A U-shaped hollow fiber pervaporation membrane module and preparation method thereof
By designing the U-shaped hollow fiber structure and vacuum-assisted impregnation lifting method to form a double-layer separation layer, the stability of the hollow fiber membrane under high temperature and high-speed fluid erosion is solved, and the permeability and vaporization separation performance and stability are significantly improved.
Patent Information
- Application Number
- CN202111390339.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-11-22
AI Technical Summary
Hollow fiber membranes are prone to tensile deformation during high-temperature environments and when flushing high-speed fluids, resulting in degradation of component short circuits and separation performance. In addition, traditional straight hollow fiber membranes are insufficient to deal with wall shear stress during high-speed fluids.
The permeable vaporization film with a U-shaped hollow fiber structure is adopted, and an ultra-thin and dense separation layer with a double-layer structure is formed on the surface of the film through a vacuum-assisted impregnation lifting method. The ends of the U-shaped structure are supported by nuts to ensure the firm deposition of the separation layer and Density.
The stable operation of the membrane is achieved under a high temperature and high-speed fluid erosion environment, and the permeability and vaporization performance of organic matter dehydration, organic matter removal from water and organic matter-organic separation, extend the end-sealing curing time, and improve the separation performance.
Smart Images

Figure HDA0003367859100000011 
Figure HDA0003367859100000012 
Figure HDA0003367859100000013
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a U-shaped hollow fiber pervaporation membrane by a vacuum-assisted impregnation and pulling method and application thereof, belonging to the technical field of membrane separation. Background Art
[0002] Pervaporation is a separation process in which a liquid contacts the feed side of a semipermeable membrane and the steam flows out of the permeate side of the membrane through a vacuum or scavenging process to generate a chemical potential difference as a driving force. The separation characteristics of the pervaporation process depend on the preferential adsorption and diffusion of components in the membrane. Therefore, compared with conventional distillation processes, the pervaporation process only requires latent heat of evaporation, which can overcome the limitations of thermodynamic vapor-liquid equilibrium and consume less energy. At present, most pervaporation membranes used for preferential alcohol permeation, preferential water permeation, and organic-organic separation are flat membranes. Compared with flat membranes, hollow fiber membranes have the advantages of high packing density and low component price.
[0003] However, it is difficult to prepare an ultra-thin, dense and uniform separation layer on the surface of the hollow fiber membrane, and as the packing density of the hollow fiber membrane increases in the module, the flow rate of the feed liquid on the membrane surface decreases, and the wall shear force on the membrane surface decreases, resulting in an increase in the concentration polarization layer, which reduces the separation performance; the traditional straight hollow fiber membrane is capped and solidified at both ends of the shell, and when it is flushed by high-speed fluid, its ability to cope with wall shear stress is low, thereby causing the module to short-circuit. Based on this, the present invention prepares a hollow fiber pervaporation membrane with a U-shaped structure, and uses its structural characteristics to solve the problems of being flushed by high-speed fluid, tensile deformation caused by high-temperature test environment, increasing the disturbance between the fluid and the curved membrane to create a better fluid morphology, and reducing the long end-capping curing time. The ultra-thin, dense and uniform separation layer is prepared on the membrane surface by the immersion-pulling method, which can be used for dehydration of organic matter, removal of organic matter from water, and organic-organic separation. Summary of the invention
[0004] The purpose of the present invention is to prepare a U-shaped hollow fiber composite membrane that can stably operate for pervaporation, and solve the problems that the hollow fiber membrane is subjected to tensile deformation under high temperature environment and high-speed fluid flushing, thereby causing component short circuit and degradation of separation membrane performance. The composite membrane prepared by the method has good separation performance and stability in the pervaporation process of dehydrating organic matter, removing organic matter from water, and separating organic matter from organic matter.
