Anti-corrosion and anti-static metal pipeline and preparation method thereof

By spraying anti-corrosion and anti-static coating composed of fluororesin base material and conductive filler on metal pipes, a conductive network and a multi-layer protection system are formed, which solves the static and corrosion problems of metal pipes when transporting crude oil or sewage, and realizes the pipeline Safe and stable operation and extended service life.

CN118959730APending Publication Date: 2024-11-15ZHENGZHOU HAITAIKE POLYMER TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411017327.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Metal pipelines are prone to static electricity and corrosion during the transportation of crude oil or sewage, resulting in safety risks and system failures. It is difficult for the existing technology to effectively prevent static electricity and corrosion.

Method used

It adopts anti-corrosion and anti-static coating composed of fluororesin base material, conductive filler (carbon fiber tube, carbon black, graphite), preservatives (isothiazolinone, quaternary ammonium salt, nitrite, phosphate) and thixotropic agent. Spray on metal pipes through a high-pressure airless sprayer to form a conductive network and a multi-layer anti-corrosion protection system.

Benefits of technology

It significantly reduces the volume resistivity of the inner wall of the pipeline, prevents electrostatic discharge, extends the service life of the pipeline, and improves the safety and stability of the conveying medium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118959730A_ABST
    Figure CN118959730A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-corrosion and anti-static metal pipeline and a preparation method thereof, and belongs to the technical field of pipeline anti-corrosion and anti-static, the metal pipeline comprises a base material layer, a primer layer and an anti-corrosion and anti-static coating, the upper surface of the base material layer is coated with the primer layer, and the upper surface of the primer layer is coated with the anti-corrosion and anti-static coating. The binding face of the anti-corrosion and anti-static coating and the primer layer is a plane, and the binding face of the primer layer and the base material layer is a wavy curved face. The anticorrosive and antistatic coating is prepared from the following components in parts by weight: 25-30 parts of fluororesin base material, 10-15 parts of conductive filler, 2-4 parts of preservative, 1-2 parts of thixotropic agent and 60-70 parts of solvent. The anti-corrosion and anti-static metal pipeline prepared by the invention can realize the anti-static performance in the pipeline, can ensure the safety and stability of crude oil during high-speed transportation in the metal pipeline, also has the anti-corrosion performance, and can more effectively prolong the service life of the metal pipeline.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pipeline anti-corrosion and anti-static technology, and specifically relates to an anti-corrosion and anti-static metal pipeline and a preparation method thereof. Background Art

[0002] The choice of metal pipe inner wall coating is crucial to the performance of the pipe. It not only provides protection for the pipe body and prevents it from being eroded by the transported medium (such as crude oil, sewage, etc.), but also has a significant drag reduction effect, thereby improving the transportation efficiency. Especially in oil pipeline transportation, the corrosion resistance and anti-static performance of the pipeline are particularly important.

[0003] Most of the metal pipes used in my country's petroleum industry are used to transport crude oil, sewage and water injection. When crude oil is transported at high speed in metal pipes, the increase in flow rate will significantly increase the possibility of static electricity. The accumulation of static electricity may not only lead to safety risks, but also affect the normal operation of the pipeline system. For metal pipes that transport sewage and water injection, the transport medium often contains a variety of additives, acids, alkalis, salts and other components, and sometimes also includes highly corrosive drilling mud and seawater. These media will produce chemical or electrochemical reactions with the inner wall of the metal pipe during long-term transportation, causing the pipe wall to gradually corrode. Over time, the corrosion phenomenon will continue to accumulate, and eventually holes may form in the pipe, affecting the airtightness of the transportation. This will not only cause sewage or water injection to leak, waste resources and pollute the environment, but also in serious cases may cause safety accidents and damage personnel and equipment.

[0004] Therefore, in order to ensure the safe and stable operation of the pipeline, developing a metal pipeline with anti-corrosion and anti-static properties has become one of the problems that technical personnel in this field urgently need to solve. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present invention discloses an anti-corrosion and anti-static metal pipe and a preparation method thereof. The metal pipe prepared by the preparation method provided by the present invention has excellent anti-corrosion and anti-static properties.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides an anti-corrosion and anti-static metal pipe, which comprises a substrate layer, a primer layer and an anti-corrosion and anti-static coating. The upper surface of the substrate layer is sprayed with the primer layer, and the upper surface of the primer layer is sprayed with the anti-corrosion and anti-static coating. The bonding surface between the anti-corrosion and anti-static coating and the primer layer is a flat surface, and the bonding surface between the primer layer and the substrate layer is a wavy curved surface.

