A multi-layer high temperature resistant fluorine-containing release film and preparation method thereof

Through the multi-layer coextrusion casting technology, the structural layer composed of polyester polymer and fluororesin and the fluorine-containing resin release layer are used to solve the problem of insufficient ductility and temperature resistance of the existing release film base material. The high temperature and tensile resistance of the bondless layer are achieved, the process is simplified and pollution is avoided.

CN114311915BActive Publication Date: 2024-11-19SHANDONG DONGYUE POLYMER MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111523035.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-13
Publication Date
2024-11-19
Estimated Expiration
2041-12-13

AI Technical Summary

Technical Problem

The existing release film substrates have insufficient ductility, insufficient temperature resistance, easy to contaminate electronic devices, and poor compatibility between the fluorine-containing resin layer and the polyester layer, and the adhesive layer is required as a transition layer, which limits its application.

Method used

A three-layer release film is prepared by multi-layer coextrusion casting. The structural layer is composed of polyester polymer, fluororesin and compatibilizer. The first and second release layers are the same or different fluororesin. By mechanical The mixing of the structural layer pellets avoids the use of adhesives and achieves high temperature and tensile resistance without the need for an adhesive layer.

Benefits of technology

A release film with excellent high temperature resistance and tensile resistance is realized, which simplifies the molding process, avoids binder contamination, and improves the application of the film material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of release films, and in particular refers to a multi-layer high-temperature resistant fluorine-containing release film and a preparation method thereof. The fluorine-containing release film of the present invention comprises a first release layer, a structural layer and a second release layer, and the release film is made by a multi-layer co-extrusion casting method, and the structural layer material comprises a polyester polymer, a fluorine resin and a functional additive, and the two release layers comprise a fluorine-containing resin. The release layer of the present invention has good high temperature resistance and tensile strength, and there is no adhesive between the structural layer and the release layer. The preparation process is simple, and the problem of contamination of the release layer by the adhesive in the prior art is avoided, so as to achieve the technical effects of high temperature resistance, tensile resistance and simple molding process of the release film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thin films, and in particular relates to a multi-layer high-temperature resistant fluorine-containing release film and a preparation method thereof. Background Art

[0002] With the development of the information age, electronic devices are becoming more and more functional and diversified, and the requirements for release films are becoming higher and higher. In the production process of electronic accessories, release films with excellent performance are indispensable.

[0003] Chinese patent CN211106113 (application number 201921296084.2) provides an environmentally friendly PET release film, including a PET base layer, two anti-stretching layers, two wear-resistant layers, and a PET release layer, but the temperature resistance and tensile resistance are insufficient. Ordinary release film substrates are generally PP, PE, PET, etc., and the release film is prepared by plasma treatment, fluorine treatment, or coating the surface of the substrate with a silicone release agent. It usually has the disadvantages of insufficient elongation, insufficient temperature resistance, and easy contamination of electronic devices. Chinese patent CN106042553A (application number 201610408694.1) provides a high temperature resistant release film, whose release layer is polymethylpentene and the support layer is a polyolefin material, but the elastic modulus of the film is too high, and it is easy to produce wrinkles during the thermoforming of electronic devices. Fluorine-containing resins usually have good temperature resistance and excellent tensile properties, and more and more research is being conducted on their application in release films. Chinese patent CN111002667A (application number 201911317773.1) provides a release film constructed of fluorine-containing resin and polyester material, including a first raw material, a second raw material and a third raw material. The first raw material is at least one of polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer, polyvinylidene fluoride and polyvinyl fluoride, the second raw material is a bonding material, and the third raw material is a polyester material. An ABC three-layer release film with a structure of a release layer-bonding layer-support layer is obtained by co-extrusion of three extruders. The release film has good high temperature resistance and low thermal shrinkage, but a bonding material is used between the first layer and the third layer, and a lamination step is required. The prepared release film has insufficient tensile properties, which limits its application in the field of membrane materials.

