Organic carrier and method thereof, conductive silver paste and method thereof, and solar cell

By using copovidone as the organic carrier of the first thixotropic agent, the problems of printing durability and dispersion of conductive silver paste in screen printing are solved, and the stability and efficient printing performance of conductive silver paste are achieved, which simplifies the The preparation process avoids the problems of blocking the web and agglomerating particles in traditional technology.

CN114283966BActive Publication Date: 2024-11-15西安宏星电子浆料科技股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111677278.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-31
Publication Date
2024-11-15
Estimated Expiration
2041-12-31

AI Technical Summary

Technical Problem

Traditional conductive silver paste is prone to blocking the grid during screen printing, which affects the photoelectric conversion efficiency of solar cells and the stability of the production process. The dispersion process of traditional thixotropic agents is complex, resulting in agglomeration of silver powder particles, affecting printing. Durability.

Method used

Copovidone is used as the first thixotropic agent, combined with organic solvents, polymer resins and additives, and prepare organic carriers. A fine and uniform conductive silver paste is obtained through simple stirring and heating methods, replacing the traditional polyamide wax thixotropic Improve printing performance and durability.

Benefits of technology

It realizes that the long-term printing of conductive silver paste is not easy to block, reduces the phenomenon of gate breakage, maintains stable photoelectric conversion efficiency, simplifies the preparation process, and avoids the problem of thixotropic agent inactivation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114283966B_ABST
    Figure CN114283966B_ABST
Patent Text Reader

Abstract

The present invention discloses an organic carrier and a method thereof, a conductive silver paste and a method thereof, and a solar cell. The organic carrier for the conductive silver paste comprises: a first thixotropic agent, a second thixotropic agent, a polymer resin, an organic solvent, and a first auxiliary agent; the first thixotropic agent is copolyvidone. The organic carrier for the conductive silver paste comprises, by weight percentage: 0.1 to 10.0 wt% of the first thixotropic agent; 0.0 to 10.0 wt% of the second thixotropic agent; 1.0 to 10.0 wt% of the polymer resin; 70.0 to 95.0 wt% of the organic solvent, and 0.05 to 5.0 wt% of the first auxiliary agent. The organic carrier of the present invention can effectively solve the problem of durability of screen printing, and has the advantages of simple preparation process and no need to worry about the deactivation of the thixotropic agent. The conductive silver paste prepared with the organic carrier has moderate viscosity, good printing performance, is not easy to produce agglomeration, and will not cause screen clogging after long-term large-scale multi-sheet printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of conductive silver paste, and in particular relates to an organic carrier and a method thereof, a conductive silver paste and a method thereof, and a solar cell. Background Art

[0002] Among the numerous renewable energy technologies, photovoltaic power generation is undoubtedly the most promising one. Among them, crystalline silicon solar cells have developed the fastest in recent years, and both the investment in research and development and the degree of industrialization are much higher than other types of photovoltaic cells. Obviously, crystalline silicon solar cells have become the mainstream technology in photovoltaic power generation technology.

[0003] Photovoltaic cells are devices that can convert light energy into electrical energy. The structure of photovoltaic cells is based on silicon material, with one side being a P-type semiconductor and the other side being an N-type semiconductor. At the junction of these two semiconductors, a semiconductor PN junction is formed due to the diffusion of electrons and holes. When sunlight shines on the photovoltaic cell, electron-hole pairs are generated in the cell. Due to the effect of the semiconductor PN junction, the electron-hole pairs are separated. Electrons flow to the N-type semiconductor region, while holes move in the opposite direction to the P-type semiconductor region. The N region is negatively charged, and the P region is positively charged, forming a potential difference between the two regions. When the circuit is connected, current is generated.

[0004] Since semiconductors are based on silicon materials, it is impossible to directly conduct current through contact with wires. Metallization is required at both ends of P-type semiconductors and N-type semiconductors to reduce resistance and allow the current generated by light to enter electronic devices through metal wires. The metallization process refers to coating or printing the conductive silver paste at the corresponding position according to the needs, and then sintering the silicon material and the metal together at high temperature.

[0005] In the production process of crystalline silicon solar cells, conductive silver paste is usually selected as the material for metallization with silicon materials. Currently, most manufacturers use screen printing as a way to apply conductive silver paste on silicon materials. Compared with other methods of applying conductive silver paste on photovoltaic silicon wafers to form grid lines, screen printing has the advantages of fast production speed and low cost. Therefore, the screen printing characteristics of conductive silver paste have always been the main focus of conductive silver paste product improvement.