[0005] The object of the present invention is achieved through the following technical solutions:
[0006] A U-shaped hollow fiber pervaporation membrane assembly, characterized in that the hollow fiber membrane is a U-shaped structure as a whole, the U-shaped structure opens upward, the two ends of the upper part of the U-shaped structure are fixed in parallel with a gap in the middle; a separation layer is provided on the outer surface of the entire hollow fiber membrane, so that the hollow fiber membrane forms a double-layer structure; nuts are used as supports for the two ends of the upper part of the U-shaped structure, and the two ends pass through the hole in the center of the nut in parallel; the two ends of the U-shaped hollow fiber pervaporation membrane are sealed and connected to the suction port on the upper end cover of the shell in a detachable manner; the lower part of the U-shaped structure is naturally located at the bottom inside the shell, a discharge port is provided on the upper side of the shell, and a feed port is provided at the bottom of the shell.
[0007] Furthermore, except for the two ends of the upper part of the U-shaped structure which are fixed in parallel, the other parts are free and not fixed or suspended, and the hollow fiber membranes are not in contact with each other.
[0008] The separation layer is selected from a membrane layer that preferentially permeates alcohol, a membrane layer that preferentially permeates water, or a membrane layer with organic-organic separation performance. The separation layer is formed on the surface of the hollow fiber membrane by a vacuum-assisted impregnation and pulling method.
[0009] The hollow fiber porous base membrane is a hollow fiber porous base membrane, which is an organic membrane selected from polyvinylidene fluoride, polysulfone, polyacrylonitrile, polyethersulfone, polytetrafluoroethylene, etc.;
[0010] The membrane with preferential alcohol permeability is selected from polyetheramide, polydimethylsiloxane, polytrimethylsilyl propyne and the like;
[0011] The membrane with preferential water permeability is selected from the group consisting of polyvinyl alcohol, polyelectrolyte complex, polyamide and polyimide membranes;
[0012] The membrane with organic-organic separation performance is selected from polyetheramide, polyurethane and other membranes.
[0013] The above-mentioned method for preparing the U-shaped hollow fiber membrane comprises the following steps:
[0014] (1) Folding the two ends of the hollow fiber porous base membrane in half, controlling the curvature of the base membrane, and shaping it with hot melt adhesive to form a U-shaped hollow fiber membrane;
[0015] (2) Use epoxy resin to bond and fix the two ends of the base film and cure for 2-5 hours;
[0016] (3) A vacuum-assisted impregnation and pulling method is used to coat the surface of the hollow fiber base membrane with a membrane material having preferential alcohol permeability, a membrane material having preferential water permeability, or a membrane material having organic-organic separation performance. During the impregnation, a vacuum is drawn at the end to make the separation layer more firmly deposited on the surface of the support, thereby improving the compactness of the membrane. During the pulling process, the end side is kept vacuumed to accelerate the volatilization of the solvent;
[0017] (4) Hang the hollow fiber membrane coated in step (3) in an oven and heat and dry it.
[0018] Preferably, when placed in the oven in step (4), the upper end is fixed with a clip so that the membrane filaments do not contact each other.
[0019] The U-shaped hollow fiber pervaporation composite membrane and its components prepared by the present invention are simple to operate and can effectively solve the problems of component short circuit, decreased membrane separation performance, long end-capping curing time, etc. due to the impact force generated by the high-speed fluid scouring of the hollow fiber fixed at both ends in a straight line in the component. At the same time, a dense and uniform ultra-thin separation layer is formed on the membrane surface through a vacuum-assisted impregnation and pulling method, thereby obtaining a higher pervaporation separation performance, and is expected to be widely used in the actual industrial field. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of a U-shaped hollow fiber pervaporation membrane of the present application;
[0021] Figure 2 It is a schematic diagram of the cross-sectional structure of the diameter surface;
[0022] Figure 3 This is the appearance of the U-shaped hollow fiber pervaporation membrane prepared in the example.
[0023] 1. U-shaped hollow fiber pervaporation membrane; 2. Hollow fiber membrane; 3. Separation layer.