[0004] In summary, ordinary release film substrates have disadvantages such as insufficient elongation, insufficient temperature resistance, and poor practicality. In addition, the compatibility between the fluorine-containing resin layer and the polyester layer in the release film is generally poor, and an adhesive layer is often required as a transition layer. The adhesive layer is easy to remain on the release layer, and when used in the production and processing of electronic devices, it may cause pollution to the electronic devices. Therefore, in order to meet practical applications, it is necessary to develop a release film that does not require an adhesive layer and has good tensile properties, high temperature resistance and environmental protection performance. Summary of the invention

[0005] In view of the above problems, the present invention provides a high temperature resistant fluorine-containing release film and a preparation method thereof. The release film comprises a first release layer, a structural layer and a second release layer from bottom to top. The release film is made by a multi-layer co-extrusion casting method. The structural layer material comprises a polyester polymer, a fluororesin and a functional additive. The two release layer materials are the same or different, and are both fluorine-containing resins. The release layer of the present invention has good high temperature resistance and tensile strength. No adhesive is contained between the structural layer and the release layer. The preparation process is simple, and the problem of adhesive contamination of the release layer in the prior art is avoided, thereby achieving the technical effects of high temperature resistance, tensile resistance and simple molding process of the release film.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention provides a multi-layer high-temperature resistant fluorine-containing release film, characterized in that it comprises a first release layer, a structural layer and a second release layer, wherein the structural layer is sandwiched between the first release layer and the second release layer, and the first release layer, the structural layer and the second release layer are made into a three-layer release film by a multi-layer co-extrusion casting method; the total thickness of the release film is 60-100 μm, the thickness ratio of the structural layer is 60-75%, the thickness ratio of the first release layer is 10-25%, and the thickness ratio of the second release layer is 10-25%; the structural layer comprises the following components by mass fraction: 76-87 wt% of a polyester polymer, 12-19 wt% of a fluororesin and 1-5 wt% of a compatibilizer, and the first release layer and the second release layer contain the same or different fluororesins.

[0008] The content of fluororesin in the structural layer can be selected according to the viscosity of the mixed resin formed by mixing and granulating it with the polyester polymer in the molten state. The content of fluororesin in the structural layer should be in the range of 12%-19%. Too large a proportion will lead to a decrease in the tensile strength of the structural layer after the mixed resin is melt-extruded and a decrease in the ductility; too low a fluororesin content will lead to poor adhesion between the structural layer and the first release layer, and between the structural layer and the second release layer.

[0009] Preferably, the polyester polymer includes one or a mixture of polycarbonate (PC), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polyethylene terephthalate (PET), and preferably, the polyester polymer is PC or PET.

[0010] Preferably, the polyester polymer has a melt index of 5-20 g / 10 min, a tensile strength of 40-70 MPa, and a tensile modulus of 400-800 MPa.

[0011] Preferably, the fluororesin is a perfluoroethylene-propylene copolymer (FEP) or an ethylene-tetrafluoroethylene copolymer (ETFE).

[0012] Preferably, the melt index of the fluororesin is 5-20g / 10min, the tensile strength is 20-50MPa, and the tensile modulus is 400-800MPa. Studies have shown that the molecular weight of a polymer is an important factor affecting its melt index, and the larger the polymer molecular weight, the higher the melt index. For ethylene-tetrafluoroethylene polymers, the larger the proportion of tetrafluoroethylene units in ETFE, the larger the melt index of the ETFE polymer. In the present invention, the melt index of the fluororesin is controlled within the range of 5-20g / 10min. Excessive melt index causes processing to become more difficult, and the smoothness and flatness of the molded film decrease, and processing costs increase.

[0013] The melt index measurement method of polyester polymers refers to GB / T 3682-2000, and the test conditions are: test temperature 300℃, nominal load 1.2kg; the melt index measurement method of fluororesin is the same as GB / T 3682-2000, and the test conditions are: test temperature 297℃, nominal load 5kg.

[0014] There is a lack of adhesion between fluororesin and most thermoplastic polymers. The first release layer and the second release layer composed of fluororesin have poor adhesion to the structural layer composed mainly of polyester polymers. Adding a compatibilizer to the structural layer can effectively improve the adhesion between the structural layer and the release layer, and avoid the problem of peeling between the structural layer and the first release layer, and between the structural layer and the second release layer during the shaping, cooling, and pulling processes after molding.