[0006] In recent years, the market has placed higher and higher demands on the photoelectric conversion efficiency of solar cells. Conductive silver paste is a key material for screen printing. The aspect ratio of the grid lines after printing directly affects the efficiency of the cell, and the requirements are becoming more and more stringent. In addition to the requirements for the aspect ratio of the silver electrode cross section, there have also been requirements for printing durability in recent years. After a long period of time and multiple printings of the conductive silver paste on the screen, the grid lines must remain unbroken, and the line shape and the aspect ratio of the cross section must not change. Traditional thixotropic agents, especially polyamide wax thixotropic agents, are limited by their own characteristics and complex dispersion processes, and are prone to plate plugging and screen blocking. And as the printing time increases, the plate plugging becomes more serious. In addition to affecting the photoelectric conversion efficiency of solar cells, it also requires downtime for processing, causing troubles in the production process. Summary of the invention

[0007] In order to solve the problem of printing durability of conductive silver paste for crystalline silicon solar cells, the present invention provides an organic carrier and method thereof, conductive silver paste and method thereof, and solar cell. The organic carrier of the present invention can effectively solve the problem of screen printing durability, and has the advantages of simple preparation process and no need to worry about deactivation of thixotropic agent.

[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0009] An organic carrier for conductive silver paste, comprising:

[0010] A first thixotropic agent, a second thixotropic agent, a polymer resin, an organic solvent and a first auxiliary agent;

[0011] The first thixotropic agent is copovidone.

[0012] As a further improvement of the present invention, the invention comprises, by weight percentage:

[0013] 0.1-10.0wt% of the first thixotropic agent; 0.0-10.0wt% of the second thixotropic agent; 1.0-10.0wt% of the polymer resin; 70.0-95.0wt% of the organic solvent; 0.05-5.0wt% of the first auxiliary agent.

[0014] As a further improvement of the present invention, the content of the first thixotropic agent is higher than that of the second thixotropic agent.

[0015] As a further improvement of the present invention, the second thixotropic agent is one or more of polyamide wax, polyamide, polyamide derivatives, castor oil derivatives, inorganic clay and silica prepared by pyrolysis.

[0016] As a further improvement of the present invention, the polymer resin is one or more of ethyl cellulose, cellulose acetate butyrate, polyvinyl butyral, polyvinyl pyrrolidone and modified acrylic resin.

[0017] As a further improvement of the present invention, the organic solvent is one or more of diethylene glycol monobutyl ether, butyl carbitol, butyl carbitol acetate, dipropylene glycol methyl ether acetate, alcohol ester dodecahydrate, triethylene glycol methyl ether, tripropylene glycol methyl ether, propylene glycol phenyl ether, pineneol, terpineol, dimethyl adipate and dibasic acid ester.

[0018] As a further improvement of the present invention, the first auxiliary agent is a surfactant, saturated and unsaturated fatty acids, saturated and unsaturated fatty acid amides or a coupling agent.

[0019] A method for preparing an organic carrier for conductive silver paste comprises the following steps:

[0020] Stir and heat the organic solvent to 50-90°C;

[0021] Add the first thixotropic agent, the second thixotropic agent, the polymer resin and the first auxiliary agent under stirring;

[0022] The organic carrier is obtained by heating and maintaining the temperature at 50-90° C. and stirring until all the raw materials are completely dissolved into a transparent, clear and uniform phase.

[0023] A conductive silver paste, measured by weight percentage, comprising:

[0024] 70.0-92.0 wt% of silver powder, 1.0-10.0 wt% of glass powder, 5.0-15.0 wt% of organic carrier, and 0.05-5.0 wt% of a second auxiliary agent;

[0025] The organic carrier is an organic carrier for the conductive silver paste.

[0026] As a further improvement of the present invention, the silver powder is spherical, flaky or irregularly shaped, and the particle size of the silver powder is 0.1 to 10 μm.

[0027] As a further improvement of the present invention, the second auxiliary agent is silicone oil, silicone oil derivative or surfactant.

[0028] A method for preparing a conductive silver paste comprises the following steps:

[0029] Mixing silver powder, glass powder, organic carrier and second auxiliary agent to obtain slurry;

[0030] Pre-dispersing the slurry;

[0031] Grinding and dispersing the pre-dispersed slurry;

[0032] The ground and dispersed slurry is stirred evenly to obtain a conductive silver slurry.

[0033] As a further improvement of the present invention, in the slurry obtained by mixing the silver powder, glass powder, organic carrier and the second auxiliary agent, the order of adding the materials is organic carrier, second auxiliary agent, glass powder and silver powder in sequence.