[0024] Figure 4 It is a structural diagram of a U-shaped hollow fiber pervaporation membrane module;
[0025] 4. Feed inlet, 5. Shell, 6. Discharge outlet, 7. Suction outlet. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is described below with specific embodiments, but the protection scope of the present invention is not limited thereto: In the following embodiments, the two ends of the hollow fiber porous base membrane are first folded in half, the curvature of the base membrane is controlled, and hot melt adhesive is used to shape the hollow fiber membrane to form a U-shaped structure; the two ends of the base membrane are bonded and fixed with epoxy resin, and cured for 2-5 hours;
[0027] Example 1
[0028] Separation layer casting liquid formula: polyetheramide 8wt%, solvent is n-butanol. The base membrane is polyvinylidene fluoride hollow fiber membrane. The separation layer is coated on the hollow fiber membrane using a lifting machine, and the operating parameters of the lifting machine are set as follows: descending speed 1cm / s, residence time 180s, rising speed 0.7cm / s, vacuum degree -0.1MPa. The upper part is fixed on the lifting machine and connected to the vacuum pump, and the lower part vertically enters the casting liquid downward. After the impregnation is completed, it is pulled out of the casting liquid and placed in an oven for drying.
[0029] The performance of the U-shaped hollow fiber pervaporation membrane obtained above was tested. Test conditions: total length of membrane fiber 30 cm, diameter 0.12 cm, module shell volume 500 cm 3 , the feed fluid flow rate is 0.9m / s, the fluid flow direction is parallel to the U-shaped structure plane of the membrane filament, and the feed liquid directly flushes the membrane filament. The pressure on the downstream side of the membrane is 100Pa, the feed liquid is a 1wt% butanol / water mixed solution, the feed temperature is 60℃, and the feed flow rate is 60L / h. Test results: butanol / water separation factor is 17.39, flux is 3029g / (m 2 h).
[0030] Example 2
[0031] Separation layer casting liquid formula: polyetheramide 10wt%, solvent is n-butanol. The base membrane is a polysulfone hollow fiber membrane. The separation layer is coated on the hollow fiber membrane using a lifting machine, and the operating parameters of the lifting machine are set as follows: descending speed 1cm / s, residence time 180s, rising speed 0.7cm / s, vacuum degree -0.1MPa. The upper part is fixed on the lifting machine and connected to the vacuum pump, and the lower part vertically enters the casting liquid downward. After the impregnation is completed, it is pulled out of the casting liquid and placed in an oven for drying.
[0032] The performance of the U-shaped hollow fiber pervaporation membrane obtained above was tested. Test conditions: total length of membrane fiber 30 cm, diameter 0.12 cm, module shell volume 500 cm 3 , the feed fluid flow rate is 0.9m / s, the fluid flow direction is parallel to the U-shaped structure plane of the membrane filament, and the feed liquid directly flushes the membrane filament. The pressure on the downstream side of the membrane is 100Pa, the feed liquid is a 1wt% butanol / water mixed solution, and the feed temperature is 60℃. Test results: butanol / water separation factor is 17.1, flux is 3107g / (m 2 h).
[0033] Example 3
[0034] Separation layer casting liquid formula: polydimethylsiloxane 6wt%, solvent is n-butanol. The base membrane is a polyethersulfone hollow fiber membrane. The separation layer is coated on the hollow fiber membrane using a lifting machine, and the operating parameters of the lifting machine are set as follows: descending speed 1cm / s, residence time 180s, rising speed 0.7cm / s, vacuum degree -0.1MPa. The upper part is fixed on the lifting machine and connected to the vacuum pump, and the lower part vertically enters the casting liquid downward. After the impregnation is completed, it is pulled out of the casting liquid and placed in an oven for drying.
[0035] The performance of the U-shaped hollow fiber pervaporation membrane obtained above was tested. Test conditions: total length of membrane fiber 30 cm, diameter 0.12 cm, module shell volume 500 cm 3 , the feed fluid flow rate is 0.9m / s, the fluid flow direction is parallel to the U-shaped structure plane of the membrane filament, and the feed liquid directly flushes the membrane filament. The pressure on the downstream side of the membrane is 100Pa, the feed liquid is a 1wt% butanol / water mixed solution, and the feed temperature is 60℃. Test results: butanol / water separation factor is 17.87, flux is 2956g / (m 2 h).