[0008] Preferably, the coating of the anti-corrosion and antistatic coating is made of the following components in parts by weight: 25-30 parts of fluororesin base material, 10-15 parts of conductive filler, 2-4 parts of preservative, 1-2 parts of thixotropic agent, and 60-70 parts of solvent.

[0009] Preferably, the fluororesin base material is one of fusible polytetrafluoroethylene, fluorinated ethylene-propylene copolymer, ethylene-tetrafluoroethylene copolymer or a combination thereof; the conductive filler is composed of carbon fiber tube, carbon black and graphite in a mass ratio of 1:(3-4):(5-6); the preservative is 3 or 4 of isothiazolinone, quaternary ammonium salt, nitrite and phosphate; the thixotropic agent is one of polyamide wax, organic bentonite and fumed silica; the solvent is one of methyl ethyl ketone, ethyl acetate and isopropanol.

[0010] The method for preparing the coating of the anti-corrosion and anti-static coating of the present invention comprises the following specific steps:

[0011] S1. Prepare raw materials: prepare fluororesin base material, conductive filler, preservative, thixotropic agent and solvent by weight;

[0012] S2. The conductive filler is gradually added to the first part of the solvent, and dispersed using a high-speed disperser for 10 to 30 minutes to obtain a uniformly dispersed conductive filler suspension;

[0013] S3. The preservative and the thixotropic agent are added to the conductive filler suspension in step S2, and the mixture is dispersed for 10 to 30 minutes using a high-speed disperser to obtain a mixed suspension;

[0014] S4. Slowly add the fluororesin base material to the mixed suspension obtained in step S3, stir and mix evenly, then add the remaining second part of the solvent, continue stirring until completely mixed, and remove undispersed particles or impurities by filtering, thereby obtaining a coating for the anti-corrosion and antistatic coating.

[0015] Preferably, the mass ratio of the first part of the solvent in step S2 to the second part of the solvent in step S4 is 1:(2-4).

[0016] The method for preparing the anti-corrosion and anti-static metal pipe of the present invention comprises the following steps:

[0017] (1) Cleaning the upper surface of the substrate layer in the metal pipe and performing sandblasting pretreatment on the upper surface of the substrate layer;

[0018] (2) uniformly coating a primer on the upper surface of the substrate layer pretreated in step (1) to form a primer layer;

[0019] (3) The anti-corrosion and anti-static coating is mixed evenly with the fluorine-containing epoxy resin curing agent, and sprayed evenly on the primer layer formed in step (2) using a high-pressure airless sprayer. After the spraying is completed, the anti-corrosion and anti-static coating is cured at room temperature to form an anti-corrosion and anti-static metal pipe.

[0020] Preferably, the primer in step (2) is one or a combination of epoxy primer, polyurethane primer, modified acrylic primer, zinc phosphate primer.

[0021] Preferably, the thickness of the primer layer in step (2) is 25 to 30 μm.

[0022] Preferably, the pressure of the high-pressure airless sprayer in step (3) is 150 to 200 bar.

[0023] Preferably, in the step (3), the mass ratio of the coating of the anti-corrosion and anti-static coating to the fluorine-containing epoxy resin curing agent is (10-15):1, and the thickness of the anti-corrosion and anti-static coating is 150-200 μm.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The present invention discloses a conductive filler (carbon fiber tube, carbon black and graphite). The carbon fiber tube has high conductivity and high strength, and they can form an effective conductive path in the material; the graphite flake structure makes it easy to form a plane contact in the material, which is helpful to form a conductive network; the carbon black can form a dense conductive network in the fluoropolymer. The present invention mixes the carbon fiber tube, carbon black and graphite according to the mass ratio as conductive fillers and adds them to the fluoropolymer base material. As the content of the conductive filler increases, the graphite will form a three-dimensional conductive network inside the coating material, allowing charges to move freely therein. When the charge is introduced into the surface of the material, the charge can be quickly dispersed through the conductive network, thereby reducing the volume resistivity of the coating material; when the charge accumulates on the surface of the fluoropolymer, the charge can be quickly neutralized through the conductive network formed by the carbon black on its surface and the conductive path formed by the carbon fiber tube in the material, thereby preventing the occurrence of electrostatic discharge events in the pipeline. The conductive base material disclosed in the present invention can be applied to the anti-corrosion and anti-static coating for metal pipelines to significantly reduce the volume resistivity of the material and form an effective conductive network, thereby achieving anti-static performance of the inner wall of the pipeline, preventing charge accumulation and electrostatic discharge, and ensuring the safety and stability of crude oil during high-speed transportation in metal pipelines.

