Method for manufacturing low capacitance transient voltage suppression diode in wafer level flip package
Through wafer-level reverse packaging technology and multiple photolithography processes, low-capacitance PIN or NIP structure diodes are formed, solving the problems of large volume and large capacitance after the existing transient voltage suppression diodes are packaged, and it is suitable for high-speed interface circuits thin, low-capacitance products.
Patent Information
- Application Number
- CN202111478196.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-12-06
AI Technical Summary
The existing transient voltage suppression diodes have problems such as large volume, thick thickness, large capacitance and inability to be used in high-speed interface circuits after packaging.
Using wafer-level inverted packaging technology, by growing an N-type epitaxial layer on a P-type substrate, performing multiple photolithography and phosphorus diffusion, forming a low-capacitance PIN or NIP structure diode, combining Ti-W and AL metallization and electroless nickel-plated gold pads to achieve thin products without additional packaging.
It realizes low capacitance, thin, and low leakage current diode products, suitable for low voltage equipment and high-speed data transmission, suitable for high-speed interface circuits, and has an adjustable package thickness.
Smart Images

Figure CN114203695B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electronics, relates to diodes, and specifically relates to a method for manufacturing a wafer-level flip-flop package low-capacitance transient voltage suppression diode. Background Art
[0002] Transient Voltage Suppressor (TVS) is a high-efficiency protection device in the form of a diode. When the two poles of a TVS diode are subjected to a reverse transient high-energy impact, it can change the high impedance between the two poles to a low impedance at a speed of 10 to the negative 12th power of seconds, absorbing up to several kilowatts of surge power, and making the voltage box between the two poles at a predetermined value, effectively protecting the precision components in the electronic circuit from damage by various surge pulses. However, existing transient voltage suppression diodes have the following defects;
[0003] (1) Ordinary TVS diode chips need to be packaged into finished products after production;
[0004] (2) Ordinary TVS diodes are large in size after packaging;
[0005] (3) Ordinary TVS diodes are thick after packaging;
[0006] (4) Ordinary transient diodes have large capacitance;
[0007] (5) Ordinary transient diodes cannot be used in high-speed interface circuits. Summary of the invention
[0008] In view of the above problems existing in the prior art, the purpose of the present invention is to provide a method for manufacturing a wafer-level flip-chip packaged low-capacitance transient voltage suppression diode with low capacitance, small packaging volume, thin product thickness, and no need for further packaging after product production.
[0009] In order to achieve the above object, the present invention adopts the following technical solution: a method for manufacturing a wafer-level flip-flop package low-capacitance transient voltage suppression diode, comprising the following steps:
[0010] a. Select a P-type substrate with a resistivity of 0.001-0.04Ω•cm and clean the substrate silicon wafer once;
[0011] b. Perform epitaxial growth on the substrate silicon wafer obtained in step a. After loading, heat it to 950±10℃, with H2 gas flow rate of 100L / min, heat it to 1800±5℃ for the second time, with H2 gas flow rate of 100L / min, pass HCl for 0.5-1 minute, etch for 2-3 minutes, with HCl gas flow rate of 1L / min, blow H2 for 2-5 minutes, keep the temperature at 1050±5℃, pass SiCl4 for 0.5-2 minutes, and grow an N-type epitaxial wafer with an epitaxial thickness of 3-4um and a resistivity of 0.001-0.4Ω•cm;
[0012] c. Cleaning the substrate silicon wafer after completing step b;
[0013] d. Perform an initial oxidation process on the substrate silicon wafer that has completed step c. First, put the silicon wafer into a quartz boat, and then put the boat into the quartz furnace tube. After the boat is put into the boat, cover the ground mouth, and introduce nitrogen at 750±3°C, and keep the temperature at 950±3°C. Stop nitrogen and replace it with oxygen. After the oxygen is introduced for 20±1 minutes, change to oxygen and hydrogen for hydrogen-oxygen synthesis. The hydrogen-oxygen synthesis time is 240±1 minute. After the hydrogen-oxygen synthesis is completed, oxygen is introduced again, and then trichloroethane is introduced, and then dry oxygen is introduced. The temperature is reduced from 950°C to 750°C, the ground mouth is removed, the boat is taken out, and the wafer is taken out of the quartz boat. The process is completed;
[0014] e. Performing a photolithography on the substrate silicon wafer with the oxide layer after completing step d, the steps are as follows:
[0015] ① Glue coating: The viscosity of the photoresist is 100±1SC, and the coating thickness is 20000±2000Å;
[0016] ② Pre-baking: Dry the coated substrate silicon wafer in an oven at 85±5℃ for 30±1 minutes;
[0017] ③ Alignment: Set the mask on the substrate silicon wafer, and expose the substrate silicon wafer with the mask set under the mercury lamp of the photolithography machine for 22±1 seconds to image the mask pattern onto the surface of the substrate silicon wafer;
[0018] ④ Development and fixing: first develop with xylene for 10±1 seconds, then fix with butyl acetate for 8±1 seconds;
[0019] ⑤ Hard film: Dry the fixed substrate silicon wafer in an oven at 140-155℃ for 30±1 minutes;
[0020] ⑥ Oxide layer corrosion: Corrode the hardened substrate silicon wafer with a corrosion solution of H 2 O: NH 4 F = 6: 1 for 10 ± 1 minutes;
[0021] ⑦ Removal of photoresist: Soak the substrate silicon wafer after the oxide layer is etched in H 2 SO 4 :H 2 O 2 =3:1 soaking solution for 10±1 minutes to remove the photoresist;
[0022] f. Performing N+ implantation on the substrate having one photolithography after completing step e, with an implantation dose of 1E15-5E15 and an implantation energy of 50-80Kev;
