Composite material and manufacturing method thereof, and semiconductor packaging structure

By oxidizing porous copper materials to form a metal oxide shell structure, the problem of high porosity in porous copper interconnect structures is solved, the strength and service reliability of the material are improved, the process flow is simplified and the cost is reduced.

CN114300411BActive Publication Date: 2024-10-15SHENZHEN INST OF ADVANCED TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111335232.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-11
Publication Date
2024-10-15
Estimated Expiration
2041-11-11

AI Technical Summary

Technical Problem

Excessive porosity in existing porous copper interconnect structures results in substandard mechanical properties and service reliability. Existing post-processing methods are time-consuming, laborious, and costly.

Method used

By oxidizing porous metal materials, a metal oxide shell structure is formed to fill the original pores and increase the density and strength of the material. Specific methods include high-temperature heat treatment, constant temperature and humidity heat treatment, oxidative solution treatment, etc. to form a copper oxide shell and improve the density and connection strength of the material.

Benefits of technology

Significantly reduces the porosity of porous copper, improves the strength and service reliability of the material, simplifies the process, reduces costs, and improves production efficiency. It also has a certain impact on the conductive properties, but the mechanical properties and reliability are significantly improved. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114300411B_ABST
    Figure CN114300411B_ABST
Patent Text Reader

Abstract

The present application relates to the field of material technology, and discloses a composite material and a method for making the same, and a semiconductor packaging structure. The composite material includes a porous metal material and a metal oxide shell structure on the inner wall of the porous structure of the porous metal material. The manufacturing method includes oxidizing the porous metal material to obtain a composite material having a metal-metal oxide core-shell structure, and the semiconductor packaging structure includes a joint made using the composite material. The above-mentioned materials, methods, and structures are used in semiconductor interconnection processes, which can effectively improve the mechanical properties and service reliability of porous copper interconnection structures, simplify the production process, reduce production costs, and promote industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of material technology, and in particular to a composite material and a manufacturing method thereof, and a semiconductor packaging structure. Background Art

[0002] The innovation of microelectronics technology has led the development of current electronic technology. With the rapid upgrading of electronic technology, microelectronics packaging technology has received increasing attention. The low-temperature sintering process of metal particles is a new type of packaging process in recent years. It promotes the diffusion of atoms on the surface of particles through the particle size effect, and then sinters them into conductors at a lower temperature. The sintered conductor has high strength and high toughness mechanical properties, and because it is composed of a single metal, it also has high electrical conductivity and high thermal conductivity. It can be used in printed electronic inks, sintered metal interconnection materials, through-hole filling sintering materials and other occasions. And the particle size effect disappears in the block formed after sintering, and the remelting temperature returns to the melting point of the bulk metal, ensuring its high-temperature reliability. Taking copper metal as an example, copper has excellent electrical and thermal conductivity, and is cheap, and is easy to prepare into micro-nanoscale particles. As a sintering filler with excellent cost performance in metal particle low-temperature sintering connection solder paste, it meets the needs of the rapidly developing electronics industry.

[0003] However, after sintering, copper particles have many holes due to their intrinsic characteristics, making it difficult to obtain a reliable sintered structure, which greatly affects their mechanical properties. Even if the porous copper interconnects obtained have excellent thermal conductivity and electrical conductivity, the high porosity makes it difficult to guarantee their service reliability. How to reduce the porosity of the sintered body and increase the density of the connection layer is the key to improving the service reliability of the porous copper interconnect structure. In recent years, it has been reported that applying high pressure and high temperature during the connection process and extending the connection process time can promote the diffusion of copper and reduce the porosity, thereby obtaining a dense porous interconnect and improving the mechanical, electrical and thermal properties. However, this post-processing method is time-consuming and labor-intensive, not suitable for industrial mass production, and has a high cost. Summary of the invention

[0004] The main technical problem solved by the present invention is to provide a composite material and a manufacturing method thereof, and a semiconductor packaging structure, which can solve the problem of substandard mechanical properties and service reliability caused by excessively high porosity in existing porous copper interconnect structures.

[0005] In order to solve the above technical problems, a technical solution adopted in the present application is: to provide a composite material, the composite material includes a porous metal material, the porous metal material includes a plurality of pore structures, and the inner wall of the pore structure includes a metal oxide shell structure.