[0026] (2) The preservatives added to the metal pipe coating of the present invention complement each other to form a multi-faceted anti-corrosion protection system. Isothiazolinone or quaternary ammonium salts can inhibit microbial activity and prevent microbial-induced corrosion; nitrites can form a protective oxide film on the inner wall of the metal pipe to prevent the metal from contacting oxygen and water in the environment, thereby reducing corrosion, while inhibiting electrochemical reactions on the metal surface and slowing down the corrosion rate; and phosphates can react with metal ions on the metal surface to form an insoluble phosphate film, which can block direct contact between the corrosive medium and the metal substrate. The present invention can more effectively extend the service life of metal pipes and reduce maintenance costs through the synergistic effect of the preservatives. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic structural diagram of an anti-corrosion and anti-static metal pipeline of the present invention.

[0028] In the figure: 1 substrate layer, 2 primer layer, 3 anti-corrosion and anti-static coating. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Combine the following Figure 1 The present invention is described in detail:

[0031] The invention discloses an anti-corrosion and anti-static metal pipe, which comprises a substrate layer 1, a primer layer 2 and an anti-corrosion and anti-static coating 3. The primer layer 2 is sprayed on the upper surface of the substrate layer 1, and the anti-corrosion and anti-static coating 3 is sprayed on the upper surface of the primer layer 2. The bonding surface between the anti-corrosion and anti-static coating 3 and the primer layer 2 is a flat surface, and the bonding surface between the primer layer 2 and the substrate layer 1 is a wavy curved surface.

[0032] Among them, the coating of the anti-corrosion and anti-static coating is made of the following components in parts by weight: 25-30 parts of fluororesin base material, 10-15 parts of conductive filler, 2-4 parts of preservative, 1-2 parts of thixotropic agent, and 60-70 parts of solvent; the fluororesin base material is one or a combination of fusible polytetrafluoroethylene, fluorinated ethylene-propylene copolymer, and ethylene-tetrafluoroethylene copolymer, the conductive filler is a carbon fiber tube, carbon black, and graphite in a mass ratio of 1: (3-4): (5-6), the preservative is 3 or 4 of isothiazolinone, quaternary ammonium salt, nitrite and phosphate, the thixotropic agent is one of polyamide wax, organic bentonite, and fumed silica; the solvent is one of methyl ethyl ketone, ethyl acetate, and isopropanol.

[0033] The preparation method of the coating of the anti-corrosion and anti-static coating of the present invention comprises the following specific steps:

[0034] S1. Prepare raw materials: prepare fluororesin base material, conductive filler, preservative, thixotropic agent and solvent by weight.

[0035] S2. gradually add the conductive filler into the first part of the solvent, and disperse it for 10 to 30 minutes using a high-speed disperser to obtain a uniformly dispersed conductive filler suspension.

[0036] S3. Add the preservative and the thixotropic agent to the conductive filler suspension in step S2 respectively, and continue to disperse using a high-speed disperser for 10 to 30 minutes to obtain a mixed suspension.

[0037] S4. Slowly add the fluororesin base material to the mixed suspension obtained in step S3, stir and mix evenly, then add the remaining second part of the solvent, continue stirring until completely mixed, and remove undispersed particles or impurities by filtering, thereby obtaining a coating for the anti-corrosion and antistatic coating.

[0038] Wherein, the mass ratio of the first part of the solvent in step S2 to the second part of the solvent in step S4 is 1:(2-4).

[0039] The present invention also provides a method for preparing an anti-corrosion and anti-static metal pipe, comprising the following steps:

[0040] (1) Clean the upper surface of the substrate layer inside the metal pipe and perform sandblasting pretreatment on the upper surface of the substrate layer.

[0041] (2) uniformly coating a primer on the upper surface of the substrate layer pretreated in step (1), wherein the primer is one of epoxy primer, polyurethane primer, modified acrylic primer, zinc phosphate primer or a combination thereof, to form a primer layer with a thickness of 25 to 30 μm.