[0036] Example 4
[0037] Separation layer casting liquid formula: polydimethylsiloxane 8wt%, solvent is n-butanol. The base membrane is polyacrylonitrile hollow fiber membrane. The separation layer is coated on the hollow fiber membrane using a lifting machine, and the operating parameters of the lifting machine are set as follows: descending speed 1cm / s, residence time 180s, rising speed 0.7cm / s, vacuum degree -0.1MPa. The upper part is fixed on the lifting machine and connected to the vacuum pump, and the lower part vertically enters the casting liquid downward. After the impregnation is completed, it is pulled out of the casting liquid and placed in an oven for drying.
[0038] The performance of the U-shaped hollow fiber pervaporation membrane obtained above was tested. Test conditions: total length of membrane fiber 30 cm, diameter 0.12 cm, module shell volume 500 cm 3 , the feed fluid flow rate is 0.9m / s, the fluid flow direction is parallel to the U-shaped structure plane of the membrane filament, and the feed liquid directly flushes the membrane filament. The pressure on the downstream side of the membrane is 100Pa, the feed liquid is a 1wt% butanol / water mixed solution, and the feed temperature is 60℃. Test results: butanol / water separation factor is 17.66, flux is 3056g / (m 2 h).
[0039] Example 5
[0040] Separation layer casting liquid formula: polytrimethylsilyl propyne 7wt%, solvent is n-butanol. The base membrane is a polyetheramide hollow fiber membrane. The separation layer is coated on the hollow fiber membrane using a lifting machine, and the operating parameters of the lifting machine are set as follows: descending speed 1cm / s, residence time 180s, rising speed 0.7cm / s, vacuum degree -0.1MPa. The upper part is fixed on the lifting machine and connected to the vacuum pump, and the lower part vertically enters the casting liquid downward. After the impregnation is completed, it is pulled out of the casting liquid and placed in an oven for drying.
[0041] The performance of the U-shaped hollow fiber pervaporation membrane obtained above was tested. Test conditions: total length of membrane fiber 30 cm, diameter 0.12 cm, module shell volume 500 cm 3 , the feed fluid flow rate is 0.9m / s, the fluid flow direction is parallel to the U-shaped structure plane of the membrane filaments, and the feed liquid directly flushes the membrane filaments. The pressure on the downstream side of the membrane is 100Pa, the feed liquid is a 1wt% butanol / water mixed solution, and the feed temperature is 60℃. Test results: butanol / water separation factor is 16.89, flux is 4156g / (m 2 h).
[0042] Example 6
[0043] Separation layer casting liquid formula: polytrimethylsilyl propyne 10wt%, solvent is n-butanol. The base membrane is polyacrylonitrile hollow fiber membrane. The separation layer is coated on the hollow fiber membrane using a lifting machine, and the operating parameters of the lifting machine are set as follows: descending speed 1cm / s, residence time 180s, rising speed 0.7cm / s, vacuum degree -0.1MPa. The upper part is fixed on the lifting machine and connected to the vacuum pump, and the lower part vertically enters the casting liquid downward. After the impregnation is completed, it is pulled out of the casting liquid and placed in an oven for drying.
[0044] The performance of the U-shaped hollow fiber pervaporation membrane obtained above was tested. Test conditions: total length of membrane fiber 30 cm, diameter 0.12 cm, module shell volume 500 cm 3 , the feed fluid flow rate is 0.9m / s, the fluid flow direction is parallel to the U-shaped structure plane of the membrane filament, and the feed liquid directly flushes the membrane filament. The pressure on the downstream side of the membrane is 100Pa, the feed liquid is a 1wt% butanol / water mixed solution, and the feed temperature is 60℃. Test results: butanol / water separation factor is 17.79, flux is 4013g / (m 2 h).