[0023] g. Perform buried layer diffusion on the substrate with N+ implantation and one-time photolithography completed in step f. First, put the silicon wafer into the quartz boat, then put the boat into the quartz furnace tube. After the boat is put into the boat, cover the ground mouth, and introduce nitrogen at 750±3℃, 6±1 liters per minute, for 30±1 minutes. The temperature is raised from 750℃ to 1150℃, and the temperature is maintained at 1150±3℃. The diffusion time is 60±1 minutes. The temperature is reduced from 1150℃ to 750℃, the ground mouth is removed, the boat is taken out, and the wafer is taken out of the quartz boat;
[0024] h. Perform secondary epitaxial growth on the substrate silicon wafer after completing step g, the steps are the same as step b, and grow an N-type epitaxial wafer with an epitaxial thickness of 3 to 5 um and a resistivity of 0.1 to 0.4 Ω•cm;
[0025] i. Performing an oxidation process on the substrate silicon wafer after completing step h, the steps are the same as step d;
[0026] j. Performing secondary photolithography on the substrate silicon wafer with the oxide layer after completing step i, the steps are the same as step e;
[0027] k. Perform phosphorus diffusion on the substrate that has completed the secondary photolithography in step j. First, place the silicon wafer in a quartz boat, and then enter the boat into the quartz furnace tube at a speed of 20±1 cm / s. After entering the boat, cover the ground mouth, and introduce nitrogen at 750±3°C at a rate of 6±1 liters per minute for 30±1 minutes. The temperature is raised from 750°C to 1100°C and maintained at 1100±3°C. Stop nitrogen and replace with oxygen. After oxygen is introduced for 5±1 minutes, replace with oxygen and phosphorus for phosphorus pre-diffusion. The phosphorus pre-diffusion time is 30±1 minutes, wherein the oxygen introduction rate is 3.5±1 L / min, the phosphorus introduction rate is 6.5±1 L / min, hydrogen and oxygen synthesis is performed for 20±1 minutes, wherein the oxygen introduction rate is 3.5±1 L / min, and then trichloroethane is introduced for 10±1 minutes, wherein the trichloroethane is 80±1 mL / min, then pass dry oxygen for 10±1 minutes, the temperature drops from 1100℃ to 750℃, remove the ground mouth, take out the boat, the boat speed is 20±1cm / s, take the slice out of the quartz boat, and the process is finished;
[0028] l, the completion of step k of the substrate silicon wafer having an oxide layer is subjected to three photolithography steps, the steps are the same as step e;
[0029] m, the three-times photolithography wafer completed in step l is p+ implanted, the implantation dose is 3 to 5E15, and the implantation energy is 50 to 80Kev;
[0030] n. After completing the p+ implantation in step m, perform photoresist removal. Soak the substrate silicon wafer after the oxide layer is etched in a H 2 SO 4 :H 2O 2 =3:1 soaking solution for 10±1 minutes to remove the photoresist;
[0031] o, to complete step n to remove the glue Chen film four times lithography, the steps are the same as step e;
[0032] p. Perform n+ implantation on the wafers that have completed four photolithography steps, with an implantation dose of 1 to 5E15 and an implantation energy of 50 to 80Kev;
[0033] q, the phosphorus diffusion is performed on the implanted sheet after completing step p, the phosphorus diffusion time is 60 ± 1 minutes, and then the dry oxygen temperature is reduced from 1050 ℃ to 750 ℃, and the remaining steps are the same as step k;
[0034] r, the phosphorus diffusion wafer is completed in step q for five photolithography steps, the same steps as step e;
[0035] s. Etch the isolation groove on the five-time photolithography wafer that has completed step r. Etch with N 2 for 5-10 minutes. Load the strip into the etcher, pass CF 4 gas at a flow rate of 100-500 mL / min, add 10-40% oxygen, ventilate for 2-3 minutes, and the etching time is 120-300 minutes;
[0036] t. Filling the isolation trench wafer after step s with glass powder;
[0037] u. Sinter the glass powder filled in step t at a sintering temperature of 470°C ± 10°C for 10 minutes. Adjust the nitrogen pressure control gauge pointer on the furnace control panel to 10-15mL / min and the hydrogen pressure control gauge pointer to 7mL / min. After sintering, take out the wafer.
[0038] v. Perform six photolithography steps on the glass powder sintered crystal circle obtained in step u, the steps of which are the same as those in step e;
[0039] w. Metallize the front side of the substrate silicon wafer after completing step v, and perform Ti-W metal sputtering and evaporation of AL metal on the substrate silicon wafer in sequence;
[0040] x. Perform seven photolithography steps on the substrate silicon wafer after completing step w. Except that the viscosity of the photoresist is 150±1SC, the remaining steps are the same as step e;
[0041] y. Performing front metal corrosion, front metal degumming and front metal alloying on the substrate silicon wafer that has completed step x;
[0042] z. Conduct electrical testing, passivation, photolithography, passivation corrosion, backside thinning, and backside stress relief corrosion on the substrate silicon wafer with the front side metal alloy completed;
[0043] aa. Thinning the back side of the substrate silicon wafer after back side stress relief etching by 150±5um to 300±5um and performing back side stress relief etching;
[0044] bb, perform back labeling photolithography and etching on the substrate silicon wafer that has completed step aa, clean it and spin dry it;
[0045] cc. Perform Ni and Au chemical plating on the front pad of the substrate silicon wafer that has completed step bb.
[0046] Preferably, in step d, the speed of the boat entering and exiting the boat is 20±1 cm / s.
[0047] Preferably, in step d, during hydrogen-oxygen synthesis, the oxygen introduction rate is 3.5±1 L / min, and the hydrogen introduction rate is 6.5±1 L / min.
[0048] Preferably, in step d, the duration of oxygen introduced after the completion of hydrogen-oxygen synthesis is 20±1 min, and the oxygen introduction rate is 3.5±1 L / min.