[0015] The compatibilizer includes one or a mixture of cyclic anhydride type, acid anhydride type, epoxy type, and imide-modified acrylic resin. Preferably, the compatibilizer is imide-modified acrylic resin.

[0016] In the presence of the imide-modified acrylic resin, a thermoplastic polyester polymer and a fluororesin are mechanically mixed and granulated at high temperature to obtain a structural layer granule. The tensile strength of the structural layer of the multi-layer high-temperature resistant fluorine-containing release film prepared using the structural layer granule is significantly improved. The compatibilizer is intended to improve the performance of the structural layer by reducing interfacial tension and by improving the interface between the polyester polymer and the fluororesin and the adhesion between the two.

[0017] The present invention also provides a method for preparing a multi-layer high temperature resistant fluorine-containing release film, which is characterized by comprising the following steps:

[0018] (1) The components of the structural layer are weighed according to the mass ratio and mixed in a high-speed mixer, and then melt-blended, extruded, granulated and dried by a twin-screw extruder to obtain structural layer pellets.

[0019] (2) Prepare three extruders A, B, and C, add fluororesin to extruders A and C respectively to extrude the first release layer and the second release layer of the release film, add the pellets in step (1) to extruder B to extrude the structural layer of the release film, the melt extruded by the three-layer extruder enters and is compounded in a casting die, the compounded multi-layer melt is shaped, cooled, pulled, and annealed to prepare a multi-layer high-temperature resistant release film, the thickness is detected and adjusted by an online thickness gauge, the film is trimmed and rolled up to obtain a multi-layer high-temperature resistant release film product.

[0020] Preferably, in the step (1), the blending time is 2-10 min, the extrusion temperature is 270-340° C., the screw speed is 15-80 r / min, and the pelletizing is dried at 100° C. for 8 h.

[0021] Preferably, in step (2), the extruder A has a screw aspect ratio of 20-30, and comprises a barrel with four heating zones, and the barrel temperatures are respectively set to: zone 1 220-340°C, zone 2 230-350°C, zone 3 230-360°C, and zone 4 230-370°C.

[0022] Preferably, in step (2), the screw aspect ratio of the extruder B is 25-30, and it comprises a barrel with four heating zones, and the barrel temperatures are respectively set to: zone 1 210-340°C, zone 2 220-340°C, zone 3 220-350°C, and zone 4 220-350°C.

[0023] Preferably, the process parameters of extruder C in step (2) are set the same as those of extruder A.

[0024] Preferably, the casting die in step (2) is a multi-channel in-mold composite casting die, and the temperature is set to 250-370°C.

[0025] One or more technical solutions provided by the present invention have at least the following technical effects:

[0026] 1. The release film prepared by the present invention has good temperature resistance, excellent tensile properties and is pollution-free.

[0027] 2. The release film prepared by the present invention has a three-layer structure as a whole, does not require an additional adhesive layer and lamination steps, has a simple molding process, has no solvent residue, and will not contaminate electronic devices during use. DETAILED DESCRIPTION

[0028] The following specific examples further illustrate the present invention. The raw materials used in the examples are all commercially available products. The tensile performance test method of the multi-layer high temperature resistant fluorine-containing release film refers to ISO 527-3 2018; the heat shrinkage test method refers to GB / T12027-2004, the heat shrinkage of the ETFE release layer is measured after constant temperature treatment in a 160°C oven for 1 hour, and the heat shrinkage of the FEP release layer is measured after constant temperature treatment in a 210°C oven for 1 hour.

[0029] Example 1

[0030] A multilayer high temperature resistant fluorine-containing release film, the release film comprises a first release layer, a structural layer, and a second release layer from top to bottom. The structural layer comprises the following components by mass fraction: ETFE: 12%; PC: 87%; fluorinated polyimide modified acrylic resin: 1%. The thickness of the structural layer is 36 μm. The first and second release layers are both ETFE layers, and the thickness is 12 μm. The melt index of ETFE is 5 g / 10 min, the tensile strength is 20.0 MPa, and the tensile modulus is 400 MPa. The melt index of PC is 5 g / 10 min, the tensile strength is 40.0 MPa, and the tensile modulus is 400 MPa.