[0045] Example 7
[0046] Separation layer casting liquid formula: polyvinyl alcohol 10wt%, solvent is water. The separation layer is coated on the hollow fiber membrane using a lifting machine, and the lifting machine operating parameters are set as follows: descending speed 1cm / s, residence time 180s, ascending speed 0.7cm / s, vacuum degree -0.1MPa. The upper part is fixed on the lifting machine and connected to the vacuum pump, and the lower part vertically enters the casting liquid downward. After the impregnation is completed, it is pulled out of the casting liquid and placed in an oven for drying.
[0047] The performance of the U-shaped hollow fiber pervaporation membrane obtained above was tested. Test conditions: total length of membrane fiber 30 cm, diameter 0.12 cm, module shell volume 500 cm 3 , the fluid flow direction is parallel to the U-shaped structure plane of the membrane filament, and the feed liquid directly flushes the membrane filament. The pressure on the downstream side of the membrane is 100Pa, the feed liquid is a 90wt% ethanol / water mixed solution, the feed temperature is 60℃, and the feed fluid flow rate is 0.9m / s. Test results: ethanol / water separation factor 1011, flux 350g / (m 2 h).
[0048] Example 8
[0049] Separation layer casting liquid formula: The casting liquid is a polyelectrolyte complex, and the solvent is water. The separation layer is coated on the hollow fiber membrane using a lifting machine, and the operating parameters of the lifting machine are set as follows: descending speed 1cm / s, residence time 180s, rising speed 0.7cm / s, vacuum degree -0.1MPa. The upper part is fixed on the lifting machine and connected to the vacuum pump, and the lower part vertically enters the casting liquid downward. After the impregnation is completed, it is pulled out of the casting liquid and placed in an oven for drying.
[0050] The performance of the U-shaped hollow fiber pervaporation membrane obtained above was tested. Test conditions: total length of membrane fiber 30 cm, diameter 0.12 cm, module shell volume 500 cm 3 , the fluid flow direction is parallel to the U-shaped structure plane of the membrane filament, and the feed liquid directly flushes the membrane filament. The pressure on the downstream side of the membrane is 100Pa, the feed liquid is a 90wt% ethanol / water mixed solution, and the feed temperature is 60℃. Test results: ethanol / water separation factor 2116, flux 2350g / (m 2 h).
[0051] Example 9
[0052] Separation layer casting liquid formula: The casting liquid is polyetheramide, and the solvent is butanol. The separation layer is coated on the hollow fiber membrane using a lifting machine, and the lifting machine operating parameters are set as follows: descending speed 1cm / s, residence time 180s, rising speed 0.7cm / s, vacuum degree -0.09MPa. The upper part is fixed on the lifting machine and connected to the vacuum pump, and the lower part vertically enters the casting liquid downward. After the impregnation is completed, it is pulled out of the casting liquid and placed in an oven for drying.
[0053] The performance of the U-shaped hollow fiber pervaporation membrane obtained above was tested. Test conditions: total length of membrane fiber 30 cm, diameter 0.12 cm, module shell volume 500 cm 3 , the feed fluid flow rate is 0.9m / s, the fluid flow direction is parallel to the U-shaped structure plane of the membrane, and the feed liquid directly flushes the membrane. The pressure on the downstream side of the membrane is 100Pa, the feed liquid is a 50wt% toluene / isooctane mixed solution, and the feed temperature is 60℃. Test results: Toluene / isooctane separation factor 10, flux 1527g / (m 2 h).
[0054] Example 10
[0055] Separation layer casting liquid formula: The casting liquid is polyetheramide, and the solvent is butanol. The separation layer is coated on the hollow fiber membrane using a lifting machine, and the operating parameters of the lifting machine are set as follows: descending speed 1cm / s, residence time 180s, rising speed 0.7cm / s, vacuum degree -0.08MPa. The upper part is fixed on the lifting machine and connected to the vacuum pump, and the lower part vertically enters the casting liquid downward. After the impregnation is completed, it is pulled out of the casting liquid and placed in an oven for drying.