[0006] Specifically, the composite material includes a central part and an outer layer part wrapping the central part, and the inner wall of the pore structure of the outer layer part includes a metal oxide shell structure.

[0007] Specifically, in the composite material, the metal is copper, and the metal oxide includes at least one of copper oxide and cuprous oxide.

[0008] In order to solve the above technical problems, another technical solution adopted in the present application is: to provide a method for manufacturing a composite material, the manufacturing method comprising: providing a porous metal material, the porous metal material comprising a plurality of pore structures; oxidizing the porous metal material to form a metal oxide shell structure on the inner wall of its pore structure.

[0009] Specifically, in the above method, the porous metal material is subjected to oxidation treatment, including: subjecting the porous metal material to at least one of high temperature heat treatment, constant temperature and constant humidity heat treatment, oxidizing solution treatment, and oxidizing plasma implantation treatment.

[0010] The temperature range of the high temperature heat treatment is 150-250° C., and the treatment time is 10-100 hours.

[0011] Specifically, in the above method, before the porous metal material is oxidized, the method further includes: cleaning the porous metal material; and coating a preset area on the surface of the porous metal material to prevent the preset area from being oxidized.

[0012] Specifically, in the above method, the metal is copper, and the metal oxide includes at least one of copper oxide or cuprous oxide.

[0013] Specifically, in the above method, a porous metal material is provided, including: sintering copper particles or porous copper films to obtain the porous metal material.

[0014] Specifically, in the above method, the copper content of the porous metal material is greater than 90%, and the porosity of the porous metal material is greater than 10%.

[0015] In order to solve the above technical problems, another technical solution adopted by the present application is: to provide a semiconductor packaging structure, which includes: a substrate; a semiconductor device, which is arranged on the substrate; and a connector, which is arranged between the substrate and the semiconductor device and is used to connect the substrate and the semiconductor device. The connector is the above composite material or the composite material made by the above method.

[0016] Different from the prior art, the present application provides a composite material and a method for making the same, as well as a semiconductor packaging structure. The composite material includes a porous metal material, the porous metal material includes a plurality of pore structures, and the inner wall of the pore structure includes a metal oxide shell structure. In the above manner, compared with the porous metal material in the prior art, a metal oxide shell inside the pore structure is added. Since the metal oxide shell is added to the original gap and the original pores are filled, the material itself becomes denser and the strength of the material is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. Among them:

[0018] Figure 1 is a schematic diagram of a semiconductor packaging structure provided by the present application;

[0019] Figure 2 It is a schematic diagram of the structure of the composite material provided in this application;

[0020] Figure 3 It is a schematic diagram of the process of manufacturing the composite material provided by the present application;

[0021] Figure 4 yes Figure 3 Schematic diagram of the process of S32;

[0022] Figure 5 is a schematic diagram of the structure of the porous metal material provided in the present application before and after oxidation treatment according to the above method;

[0023] Figure 6 It is a comparison diagram of the scanning electron microscope morphology, XRD image analysis, shear strength and resistivity of the porous metal sample before and after oxidation treatment in Example 1 provided in the present application;

[0024] Figure 7 It is a comparison diagram of the scanning electron microscope morphology, XRD image analysis, shear strength and resistivity of the porous metal sample before and after oxidation treatment in Example 2 provided in the present application;

[0025] Figure 8 This is a comparison diagram of the scanning electron microscope morphology and shear strength of the porous metal sample after oxidation treatment and the original porous metal sample in Example 3 provided by the present application before and after the device is formed into a device and subjected to 1000 power cycles;

[0026] Fig. 9This is a scanning electron microscope morphology image of the porous metal sample after non-oxidation treatment in Comparative Example 1 provided in the present application. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. It will be understood that the specific embodiments described herein are only used to explain the present application, rather than to limit the present application. It should also be noted that, for ease of description, only some but not all structures related to the present application are shown in the drawings. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.

[0028] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0029] See also Figure 1 , Figure 1 It is a schematic diagram of a semiconductor packaging structure provided in the present application. The semiconductor packaging structure 100 includes a semiconductor chip 110, a porous copper joint 120, and a substrate 130. The semiconductor chip 110 is connected to the substrate 130 through the porous copper joint 120.