[0034] A solar cell, characterized in that the electrodes or grid lines of the solar cell are made of the conductive silver paste.

[0035] Compared with the prior art, the present invention has the following advantages:

[0036] The present invention uses copolyvidone as the first thixotropic agent to replace the traditional polyamide wax thixotropic agent to prepare an organic carrier. Since the polyamide wax thixotropic agent is insoluble in organic solvents and has a complicated dispersion process, the organic carrier is prone to contain fine undispersed particles, which further causes silver powder agglomeration particles in the subsequent conductive silver paste production process. Copolyvidone as the first thixotropic agent has the characteristics of being completely soluble in organic solvents, having a simple dispersion process, and being highly compatible with various types of thixotropic agents, polymer resins and additives. Therefore, the organic carrier obtained by using copolyvidone as the first thixotropic agent can obtain a conductive silver paste that is delicate and does not block the plate during long-term printing, effectively solving the problem of printing durability.

[0037] The solar cell of the invention has an electrode or a grid line prepared by using a conductive silver paste, and an organic carrier is prepared by using copolyvidone as a first thixotropic agent. The conductive silver paste prepared by using the organic carrier has moderate viscosity, good printing performance, is not easy to agglomerate, and will not cause screen clogging after long-term large-scale printing of multiple sheets. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The present invention is a flow chart of a method for preparing an organic carrier for conductive silver paste;

[0039] Figure 2 The present invention is a flow chart of a method for preparing a conductive silver paste. DETAILED DESCRIPTION

[0040] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0041] The theories or mechanisms described and disclosed in the present invention, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0042] In the present invention, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0043] In the present invention, unless otherwise specified, “comprising”, “including”, “containing”, “having” or similar terms cover the meanings of “consisting of” and “mainly consisting of”, for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a”.

[0044] In the present invention, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0045] The present invention provides an organic carrier for a conductive silver paste for solar cells, wherein the organic carrier comprises a first thixotropic agent, a second thixotropic agent, a polymer resin, an organic solvent and a first auxiliary agent; the first thixotropic agent is copolyvidone. Specifically, the content of each component is calculated by weight percentage and includes:

[0046] 70.0-95.0wt% of organic solvent, 0.1-10.0wt% of first thixotropic agent, 0.0-10.0wt% of second thixotropic agent, 1.0-10.0wt% of polymer resin, 0.05-5.0wt% of first auxiliary agent. In the present invention, the sum of the percentages of all components in the formula is equal to 100%.

[0047] The most core feature of the present invention is that the first thixotropic agent is a new type of thixotropic agent, specifically copolyvidone (PVP / VA).

[0048] Copolyvidone (PVP / VA) is a linear copolymer of N-vinyl pyrrolidone (NVP) and vinyl acetate (VA), wherein the molar ratio of NVP and VA in the copolyvidone ranges from (20 / 80) to (80 / 20).

[0049] As a preferred embodiment, the content of the first thixotropic agent copolyvidone is higher than that of the second thixotropic agent polyamide wax in the conductive silver paste. In this case, the number of broken grids is significantly reduced after the organic carrier is used.

[0050] In a preferred embodiment, the ratio of NVP and VA monomers in copolyvidone ranges from (20 / 80) to (80 / 20), for example, (20 / 80) to 80 / 20), (20 / 80) to (50 / 50), (30 / 70) to (40 / 60), 50 / 50, 80 / 20, 20 / 80, etc.

[0051] In a preferred embodiment, the organic solvent content is 70.0-95.0 wt%, for example, 70.0-85.0 wt%, 80.0-95.0 wt%, 80.0-90.0 wt%, 70.0 wt%, 85 wt%, and the like.

[0052] In a preferred embodiment, the first thixotropic agent is 0.1-10.0 wt%, for example, 0.1-10.0 wt%, 0.1-8.0 wt%, 1-5.0 wt%, 5-10.0 wt%, 6 wt%, and the like.

[0053] In a preferred embodiment, the second thixotropic agent is 0.0-10.0 wt%, for example, 0.1-8.0 wt%, 2-5.0 wt%, 5-9.0 wt%, 6-10.0 wt%, 7 wt%, and the like.

[0054] In a preferred embodiment, the polymer resin is 1.0-10.0 wt%, for example, 1.0-6 wt%, 3-10.0 wt%, 1.0-10.0 wt%, 4-8 wt%, 5 wt%, and the like.