[0056] The performance of the U-shaped hollow fiber pervaporation membrane obtained above was tested. Test conditions: total length of membrane fiber 30 cm, diameter 0.12 cm, module shell volume 500 cm 3 , the feed fluid flow rate is 0.9m / s, the fluid flow direction is parallel to the U-shaped structure plane of the membrane, and the feed liquid directly flushes the membrane. The pressure on the downstream side of the membrane is 100Pa, the feed liquid is a 50wt% benzene / cyclohexane mixed solution, and the feed temperature is 60℃. Test results: toluene / isooctane separation factor 4.1, flux 127g / (m 2 h).
Claims
1. A method for preparing a U-shaped hollow fiber pervaporation membrane module, characterized in that: The hollow fiber membrane is a U-shaped structure as a whole, with the U-shaped structure opening upward, and the two ends of the upper part of the U-shaped structure are fixed in parallel with a gap in the middle; a separation layer is provided on the outer surface of the entire hollow fiber membrane, so that the hollow fiber membrane forms a double-layer structure; nuts are used as supports at the two ends of the upper part of the U-shaped structure, and the two ends pass through the hole in the center of the nut in parallel; the two ends of the U-shaped hollow fiber pervaporation membrane are sealed and connected to the suction port on the upper end cover of the shell when detachable; the lower part of the U-shaped structure is naturally located at the bottom of the shell, and a discharge port is provided on the upper side of the shell, and a feed port is provided at the bottom of the shell; The U-shaped hollow fiber membrane preparation method comprises the following steps: (1) Folding the two ends of the hollow fiber porous base membrane in half, controlling the curvature of the base membrane, and shaping it with hot melt adhesive to form a U-shaped hollow fiber membrane; (2) Use epoxy resin to bond the two ends of the base film and cure for 2-5 hours; (3) A vacuum-assisted impregnation and pulling method is used to coat the surface of the hollow fiber base membrane with a membrane material having preferential alcohol permeability, a membrane material having preferential water permeability, or a membrane material having organic-organic separation performance. During the impregnation, a vacuum is drawn at the end to make the separation layer more firmly deposited on the surface of the support, thereby improving the density of the membrane. During the pulling process, the end side is kept vacuumed to accelerate the volatilization of the solvent; (4) hanging the coated hollow fiber membrane in step (3) in an oven for heating and drying; When the film is suspended in the oven in step (4), the upper end is fixed with a clip so that the film filaments do not touch each other; The membrane having a preferential alcohol permeability is selected from polyetheramides.
2. The method for preparing a U-shaped hollow fiber pervaporation membrane module according to claim 1, characterized in that: The U-shaped structure has two ends at the upper part which are fixed in parallel, while the rest of the structure is suspended in the air, and the hollow fiber membranes do not contact each other.
3. The method for preparing a U-shaped hollow fiber pervaporation membrane module according to claim 1, characterized in that: The separation layer is selected from a membrane layer that preferentially permeates alcohol, a membrane layer that preferentially permeates water, or a membrane layer with organic-organic separation performance. The separation layer is formed on the surface of the hollow fiber membrane by a vacuum-assisted impregnation and pulling method.
4. The method for preparing a U-shaped hollow fiber pervaporation membrane module according to claim 1, characterized in that: The hollow fiber porous base membrane is a hollow fiber porous base membrane, which is an organic membrane selected from polyvinylidene fluoride, polysulfone, polyacrylonitrile, polyethersulfone, and polytetrafluoroethylene.
5. The method for preparing a U-shaped hollow fiber pervaporation membrane module according to claim 1, characterized in that: The preferentially water permeable membrane is selected from polyvinyl alcohol, polyelectrolyte complex, polyamide and polyimide membranes.
6. The method for preparing a U-shaped hollow fiber pervaporation membrane module according to claim 1, characterized in that: The membrane with organic-organic separation performance is selected from polyetheramide and polyurethane membrane.
Citation Information
Patent Citations
Preparation method for PDMS / PAN pervaporation hollow fiber membrane
CN104138717A
U-shaped hollow fiber pervaporation membrane assembly
CN216498606U
Hollow fiber composite membrane module and method for producing same
WO2018003949A1