] Next, the sintered body was sintered at normal pressure for 10 hours at a sintering temperature of 950° C. in an oxygen gas flow to produce a sintered body. The sintered body was then machined to be finished into the shape of a sputtering target.

[0063] The sputtering target obtained in Comparative Example 1 was evaluated and found to have a relative density of 98.3% and a volume resistivity of 3.3×10 5 Ω·cm. In addition, the work function of the sputtering target was measured and the result was 4.2 eV. It should be noted that the component analysis of the sputtering target confirmed that there was almost no change compared with the ratio when the raw materials were charged.

[0064] (Comparative Examples 2 and 3)

[0065] In Comparative Examples 2 and 3, only WO 3 Powder, no CuO powder was used. 3.0 mm zirconia beads were used to 3 The powder was mixed and pulverized in a wet ball mill for 24 hours to obtain a mixed powder with a median particle size of 0.8 μm or less. 2 The mixed powder was pressurized under the condition of 1800 kgf / cm 2 CIP was performed under the conditions of , thereby producing a molded body.

[0066] Next, the sintering temperature was set to 1100° C. (Comparative Example 2) or 940° C. (Comparative Example 3) in an oxygen gas flow, and atmospheric sintering was performed for 10 hours to produce a sintered body. The sintered body was then machined to a sputtering target shape.

[0067] The sputtering targets obtained in Comparative Examples 2 and 3 were evaluated. The results showed that the relative density was less than 95%, and the volume resistivity was greater than 1.0×10 3 Ω·cm. In addition, the work function of the sputtering target was measured and the result was 4.4 eV. It should be noted that the composition analysis of the sputtering target confirmed that there was almost no change compared with the ratio when the raw materials were charged.

[0068] (Comparative Example 4)

[0069] Preparation of CuO powder and WO 3 Powder, CuO:WO 3 =30:70 (mol%). Then, the powders were mixed and pulverized in a wet ball mill for 24 hours using 3.0 mm zirconia beads to obtain a mixed powder with a median particle size of 0.8 μm or less. The surface pressure was 400 kgf / cm 2 The mixed powder was pressurized under the condition of 1800 kgf / cm 2 CIP was performed under the conditions of , thereby producing a molded body.

[0070] Next, the sintered body was sintered at normal pressure for 10 hours at a sintering temperature of 850° C. in an oxygen gas flow to produce a sintered body. The sintered body was then machined to be finished into the shape of a sputtering target.

[0071] The sputtering target obtained in Comparative Example 4 was evaluated and found to have a volume resistivity of 3.1×10 4 Ω·cm.

[0072] Next, sputtering film formation was performed using the sputtering target of Example 3. The film formation conditions are as follows. The work function of the obtained sputtered film was measured and found to be 4.6 eV in Ar gas and 4.6 eV in Ar gas + 6% O. 2 The work function was 4.8 eV, which was the expected high work function. It should be noted that the composition of the sputtered film was analyzed, and it was confirmed that there was almost no change in the ratio compared with the ratio when the raw materials were charged.

[0073] (film forming conditions)

[0074] Equipment: SPL-500 sputtering equipment manufactured by CANON ANELVA

[0075] Substrate: Silicon substrate

[0076] Film forming power density: 1.0W / cm 2

[0077] Film forming atmosphere: Ar or Ar+6%O 2

[0078] Gas pressure: 0.5Pa

[0079] Film thickness: 50nm

[0080] Industrial Applicability

[0081] The Cu-WO sputtering target of the embodiment of the present invention has a low volume resistivity, can be DC sputtered, has a high relative density, does not break or crack during film formation, and can be used at a practical and commercial level. The present invention can be used to form a transparent electrode in a light-emitting element such as an organic electroluminescent element.

Claims

1. A Cu-WO sputtering target, which is a sputtering target containing tungsten (W), copper (Cu), oxygen (O) and inevitable impurities, in, The volume resistivity of the Cu-WO sputtering target is 1.0×10 3 Ω·cm or less, and the Cu—WO sputtering target satisfies a work function of 4.5 eV or more.

2. The Cu-WO sputtering target according to claim 1, in, The relative density of the Cu-WO sputtering target is above 95%.

3. The Cu-WO sputtering target according to claim 1 or 2, in, The content ratio of W and Cu satisfies 0.8≤W / (Cu+W)<1 in terms of atomic ratio.

4. An oxide thin film, which is a thin film containing tungsten (W), copper (Cu), oxygen (O) and inevitable impurities, in, The content ratio of W and Cu satisfies 0.8≤W / (Cu+W)<1 in terms of atomic ratio, and the oxide thin film satisfies a work function of 4.5 eV or more.