[0030] The semiconductor chip 110 is a semiconductor device that is manufactured by etching and wiring on a semiconductor sheet and can achieve a certain function, which is not specifically limited here.

[0031] The substrate 130 is a basic material for manufacturing a PCB (Printed Circuit Board). Generally, the substrate is a copper-clad laminate, which is not specifically limited here.

[0032] Among them, the material of the porous copper joint 120 is the composite material provided in this application or the composite material produced by the method provided in this application. The structure and production method of the composite material of the porous copper joint 120 are introduced through several embodiments below.

[0033] See also Figure 2 , Figure 21 is a schematic diagram of the structure of the composite material provided in the present application. Specifically, the porous copper joint 120 is made of a composite material 200. The composite material 200 includes a porous metal material. The porous metal material includes a plurality of pore structures 121. The inner wall of the pore structure 121 includes a metal oxide shell structure 122. The composite material 200 can be divided into a central part and an outer layer part wrapping the central part. The inner wall of the pore structure 121 of the outer layer part includes a metal oxide shell structure 122.

[0034] Among them, porous metal materials are metals with a large number of directional or random holes dispersed inside. The diameter of these holes is about 2um to 3mm. Due to different design requirements for holes, the holes can be foam-shaped, lotus-shaped, honeycomb-shaped, etc. Porous metal materials can also be divided into two categories according to the shape of their holes: independent hole type and continuous hole type. Independent materials have the characteristics of small specific gravity, good rigidity and specific strength, good vibration and sound absorption performance; in addition to the above characteristics, continuous materials also have the characteristics of good permeability and air permeability. Because porous metal materials have the characteristics of structural materials and functional materials, they are widely used in aerospace, transportation, construction engineering, mechanical engineering, electrochemical engineering, environmental protection engineering and other fields.

[0035] Compared with the porous metal material in the prior art, the present embodiment adds a metal oxide shell structure 122 to the inner wall of the pore structure 121. Since the metal oxide shell is added to the original gap and fills the original hole, the material itself is more dense and the strength of the material is increased.

[0036] In one embodiment, the metal may be copper, and the metal oxide disposed on the inner wall of the pore structure may be copper oxides such as copper oxide and cuprous oxide. Specifically, the copper particles are sintered at low temperature to form porous copper. Among them, copper is electrically conductive and has excellent thermal conductivity, and is cheap, so it is convenient to prepare it into micro-nanoscale particles, which are used as sintering fillers with excellent cost performance in solder paste for low-temperature sintering of metal particles, meeting the needs of the rapidly developing electronics industry. However, after sintering, the copper particles have many holes due to their intrinsic characteristics, making it difficult to obtain a reliable sintering structure, which greatly affects their mechanical properties. Even if the porous copper interconnects obtained have excellent thermal conductivity and electrical conductivity, the high porosity makes it difficult to ensure their service reliability. By adding copper oxide to the inner wall of the pore structure in the manner of this embodiment, the porosity of the porous copper can be reduced, the density of the porous copper can be increased, and the strength of the material can be improved.

[0037] See also Figure 3 , Figure 3 : is a schematic diagram of a process for preparing a composite material provided in the present application, the method comprising:

[0038] S31: Provide a porous metal material, wherein the porous metal material includes a plurality of pore structures.

[0039] Specifically, the porous metal material is produced by sintering copper particles or porous copper films.

[0040] Specifically, the copper content of the porous metal material is greater than 90%, and the porosity of the porous metal material is greater than 10%.

[0041] S32: performing oxidation treatment on the porous metal material to form a metal oxide shell structure on the inner wall of the pore structure of the porous metal material.

[0042] Optionally, the method of performing oxidation treatment includes at least one of high temperature heat treatment, constant temperature and constant humidity heat treatment, oxidizing solution treatment, and oxidizing plasma implantation treatment.

[0043] Specifically, the temperature range of the high temperature heat treatment is 150-250° C., and the treatment time is 10-100 hours.