[0055] In a preferred embodiment, the first auxiliary agent is 0.05-5.0 wt%, for example, 0.05-3 wt%, 1-4 wt%, 3-5.0 wt%, 4 wt%, 2.5 wt%, and the like.

[0056] The second thixotropic agent is a conventional thixotropic agent, which includes but is not limited to commercially available polyamide wax, polyamide, polyamide derivatives, castor oil derivatives, inorganic clay, pyrogenic silica, etc., and one or more of them can be selected.

[0057] For example MAX, PLUS, ST, 6500.

[0058] The above-mentioned polymer resin includes but is not limited to ethyl cellulose (EC), cellulose acetate butyrate (CAB), polyvinyl butyral (PVB), polyvinyl pyrrolidone (PVP), and modified acrylic resin, and one or more kinds of them can be selected.

[0059] The organic solvent can be a mixture of one or more organic solvents, including but not limited to the following solvents: DOWANOLTM Series solvents, alcohol ester twelve, pineol, terpineol, dimethyl adipate, DBE, etc. For example, the organic solvent is diethylene glycol monobutyl ether, butyl carbitol, butyl carbitol acetate, dipropylene glycol methyl ether acetate, alcohol ester twelve, triethylene glycol methyl ether, tripropylene glycol methyl ether, propylene glycol phenyl ether, pineol, terpineol, dimethyl adipate or divalent acid ester.

[0060] The first auxiliary agent includes but is not limited to a surfactant, for example, saturated and unsaturated fatty acids, saturated and unsaturated fatty acid amides, and a coupling agent;

[0061] The surfactant may preferably be a polyoxyethylene surfactant (Ex: TritonX100, Tween20); wherein the unsaturated fatty acid is preferably oleic acid.

[0062] The following describes the preparation method of the organic vehicle containing the first thixotropic agent and the corresponding conductive silver paste for printing. The present invention is not limited to the following embodiments.

[0063] Comparative Example 1

[0064] In a specific embodiment, the raw material ratio of the organic carrier V1 is:

[0065] Polyamide wax MAX4.5wt%, ethyl cellulose EC 1.0wt%, cellulose acetate butyrate CAB 1.0wt%, polyvinyl butyral PVB3.0 wt%, oleic acid 1.0wt%, organic solvent 89.5wt%, wherein the organic solvent is a mixed solvent of diethylene glycol monobutyl ether, butyl carbitol acetate, alcohol ester dodecanedioic acid dimethyl ester.

[0066] Example 1

[0067] In a specific embodiment, the raw material ratio of the organic carrier V2 is: copolyvidone PVP / VA 1.5wt%, ethyl cellulose EC 1.0wt%, cellulose acetate butyrate CAB 1.0wt%, polyvinyl butyral PVB 3.0wt%, oleic acid 1.0wt%, and organic solvent 92.5wt%, wherein the organic solvent is a mixed solvent of diethylene glycol monobutyl ether, butyl carbitol acetate, alcohol ester dodecanedioic acid and dimethyl adipate.

[0068] Example 2

[0069] In a specific embodiment, the raw material ratio of the organic carrier V3 is: copolyvidone PVP / VA 2.5wt%, ethyl cellulose EC 1.0wt%, cellulose acetate butyrate CAB 1.0wt%, polyvinyl butyral PVB 3.0wt%, oleic acid 1.0wt%, and organic solvent 91.5wt%, wherein the organic solvent is a mixed solvent of diethylene glycol monobutyl ether, butyl carbitol acetate, alcohol ester dodecanedioic acid and dimethyl adipate.

[0070] Example 3

[0071] In a specific embodiment, the raw material ratio of the organic carrier V4 is: copolyvidone PVP / VA 3.5wt%, ethyl cellulose EC 1.0wt%, cellulose acetate butyrate CAB 1.0wt%, polyvinyl butyral PVB 3.0wt%, oleic acid 1.0wt%, and organic solvent 90.5wt%, wherein the organic solvent is a mixed solvent of diethylene glycol monobutyl ether, butyl carbitol acetate, alcohol ester dodecanedioic acid and dimethyl adipate.

[0072] The preparation method of the organic carrier of the present invention is different from the traditional preparation method of the organic carrier containing polyamide wax thixotropic agent. The traditional polyamide wax thixotropic agent must undergo a thermal activation process, but its temperature range and heating time must be well and accurately controlled to avoid the deactivation of the polyamide wax thixotropic agent.

[0073] The preparation method of the organic carrier of the present invention is relatively simple, and the copolyvidone (PVP / VA) is composed of other components, and other components such as polymer resin, additives, and even polyamide wax thixotropic agents have good compatibility. Therefore, the preparation method of the organic carrier of the present invention is simpler than that of the organic carrier containing the polyamide wax thixotropic agent.

