Ferrite sintered body and wound coil parts

By adjusting the composition ratios of Fe2O3, CuO, NiO, ZnO, B and Nb in the ferrite sintered body, the thermal impact flexural strength and intersection frequency of ferrite are improved, and the existing ferrite materials are solved in the heat The problem of insufficient heat resistance after impact is suitable for coiled coil components in high-temperature environments and improves the high-frequency noise absorption capacity.

CN114300229BActive Publication Date: 2024-12-06MURATA MFG CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111162719.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-10-07
Filing Date
2021-09-30
Publication Date
2024-12-06
Estimated Expiration
2041-09-30

AI Technical Summary

Technical Problem

The existing ferrite materials lack heat resistance and flexural strength after thermal shock, and the intersection frequency is low, which affects the performance of the coil device.

Method used

Ferrite sintered body containing Fe2O3, CuO, NiO, ZnO, B and Nb is used to increase the thermal impact flexural strength and intersection frequency of ferrite through specific composition ratios and manufacturing processes, and apply it to the coil. In the ceramic core of the linear coil component.

Benefits of technology

It realizes high flexural strength and high intersection frequency after thermal shock, and is suitable for coiled coil components in high temperature environments, effectively removing high-frequency noise.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114300229B_ABST
    Figure CN114300229B_ABST
Patent Text Reader

Abstract

The present invention provides a ferrite sintered body having high flexural strength after thermal shock and high crossover frequency. A ferrite sintered body comprising 45.0 mol% to 49.7 mol% of Fe calculated as Fe2O3, 2.0 mol% to 8.0 mol% of Cu calculated as CuO, 25.0 mol% to 45.0 mol% of Ni calculated as NiO, and 1.0 mol% to 20.0 mol% of Zn calculated as ZnO, and comprising 5 ppm to 25 ppm of B calculated as a single substance of B, and 6 ppm to 25 ppm of Nb calculated as a single substance of Nb, when Fe, Cu, Ni, and Zn are converted to Fe2O3, CuO, NiO, and ZnO, respectively, and the total amount of the Fe2O3, CuO, NiO, and ZnO is set to 100 parts by weight.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a ferrite sintered body and a wound coil component. Background Art

[0002] Patent document 1 discloses a winding type coil device using a drum core having a winding core and a flange portion. According to the coil device described in patent document 1, a first mounting protrusion formed on a flange portion at one end of the winding core portion and a second mounting protrusion formed on a flange portion at the other end of the winding core portion are arranged in an offset manner, so that the coil device has excellent heat shock resistance.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2018-125397 Summary of the invention

[0006] Patent Document 1 describes that the drum core is produced by molding and sintering a ferrite material such as Ni-Zn ferrite or Mn-Zn ferrite. However, if the ferrite material used in the drum core does not have sufficient heat resistance, there is a risk that the heat shock resistance of the coil device as a final product will be reduced.

[0007] Furthermore, from the viewpoint of effectively removing high-frequency noise components, it is also desirable that the crossover frequency at which the reactance X and the resistance R are equal be high.

[0008] The present invention has been made to solve the above problems, and an object of the present invention is to provide a ferrite sintered body having high flexural strength after thermal shock and high crossover frequency. Another object of the present invention is to provide a wound coil component having the ferrite sintered body as a ceramic core.

[0009] The ferrite sintered body of the present invention contains 45.0 mol% to 49.7 mol% of Fe calculated as Fe2O3, 2.0 mol% to 8.0 mol% of Cu calculated as CuO, 25.0 mol% to 45.0 mol% of Ni calculated as NiO, and 1.0 mol% to 20.0 mol% of Zn calculated as ZnO. When Fe, Cu, Ni and Zn are converted into Fe2O3, CuO, NiO and ZnO respectively and the total amount of the above-mentioned Fe2O3, the above-mentioned CuO, the above-mentioned NiO and the above-mentioned ZnO is set to 100 parts by weight, it contains 5 ppm to 25 ppm of B calculated as a single substance of B, and 6 ppm to 25 ppm of Nb calculated as a single substance of Nb.