[0042] (3) The anti-corrosion and anti-static coating prepared above is mixed evenly with a fluorine-containing epoxy resin curing agent (the mass ratio of the coating to the fluorine-containing epoxy resin curing agent is (10-15): 1), and the primer layer formed in step (2) is evenly sprayed using a high-pressure airless sprayer at a pressure of 150-200 bar. After the spraying is completed, the anti-corrosion and anti-static coating is cured at room temperature to form a 150-200 μm thick anti-corrosion and anti-static coating, thereby obtaining an anti-corrosion and anti-static metal pipe.

[0043] The technical solution of the present invention is further described below in conjunction with specific embodiments:

[0044] Example 1

[0045] In this embodiment, an anti-corrosion and anti-static metal pipe is provided, and the metal pipe includes a substrate layer 1, a primer layer 2 and an anti-corrosion and anti-static coating 3. The upper surface of the substrate layer 1 is sprayed with the primer layer 2, and the upper surface of the primer layer 2 is sprayed with the anti-corrosion and anti-static coating 3. The bonding surface between the anti-corrosion and anti-static coating 3 and the primer layer 2 is a flat surface, and the bonding surface between the primer layer 2 and the substrate layer 1 is a wavy curved surface.

[0046] The preparation method of the coating of the anti-corrosion and anti-static coating in this embodiment comprises the following specific steps:

[0047] S1. Prepare, by weight, 30 parts of fusible polytetrafluoroethylene, 15 parts of conductive filler (carbon fiber tube, carbon black, graphite = 1:3:5), 4 parts of preservative (isothiazolinone, quaternary ammonium salt, nitrite), 2 parts of organic bentonite and 70 parts of methyl ethyl ketone.

[0048] S2. The conductive filler was gradually added into 17 parts of methyl ethyl ketone solvent, and dispersed for 25 minutes using a high-speed disperser to obtain a uniformly dispersed conductive filler suspension.

[0049] S3. Add the preservative and the thixotropic agent to the conductive filler suspension in step S2 respectively, and continue to disperse using a high-speed disperser for 25 minutes to obtain a mixed suspension.

[0050] S4. Slowly add the fluororesin base material to the mixed suspension obtained in step S3, stir and mix evenly, then add the remaining 53 parts of methyl ethyl ketone solvent, continue stirring until completely mixed, and remove undispersed particles or impurities by filtering, thereby obtaining a coating for anti-corrosion and antistatic coating.

[0051] The method for preparing the anti-corrosion and anti-static metal pipe in this embodiment comprises the following steps:

[0052] (1) Clean the upper surface of the substrate layer inside the metal pipe and perform sandblasting pretreatment on the upper surface of the substrate layer.

[0053] (2) Evenly coating the epoxy primer on the upper surface of the substrate layer pretreated in step (1) to form a primer layer with a thickness of 30 μm.

[0054] (3) The anti-corrosion and anti-static coating prepared above was mixed evenly with a fluorine-containing epoxy resin curing agent at a mass ratio of 12:1, and the primer layer formed in step (2) was evenly sprayed using a high-pressure airless sprayer at a pressure of 200 bar. After the spraying was completed, the anti-corrosion and anti-static coating was cured at room temperature to form an anti-corrosion and anti-static coating with a thickness of 160 μm, thereby obtaining an anti-corrosion and anti-static metal pipe.

[0055] Example 2

[0056] In this embodiment, an anti-corrosion and anti-static metal pipe is provided, and the metal pipe includes a substrate layer 1, a primer layer 2 and an anti-corrosion and anti-static coating 3. The upper surface of the substrate layer 1 is sprayed with the primer layer 2, and the upper surface of the primer layer 2 is sprayed with the anti-corrosion and anti-static coating 3. The bonding surface between the anti-corrosion and anti-static coating 3 and the primer layer 2 is a flat surface, and the bonding surface between the primer layer 2 and the substrate layer 1 is a wavy curved surface.

[0057] The preparation method of the coating of the anti-corrosion and anti-static coating in this embodiment comprises the following specific steps:

[0058] S1. Prepare, by weight, 25 parts of fluorinated ethylene-propylene copolymer, 10 parts of conductive filler (carbon fiber tube, carbon black, graphite = 1:3:6), 3 parts of preservatives (isothiazolinone, nitrite and phosphate), 1 part of fumed silica and 60 parts of ethyl acetate.

[0059] S2. The conductive filler was gradually added into 20 parts of ethyl acetate solvent, and dispersed for 10 minutes using a high-speed disperser to obtain a uniformly dispersed conductive filler suspension.