[0074] Combination Figure 1 The method for preparing the organic carrier of the present invention comprises the following steps:

[0075] Step 1: Add the organic solvent into the reaction vessel according to the weight percentage, stir and heat to the appropriate temperature.

[0076] Step 2: Prepare the raw materials by weight percentage, and add various raw materials under stirring: thixotropic agent, polymer resin and other additives, etc., without limiting the order of addition.

[0077] In combination with Example 1, for example, 1.5 wt % of copovidone PVP / VA, 1.0 wt % of ethyl cellulose EC, 1.0 wt % of cellulose acetate butyrate CAB, 3.0 wt % of polyvinyl butyral PVB, 1.0 wt % of oleic acid, and 92.5 wt % of an organic solvent are added in sequence.

[0078] Step 3: Heat and keep warm, stir until all raw materials are completely dissolved into a transparent, clear, uniform phase, and then the organic carrier for the conductive silver paste of solar cells can be obtained.

[0079] In a preferred embodiment, the temperature is 50-90°C, such as 50-70°C, 60-90°C, 65-85°C, 75°C, 80°C, etc. As in Example 1, the temperature is 60°C.

[0080] The preferred technical solution is that the stirring does not need to be restricted to stirring parameters such as speed, mode, rotor, and blades. The core purpose is to stir evenly.

[0081] In order to solve the problems of poor long-term printing performance and complicated preparation process caused by polyamide wax thixotropic agents, the present invention develops an organic carrier for conductive silver paste that does not use polyamide wax, and uses copolyvidone to replace polyamide wax. The prepared conductive silver paste for solar cells is more stable and not easy to agglomerate; during screen printing, the conductive silver paste is easier to pass through the screen, so that the broken grid phenomenon is reduced, so that during the production process, the stable photoelectric conversion efficiency of the solar cell can be maintained; there is no need to clean and wipe the screen due to blockage, which causes the trouble of downtime.

[0082] The technical solution of the present invention further includes providing a conductive silver paste containing the organic carrier for making solar cell electrodes and grid lines. The conductive silver paste comprises, by weight percentage, 70.0-92.0wt% of silver powder, 1.0-10.0wt% of glass powder, 5.0-15.0wt% of organic carrier, and 0.05-5.0wt% of a second auxiliary agent. In the present invention, the sum of the percentages of all components in the formula is equal to 100%.

[0083] The silver powder includes but is not limited to spherical, flake, and irregularly shaped silver powders, and the particle size range is 0.1 to 10 μm.

[0084] The second auxiliary agent includes but is not limited to silicone oil (PDMS), silicone oil derivatives, surfactants, and the like.

[0085] In a preferred embodiment, the silver powder is 70.0-92.0 wt %, for example, 70.0-80.0 wt %, 80-92.0 wt %, 75-89 wt %, 85 wt %, and the like.

[0086] In a preferred embodiment, the glass powder is 1.0-10.0 wt%, for example, 1.0-6.0 wt%, 5-10.0 wt%, 3-8 wt%, 5 wt%, and the like.

[0087] In a preferred embodiment, the organic vehicle is 5.0-15.0 wt%, for example, 5.0-10.0 wt%, 7-15.0 wt%, 5.0-12.0 wt%, 6-15.0 wt%, 12.0 wt%, and the like.

[0088] In a preferred embodiment, the second auxiliary agent is 0.05-5.0 wt%, for example, 0.05-3.0 wt%, 1-5.0 wt%, 2-4 wt%, 3 wt%, 2.5 wt%, and the like.

[0089] Embodiments and a preparation method of the conductive silver paste are described below, but the present invention is not limited to the following embodiments.

[0090] Comparative Example 2

[0091] In a specific embodiment, the raw material ratio of the conductive silver paste P1 is: silver powder A, 66.6wt%; silver powder B, 22.2wt%; glass powder C, 2.1wt%; glass powder D, 0.4wt%; organic carrier V1, 8.2wt%; PDMS, 0.5wt%. (Using the organic carrier V1 of the comparative example)

[0092] Example 4

[0093] In a specific embodiment, the raw material ratio of the conductive silver paste P2 is: silver powder A, 66.6wt%; silver powder B, 22.2wt%; glass powder C, 2.1wt%; glass powder D, 0.4wt%; organic carrier V2, 8.2wt%; PDMS, 0.5wt%. (The organic carrier V2 of Example 1 is used)