[0010] The winding type coil component of the present invention comprises: a ceramic core, which is composed of the ferrite sintered body of the present invention; an electrode, which is formed on an end face in the height direction of the flange portion of the above-mentioned ceramic core; and a winding, which is wound around the axial core portion of the above-mentioned ceramic core, and the end portion is electrically connected to the above-mentioned electrode.

[0011] According to the present invention, a ferrite sintered body having high flexural strength after thermal shock and high intersection frequency can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 This is a front view schematically showing an example of the wound wire coil component of the present invention.

[0013] Figure 2 It is a schematic representation of the composition Figure 1 A perspective view of an example of a ceramic core of a wound coil component is shown.

[0014] Explanation of symbols

[0015] 10 Wound coil parts

[0016] 20 Ceramic core

[0017] 30 Shaft core

[0018] 31, 32 Main surface of the shaft core

[0019] 33, 34 Side of the shaft core

[0020] 40 Flange

[0021] 41, 42 Main surface of flange portion

[0022] 43, 44 Side of flange

[0023] 45, 46 End surface of flange

[0024] 50 electrodes

[0025] 55 Reel

[0026] Ld Length direction

[0027] Td height direction

[0028] Wd width direction DETAILED DESCRIPTION

[0029] Hereinafter, the ferrite sintered body and the wound coil component of the present invention will be described.

[0030] However, the present invention is not limited to the following configurations, and can be appropriately modified and applied within the scope of the present invention. It should be noted that a configuration in which two or more of the preferred configurations of the present invention described below are combined is also the present invention.

[0031] [Ferrite sintered body]

[0032] The ferrite sintered body of the present invention contains Fe, Cu, Ni, Zn, B and Nb.

[0033] The ferrite sintered body of the present invention contains 45.0 mol% to 49.7 mol% of Fe calculated as Fe2O3, 2.0 mol% to 8.0 mol% of Cu calculated as CuO, 25.0 mol% to 45.0 mol% of Ni calculated as NiO, and 1.0 mol% to 20.0 mol% of Zn calculated as ZnO.

[0034] The ferrite sintered body of the present invention contains 5ppm to 25ppm of B calculated as a single substance and 6ppm to 25ppm of Nb calculated as a single substance, when Fe, Cu, Ni and Zn are converted into Fe2O3, CuO, NiO and ZnO, respectively, and the total amount of the above-mentioned Fe2O3, the above-mentioned CuO, the above-mentioned NiO and the above-mentioned ZnO is set to 100 parts by weight.

[0035] By setting the composition of ferrite in the ferrite sintered body of the present invention within the above range, the flexural strength after thermal shock can be increased and the crossover frequency can be increased.

[0036] The content of each element can be determined by analyzing the composition of the sintered body using inductively coupled plasma atomic emission spectrometry / mass spectrometry (ICP-AES / MS).

[0037] The ferrite sintered body of the present invention preferably further contains 100 ppm or less of Mo in terms of Mo element when the total amount of the Fe2O3, CuO, NiO and ZnO is 100 parts by weight. If the ferrite sintered body contains Mo in the above range, the flexural strength after thermal shock can be further improved.

[0038] When the ferrite sintered body of the present invention contains Mo, the lower limit of the Mo content is not particularly limited, but it is preferred that when the total amount of the above-mentioned Fe2O3, the above-mentioned CuO, the above-mentioned NiO and the above-mentioned ZnO is set to 100 parts by weight, it contains Mo in an amount of 3 ppm or more calculated as a single substance of Mo.

[0039] In the ferrite sintered body of the present invention, the ratio of ZnO to NiO (Zn / Ni) is preferably 0.52 or less. If the Zn / Ni ratio is 0.52 or less, the crossover frequency can be further increased, thereby obtaining a noise absorbing component that can effectively remove high-frequency noise.

[0040] In the ferrite sintered body of the present invention, the lower limit of the ratio of the ZnO to the NiO (Zn / Ni) is not particularly limited, but the ratio of the ZnO to the NiO (Zn / Ni) is, for example, 0.01 or more.

[0041] The ferrite sintered body of the present invention is preferably produced as follows.