[0031] The preparation steps of the release film are as follows:

[0032] (1) The components of the structural layer were weighed according to the mass ratio and mixed in a high-speed mixer for 4 minutes, and then melt-blended by a twin-screw extruder. The extrusion temperature was controlled at 280°C and the screw speed was 30 r / min. After traction granulation, the mixture was dried at 100°C for 8 hours and sealed for use.

[0033] (2) The extrusion cast film unit used contains three extruders, wherein extruders A and C are used to extrude two layers of outer release films, and extruder B is used to extrude a structural layer film. The melt extruded by the three-layer extruder passes through a multi-channel in-mold composite casting die head. The composite multi-layer melt is subjected to shaping, cooling, pulling, annealing and other steps to prepare a multi-layer high-temperature resistant release film. The thickness is detected and adjusted by an online thickness gauge, and the film is trimmed and rolled up to obtain a multi-layer high-temperature resistant release film product.

[0034] The preparation process parameters of the release film are as follows:

[0035] A extruder: The extruder for processing ETFE resin uses a screw with an aspect ratio of 30 and a barrel with four heating zones. The temperature is set to 260°C for zone 1, 270°C for zone 2, 280°C for zone 3, and 290°C for zone 4. The thickness of the first release layer is adjusted to 12μm.

[0036] B Extruder: The extruder for processing the structural layer mixture has a screw with an aspect ratio of 25 and a barrel with four heating zones. The temperature is set at 240°C for zone 1, 250°C for zone 2, 260°C for zone 3, and 270°C for zone 4. The extrusion thickness is adjusted to 36μm.

[0037] C extruder: The process parameters are set the same as those of A extruder.

[0038] Multi-channel die: The temperature was set to 295°C. After each section of the equipment reached the set temperature and was kept warm for 0.5h, the feeding production began. The mechanical properties of each layer of the obtained release film are shown in Table 1.

[0039] Example 2

[0040] A multilayer high temperature resistant fluorine-containing release film is as in Example 1, except that the structural layer includes the following components by mass fraction: ETFE: 19%; PC: 76%; fluorinated polyimide modified acrylic resin: 5%. The melt index of ETFE is 20g / 10min, the tensile strength is 50.0MPa, and the tensile modulus is 800MPa. The melt index of PC is 20g / 10min, the tensile strength is 70.0MPa, and the tensile modulus is 800MPa. The preparation steps of the release film of this embodiment are the same as those of Example 1, and the mechanical property test results of each layer of the obtained release film are shown in Table 1.

[0041] Example 3

[0042] A multilayer high temperature resistant fluorine-containing release film, the release film comprises a first release layer, a structural layer, and a second release layer from top to bottom. The structural layer comprises the following components by mass fraction: 5% fluororesin ETFE; 80% polyethylene terephthalate (PET); 5% fluorinated polyimide modified acrylic resin. The thickness of the structural layer is 70 μm. The first and second release layers are both ETFE layers, and the thickness is 15 μm. The melt index of ETFE is 10 g / 10 min, the tensile strength is 35.0 MPa, and the tensile modulus is 430 MPa. The melt index of PET is 10 g / 10 min, the tensile strength is 40.0 MPa, and the tensile modulus is 450 MPa.

[0043] The preparation steps of the release film are as follows:

[0044] (1) The components of the structural layer were weighed according to the above mass ratio and mixed in a high-speed mixer for 4 minutes. The mixture was then melt-blended by a twin-screw extruder. The extrusion temperature was controlled at 270°C and the screw speed was 30 r / min. After granulation, the mixture was dried at 100°C for 8 hours and sealed for later use.

[0045] (2) The extrusion cast film unit used contains three extruders, wherein extruders A and C are used to extrude the first and second release films, and extruder B is used to extrude the structural layer film. The melt extruded by the three-layer extruder passes through a multi-channel in-mold composite casting die head. The composite multi-layer melt is subjected to shaping, cooling, pulling, annealing and other steps to prepare a multi-layer high-temperature resistant release film. The thickness is detected and adjusted by an online thickness gauge, and the film is trimmed and rolled up to obtain a multi-layer high-temperature resistant release film product.