[0060] S3. Add the preservative and the thixotropic agent to the conductive filler suspension in step S2 respectively, and continue to disperse using a high-speed disperser for 25 minutes to obtain a mixed suspension.

[0061] S4. Slowly add the fluororesin base material to the mixed suspension obtained in step S3, stir and mix evenly, then add the remaining 40 parts of ethyl acetate solvent, continue stirring until completely mixed, and remove undispersed particles or impurities by filtering, thereby obtaining a coating for anti-corrosion and antistatic coating.

[0062] The method for preparing the anti-corrosion and anti-static metal pipe in this embodiment comprises the following steps:

[0063] (1) Clean the upper surface of the substrate layer inside the metal pipe and perform sandblasting pretreatment on the upper surface of the substrate layer.

[0064] (2) A polyurethane primer is evenly coated on the upper surface of the substrate layer pretreated in step (1) to form a primer layer with a thickness of 25 μm.

[0065] (3) The anti-corrosion and anti-static coating prepared above is mixed evenly with a fluorine-containing epoxy resin curing agent at a mass ratio of 10:1, and a high-pressure airless sprayer is used to evenly spray the primer layer formed in step (2) at a pressure of 150 bar. After the spraying is completed, it is cured at room temperature to form an anti-corrosion and anti-static coating with a thickness of 150 μm, that is, an anti-corrosion and anti-static metal pipe is obtained.

[0066] Example 3

[0067] In this embodiment, an anti-corrosion and anti-static metal pipe is provided, and the metal pipe includes a substrate layer 1, a primer layer 2 and an anti-corrosion and anti-static coating 3. The upper surface of the substrate layer 1 is sprayed with the primer layer 2, and the upper surface of the primer layer 2 is sprayed with the anti-corrosion and anti-static coating 3. The bonding surface between the anti-corrosion and anti-static coating 3 and the primer layer 2 is a flat surface, and the bonding surface between the primer layer 2 and the substrate layer 1 is a wavy curved surface.

[0068] The preparation method of the coating of the anti-corrosion and anti-static coating in this embodiment comprises the following specific steps:

[0069] S1. Prepare, by weight, 28 parts of ethylene-tetrafluoroethylene copolymer, 12 parts of conductive filler (carbon fiber tube, carbon black, graphite = 1:4:5), 4 parts of preservative (quaternary ammonium salt, nitrite and phosphate), 2 parts of polyamide wax and 65 parts of isopropyl alcohol.

[0070] S2. The conductive filler was gradually added into 13 parts of isopropanol solvent and dispersed for 30 minutes using a high-speed disperser to obtain a uniformly dispersed conductive filler suspension.

[0071] S3. Add the preservative and the thixotropic agent to the conductive filler suspension in step S2 respectively, and continue to disperse using a high-speed disperser for 30 minutes to obtain a mixed suspension.

[0072] S4. Slowly add the fluororesin base material to the mixed suspension obtained in step S3, stir and mix evenly, then add the remaining 52 parts of ethyl acetate solvent, continue stirring until completely mixed, and remove undispersed particles or impurities by filtering, thereby obtaining a coating for anti-corrosion and antistatic coating.

[0073] The method for preparing the anti-corrosion and anti-static metal pipe in this embodiment comprises the following steps:

[0074] (1) Clean the upper surface of the substrate layer inside the metal pipe and perform sandblasting pretreatment on the upper surface of the substrate layer.

[0075] (2) The modified acrylic primer is evenly coated on the upper surface of the substrate layer pretreated in step (1) to form a primer layer with a thickness of 28 μm.

[0076] (3) The anti-corrosion and anti-static coating prepared above was mixed evenly with a fluorine-containing epoxy resin curing agent at a mass ratio of 15:1, and the primer layer formed in step (2) was evenly sprayed using a high-pressure airless sprayer at a pressure of 180 bar. After the spraying was completed, the anti-corrosion and anti-static coating was cured at room temperature to form an anti-corrosion and anti-static coating with a thickness of 200 μm, thereby obtaining an anti-corrosion and anti-static metal pipe.

[0077] Example 4

[0078] In this embodiment, an anti-corrosion and anti-static metal pipe is provided, and the metal pipe includes a substrate layer 1, a primer layer 2 and an anti-corrosion and anti-static coating 3. The upper surface of the substrate layer 1 is sprayed with the primer layer 2, and the upper surface of the primer layer 2 is sprayed with the anti-corrosion and anti-static coating 3. The bonding surface between the anti-corrosion and anti-static coating 3 and the primer layer 2 is a flat surface, and the bonding surface between the primer layer 2 and the substrate layer 1 is a wavy curved surface.