[0049] Preferably, in step d, the duration of the trichloroethane introduced is 10±1 min, and the rate of introduction of trichloroethane is 80±1 mL / min.
[0050] Preferably, the etching in step bb is that the substrate silicon wafer is etched with a chemical etching solution of HNO 3 :HF:CH 3 COOH:H 2 O = 5:1:3:20 at 12-18° C. for 10±1 min.
[0051] Preferably, in step cc, the front pad metal chemical plating of Ni and Au is performed on the substrate silicon wafer, and the steps are:
[0052] S1. One-time nickel plating: PH value 8.5-9.0, immersed in 95±3℃ nickel plating solution, nickel plating 90±6s;
[0053] S2. Nickel sintering: sinter at 575℃ for 35±1min, then cool to 500℃ at a rate of 1.5℃ / min, with a nitrogen flow rate of 2±0.5LPM during cooling;
[0054] S3. Nitric acid treatment: Boil the silicon wafer in 1:1 nitric acid at 95±5℃ for 4±1min;
[0055] S4. Secondary nickel plating: immerse in 100±3℃ nickel plating solution;
[0056] S5. Gold plating: Gold plating for 20-25 seconds, check and confirm that the temperature of the gold plating solution is 110±5℃.
[0057] Compared with the prior art, the present invention has the following beneficial effects:
[0058] 1. The present invention first grows a first epitaxial layer n++ region on a p substrate, then performs a buried layer process to make an N+ region, and then performs a second epitaxial process to make an N- region. The second epitaxial type is different from the first epitaxial type, and is a layer of high resistivity N-type epitaxial layer; after this process, the TVS tube and the low capacitance diodes D1 and D2 are adjusted; wherein the n++ isolation region can be used as the n-type region of the TVS diode, and is connected to the highly doped P++ substrate, and an N+ region is formed on the surface of the P-type region, thereby forming an avalanche diode with a low breakdown voltage, and the adjustment of its concentration can adjust the reverse breakdown voltage value of the TVS diode.
[0059] 2. The present invention forms highly doped P+ and N+ regions on the N-epitaxial structure, and forms a PIN low capacitance diode D2 with P+ / N- / N++, and forms a NIP low capacitance diode D1 with N+ / N- / P++.
[0060] 3. The present invention introduces the positive and negative electrodes to the front side of the chip through phosphorus diffusion, and the product thickness is adjusted according to the back thinning thickness (100-400) ±5um range; the front side is metallized, and the substrate silicon wafer is sequentially subjected to Ti-W metal sputtering and AL metal evaporation; the completed substrate silicon wafer is subjected to chemical plating of Ni and Au on the front pad metal, and the chemically plated Ni and Au are used as the pad metal to weld the wafer on the circuit board after dicing. The product does not require further packaging process.
[0061] 4. The product of the present invention has the following outstanding characteristics:
[0062] (1) Low voltage: Application in portable devices (PAD, ultra-thin notebook computers) that operate at low voltage.
[0063] (2) Low capacitance: high-speed data transmission; such as T1 / E1, Ethernet, USB and video.
[0064] (3) Low leakage current: for portable low power devices.
[0065] (4) Fast operation speed: Applied to high-speed interface circuits.
[0066] (5) The same type of wafer-level packaging: the packaging thickness is adjustable. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1 .Top view of low capacitance wafer-level TVS product;
[0068] Figure 2 . This is a low capacitance design structure diagram of the TVS product of the present invention;
[0069] Figure 3 . Flow chart (1)-(12) of the TVS product of the present invention;
[0070] Figure 4 . is the TVS product flow chart (13)-(18) of the present invention. DETAILED DESCRIPTION
[0071] The present invention will be further explained and illustrated below in conjunction with the accompanying drawings and specific embodiments;
[0072] A method for manufacturing a wafer-level flip-chip package low-capacitance transient voltage suppression diode comprises the following steps:
[0073] a. Use P-type substrate with resistivity of 0.001-0.04Ω•cm to clean the substrate epitaxial silicon wafer once;
[0074] b. Perform epitaxial growth on the substrate silicon wafer after step a. After loading, heat it to 950±10℃ for 8-15 minutes with H2 gas flow rate of 100L / min. Heat it to 1800±5℃ for 5-8 minutes with H2 gas flow rate of 100L / min. Pass HCl for 0.5-1 minute. Etch with HCl for 2-3 minutes with HCl gas flow rate of 1L / min. Blow H2 gas for 2-5 minutes. Keep the temperature at 1050±5℃ and pass SiCl4 for 0.5-2 minutes to grow N-type epitaxial wafers with epitaxial thickness of 3-4um and resistivity of 0.001-0.4Ω•cm.