[0094] Example 5

[0095] In a specific embodiment, the raw material ratio of the conductive silver paste P3 is: silver powder A, 66.6wt%; silver powder B, 22.2wt%; glass powder C, 2.1wt%; glass powder D, 0.4wt%; organic carrier V3, 8.2wt%; PDMS, 0.5wt%. (The organic carrier V3 of Example 2 is used)

[0096] Example 6

[0097] In a specific embodiment, the raw material ratio of the conductive silver paste P4 is: silver powder A, 66.6wt%; silver powder B, 22.2wt%; glass powder C, 2.1wt%; glass powder D, 0.4wt%; organic carrier V4, 8.2wt%; PDMS, 0.5wt%. (The organic carrier V4 of Example 3 is used)

[0098] In this embodiment, the particle size of the silver powder D50 is not greater than 3 μm.

[0099] Combination Figure 2The present invention also provides a method for preparing a conductive silver paste for solar cells, comprising the following steps:

[0100] Step 1: Prepare the raw materials according to weight percentage. Put silver powder A, silver powder B, glass powder C, glass powder D, organic carrier, and PDMS into a pre-dispersed container.

[0101] As in Example 5, silver powder A, 66.6 wt %; silver powder B, 22.2 wt %; glass powder C, 2.1 wt %; glass powder D, 0.4 wt %; organic carrier V2, 8.2 wt %; PDMS, 0.5 wt %.

[0102] A preferred technical solution is that the raw materials are added into the pre-dispersion container in the order of organic carrier V2, PDMS, glass powders C and D, and silver powders A and B.

[0103] Step 2: Place the pre-dispersion container on the rotary dispersing device for pre-dispersion.

[0104] Step 3: Roll the pre-dispersed slurry with a three-roll mill for 5 to 10 times. Further grinding and dispersion. The number of rolling times depends on the actual situation.

[0105] Step 4: Pass the ground slurry through a mixer or deaerator for overall mixing;

[0106] The prepared conductive silver pastes P1 to P4 were screen-printed, sintered, and tested on 50 polycrystalline silicon wafers using a screen with an opening of 25 μm.

[0107] The specific embodiments and the properties of the conductive silver paste and the solar cell electrode are shown in Table 1 below:

[0108] Table 1

[0109]

[0110] It can be concluded from the test results in the above table that the conductive silver paste made of the improved organic carrier of the present invention is superior to the conductive silver paste made of the traditional organic carrier in performance tests.

[0111] In the examples, in addition to comparing the effects of the first thixotropic agent and the second thixotropic agent, the effects of mixing the two thixotropic agents are also compared.

[0112] Example 7

[0113] In a specific embodiment, the raw material ratio of the organic carrier V5 is: polyamide wax MAX 3.0wt%, copovidone PVP / VA 1.0wt%, ethyl cellulose EC 1.0wt%, cellulose acetate butyrate CAB 1.0wt%, polyvinyl butyral PVB 3.0wt%, oleic acid 1.0wt%, organic solvent 90.0wt%, wherein the organic solvent is diethylene glycol monobutyl ether.

[0114] Example 8

[0115] In a specific embodiment, the raw material ratio of the organic carrier V6 is: polyamide wax MAX 2.0wt%, copolyvidone PVP / VA 2.0wt%, ethyl cellulose EC 1.0wt%, cellulose acetate butyrate CAB 1.0wt%, polyvinyl butyral PVB 3.0wt%, oleic acid 1.0wt%, organic solvent 90.0wt%, wherein the organic solvent is diethylene glycol monobutyl ether, butyl carbitol acetate, alcohol ester dodecanedioic acid dimethyl ester.

[0116] Example 9

[0117] In a specific embodiment, the raw material ratio of the organic carrier V7 is: polyamide wax MAX1.0wt%, copolyvidone PVP / VA2.5wt%, ethyl cellulose EC1.0wt%, cellulose acetate butyrate CAB1.0wt%, polyvinyl butyral PVB3.0wt%, oleic acid 1.0wt%, organic solvent 90.5wt%, wherein the organic solvent is a mixture of diethylene glycol monobutyl ether, butyl carbitol acetate, alcohol ester dodecahydrate, and dimethyl adipate. Among them, this embodiment uses an activated polyamide wax as the second thixotropic agent, and mixes another prepared copolyvidone as the first thixotropic agent.

[0118] Example 10

[0119] In a specific embodiment, the raw material ratio of the conductive silver paste P5 is: silver powder A, 66.6wt%; silver powder B, 22.2wt%; glass powder C, 2.1wt%; glass powder D, 0.4wt%; organic carrier V5, 8.2wt%; PDMS, 0.5wt%. (The organic carrier V5 of Example 7 is used).