[0079] The preparation method of the coating of the anti-corrosion and anti-static coating in this embodiment comprises the following specific steps:

[0080] S1. Prepare, by weight, 30 parts of ethylene-tetrafluoroethylene copolymer, 12 parts of conductive filler (carbon fiber tube, carbon black, graphite = 1:4:6), 3 parts of preservative (isothiazolinone, quaternary ammonium salt, nitrite and phosphate), 2 parts of polyamide wax and 70 parts of isopropyl alcohol.

[0081] S2. The conductive filler was gradually added into 14 parts of isopropanol solvent, and dispersed for 25 minutes using a high-speed disperser to obtain a uniformly dispersed conductive filler suspension.

[0082] S3. Add the preservative and the thixotropic agent to the conductive filler suspension in step S2 respectively, and continue to disperse using a high-speed disperser for 30 minutes to obtain a mixed suspension.

[0083] S4. Slowly add the fluororesin base material to the mixed suspension obtained in step S3, stir and mix evenly, then add the remaining 56 parts of ethyl acetate solvent, continue stirring until completely mixed, and remove undispersed particles or impurities by filtering, thereby obtaining a coating for anti-corrosion and antistatic coating.

[0084] The method for preparing the anti-corrosion and anti-static metal pipe in this embodiment comprises the following steps:

[0085] (1) Clean the upper surface of the substrate layer inside the metal pipe and perform sandblasting pretreatment on the upper surface of the substrate layer.

[0086] (2) Evenly coating the zinc phosphate primer on the upper surface of the substrate layer pretreated in step (1) to form a primer layer with a thickness of 26 μm.

[0087] (3) The anti-corrosion and anti-static coating prepared above was mixed evenly with a fluorine-containing epoxy resin curing agent at a mass ratio of 10:1, and the primer layer formed in step (2) was evenly sprayed using a high-pressure airless sprayer at a pressure of 200 bar. After the spraying was completed, the anti-corrosion and anti-static coating was cured at room temperature to form an anti-corrosion and anti-static coating with a thickness of 180 μm, thereby obtaining an anti-corrosion and anti-static metal pipe.

[0088] Comparative Example 1

[0089] The difference between this comparative example and Example 1 is that only carbon black is used as the conductive filler, and the other components and preparation processes are exactly the same.

[0090] The preparation method of the coating of the anticorrosion and antistatic coating in this comparative example comprises the following specific steps:

[0091] S1. Prepare, by weight, 30 parts of fusible polytetrafluoroethylene, 15 parts of conductive filler (carbon black), 4 parts of preservative (isothiazolinone, quaternary ammonium salt, nitrite), 2 parts of organic bentonite and 70 parts of methyl ethyl ketone.

[0092] S2. The conductive filler was gradually added into 17 parts of methyl ethyl ketone solvent, and dispersed for 25 minutes using a high-speed disperser to obtain a uniformly dispersed conductive filler suspension.

[0093] S3. Add the preservative and the thixotropic agent to the conductive filler suspension in step S2 respectively, and continue to disperse using a high-speed disperser for 25 minutes to obtain a mixed suspension.

[0094] S4. Slowly add the fluororesin base material to the mixed suspension obtained in step S3, stir and mix evenly, then add the remaining 53 parts of methyl ethyl ketone solvent, continue stirring until completely mixed, and remove undispersed particles or impurities by filtering, thereby obtaining a coating for anti-corrosion and antistatic coating.

[0095] The preparation method of the anti-corrosion and anti-static metal pipe in this comparative example comprises the following steps:

[0096] (1) Clean the upper surface of the substrate layer inside the metal pipe and perform sandblasting pretreatment on the upper surface of the substrate layer.

[0097] (2) Evenly coating the epoxy primer on the upper surface of the substrate layer pretreated in step (1) to form a primer layer with a thickness of 30 μm.

[0098] (3) The anti-corrosion and anti-static coating prepared above was mixed evenly with a fluorine-containing epoxy resin curing agent at a mass ratio of 12:1, and the primer layer formed in step (2) was evenly sprayed using a high-pressure airless sprayer at a pressure of 200 bar. After the spraying was completed, the anti-corrosion and anti-static coating was cured at room temperature to form an anti-corrosion and anti-static coating with a thickness of 160 μm, thereby obtaining an anti-corrosion and anti-static metal pipe.