[0075] c. Complete step b to clean the substrate epitaxial wafer once;
[0076] d. Perform an initial oxidation process on the substrate silicon wafer that has completed step c. First, place the silicon wafer in a quartz boat, then enter the boat into the quartz furnace tube at a boat speed of 20±1 cm / s. After entering the boat, cover the ground mouth, and introduce nitrogen at 750±3°C at 6±1 L / min for 30±1 min. The temperature is raised from 750°C to 950°C and maintained at 950±3°C. Stop nitrogen and replace with oxygen. Oxygen is introduced for 20±1 min. Then, oxygen and hydrogen are used for hydrogen-oxygen synthesis. The hydrogen-oxygen synthesis time is 240±1 min, wherein the oxygen introduction rate is 3.5±1 L / min and the hydrogen introduction rate is 6.5±1 L / min. After the hydrogen-oxygen synthesis is completed, oxygen is introduced for 20±1 min, wherein the oxygen introduction rate is 3.5±1 L / min and the hydrogen introduction rate is 6.5±1 L / min. After the hydrogen-oxygen synthesis is completed, oxygen is introduced again for 20±1 min, wherein the oxygen introduction rate is 3.5±1 L / min, then pass trichloroethane for 10±1min, where trichloroethane is 80±1mL / min, then pass dry oxygen for 120±1min, the temperature drops from 950℃ to 750℃, remove the ground mouth, take out the boat, the boat speed is 20±1cm / s, take the slice on the quartz boat, and the process is finished;
[0077] e. Performing a photolithography on the substrate silicon wafer with the oxide layer after completing step d, the steps are as follows:
[0078] ① Glue coating: The viscosity of the photoresist is 100±1SC, and the coating thickness is 20000±2000Å;
[0079] ② Pre-baking: Dry the coated substrate silicon wafer in an oven at 85±5℃ for 30±1 minutes;
[0080] ③ Alignment: Set the mask on the substrate silicon wafer, and expose the substrate silicon wafer with the mask set under the mercury lamp of the photolithography machine for 22±1 seconds to image the mask pattern onto the surface of the substrate silicon wafer;
[0081] ④ Development and fixing: first develop with xylene for 10±1 seconds, then fix with butyl acetate for 8±1 seconds;
[0082] ⑤ Hard film: Dry the fixed substrate silicon wafer in an oven at 140-155℃ for 30±1 minutes;
[0083] ⑥ Oxide layer corrosion: Corrode the hardened substrate silicon wafer with a corrosion solution of H 2 O: NH 4 F = 6: 1 for 10 ± 1 min;
[0084] ⑦ Removal of photoresist: Soak the substrate silicon wafer after the oxide layer is etched in H 2 SO 4 :H 2 O 2 =3:1 soaking solution for 10±1min to remove the photoresist;
[0085] f. Performing N+ implantation on the substrate having one photolithography after completing step e, with an implantation dose of 1E15-5E15 and an implantation energy of 50-80Kev;
[0086] g. Perform buried layer diffusion on the N+ implanted layer after step f, the steps are as follows:
[0087] For the substrate piece of the first photolithography, first put the silicon wafer into the quartz boat, then put the boat into the quartz furnace tube, the boat speed is 20±1cm / s, after the boat is put into the boat, cover the ground mouth, introduce nitrogen at 750±3℃, 6±1 L / min, 30±1 min, the temperature is raised from 750℃ to 1150℃, the temperature is maintained at 1150±3℃, the diffusion time is 60±1 min, the temperature is reduced from 1150℃ to 750℃, remove the ground mouth, take out the boat at a speed of 20±1cm / s, take the wafer on the quartz boat, and the process is completed;
[0088] h. Secondary epitaxial growth: perform secondary epitaxial growth on the substrate silicon wafer that has completed step g. After loading, heat it to 950±10°C for 8-15 min, with a H 2 gas flow rate of 100L / min. Heat it again to 1800±5°C for 5-8 min, with a H 2 gas flow rate of 100L / min. Pass HCl for 0.5-1 min, HCl corrosion for 2-3 min, HCl gas flow rate of 1L / min, blow H 2 for 2-5 min, keep the temperature constant at 1050±5°C, pass SiCl 4 for 0.5-2min, and grow an N-type epitaxial wafer with an epitaxial thickness of 3-5um and a resistivity of 0.1-0.4Ω•cm.
[0089] i. Oxidation: The substrate silicon wafer that has completed step h is subjected to an oxidation process. First, the silicon wafer is placed in a quartz boat, and then the boat is fed into the quartz furnace tube at a boat speed of 20±1 cm / s. After the boat is fed, the ground mouth is covered and nitrogen is introduced at 750±3°C at 6±1 L / min for 30±1 minutes. The temperature is raised from 750°C to 950°C and maintained at 950±3°C. Nitrogen is stopped and replaced with oxygen. After oxygen is introduced for 20±1 minutes, oxygen and hydrogen are used for hydrogen-oxygen synthesis. The hydrogen-oxygen synthesis time is 240±1 minutes, wherein the oxygen introduction rate is 3.5±1 L / min and the hydrogen introduction rate is 6.5±1 L / min. After the hydrogen-oxygen synthesis is completed, oxygen is introduced for 20±1 minutes, wherein the oxygen introduction rate is 3.5±1 L / min, and then trichloroethane is introduced for 10±1 min, where trichloroethane is 80±1mL / min, then dry oxygen is passed for 120±1min, the temperature is reduced from 950℃ to 750℃, the ground mouth is removed, the boat is taken out, the boat speed is 20±1cm / s, the slice is taken out of the quartz boat, and the process is completed;
[0090] j. Secondary photolithography: Perform secondary photolithography on the substrate silicon wafer with the oxide layer after completing step i, and the steps are as follows:
[0091] ① Glue coating: The viscosity of the photoresist is 100±1SC, and the coating thickness is 20000±2000Å;
[0092] ② Pre-baking: Dry the coated substrate silicon wafer in an oven at 85±5℃ for 30±1 minutes;
[0093] ③ Alignment: Set the mask on the substrate silicon wafer, and expose the substrate silicon wafer with the mask set under the mercury lamp of the photolithography machine for 22±1 seconds to image the mask pattern onto the surface of the substrate silicon wafer;
[0094] ④ Development and fixing: first develop with xylene for 10±1 seconds, then fix with butyl acetate for 8±1 seconds;
[0095] ⑤ Hard film: Dry the fixed substrate silicon wafer in an oven at 140-155℃ for 30±1 minutes;
[0096] ⑥ Oxide layer corrosion: Corrode the hardened substrate silicon wafer with a corrosion solution of H2O: NH4F = 6: 1 for 10 ± 1 minutes;
[0097] ⑦ Removal of photoresist: Soak the substrate silicon wafer after the oxide layer is corroded in H2SO4:H2O2=3:1 soaking solution for 10±1 minutes to remove the photoresist;
[0098] k. Pre-diffusion of phosphorus: Phosphorus diffusion is performed on the substrate that has completed the secondary photolithography in step j. First, the silicon wafer is placed in a quartz boat, and then the boat is placed in the quartz furnace tube at a speed of 20±1cm / s. After the boat is placed, the ground mouth is covered and nitrogen is introduced at 750±3℃ at a rate of 6±1 liters per minute for 30±1 minutes. The temperature is raised from 750℃ to 1100℃ and maintained at 1100±3℃. The nitrogen is stopped and replaced with oxygen. After 5±1 minutes of oxygen introduction, oxygen and phosphorus are replaced for pre-diffusion of phosphorus. During the pre-diffusion of phosphorus The reaction time is 30±1 minutes, wherein the oxygen introduction rate is 3.5±1 liters per minute, the phosphorus introduction rate is 6.5±1 liters per minute, the hydrogen and oxygen synthesis is 20±1 minutes, wherein the oxygen introduction rate is 3.5±1 liters per minute, and then trichloroethane is introduced for 10±1 minutes, wherein trichloroethane is 80±1 milliliters per minute, and then dry oxygen is introduced for 10±1 minutes, the temperature is reduced from 1100°C to 750°C, the ground mouth is removed, the boat is taken out, the boat speed is 20±1cm / s, the slice is taken out of the quartz boat, and the process is completed.