[0044] Compared with the prior art, the method for making the composite material provided in this embodiment forms a metal oxide shell inside the pore structure by oxidizing the original porous metal material. Compared with the long-term high temperature and high pressure treatment in the prior art, the manufacturing method is simpler. The metal oxide shell is added to the original gap to fill the original hole, making the material itself more dense and improving the strength of the material. In addition, the cost is reduced in the process flow and the manufacturing efficiency is improved.

[0045] See also Figure 4 , Figure 4 yes Figure 3 In the flowchart of S32, S32 may further include:

[0046] S321: Cleaning the porous metal material.

[0047] Specifically, a special cleaning agent is used to clean dirt and possible organic residues on the surface of the porous metal material to keep its surface and porous structure clean.

[0048] S322: performing coating treatment on a preset area on the surface of the porous metal material.

[0049] Specifically, a predetermined area on the surface of the porous metal material is plated by a coating process to prevent the predetermined area from being oxidized during the oxidation process.

[0050] S323: placing the porous metal material in an oxidizing environment for oxidation treatment.

[0051] Optionally, in the high temperature heat treatment method, the porous metal material is placed in an atmospheric environment with a temperature ranging from 150 to 250° C., and the treatment time is 10 to 100 hours.

[0052] See also Figure 5 , Figure 5 It is a schematic diagram of the structure of the porous metal material provided in the present application before and after oxidation treatment according to the above method, wherein the porous copper joint 120 includes a plurality of pore structures 121 inside. After oxidation treatment, a metal oxide shell structure 122 is generated on the inner wall of the pore structure 121, thereby forming a copper-copper oxide core-shell structure inside the porous copper joint 120, wherein the central part is a porous copper core structure, the outer part is a copper oxide shell structure, and the central part is wrapped by the outer part.

[0053] Specifically, copper absorbs oxygen atoms to form copper oxide after oxidation. The density of pure copper is 8.9 g / cm 3 , the density of copper oxide is 6g / cm 3 Understandably, since copper oxide has a lower density than pure copper, the volume of the generated copper oxide will increase and occupy more space, thereby filling the pore structure of the porous copper joint, forming a denser structure, and improving the connection strength and service reliability of the porous copper joint.

[0054] See also Figure 6 , Figure 6 It is a comparison chart of the scanning electron microscope morphology, XRD image analysis, shear strength and resistivity of the porous metal sample before and after oxidation treatment in Example 1 provided in the present application.

[0055] Specifically, the scanning electron microscope morphology is the morphology obtained by observing with a scanning electron microscope. The scanning electron microscope (SEM) is an observation method between the transmission electron microscope and the optical microscope. It uses a focused narrow high-energy electron beam to scan the sample, and stimulates various physical information through the interaction between the beam and the material. This information is collected, amplified, and re-imaged to achieve the purpose of characterizing the microscopic morphology of the material. The combination of a scanning electron microscope and other analytical instruments can also perform micro-region composition analysis of the material while observing the microscopic morphology.

[0056] Specifically, XRD is X-ray diffraction technology. When a beam of monochromatic X-rays is incident on a crystal, since the crystal is composed of unit cells of atoms arranged regularly, the distance between these regularly arranged atoms is of the same order of magnitude as the wavelength of the incident X-rays. Therefore, the X-rays scattered by different atoms interfere with each other, and strong X-ray diffraction is generated in certain special directions. The orientation and intensity of the diffraction line in space are closely related to the crystal structure. The diffraction pattern produced by each crystal reflects the atomic distribution law inside the crystal. By performing X-ray diffraction on the material and analyzing its diffraction spectrum, information such as the composition of the material, the structure or morphology of the atoms or molecules inside the material, etc. can be obtained.

[0057] Specifically, shear strength is the ultimate strength generated when the material is sheared. It is numerically equal to the tangential stress value on the shear surface, that is, the ratio of the shear force formed on the shear surface to the damage area. It reflects the maximum ability of the material to resist shear damage. The shear strength can be obtained through shear strength test.

[0058] Specifically, resistivity is a physical quantity used to represent the resistance characteristics of a material. Its numerical value is equal to the resistance value of a conductor made of the material with a length of 1 meter and a cross-sectional area of ​​1 square meter. It reflects the material's property of hindering electric current. Resistivity can be obtained through resistivity testing.