[0120] Embodiment 11

[0121] In a specific embodiment, the raw material ratio of the conductive silver paste P6 is: silver powder A, 66.6wt%; silver powder B, 22.2wt%; glass powder C, 2.1wt%; glass powder D, 0.4wt%; organic carrier V6, 8.2wt%; PDMS, 0.5wt%. (The organic carrier V6 of Example 8 is used).

[0122] Example 12

[0123] In a specific embodiment, the raw material ratio of the conductive silver paste P7 is: silver powder A, 66.6wt%; silver powder B, 22.2wt%; glass powder C, 2.1wt%; glass powder D, 0.4wt%; organic carrier V7, 8.2wt%; PDMS, 0.5wt%. (The organic carrier V7 of Example 9 is used).

[0124] The prepared conductive silver pastes P5-P7 were screen printed, sintered and tested on 50 polycrystalline silicon wafers using a screen with an opening of 25 μm, and compared with P1 in Comparative Example 2.

[0125] The specific embodiments and the properties of the conductive silver paste and the solar cell electrode are shown in Table 2 below:

[0126] Table 2

[0127]

[0128] It can be concluded from the test results in the above table that the conductive silver paste made by mixing the traditional organic carrier with the organic carrier of the present invention has better test performance than the conductive silver paste made by simply using the polyamide wax organic carrier, especially the conductive silver paste in which the content of the first thixotropic agent copolyvidone is higher than that of the second thixotropic agent polyamide wax, and the number of broken grids is significantly reduced.

[0129] The conductive silver paste prepared with the organic carrier of the invention has moderate viscosity, good printing performance, is not easy to generate agglomeration, and will not cause screen clogging after long-term, large-scale, and multi-sheet printing.

[0130] Embodiment 13

[0131] In a specific embodiment, the organic carrier raw material ratio is: 10.0wt% of the first thixotropic agent; 1.0wt% of the second thixotropic agent; 1.0wt% of the polymer resin; 0.05wt% of the first auxiliary agent; the remaining amount of organic solvent; the first thixotropic agent is copolyvidone; the second thixotropic agent is selected from silica prepared by thermal decomposition. The polymer resin is selected from ethyl cellulose and cellulose acetate butyrate. The organic solvent is butyl carbitol. The first auxiliary agent is selected from unsaturated fatty acid amide.

[0132] Embodiment 14

[0133] In a specific embodiment, the organic carrier raw material ratio is: 5wt% of the first thixotropic agent; 1wt% of the second thixotropic agent; 10.0wt% of the polymer resin; 5.0wt% of the first auxiliary agent; the rest of the organic solvent; the first thixotropic agent is copolyvidone; the second thixotropic agent is polyamide; the polymer resin is ethyl cellulose, cellulose acetate butyrate, polyvinyl butyral and polyvinyl pyrrolidone. The organic solvent is alcohol ester dodeca, triethylene glycol methyl ether and tripropylene glycol methyl ether. The first auxiliary agent is TritonX100 and Tween20.

[0134] Embodiment 15

[0135] In a specific embodiment, the organic carrier raw material ratio is: 8.0wt% of the first thixotropic agent; 4.0wt% of the second thixotropic agent; 8.5wt% of the polymer resin; 4.5wt% of the first auxiliary agent; the rest of the organic solvent; the first thixotropic agent is copolyvidone; the second thixotropic agent is polyamide wax and polyamide. The polymer resin is polyvinyl butyral, polyvinyl pyrrolidone and modified acrylic resin. The organic solvent is terpineol, dimethyl adipate and dibasic acid ester. The first auxiliary agent is oleic acid.

[0136] Example 16

[0137] In a specific embodiment, the organic carrier raw material ratio is: 3.0wt% of the first thixotropic agent; 0.2wt% of the second thixotropic agent; 3.2wt% of the polymer resin; 2.2wt% of the first auxiliary agent; the rest is an organic solvent; the first thixotropic agent is copolyvidone; the second thixotropic agent is a castor oil derivative. The polymer resin is polyvinyl pyrrolidone. The organic solvent is DOWANOL TM The first auxiliary agent is unsaturated fatty acid amide.