[0042] First, Fe2O3, CuO, NiO, ZnO, B4C and Nb2O5 are weighed so that the composition after firing becomes a predetermined composition, and the raw materials are put into a ball mill together with pure water and PSZ (partially stabilized zirconia) balls, and wet mixed and crushed for a predetermined time (e.g., 4 to 8 hours). After evaporation and drying, they are pre-calcined at a predetermined temperature (e.g., 700°C to 800°C) for a predetermined time (e.g., 2 to 5 hours), thereby preparing a pre-calcined product (pre-calcined powder).

[0043] The obtained precalcined product (precalcined powder) was put into a ball mill together with pure water, polyvinyl alcohol as a binder, a dispersant, a plasticizer and PSZ balls, and mixed and pulverized in a wet manner. The slurry obtained by the mixed and pulverized was dried in a spray dryer and granulated to produce a granular powder.

[0044] A mold is prepared, and the prepared granular powder is pressure-molded to form a compact.

[0045] Next, the molded body is fired in a firing furnace at a predetermined temperature (eg, 1100° C. to 1200° C.) for a predetermined time (eg, 2 hours to 5 hours). Through the above production steps, a ferrite sintered body can be obtained.

[0046] Hereinafter, examples will be shown which more specifically disclose the ferrite sintered body of the present invention, but it should be noted that the present invention is not limited to these examples.

[0047] (Example 1)

[0048] Fe2O3, CuO, NiO, ZnO, B4C and Nb2O5 were weighed so that the composition after firing would be the composition shown in Table 1, and the raw materials were put into a ball mill together with pure water and PSZ balls, and wet mixed and pulverized for 4 hours. After evaporation and drying, they were pre-calcined at 800°C for 2 hours to prepare a pre-calcined product.

[0049] The calcined product was put into a ball mill together with pure water, polyvinyl alcohol as a binder, a dispersant, a plasticizer and PSZ balls, and mixed and pulverized. The slurry obtained by the mixed and pulverized was dried in a spray dryer and granulated to produce a granular powder.

[0050] The prepared granular powder was compacted to produce a compact having the following dimensions after firing.

[0051] ·4mm×2mm×1.5mm single plate specimen, or,

[0052] Ring-shaped test piece with an outer diameter of 20 mm, an inner diameter of 12 mm, and a thickness of 1.5 mm.

[0053] The produced compact was fired at 1100° C. for 2 hours. Samples 1 to 27 were thus produced.

[0054] For each single plate sample, the composition of the sintered body was analyzed using ICP-AES / MS, thereby determining the content of each element. The results are shown in Table 1. For Fe, Cu, Ni, and Zn, the values ​​converted into oxides are shown in Table 1, and for B and Nb, the values ​​converted into simple substances are shown in Table 1. In addition, Table 1 also shows the ratio of ZnO to NiO (Zn / Ni).

[0055] The flexural strength of each single-plate specimen was measured by a three-point bending test.

[0056] First, the flexural strength of the sample after firing was measured and this was defined as the initial flexural strength. In addition, the sample kept at 125°C was put into water at 25°C and subjected to a heat shock of 100°C, thereby measuring the flexural strength after the heat shock. The results are shown in Table 1.

[0057] The flexural strength was measured on 10 specimens and the average value was taken.

[0058] Each ring-shaped sample was placed in a magnetic permeability measuring fixture (Agilent Technologies, Inc., 16454A-s) and measured for magnetic permeability μ at 25±2°C and a measuring frequency of 1 MHz using an impedance analyzer (Agilent Technologies, Inc., E4991A). In addition, the frequency characteristics of reactance X and resistance R were measured to find the crossover point frequency at which X and R were equal. The results are shown in Table 1.

[0059]

[0060] In Table 1, samples marked with an asterisk are comparative examples outside the scope of the present invention.

[0061] According to Table 1, for a composite containing 45.0 mol% to 49.7 mol% of Fe in terms of Fe2O3, 2.0 mol% to 8.0 mol% of Cu in terms of CuO, 25.0 mol% to 45.0 mol% of Ni in terms of NiO, and 1.0 mol% to 20.0 mol% of Zn in terms of ZnO, and after converting Fe, Cu, Ni and Zn into Fe2O3, CuO, NiO and ZnO respectively and converting the above Fe 2O3, the above-mentioned CuO, the above-mentioned NiO and the above-mentioned ZnO when the total amount is set to 100 parts by weight, samples 2 to 4, 7 to 10, 12 to 14, 17 to 19 and 22 to 24 containing 5ppm to 25ppm of B calculated as B element and 6ppm to 25ppm of Nb calculated as Nb element can obtain ferrite sintered bodies having a magnetic permeability μ of greater than 20, a flexural strength after thermal shock at 100°C of greater than 100N and a crossover frequency of greater than 20MHz.