[0046] The process parameters for preparing the release film are as follows:

[0047] A extruder: The extruder for processing ETFE resin uses a screw with an aspect ratio of 30 and a barrel with four heating zones. The temperature is set at 260°C for zone 1, 270°C for zone 2, 280°C for zone 3, and 290°C for zone 4. The film thickness is adjusted to 15μm.

[0048] B Extruder: The extruder for processing the structural layer mixture has a screw with an aspect ratio of 25 and a barrel with four heating zones. The temperature is set at 230°C for zone 1, 240°C for zone 2, 250°C for zone 3, and 260°C for zone 4. The film thickness is adjusted to 70μm.

[0049] C extruder: The process parameters are set the same as those of A extruder.

[0050] Multi-channel die: The temperature was set to 295°C. After each section of the equipment reached the set temperature and was kept warm for 0.5h, the feeding and production began. The mechanical properties test results of each layer of the obtained release film are shown in Table 1.

[0051] Example 4

[0052] A multi-layer high temperature resistant fluorine-containing release film and a preparation method thereof, wherein the release film comprises a first release layer, a structural layer, and a second release layer from top to bottom. The structural layer is a mixed layer of 12% fluororesin FEP, 85% polycarbonate (PC), and 3% fluoropolyimide modified acrylic resin, with a thickness of 70 μm. The first release layer and the second release layer are both FEP resin layers, with thicknesses of 10 μm and 15 μm, respectively. The melt index of the fluororesin FEP is 10 g / 10 min, the tensile strength is 35.0 MPa, and the tensile modulus is 430 MPa. The melt index of PC is 10 g / 10 min, the tensile strength is 40.0 MPa, and the tensile modulus is 450 MPa.

[0053] The preparation method steps are as follows:

[0054] (1) The components of the structural layer, namely, 12% fluororesin FEP, 85% polycarbonate (PC), and 3% fluoropolyimide-modified acrylic resin, were weighed according to the mass ratio and mixed in a high-speed mixer for 4 minutes. The mixture was then melt-blended in a twin-screw extruder with the extrusion temperature controlled at 340°C and the screw speed at 30 r / min. After granulation, the mixture was dried at 100°C for 8 hours and sealed for later use.

[0055] (2) The extrusion cast film unit used contains three extruders, wherein extruders A and C are used to extrude the first and second release films, and extruder B is used to extrude the structural layer film. The melt extruded by the three-layer extruder passes through a multi-channel in-mold composite casting die head. The composite multi-layer melt is subjected to shaping, cooling, pulling, annealing and other steps to prepare a multi-layer high-temperature resistant release film. The thickness is detected and adjusted by an online thickness gauge, and the film is trimmed and rolled up to obtain a multi-layer high-temperature resistant release film product.

[0056] The process parameters for preparing the release film are as follows:

[0057] A extruder: The extruder for processing FEP resin uses a screw with an aspect ratio of 30 and a barrel with four heating zones. The temperature is set to 330°C in zone 1, 340°C in zone 2, 350°C in zone 3, and 360°C in zone 4. The film thickness is adjusted to 10 μm.

[0058] B Extruder: The extruder for processing the structural layer mixture has a screw with an aspect ratio of 25 and a barrel with four heating zones. The temperature is set at 240°C for zone 1, 250°C for zone 2, 260°C for zone 3, and 270°C for zone 4. The film thickness is adjusted to 70μm.

[0059] C extruder: The process parameters are set the same as those of A extruder, with a thickness of 15 μm.

[0060] Multi-channel die head: The temperature is set to 360°C. After each section of the equipment reaches the set temperature and is kept warm for 0.5h, feed production begins.

[0061] The mechanical property test results of each layer of the obtained release film are shown in Table 1.