[0099] 1. Perform photolithography three times on the substrate silicon wafer with the oxide layer after completing step k, the steps are as follows:
[0100] ① Glue coating: The viscosity of the photoresist is 100±1SC, and the coating thickness is 20000±2000Å;
[0101] ② Pre-baking: Dry the coated substrate silicon wafer in an oven at 85±5℃ for 30±1 minutes;
[0102] ③ Alignment: Set the mask on the substrate silicon wafer, and expose the substrate silicon wafer with the mask set under the mercury lamp of the photolithography machine for 22±1 seconds to image the mask pattern onto the surface of the substrate silicon wafer;
[0103] ④ Development and fixing: first develop with xylene for 10±1 seconds, then fix with butyl acetate for 8±1 seconds;
[0104] ⑤ Hard film: Dry the fixed substrate silicon wafer in an oven at 140-155℃ for 30±1 minutes;
[0105] ⑥ Oxide layer corrosion: Corrode the hardened substrate silicon wafer with a corrosion solution of H2O: NH4F = 6: 1 for 10 ± 1 minutes;
[0106] ⑦ Removal of photoresist: Soak the substrate silicon wafer after the oxide layer is corroded in H2SO4:H2O2=3:1 soaking solution for 10±1 minutes to remove the photoresist;
[0107] m, the three-times photolithography wafer completed in step l is p+ implanted, the implantation dose is 3 to 5E15, and the implantation energy is 50 to 80Kev;
[0108] n. Remove the p+ implantation after step m, and soak the substrate silicon wafer after the oxide layer is etched in a H2SO4:H2O2=3:1 soaking solution for 10±1 minutes to remove the photoresist;
[0109] o. Perform four photolithography steps on the debonded old film after step n, the steps are as follows:
[0110] ① Glue coating: The viscosity of the photoresist is 100±1SC, and the coating thickness is 20000±2000Å;
[0111] ② Pre-baking: Dry the coated substrate silicon wafer in an oven at 85±5℃ for 30±1 minutes;
[0112] ③ Alignment: Set the mask on the substrate silicon wafer, and expose the substrate silicon wafer with the mask set under the mercury lamp of the photolithography machine for 22±1 seconds to image the mask pattern onto the surface of the substrate silicon wafer;
[0113] ④ Development and fixing: first develop with xylene for 10±1 seconds, then fix with butyl acetate for 8±1 seconds;
[0114] ⑤ Hard film: Dry the fixed substrate silicon wafer in an oven at 140-155℃ for 30±1 minutes;
[0115] ⑥ Oxide layer corrosion: Corrode the hardened substrate silicon wafer with a corrosion solution of H2O: NH4F = 6: 1 for 10 ± 1 minutes;
[0116] ⑦ Removal of photoresist: Soak the substrate silicon wafer after the oxide layer is corroded in H2SO4:H2O2=3:1 soaking solution for 10±1 minutes to remove the photoresist;
[0117] p, the four-times photolithography wafer completed in step l is subjected to n+ implantation, the implantation dose is 1 to 5E15, and the implantation energy is 50 to 80Kev;
[0118] q. Re-diffusion of phosphorus: Phosphorus diffusion is performed on the implanted wafers that have completed step p. First, the silicon wafer is placed in a quartz boat, and then the boat is placed in the quartz furnace tube at a speed of 20±1 cm / s. After the boat is placed, the ground mouth is covered and nitrogen is introduced at 750±3°C at a rate of 6±1 liters per minute for 30±1 minutes. The temperature is raised from 750°C to 1050°C and maintained at 1050±3°C. The nitrogen is stopped and replaced with oxygen. After 5±1 minutes of oxygen introduction, the phosphorus diffusion is performed with oxygen and phosphorus. The phosphorus diffusion time is 6 0±1 minute, wherein the oxygen introduction rate is 3.5±1 liters per minute, the phosphorus introduction rate is 6.5±1 liters per minute, hydrogen and oxygen synthesis is 20±1 minutes, wherein the oxygen introduction rate is 3.5±1 liters per minute, then trichloroethane is introduced for 10±1 minutes, wherein trichloroethane is 80±1 milliliters per minute, then dry oxygen is introduced for 10±1 minutes, the temperature is reduced from 1050°C to 750°C, the grinding mouth is removed, the boat is taken out, the boat speed is 20±1cm / s, the slice is taken out of the quartz boat, and the process is finished;
[0119] r. Perform five photolithography steps on the phosphorus diffusion wafer after completing step q, wherein the steps are as follows:
[0120] ① Glue coating: The viscosity of the photoresist is 100±1SC, and the coating thickness is 20000±2000Å;
[0121] ② Pre-baking: Dry the coated substrate silicon wafer in an oven at 85±5℃ for 30±1 minutes;
[0122] ③ Alignment: Set the mask on the substrate silicon wafer, and expose the substrate silicon wafer with the mask set under the mercury lamp of the photolithography machine for 22±1 seconds to image the mask pattern onto the surface of the substrate silicon wafer;
[0123] ④ Development and fixing: first develop with xylene for 10±1 seconds, then fix with butyl acetate for 8±1 seconds;
[0124] ⑤ Hard film: Dry the fixed substrate silicon wafer in an oven at 140-155℃ for 30±1 minutes;