[0138] Embodiment 17

[0139] In a specific embodiment, the raw material ratio of the conductive silver paste is: silver powder A, 50wt%; silver powder B, 39wt%; glass powder C, 0.5wt%; glass powder D, 0.5wt%; organic vehicle, 5.0wt%; TritonX100, 5.0wt%. (The organic vehicle of Example 12 is used)

[0140] Embodiment 18

[0141] In a specific embodiment, the raw material ratio of the conductive silver paste is: silver powder A, 54.95wt%; silver powder B, 20wt%; glass powder C, 5wt%; glass powder D, 5wt%; organic vehicle, 15.0wt%; Tween20, 0.05wt%. (The organic vehicle of Example 13 is used)

[0142] Embodiment 19

[0143] In a specific embodiment, the raw material ratio of the conductive silver paste is: silver powder A, 60wt%; silver powder B, 10wt%; glass powder C, 5.5wt%; glass powder D, 5.5wt%; organic vehicle, 14wt%; stearic acid, 5wt%. (The organic vehicle of Example 14 is used)

[0144] The conductive silver pastes prepared in Examples 16 to 18 were screen-printed, sintered, and tested on 50 polycrystalline silicon wafers using a screen with an opening of 25 μm.

[0145] The test results show that the organic carrier obtained by using copolyvidone as the first thixotropic agent in the present invention can obtain a conductive silver paste that is fine and does not clog the plate during long-term printing, effectively solving the problem of printing durability.

[0146] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

[0147] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A conductive silver paste for forming grid lines by screen printing, characterized in that: Calculated by weight percentage, including: 70.0-92.0wt% of silver powder, 1.0-10.0wt% of glass powder, 5.0-15.0wt% of organic carrier, 0.05-5.0wt% of second auxiliary agent; The organic carrier comprises: A first thixotropic agent, a second thixotropic agent, a polymer resin, an organic solvent and a first auxiliary agent; The first thixotropic agent is copolyvidone; Calculated by weight percentage, including: 0.1~10.0wt% of the first thixotropic agent; 0.1~10.0wt% of the second thixotropic agent; 1.0~10.0wt% of the polymer resin; 70.0~95.0wt% of the organic solvent; 0.05~5.0wt% of the first auxiliary agent; The content of the first thixotropic agent is higher than the content of the second thixotropic agent; The second thixotropic agent is one or more of polyamide wax, polyamide, polyamide derivatives, castor oil derivatives, inorganic clay and silica prepared by pyrolysis; Copolyvidone is a linear copolymer of N-vinyl pyrrolidone NVP and vinyl acetate VA; the molar ratio of the two monomers NVP and VA in copolyvidone ranges from (20 / 80) to (80 / 20); The polymer resin is one or more of ethyl cellulose, cellulose acetate butyrate, polyvinyl butyral, polyvinyl pyrrolidone and modified acrylic resin; The organic solvent is one or more of diethylene glycol monobutyl ether, butyl carbitol, butyl carbitol acetate, dipropylene glycol methyl ether acetate, alcohol ester dodecahydrate, triethylene glycol methyl ether, tripropylene glycol methyl ether, propylene glycol phenyl ether, terpineol, terpineol, dimethyl adipate and dibasic acid ester; The first auxiliary agent is a surfactant, saturated and unsaturated fatty acids, saturated and unsaturated fatty acid amides or a coupling agent; The second auxiliary agent is a silicone oil derivative or a surfactant.

2. The conductive silver paste according to claim 1, characterized in that: The method for preparing the organic carrier for conductive silver paste comprises the following steps: Stir and heat the organic solvent to 50-90°C; Add the first thixotropic agent, the second thixotropic agent, the polymer resin and the first auxiliary agent under stirring; The organic carrier is obtained by heating and maintaining the temperature at 50-90°C and stirring until all the raw materials are completely dissolved into a transparent and clear uniform phase.

3. The conductive silver paste according to claim 1, characterized in that: The silver powder is spherical, flaky or irregularly shaped, and the particle size of the silver powder is 0.1-10 μm.

4. The method for preparing a conductive silver paste according to any one of claims 1 to 3, characterized in that: The following steps are involved: Mixing silver powder, glass powder, organic carrier and second auxiliary agent to obtain slurry; Pre-dispersing the slurry; Grinding and dispersing the pre-dispersed slurry; The ground and dispersed slurry is stirred evenly to obtain a conductive silver slurry.

5. The method for preparing a conductive silver paste according to claim 4, characterized in that: In the slurry obtained by mixing the silver powder, glass powder, organic carrier and the second auxiliary agent, the order of adding the materials is organic carrier, second auxiliary agent, glass powder and silver powder.

6. A solar cell, characterized in that: The electrodes or grid lines of the solar cell are made of the conductive silver paste according to any one of claims 1 to 3.