[0059] Through the above characteristics and parameters, the morphology, structure, connection strength and conductivity of porous metal materials can be analyzed and compared.

[0060] In Example 1 provided in the present application, the raw material sample used is a 3 mm × 3 mm copper particle sintered interconnect joint with an average porosity of 28%, an average shear strength of 27.1 MPa, and an average resistivity of 1.0 × 10 -6 The joint is oxidized by high temperature heat treatment to obtain a copper-copper oxide strengthening structure.

[0061] Specifically, the high-temperature heat treatment includes: cleaning the joint to clean the dirt and possible organic residues on the surface to keep the surface and porous structure clean; coating the preset area on the surface of the joint to prevent the preset area from being oxidized; placing the joint in an air oven and heating it to 200°C for 50-100 hours.

[0062] The samples after high temperature heat treatment were observed by scanning electron microscope, EDS, XRD image analysis, shear strength test, resistivity test, and compared with those before high temperature heat treatment. The results are as follows Figure 6As shown. The scanning electron microscope photos of the treated samples show that the original copper sintered porous structure is partially filled with copper oxide. EDS and XRD can detect that copper and copper oxide coexist in the sintered structure. The porosity of the sample is significantly reduced from 28% before treatment to 8.9%. The shear strength continues to increase with the increase of high temperature heat treatment time, from 27.1MPa to 39.0MPa. The resistivity increases to a certain extent, from 1.0×10 -6 Ω rises to 9.6×10 -6 Ω.

[0063] It can be seen that after high-temperature heat treatment, the porosity of the copper particle sintered interconnect joint is significantly reduced, and the shear strength is greatly improved, which can improve the mechanical properties and service reliability of the joint, but the conductive performance is reduced.

[0064] See also Figure 7 , Figure 7 It is a comparison chart of the scanning electron microscope morphology, XRD image analysis, shear strength and resistivity of the porous metal sample before and after oxidation treatment in Example 2 provided in the present application.

[0065] In Example 2 provided in the present application, the raw material sample used is a 3 mm × 3 mm copper particle sintered interconnect joint with an average porosity of 28%, an average shear strength of 27.1 MPa, and an average resistivity of 1.0 × 10 -6 The joint is oxidized by constant temperature and constant humidity heat treatment to obtain a copper-copper oxide reinforced structure.

[0066] Specifically, the constant temperature and constant humidity heat treatment includes: cleaning the joint to clean the dirt and possible organic residues on the surface to keep the surface and porous structure clean; coating the preset area on the surface of the joint to prevent the preset area from being oxidized; placing the joint in an atmospheric environment with a temperature of 85°C and a humidity of 85RH for 50-100 hours.

[0067] The samples after constant temperature and humidity heat treatment were observed by scanning electron microscope, EDS, XRD image analysis, shear strength test, resistivity test, and compared with those before constant temperature and humidity heat treatment. The results are as follows Figure 7 The scanning electron microscope photos of the treated samples show that an oxide film has grown on the surface of the original copper sintered porous structure. EDS and XRD can detect that copper and copper oxide coexist in the sintered structure. The porosity of the sample has decreased to a certain extent, from 28% to 20.1%. The shear strength continues to increase with the increase of the constant temperature and constant humidity heat treatment time, from 27.1MPa to 33.4MPa. The resistivity has not increased significantly, from 1.0×10 -6 Ω slightly increased to 1.6×10 -6 Ω.

[0068] It can be seen that after constant temperature and constant humidity heat treatment, the porosity of the copper particle sintered interconnect joint is reduced to a certain extent, and the shear strength is improved to a certain extent, which can improve the mechanical properties and service reliability of the joint, and at the same time has almost no effect on its conductive properties.

[0069] See also Figure 8 , Figure 8 It is a comparison diagram of the scanning electron microscope morphology and shear strength of the porous metal sample after oxidation treatment and the original porous metal sample in Example 3 provided in the present application before and after the device is formed into a power cycle for 1000 times.

[0070] In Example 3 provided in the present application, the raw material sample used was a 2.7 mm×3.4 mm copper particle sintered interconnect joint with an average porosity of 20% and an average shear strength of 34 MPa. The power cycle was set to be performed in two groups separately.