[0125] ⑥ Oxide layer corrosion: Corrode the hardened substrate silicon wafer with a corrosion solution of H2O: NH4F = 6: 1 for 10 ± 1 minutes;
[0126] ⑦ Removal of photoresist: Soak the substrate silicon wafer after the oxide layer is corroded in H2SO4:H2O2=3:1 soaking solution for 10±1 minutes to remove the photoresist;
[0127] s. Etch the isolation grooves on the wafer that has completed the five-time photolithography in step r, and etch with N2 gas for 5-10 minutes. Load the strip into the etcher, pass CF4 gas at a flow rate of 100-500 ml / min, add 10-40% oxygen, and ventilate for 2-3 minutes. The etching time is 120-300 minutes.
[0128] t. Glass powder filling: Fill the isolation trench wafer that has completed step s with glass powder.
[0129] u. Glass powder sintering: Sinter the glass powder filled in step t, sintering temperature: 470℃±10℃, sintering time: 10 minutes, adjust the nitrogen pressure control gauge pointer on the furnace control panel to 10-15ml / min, and adjust the hydrogen pressure control gauge pointer to 7 ml / min. After sintering, take out the wafer.
[0130] v. Perform six photolithography steps on the glass powder sintered crystal circle after completing step u, wherein the steps are as follows:
[0131] ① Glue coating: The viscosity of the photoresist is 100±1SC, and the coating thickness is 20000±2000Å;
[0132] ② Pre-baking: Dry the coated substrate silicon wafer in an oven at 85±5℃ for 30±1 minutes;
[0133] ③ Alignment: Set the mask on the substrate silicon wafer, and expose the substrate silicon wafer with the mask set under the mercury lamp of the photolithography machine for 22±1 seconds to image the mask pattern onto the surface of the substrate silicon wafer;
[0134] ④ Development and fixing: first develop with xylene for 10±1 seconds, then fix with butyl acetate for 8±1 seconds;
[0135] ⑤ Hard film: Dry the fixed substrate silicon wafer in an oven at 140-155℃ for 30±1 minutes;
[0136] ⑥ Oxide layer corrosion: Corrode the hardened substrate silicon wafer with a corrosion solution of H2O: NH4F = 6: 1 for 10 ± 1 minutes;
[0137] ⑦ Removal of photoresist: Soak the substrate silicon wafer after the oxide layer is corroded in H2SO4:H2O2=3:1 soaking solution for 10±1 minutes to remove the photoresist;
[0138] w. Metallization of the front side of the substrate silicon wafer: metallization is performed on the front side of the substrate silicon wafer after completing step v, wherein the steps are: Ti-W metal sputtering and Al metal evaporation are performed on the substrate silicon wafer in sequence;
[0139] x. Perform seven photolithography steps on the substrate silicon wafer after completing step w, the steps are as follows:
[0140] ① Glue coating: The viscosity of the photoresist is 150±1SC, and the coating thickness is 20000±2000Å;
[0141] ② Pre-baking: Dry the coated substrate silicon wafer in an oven at 85±5℃ for 30±1 minutes;
[0142] ③ Alignment: Set the mask on the substrate silicon wafer, and expose the substrate silicon wafer with the mask set under the mercury lamp of the photolithography machine for 22±1 seconds to image the mask pattern onto the surface of the substrate silicon wafer;
[0143] ④ Development and fixing: first develop with xylene for 10±1 seconds, then fix with butyl acetate for 8±1 seconds;
[0144] ⑤ Hard film: Dry the fixed substrate silicon wafer in an oven at 140-155℃ for 30±1 minutes;
[0145] ⑥ Oxide layer corrosion: Corrode the hardened substrate silicon wafer with a corrosion solution of H 2 O: NH 4 F = 6: 1 for 10 ± 1 minutes;
[0146] ⑦ Removal of photoresist: Soak the substrate silicon wafer after the oxide layer is corroded in H 2 SO 4 :H2O2=3:1 soaking solution for 10±1 minutes to remove the photoresist;
[0147] y. Performing front metal corrosion, front metal degumming and front metal alloying on the substrate silicon wafer that has completed step x;
[0148] z. Conduct electrical testing, passivation, photolithography, passivation corrosion, backside thinning, and backside stress relief corrosion on the substrate silicon wafer with the front side metal alloy completed;
[0149] aa. Thin the back side of the substrate silicon wafer after back side stress relief corrosion by (150-300) ±5um, i.e., the packaging thickness, and back side stress relief corrosion;
[0150] bb. Perform back label photolithography and etching on the substrate silicon wafer after completing step aa, the steps are as follows:
[0151] The substrate silicon wafer is etched with a chemical etching solution of HNO 3 :HF:CH 3 COOH:H 2 O=5:1:3:20 at 12-18°C for 10±1min, cleaned and dried;
[0152] cc, the substrate silicon wafer that has completed step bb is subjected to chemical metal plating of Ni and Au on the front pad, the steps are as follows:
[0153] S1. One-time nickel plating: pH value is 8.5-9.0 when tested with pH test paper, immersed in 95±3℃ nickel plating solution, nickel plating for 90±6 seconds;
[0154] S2. Nickel sintering: sinter at 575℃ for 35±1min, then cool to 500℃ at 1.5℃ / min. Nitrogen flow rate during cooling: 2±0.5 LPM.