[0099] Comparative Example 2

[0100] The difference between this comparative example and Example 1 is that the preservative uses a quaternary ammonium salt, and the other components and preparation processes are exactly the same.

[0101] The preparation method of the coating of the anticorrosion and antistatic coating in this comparative example comprises the following specific steps:

[0102] S1. Prepare, by weight, 30 parts of fusible polytetrafluoroethylene, 15 parts of conductive filler (carbon black), 4 parts of preservative (quaternary ammonium salt), 2 parts of organic bentonite and 70 parts of methyl ethyl ketone.

[0103] S2. The conductive filler was gradually added into 17 parts of methyl ethyl ketone solvent, and dispersed for 25 minutes using a high-speed disperser to obtain a uniformly dispersed conductive filler suspension.

[0104] S3. Add the preservative and the thixotropic agent to the conductive filler suspension in step S2 respectively, and continue to disperse using a high-speed disperser for 25 minutes to obtain a mixed suspension.

[0105] S4. Slowly add the fluororesin base material to the mixed suspension obtained in step S3, stir and mix evenly, then add the remaining 53 parts of methyl ethyl ketone solvent, continue stirring until completely mixed, and remove undispersed particles or impurities by filtering, thereby obtaining a coating for anti-corrosion and antistatic coating.

[0106] The preparation method of the anti-corrosion and anti-static metal pipe in this comparative example comprises the following steps:

[0107] (1) Clean the upper surface of the substrate layer inside the metal pipe and perform sandblasting pretreatment on the upper surface of the substrate layer.

[0108] (2) Evenly coating the epoxy primer on the upper surface of the substrate layer pretreated in step (1) to form a primer layer with a thickness of 30 μm.

[0109] (3) The anti-corrosion and anti-static coating prepared above was mixed evenly with a fluorine-containing epoxy resin curing agent at a mass ratio of 12:1, and the primer layer formed in step (2) was evenly sprayed using a high-pressure airless sprayer at a pressure of 200 bar. After the spraying was completed, the anti-corrosion and anti-static coating was cured at room temperature to form an anti-corrosion and anti-static coating with a thickness of 160 μm, thereby obtaining an anti-corrosion and anti-static metal pipe.

[0110] Detection:

[0111] (1) Antistatic property: The antistatic property of Examples 1 to 4 and Comparative Examples 1 and 2 was tested using a surface resistance tester. The sample size was 10 cm long and 5 cm wide. The unit is MΩ·cm.

[0112] (2) Acid and alkali corrosion resistance: The metal pipes prepared in Examples 1-4 and Comparative Examples 1-2 were tested for their resistance to acid and alkali corrosion. The metal pipe samples were immersed in a strong acid corrosive liquid of sulfuric acid and a strong alkaline corrosive liquid of sodium hydroxide, with the pH of the strong acid corrosive liquid being about 3 and the pH of the strong alkaline corrosive liquid being about 12. The samples were kept for 48 hours respectively, and the condition of the inner wall of the pipe was observed.

[0113] Table 1 Performance test results of Examples 1-4 and Comparative Examples 1-2

[0114]

[0115]

[0116] It can be seen from Table 1 above that the metal pipes prepared in Examples 1-4 of the present invention have excellent antistatic properties compared to the metal pipes prepared in Comparative Document 1, and can conduct static electricity in time, playing a good antistatic role. Although Comparative Document 1 uses carbon black as a conductive filler, it can also conduct static electricity, but its antistatic effect is not as good as that of the sample in the embodiment of the present invention. This is because the conductive base materials used in the present invention are carbon fiber tubes, carbon black and graphite. Through the synergistic effect between them, an effective conductive network can be formed inside the material, thereby achieving the antistatic performance of the inner wall of the pipeline, preventing charge accumulation and static discharge, and ensuring that crude oil is in the metal pipeline. At the same time, after the metal pipes prepared in Examples 1-4 of the present invention were immersed in strong acidic corrosive liquids and strong alkaline corrosive liquids for 48 hours, the inner wall surface of the pipes was intact, while the inner wall surface of the pipes in Comparative Document 2 fell off. This is because the anti-corrosion added by the present invention can form a multi-faceted anti-corrosion protection system. Isothiazolinone and quaternary ammonium salts can inhibit microbial activity and prevent microbial-induced corrosion, while nitrites and phosphates mainly prevent chemical and electrochemical corrosion by forming a protective film and electrochemical action. Such a comprehensive anti-corrosion strategy can more effectively extend the service life of metal pipes.