[0062] For samples 2 to 4, 8 to 10, 13, 14, 17 to 19, and 22 to 24 having a Zn / Ni ratio of 0.52 or less, the crossover frequency can be further increased. Specifically, the crossover frequency can be made 40 MHz or more.

[0063] (Example 2)

[0064] In the composition of sample 3 in Table 1, MoO3 was converted into Mo simple substance and contained 3 ppm, 30 ppm, 50 ppm or 100 ppm in the composition after firing, and the same evaluation as in Example 1 was performed. The method for measuring the Mo content was the same as in Example 1. The results are shown in Table 2.

[0065]

Table 2

[0066]

[0067] According to Table 2, samples 31, 32, 33 and 34 containing 100 ppm or less of Mo in terms of Mo element conversion can further improve the flexural strength after heat shock at 100°C.

[0068] [Wound coil parts]

[0069] The wound coil component of the present invention comprises the ferrite sintered body of the present invention as a ceramic core. As described above, the ferrite sintered body of the present invention has high bending strength even when subjected to thermal shock, and can be used favorably as a wound coil component used in a high temperature environment such as in-vehicle applications.

[0070] Figure 1 This is a front view schematically showing an example of the wound wire coil component of the present invention. Figure 2 It is a schematic representation of the composition Figure 1 A perspective view of an example of a ceramic core of a wound coil component is shown.

[0071] Figure 1 and Figure 2 This is a schematic diagram and its dimensions, aspect ratio, etc. may differ from the actual product.

[0072] Figure 1 The wound coil component 10 shown includes a ceramic core 20, an electrode 50, and a winding (coil) 55. The ceramic core 20 is made of the ferrite sintered body of the present invention.

[0073] like Figure 2 As shown, the ceramic core 20 includes an axial core portion 30 and a pair of flange portions 40 formed at both ends of the axial core portion 30. The axial core portion 30 and the flange portion 40 are formed integrally.

[0074] In this manual, if Figure 1 and Figure 2 As shown, the direction in which the pair of flanges 40 are arranged is defined as the length direction Ld, and in the direction perpendicular to the length direction Ld, Figure 1 and Figure 2 The up-down direction of is defined as a height direction (thickness direction) Td, and the direction perpendicular to both the length direction Ld and the height direction Td is defined as a width direction Wd.

[0075] The shaft core 30 is formed, for example, in a rectangular parallelepiped shape extending in the length direction Ld. The central axis of the shaft core 30 extends substantially parallel to the length direction Ld. The shaft core 30 has a pair of main surfaces 31 and 32 facing each other in the height direction Td and a pair of side surfaces 33 and 34 facing each other in the width direction Wd.

[0076] In this specification, the rectangular parallelepiped includes a cuboid with chamfered corners and ridges, a cuboid with rounded corners and ridges, etc. In addition, concavities and convexities may be formed on part or all of the main surface and the side surfaces.

[0077] A pair of flanges 40 are provided at both ends of the longitudinal direction Ld of the shaft core 30. Each flange 40 is formed into a thin rectangular parallelepiped shape in the longitudinal direction Ld. Each flange 40 is formed to extend around the shaft core 30 in the height direction Td and the width direction Wd. Specifically, the planar shape of each flange 40 when viewed from the longitudinal direction Ld is formed to extend in the height direction Td and the width direction Wd relative to the shaft core 30.

[0078] Each flange portion 40 has a pair of main surfaces 41 and 42 facing each other in the length direction Ld, a pair of side surfaces 43 and 44 facing each other in the width direction Wd, and a pair of end surfaces 45 and 46 facing each other in the height direction Td. The main surface 41 of one flange portion 40 faces the main surface 41 of another flange portion 40.