[0155] S3. Nitric acid treatment: Boil the silicon wafer in 1:1 nitric acid at 95±5℃ for 4±1 minutes;
[0156] S4. Secondary nickel plating: immerse in 100±3℃ nickel plating solution;
[0157] S5. Gold plating: Gold plating time: 20-25 seconds Check and confirm that the gold plating solution temperature is 110±5℃.
Claims
1. A method for manufacturing a wafer-level flip-flop package low-capacitance transient voltage suppression diode, characterized in that: The following steps are involved: a. Select a P-type substrate with a resistivity of 0.001-0.04Ω•cm and clean the substrate silicon wafer once; b. Perform epitaxial growth on the substrate silicon wafer obtained in step a. After loading, heat it to 950±10℃, with H 2 gas flow rate of 100L / min, heat it to 1800±5℃, with H 2 gas flow rate of 100L / min, pass HCl for 0.5-1 minute, etch for 2-3 minutes, with HCl gas flow rate of 1L / min, blow H 2 for 2-5 minutes, keep the temperature at 1050±5℃, pass SiCl 4 for 0.5-2 minutes, and grow an N-type epitaxial wafer with an epitaxial thickness of 3-4um and a resistivity of 0.001-0.4Ω•cm; c. Cleaning the substrate silicon wafer after completing step b; d. Perform an initial oxidation process on the substrate silicon wafer that has completed step c. First, put the silicon wafer into a quartz boat, and then put the boat into the quartz furnace tube. After the boat is put into the boat, cover the ground mouth, and introduce nitrogen at 750±3°C, and keep the temperature at 950±3°C. Stop nitrogen and replace it with oxygen. After the oxygen is introduced for 20±1 minutes, change to oxygen and hydrogen for hydrogen-oxygen synthesis. The hydrogen-oxygen synthesis time is 240±1 minute. After the hydrogen-oxygen synthesis is completed, oxygen is introduced again, and then trichloroethane is introduced, and then dry oxygen is introduced. The temperature is reduced from 950°C to 750°C, the ground mouth is removed, the boat is taken out, and the wafer is taken out of the quartz boat. The process is completed; e. Performing a photolithography on the substrate silicon wafer with the oxide layer after completing step d, the steps are as follows: ① Glue coating: The viscosity of the photoresist is 100±1SC, and the coating thickness is 20000±2000Å; ② Pre-baking: Dry the coated substrate silicon wafer in an oven at 85±5℃ for 30±1 minutes; ③ Alignment: Set the mask on the substrate silicon wafer, and expose the substrate silicon wafer with the mask set under the mercury lamp of the photolithography machine for 22±1 seconds to image the mask pattern onto the surface of the substrate silicon wafer; ④ Development and fixing: first develop with xylene for 10±1 seconds, then fix with butyl acetate for 8±1 seconds; ⑤ Hard film: Dry the fixed substrate silicon wafer in an oven at 140-155℃ for 30±1 minutes; ⑥ Oxide layer corrosion: Corrode the hardened substrate silicon wafer with a corrosion solution of H 2 O: NH 4 F = 6: 1 for 10 ± 1 minutes; ⑦ Removal of photoresist: Soak the substrate silicon wafer after the oxide layer is etched in H 2 SO 4 :H 2 O 2 =3:1 soaking solution for 10±1 minutes to remove the photoresist; f. Performing N+ implantation on the substrate having one photolithography after completing step e, with an implantation dose of 1E15-5E15 and an implantation energy of 50-80Kev; g. Perform buried layer diffusion on the substrate with N+ implantation and one-time photolithography completed in step f. First, put the silicon wafer into the quartz boat, then put the boat into the quartz furnace tube. After the boat is put into the boat, cover the ground mouth, and introduce nitrogen at 750±3℃, 6±1 liters per minute, for 30±1 minutes. The temperature is raised from 750℃ to 1150℃, and the temperature is maintained at 1150±3℃. The diffusion time is 60±1 minutes. The temperature is reduced from 1150℃ to 750℃, the ground mouth is removed, the boat is taken out, and the wafer is taken out of the quartz boat; h. Perform secondary epitaxial growth on the substrate silicon wafer after completing step g, the steps are the same as step b, and grow an N-type epitaxial wafer with an epitaxial thickness of 3 to 5 um and a resistivity of 0.1 to 0.4 Ω•cm; i. Performing an oxidation process on the substrate silicon wafer after completing step h, the steps are the same as step d; j. Performing secondary photolithography on the substrate silicon wafer with the oxide layer after completing step i, the steps are the same as step e; k. Perform phosphorus diffusion on the substrate that has completed the secondary photolithography in step j. First, place the silicon wafer in a quartz boat, and then enter the boat into the quartz furnace tube at a speed of 20±1 cm / s. After entering the boat, cover the ground mouth, and introduce nitrogen at 750±3°C at a rate of 6±1 liters per minute for 30±1 minutes. The temperature is raised from 750°C to 1100°C and maintained at 1100±3°C. Stop nitrogen and replace with oxygen. After oxygen is introduced for 5±1 minutes, replace with oxygen and phosphorus for phosphorus pre-diffusion. The phosphorus pre-diffusion time is 30±1 minutes, wherein the oxygen introduction rate is 3.5±1 L / min, the phosphorus introduction rate is 6.5±1 L / min, hydrogen and oxygen synthesis is performed for 20±1 minutes, wherein the oxygen introduction rate is 3.5±1 L / min, and then trichloroethane is introduced for 10±1 minutes, wherein the trichloroethane is 80±1 mL / min, then pass dry oxygen for 10±1 minutes, the temperature drops from 1100℃ to 750℃, remove the ground mouth, take out the boat, the boat speed is 20±1cm / s, take the slice