Magnesium ion battery negative electrode material with core-shell structure and preparation method and application thereof

By preparing a carbon-coated core-shell structured magnesium-ion battery anode material, the problems of uneven size and high energy consumption of multi-element alloy-based materials in the prior art have been solved, and the improvement of high specific capacity, long cycle life and high rate performance has been achieved.

CN114361418BActive Publication Date: 2024-11-05SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111661720.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-30
Publication Date
2024-11-05
Estimated Expiration
2041-12-30

AI Technical Summary

Technical Problem

Existing magnesium-ion battery multi-element alloy-based anode materials suffer from problems such as uneven size, uneven element distribution, and high energy consumption during preparation, making it difficult to meet the requirements of high specific capacity, long cycle life, and high rate capability.

Method used

Using metal-organic framework materials as precursors, a carbon-coated core-shell structured magnesium-ion battery anode material is prepared by solvothermal reaction and calcination. The specific steps include solvothermal synthesis of porous metal-organic framework, heating of mixed solution, centrifugation and washing, and calcination in a hydrogen-argon mixed atmosphere to form a uniform core-shell structure.

Benefits of technology

The prepared anode material has a uniform micron-scale sheet structure and uniform core-shell composite metal nanoparticles, which improves the migration dynamics of Mg2+, alleviates the volume expansion during charge and discharge, and exhibits excellent cycle stability and high first-cycle coulombic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114361418B_ABST
    Figure CN114361418B_ABST
Patent Text Reader

Abstract

The present invention discloses a magnesium ion battery negative electrode material with a core-shell structure and a preparation method and application thereof. a+ The metal organic framework coordinated with organic ligands is used as a precursor, and a part of the metal ions X in the precursor framework is replaced by cation exchange method. a+ Replaced by another metal ion Y b+ , a bimetallic organic framework is obtained, and finally a carbon-coated core-shell X@Y particle can be obtained by heat treatment in an inert atmosphere. The X@Y particle has uniform size and distribution, and exhibits a core-shell structure, wherein the core is X and the shell is Y. The preparation process of the present invention is simple and environmentally friendly. The obtained product has uniform size, uniform distribution, and stable structure, and is suitable for use as a negative electrode material for a magnesium ion battery. At the same time, the magnesium ion battery prepared using the negative electrode material has excellent electrochemical properties. The composite material and its design strategy proposed in the present invention promote the development of magnesium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electrochemical energy storage, and specifically relates to a magnesium ion battery negative electrode material and a preparation method and application thereof, and in particular relates to a magnesium ion battery negative electrode material with a core-shell structure and a preparation method and application thereof. Background Art

[0002] Due to the abundant reserves and low price of magnesium, magnesium-ion battery system has attracted widespread attention as a battery system to replace lithium-ion batteries in the "post-lithium era". Secondly, magnesium metal has a lower electrode potential (-2.37V vs. SHE) and a higher volumetric capacity (3833mAh·cm -3 ). More importantly, the dendrite-free property of magnesium can largely ensure the high stability and high safety of the battery system during operation. However, the research on magnesium-ion batteries is still in its infancy, which is mainly limited by two aspects: (1) Due to the chemical characteristics of magnesium, only solutions that neither provide nor accept protons can be used as electrolytes. Most traditional electrolytes will react with magnesium and form a layer on the electrode surface that cannot conduct Mg. 2+ The passivation film makes it difficult for magnesium to dissolve and deposit reversibly; (2) due to Mg 2+ With two charges, the charge density is high, and Mg 2+ The smaller ionic radius of Mg 2+ The interaction force with the electrode material is strong, making Mg 2+ It is difficult to embed into electrode materials, and its diffusion and migration in electrode materials are extremely slow.

[0003] In order to solve the problem that magnesium is incompatible with most electrolytes, a class of materials such as Bi, Sn and Ga based on alloying reaction mechanism has been widely studied (Niu, JZ; Zhang, ZH; Aurbach, D., Alloy Anode Materials for Rechargeable Mg Ion Batteries. Advanced Energy Materials 2020, 10, 2000697.). However, this type of material will experience a large volume expansion during the charge and discharge process, and each material has its own shortcomings. Therefore, the above-mentioned single element alloy-based materials may be difficult to meet the requirements of magnesium ion batteries for high specific capacity, long cycle life and high rate. Multi-element alloy-based negative electrodes such as BiSb, SnSb and BiSn can introduce certain new properties while combining the advantages of each element to become better magnesium ion battery negative electrode materials. However, the existing multi-element alloy-based material preparation process is limited to magnetron sputtering or traditional casting methods, but these methods often have problems such as large size of the prepared multi-element alloy materials, uneven distribution of each element and high energy consumption. For example, Niu et al. synthesized a bismuth-tin-magnesium alloy using a traditional casting process, and then obtained porous bismuth-tin as a negative electrode active material for magnesium-ion batteries by dealloying in a 2wt% tartaric acid aqueous solution. However, the bismuth-tin-magnesium alloy undergoes violent agglomeration during high-temperature (740°C) casting, resulting in a larger size of the bismuth-tin obtained after dealloying. More importantly, the process is difficult to achieve uniform distribution of bismuth and tin at the nanoscale and high energy consumption caused by high temperature (Niu, J.; Gao, H.; Ma, W.; Luo, F.; Yin, K.; Peng, Z.; Zhang, Z., Dual phase enhanced superior electrochemical performance of nanoporous bismuth-tin alloyanodes for magnesium-ion batteries. Energy Storage Materials 2018, 14, 351-360.). Therefore, it is very desirable and valuable to explore a multi-element alloy-based magnesium-ion battery negative electrode material with uniform size, uniform distribution and specific structure and a preparation method thereof. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the existing method for preparing multi-element alloy-based negative electrode materials for magnesium ion batteries, and to provide a carbon-coated core-shell particle prepared using a metal organic framework (MOFs) material as a precursor, a preparation method, and an application in a magnesium ion battery. The process for synthesizing the carbon-coated core-shell particle is simple, environmentally friendly, safe and controllable, and time-consuming and energy-saving. The carbon-coated core-shell particle prepared by the preparation method of the present invention has excellent magnesium storage performance when used as a negative electrode material for a magnesium ion battery.