[0062] Table 1. Mechanical properties of the structural layer, the first release layer, and the second release layer of the release film of the embodiment

[0063] project Example 1 Example 2 Example 3 Example 4 Tensile strength of structural layer / MPa 30.8 48.9 28.7 31.2 Tensile strength of the first release layer / MPa 18.5 46.7 36.2 34.7 Second release layer tensile strength / MPa 19.3 47.9 35.4 33.5 Elongation at break of the first release layer / % 267 236 247 146 Elongation at break of the second release layer / % 282 228 254 137 Thermal shrinkage of the first release layer / % 2.2 2.4 2.3 2.1 Thermal shrinkage of the second release layer / % 2.3 2.3 2.1 2.0

[0064] As can be seen from the above table, the release layer raw material of the high temperature resistant fluorine-containing release film prepared by the present invention is ETFE or FEP material, which has excellent heat shrinkage and tensile properties. The release film is a three-layer structure formed by co-extrusion, does not require an additional bonding layer and lamination steps, has a simple molding process, has no solvent residue on the surface of the release layer, and will not pollute electronic devices during use. At the same time, the structural layer uses polyester polymers instead of fluororesin polymers, which reduces the cost of the release film material.

Claims

1. A multi-layer high temperature resistant fluorine-containing release film, characterized in that: It comprises a first release layer, a structural layer and a second release layer, wherein the structural layer is sandwiched between the first release layer and the second release layer, and the first release layer, the structural layer and the second release layer are made into a three-layer release film by a multi-layer co-extrusion casting method; the total thickness of the release film is 60-100 μm, the thickness ratio of the structural layer is 60-75%, the thickness ratio of the first release layer is 10-25%, and the thickness ratio of the second release layer is 10-25%; The structural layer comprises the following components by mass fraction: 76% polycarbonate, 19% ethylene-tetrafluoroethylene copolymer and 5% fluorinated polyimide modified acrylic resin. The first release layer and the second release layer are ethylene-tetrafluoroethylene copolymer, The melt index of polycarbonate is 20 g / 10 min, the tensile strength is 70.0 MPa, and the tensile modulus is 800 MPa; The melt index of ethylene-tetrafluoroethylene copolymer is 20 g / 10 min, the tensile strength is 50.0 MPa, and the tensile modulus is 800 MPa; The melt index measurement method of polycarbonate refers to GB / T 3682-2000, and the test conditions are: test temperature 300℃, nominal load 1.2kg; The melt index measurement method of ethylene-tetrafluoroethylene copolymer refers to GB / T 3682-2000, and the test conditions are: test temperature 297°C, nominal load 5kg.

2. The method for preparing a multi-layer high temperature resistant fluorine-containing release film according to claim 1, characterized in that: The following steps are involved: (1) The components of the structural layer are weighed according to the mass ratio and mixed in a high-speed mixer, and then melt-blended, extruded, granulated and dried by a twin-screw extruder to obtain structural layer pellets; (2) Prepare three extruders A, B, and C, add ethylene-tetrafluoroethylene copolymer to extruders A and C respectively, for extruding the first release layer and the second release layer of the release film, add the pellets in step (1) to extruder B, for extruding the structural layer of the release film, the melt extruded by the three-layer extruder enters and is compounded in a casting die, the compounded multi-layer melt is shaped, cooled, pulled, and annealed to prepare a multi-layer high-temperature resistant release film, the thickness is detected and adjusted by an online thickness gauge, the film is trimmed and rolled up, and a multi-layer high-temperature resistant fluorine-containing release film product is obtained.

3. The preparation method according to claim 2, characterized in that: In the step (1), the blending time is 2-10 min, the extrusion temperature is 270-340° C., the screw speed is 15-80 r / min, and after traction granulation, the granules are dried at 100° C. for 8 h.

4. The preparation method according to claim 2, characterized in that: In the step (2), the screw length-diameter ratio of extruder A is 20-30, and it comprises a barrel with four heating zones, and the barrel temperatures are respectively set to: 220-340°C for zone 1, 230-350°C for zone 2, 230-360°C for zone 3, and 230-370°C for zone 4; the screw length-diameter ratio of extruder B is 25-30, and it comprises a barrel with four heating zones, and the barrel temperatures are respectively set to: 210-340°C for zone 1, 220-340°C for zone 2, 220-350°C for zone 3, and 220-350°C for zone 4; the process parameters of extruder C are set the same as those of extruder A.

5. The preparation method according to claim 2, characterized in that: The casting die in step (2) is a multi-channel in-mold composite casting die, and the temperature is set to 250-370°C.