out of the quartz boat, and the process is finished; l, the completion of step k of the substrate silicon wafer having an oxide layer is subjected to three photolithography steps, the steps are the same as step e; m, the three-times photolithography wafer completed in step l is p+ implanted, the implantation dose is 3 to 5E15, and the implantation energy is 50 to 80Kev; n. After completing the p+ implantation in step m, perform photoresist removal. Soak the substrate silicon wafer after the oxide layer is etched in a H 2 SO 4 :H 2 O 2=3:1 soaking solution for 10±1 minutes to remove the photoresist; o, to complete step n to remove the glue Chen film four times lithography, the steps are the same as step e; p. Perform n+ implantation on the wafers that have completed four photolithography steps, with an implantation dose of 1 to 5E15 and an implantation energy of 50 to 80Kev; q, the phosphorus diffusion is performed on the implanted sheet after completing step p, the phosphorus diffusion time is 60 ± 1 minutes, and then the dry oxygen temperature is reduced from 1050 ℃ to 750 ℃, and the remaining steps are the same as step k; r, the phosphorus diffusion wafer is completed in step q for five photolithography steps, the same steps as step e; s. Etch the isolation groove on the five-time photolithography wafer that has completed step r. Etch with N 2 for 5-10 minutes. Load the strip into the etcher, pass CF 4 gas at a flow rate of 100-500 mL / min, add 10-40% oxygen, ventilate for 2-3 minutes, and the etching time is 120-300 minutes; t. Filling the isolation trench wafer after step s with glass powder; u. Sinter the glass powder filled in step t at a sintering temperature of 470°C ± 10°C for 10 minutes. Adjust the nitrogen pressure control gauge pointer on the furnace control panel to 10-15mL / min and the hydrogen pressure control gauge pointer to 7mL / min. After sintering, take out the wafer. v. Perform six photolithography steps on the glass powder sintered crystal circle obtained in step u, the steps of which are the same as those in step e; w. Metallize the front side of the substrate silicon wafer after completing step v, and perform Ti-W metal sputtering and evaporation of AL metal on the substrate silicon wafer in sequence; x. Perform seven photolithography steps on the substrate silicon wafer after completing step w. Except that the viscosity of the photoresist is 150±1SC, the remaining steps are the same as step e; y. Performing front metal corrosion, front metal degumming and front metal alloying on the substrate silicon wafer that has completed step x; z. Conduct electrical testing, passivation, photolithography, passivation corrosion, backside thinning, and backside stress relief corrosion on the substrate silicon wafer with the front side metal alloy completed; aa. Thinning the back side of the substrate silicon wafer after back side stress relief etching by 150±5um to 300±5um and performing back side stress relief etching; bb, perform back labeling photolithography and etching on the substrate silicon wafer that has completed step aa, clean it and spin dry it; cc. Perform Ni and Au chemical plating on the front pad of the substrate silicon wafer that has completed step bb.
2. The method for manufacturing a wafer-level flip-chip package low-capacitance transient voltage suppression diode as claimed in claim 1, characterized in that: In step d, the boat speeds entering and exiting the boat are both 20±1 cm / s.
3. The method for manufacturing a wafer-level flip-chip package low-capacitance transient voltage suppression diode as claimed in claim 2, characterized in that: In step d, during hydrogen-oxygen synthesis, the oxygen introduction rate is 3.5±1 L / min, and the hydrogen introduction rate is 6.5±1 L / min.
4. The method for manufacturing a wafer-level flip-flop package low-capacitance transient voltage suppression diode according to claim 2 or 3, characterized in that: In step d, the duration of oxygen introduced after the completion of hydrogen-oxygen synthesis is 20±1 min, and the oxygen introduction rate is 3.5±1 L / min.
5. The method for manufacturing a wafer-level flip-chip package low-capacitance transient voltage suppression diode as claimed in claim 4, characterized in that: In step d, the duration of the introduction of trichloroethane is 10±1 min, and the introduction rate of trichloroethane is 80±1 mL / min.
6. The method for manufacturing a wafer-level flip-chip packaged low-capacitance transient voltage suppressor diode according to claim 1, 2, 3 or 5, characterized in that: The etching described in step bb is that the substrate silicon wafer is etched with a chemical etching solution of HNO 3 :HF:CH 3 COOH:H 2 O =5:1:3:20 at 12-18° C. for 10±1 min.
7. The method for manufacturing a wafer-level flip-chip package low-capacitance transient voltage suppression diode as claimed in claim 6, characterized in that: In the step cc, the front pad metal of the substrate silicon wafer is chemically plated with Ni and Au, and the steps are as follows: S1. One-time nickel plating: PH value 8.5-9.0, immersed in 95±3℃ nickel plating solution, nickel plating 90±6s; S2. Nickel sintering: sinter at 575℃ for 35±1min, then cool to 500℃ at a rate of 1.5℃ / min, with a nitrogen flow rate of 2±0.5LPM during cooling; S3. Nitric acid treatment: Boil the silicon wafer in 1:1 nitric acid at 95±5℃ for 4±1min; S4. Secondary nickel plating: immerse in 100±3℃ nickel plating solution; S5. Gold plating: Gold plating for 20-25 seconds, check and confirm that the temperature of the gold plating solution is 110±5℃.