[0079] For example, the main surface 41 of each flange portion 40 is formed so that its entire surface extends substantially perpendicularly to the direction in which the central axis of the shaft core portion 30 extends (i.e., the length direction Ld). That is, the entire main surface 41 of each flange portion 40 is formed so as to extend substantially parallel to the height direction Td. However, the main surface 41 of each flange portion 40 may also be formed as an inclined surface.

[0080] like Figure 1 As shown, the electrode 50 is provided on one end surface 46 in the height direction Td of each flange portion 40. For example, when the wound coil component 10 is mounted on a circuit board, the electrode 50 is electrically connected to the electrode of the circuit board. The electrode 50 is composed of, for example, a Ni-based alloy such as nickel (Ni)-chromium (Cr), Ni-copper (Cu), silver (Ag), Cu, tin (Sn), etc.

[0081] The winding wire 55 is wound around the shaft core 30. The winding wire 55 has a structure in which a core wire mainly composed of a conductive material such as Cu is covered with an insulating material such as polyurethane or polyester. Both ends of the winding wire 55 are electrically connected to the electrodes 50, respectively.

[0082] The wound wire type coil component of the present invention is produced, for example, as follows.

[0083] As described in the above [Ferrite sintered body], the granular powder is pressed and formed into a molded body. Next, the molded body is fired in a firing furnace at a predetermined temperature (e.g., 1100°C to 1200°C) for a predetermined time (e.g., 2 hours to 5 hours). The obtained sintered body is put into a drum and ground with a grinding material. The above manufacturing process can obtain Figure 2 Ceramic core shown.

[0084] Next, an electrode is formed on the end surface of the flange of the ceramic core. For example, a conductive paste containing Ag and glass frit is applied to the end surface of the flange, sintered under predetermined conditions (e.g., 800° C. to 820° C.) to form a base metal layer, and then a Ni plating film and a Sn plating film are sequentially formed on the base metal layer by electroplating to form an electrode.

[0085] Then, after the winding wire is wound around the axial core of the ceramic core, the end of the winding wire is joined to the electrode by a known method such as thermal compression. Figure 1 The wound coil component shown.

[0086] The wound wire coil component of the present invention is not limited to the above-mentioned embodiment, and various applications and modifications can be made within the scope of the present invention.

[0087] In the winding type coil component of the present invention, the shape and size of the axial core of the ceramic core, the shape and size of the flange of the ceramic core, the thickness (wire diameter), the number of turns (number of turns), the cross-sectional shape and the number of roots of the winding wire are not particularly limited and can be appropriately changed according to the desired characteristics and installation location. In addition, the position and number of electrodes can also be appropriately set according to the number of roots and purpose of the winding wire.

Claims

1. A ferrite sintered body comprising 45.0 mol% to 49.7 mol% of Fe calculated as Fe2O3, 2.0 mol% to 8.0 mol% of Cu calculated as CuO, 25.0 mol% to 45.0 mol% of Ni calculated as NiO, and 1.0 mol% to 20.0 mol% of Zn calculated as ZnO, When Fe, Cu, Ni and Zn are converted into Fe2O3, CuO, NiO and ZnO respectively and the total amount of Fe2O3, CuO, NiO and ZnO is set to 100 parts by weight, it contains 5ppm to 25ppm of B calculated as a single substance of B and 6ppm to 25ppm of Nb calculated as a single substance of Nb.

2. The ferrite sintered body according to claim 1, wherein When the total amount of the Fe2O3, the CuO, the NiO and the ZnO is 100 parts by weight, the Fe2O3, the CuO, the NiO and the ZnO further contain 100 ppm or less of Mo in terms of Mo single substance.

3. The ferrite sintered body according to claim 1 or 2, wherein: The ratio of the ZnO to the NiO, that is, Zn / Ni, is 0.52 or less in terms of molar ratio.

4. A wound coil component, comprising: A ceramic core, comprising a ferrite sintered body as claimed in any one of claims 1 to 3; an electrode formed on one end surface in the height direction of the flange portion of the ceramic core; and The winding wire is wound around the axial core of the ceramic core, and the end portion is electrically connected to the electrode.

Citation Information

Patent Citations

  • Coil device

    JP2018125397A

  • Ferrite sintered body and wound coil component

    CN114300230A

  • Ferrite sintered body and wound coil component

    CN114300231A