[0117] The above is a detailed introduction to an anti-corrosion and anti-static metal pipe and a preparation method thereof disclosed in the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. An anti-corrosion and anti-static metal pipe, characterized in that: The metal pipe includes a substrate layer, a primer layer and an anti-corrosion and anti-static coating. The upper surface of the substrate layer is sprayed with the primer layer, and the upper surface of the primer layer is sprayed with the anti-corrosion and anti-static coating. The bonding surface between the anti-corrosion and anti-static coating and the primer layer is a flat surface, and the bonding surface between the primer layer and the substrate layer is a wavy curved surface.

2. The anti-corrosion and anti-static metal pipe according to claim 1, characterized in that: The coating of the anticorrosive and antistatic coating is made of the following components in parts by weight: 25-30 parts of fluororesin base material, 10-15 parts of conductive filler, 2-4 parts of preservative, 1-2 parts of thixotropic agent and 60-70 parts of solvent.

3. The anti-corrosion and anti-static metal pipe according to claim 2 is characterized in that: The fluororesin base material is one of fusible polytetrafluoroethylene, fluorinated ethylene-propylene copolymer, ethylene-tetrafluoroethylene copolymer or a combination thereof; the conductive filler is carbon fiber tube, carbon black, graphite in a mass ratio of 1: (3-4): (5-6) composition; the preservative is 3 or 4 of isothiazolinone, quaternary ammonium salt, nitrite and phosphate; the thixotropic agent is one of polyamide wax, organic bentonite and fumed silica; the solvent is one of methyl ethyl ketone, ethyl acetate and isopropyl alcohol.

4. The anti-corrosion and anti-static metal pipe according to claim 3 is characterized in that: The preparation method of the coating of the anti-corrosion and anti-static coating comprises the following specific steps: S1. Prepare raw materials: prepare fluororesin base material, conductive filler, preservative, thixotropic agent and solvent by weight; S2. The conductive filler is gradually added to the first part of the solvent, and dispersed using a high-speed disperser for 10 to 30 minutes to obtain a uniformly dispersed conductive filler suspension; S3. The preservative and the thixotropic agent are added to the conductive filler suspension in step S2, and the mixture is dispersed for 10 to 30 minutes using a high-speed disperser to obtain a mixed suspension; S4. Slowly add the fluororesin base material to the mixed suspension obtained in step S3, stir and mix evenly, then add the remaining second part of the solvent, continue stirring until completely mixed, and remove undispersed particles or impurities by filtering, thereby obtaining a coating for the anti-corrosion and antistatic coating.

5. The anti-corrosion and anti-static metal pipe according to claim 4, characterized in that: The mass ratio of the first part of the solvent in step S2 to the second part of the solvent in step S4 is 1:(2-4).

6. The method for preparing the anti-corrosion and anti-static metal pipe according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) Cleaning the upper surface of the substrate layer in the metal pipe and performing sandblasting pretreatment on the upper surface of the substrate layer; (2) uniformly coating a primer on the upper surface of the substrate layer pretreated in step (1) to form a primer layer; (3) The anti-corrosion and anti-static coating is mixed evenly with the fluorine-containing epoxy resin curing agent, and sprayed evenly on the primer layer formed in step (2) using a high-pressure airless sprayer. After the spraying is completed, the anti-corrosion and anti-static coating is cured at room temperature to form an anti-corrosion and anti-static metal pipe.

7. The method for preparing the anti-corrosion and anti-static metal pipe according to claim 6, characterized in that: The primer in step (2) is one of epoxy primer, polyurethane primer, modified acrylic primer, zinc phosphate primer or a combination thereof.

8. The method for preparing the anti-corrosion and anti-static metal pipe according to claim 7, characterized in that: The thickness of the primer layer in step (2) is 25 to 30 μm.

9. The method for preparing the anti-corrosion and anti-static metal pipe according to claim 6, characterized in that: In step (3), the pressure of the high-pressure airless sprayer is 150 to 200 bar.

10. The method for preparing the anti-corrosion and anti-static metal pipe according to claim 9, characterized in that: In the step (3), the mass ratio of the anti-corrosion and anti-static coating to the fluorine-containing epoxy resin curing agent is (10-15):1, and the thickness of the anti-corrosion and anti-static coating is 150-200 μm.