[0071] One group of samples was not treated, and SiC-MOSFET chips of the same size were connected to the DBC substrate to form a device, and then the service reliability was evaluated by 1000 power cycles (40℃-175℃); the other group of samples was oxidized by high-temperature heat treatment, specifically heating to 200℃ in the atmosphere for 100 hours. After the high-temperature heat treatment, the samples were then connected to SiC-MOSFET chips of the same size to the DBC substrate to form a device, and then the service reliability was evaluated by 1000 power cycles (40℃-175℃).

[0072] The samples after power cycling were observed by scanning electron microscopy and shear strength tested, and compared with those before power cycling. The results are as follows: Figure 8 As shown. Among them, after 1000 power cycles, the scanning electron microscope photos of the original sample showed that there were many cracks inside it, and the shear strength also dropped significantly; after 1000 power cycles of the oxidized sample, the scanning electron microscope photos showed that there were fewer cracks inside it, and the shear strength did not drop significantly. Further comparison shows that the shear strength of the oxidized sample is higher than that of the original sample before and after the power cycle. It can be seen that oxidation treatment of copper particle sintered interconnects can significantly improve their service reliability in practical applications.

[0073] See also Fig. 9 , Fig. 9 This is a scanning electron microscope morphology image of the porous metal sample after non-oxidation treatment in Comparative Example 1 provided in the present application.

[0074] In Comparative Example 1 provided in the present application, the raw material sample used is a 3 mm × 3 mm copper particle sintered interconnect joint with an average porosity of 28%, an average shear strength of 27.1 MPa, and an average resistivity of 1.1 × 10 -6 Ω, the joint was subjected to non-oxidative treatment to obtain a comparative sample.

[0075] Specifically, the non-oxidative treatment of the joint includes: cleaning the joint to clean the dirt and possible organic residues on the surface to keep the surface and porous structure clean; placing the joint in a vacuum environment, heating it to 200° C., and treating it for 50-100 hours.

[0076] The non-oxidized comparative samples were observed by scanning electron microscopy, EDS, XRD image analysis, shear strength test, resistivity test, and the scanning electron microscopy morphology was obtained as shown in the figure. Fig. 9 The scanning electron microscope photos of the comparison samples show that the original copper sintered porous structure and metal phase structure have not changed much; at the same time, the shear strength of the comparison sample is 28MPa, the porosity is 27.6%, and the resistivity is 0.9×10 -6 Ω, which has not changed much compared with the original samples.

[0077] It can be seen that non-oxidation treatment of copper particle sintered interconnects cannot change their structure and properties. On the contrary, oxidation treatment of copper particle sintered interconnects can reduce their porosity and increase their strength, thereby improving their mechanical properties and service reliability.

[0078] The above description is only an implementation method of the present application, and does not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made according to the description and drawings of the present application, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A method for preparing a composite material, characterized in that: Sintering the copper particles or the porous copper film to obtain a porous metal material, wherein the porous metal material includes a plurality of pore structures; Performing a cleaning operation on the porous metal material; A predetermined area on the surface of the porous metal material is subjected to a coating treatment to prevent the predetermined area from being subjected to an oxidation treatment; the composite material is used to connect a substrate and a semiconductor device in a semiconductor packaging structure; The porous metal material is subjected to at least one of high-temperature heat treatment, constant temperature and constant humidity heat treatment, and oxidative plasma implantation treatment to form a metal oxide shell structure on the inner wall of the pore structure; wherein the temperature range of the high-temperature heat treatment is 150-250°C, and the treatment time is 10-100 hours; wherein the metal oxide includes at least one of copper oxide or cuprous oxide.

2. The method according to claim 1, characterized in that: The copper content of the porous metal material is greater than 90%, and the porosity of the porous metal material is greater than 10%.

3. The method according to claim 1, characterized in that The composite material includes a central part and an outer layer part wrapping the central part, and the inner wall of the pore structure of the outer layer part includes the metal oxide shell structure.

4. A semiconductor packaging structure, characterized in that: The semiconductor packaging structure comprises: substrate; A semiconductor device is disposed on the substrate; A joint is arranged between the substrate and the semiconductor device and is used to connect the substrate and the semiconductor device. The joint is a composite material made by the method according to any one of claims 1 to 3.