[0005] The present invention is achieved through the following technical solutions.

[0006] A method for preparing a magnesium ion battery negative electrode material with a core-shell structure comprises the following steps:

[0007] (1) dissolving a metal salt and an organic ligand in an organic solvent to perform a solvothermal reaction, and after the reaction, centrifuging, washing, and drying to obtain a porous metal organic framework having metal ions and organic ligands coordinated thereto;

[0008] (2) dispersing the porous metal organic framework solid powder dried in step (1) in a solvent to obtain a mixture solution, heating it under stirring, dissolving another metal salt in the solvent, adding the obtained solution to the aforementioned mixture solution for reaction, and centrifuging, washing, and drying after the reaction to obtain a porous bimetallic organic framework;

[0009] (3) The porous bimetallic organic framework solid powder dried in step (2) is placed in a tube furnace and calcined in a hydrogen-argon mixed atmosphere to obtain carbon-coated core-shell X@Y nanoparticles.

[0010] Preferably, the metal salt in step (1) is one of BiCl3, BiI3 and Bi(NO3)3·5H2O.

[0011] Preferably, the organic ligand in step (1) is one of benzene-1,3,5-tribenzoic acid, 1,3,5-benzenetricarboxylic acid and 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine.

[0012] Preferably, the molar ratio of the metal salt to the organic ligand in step (1) is 1:(1-15).

[0013] Preferably, the solvent in step (1) is a mixture of one or more organic solvents such as methanol, ethanol, ethylene glycol and N,N-dimethylformamide.

[0014] Preferably, the reaction temperature of the solvent thermal reaction in step (1) is 100-160° C., and the reaction time is 12-48 h.

[0015] Preferably, the other metal salt in step (2) is one of SnCl2, SnSO4 and SnC2O4.

[0016] Preferably, the mass ratio of the porous metal organic framework in step (1) to the another metal salt in step (2) is (10-1):1.

[0017] Preferably, the solvent in step (2) is one or a mixture of organic solvents such as methanol, ethanol, ethylene glycol and N,N-dimethylformamide.

[0018] Preferably, the heating temperature in step (2) is 50-90°C.

[0019] Preferably, the reaction time in step (2) is 0.5-12 h.

[0020] Preferably, the calcination procedure in step (3) is: heating to 300-800° C. at a heating rate of 1-5° C. / min and maintaining for 0.5-10 h.

[0021] The present invention provides a magnesium ion battery negative electrode material with a core-shell structure obtained by the above-mentioned preparation method. The negative electrode material has a uniform size and is a micron sheet structure as a whole, and the sheet is coated with composite metal X@Y nanoparticles with a core-shell structure that are evenly distributed.

[0022] The composite metal X@Y nanoparticles have a core-shell structure, wherein the core is X and the shell is Y, wherein the size of the core is 10-150nm and the thickness of the shell is 0.5-40nm. X in the composite metal X@Y nanoparticles is preferably Bi and Y is preferably Sn.

[0023] The carbon-coated core-shell X@Y nanoparticles with a core-shell structure prepared by the above preparation method are used as negative electrode active materials in magnesium ion batteries.

[0024] Compared with the prior art, the present invention has the following advantages:

[0025] (1) The preparation process of the present invention is simple, environmentally friendly, safe and controllable, and consumes little time and energy, thus providing a new approach for the preparation of multi-metal / carbon composite materials.

[0026] (2) A magnesium ion battery negative electrode material prepared by the present invention has a micron-level sheet structure as a whole, and has uniform size, uniform distribution and stable structure. The composite metal particles coated in the sheet have a core-shell structure, wherein the size of the core is 10-150nm and the thickness of the shell is 0.5-40nm.

[0027] (3) The magnesium ion battery negative electrode material with a core-shell structure prepared by the present invention can be used in magnesium ion batteries to accelerate the Mg 2+Migration kinetics, alleviating volume expansion during charge and discharge, with excellent cycle stability and high first-cycle coulombic efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 are scanning electron microscope photographs of different magnifications of the bismuth-based metal organic framework Bi-BTC prepared in Example 1 of the present invention;

[0029] Figure 2 These are scanning electron microscope photographs of different magnifications of the bismuth-tin-based metal organic framework BiSn-BTC prepared in Example 1 of the present invention;

[0030] Figure 3 is a scanning electron microscope photograph of the carbon-coated core-shell Bi@Sn particles prepared in Example 1 of the present invention;

[0031] Figure 4 is a transmission electron microscope photograph of the carbon-coated core-shell Bi@Sn particles prepared in Example 1 of the present invention;

[0032] Figure 5 is a scanning transmission electron microscope photograph of the carbon-coated core-shell Bi@Sn particles prepared in Example 1 of the present invention;

[0033] Figure 6 This is a cycle performance diagram of a battery assembled using the carbon-coated core-shell Bi@Sn particles prepared in Example 1 of the present invention as the negative electrode material for a magnesium ion battery. DETAILED DESCRIPTION

[0034] In order to better understand the present invention, the specific implementation of the present invention is further described in detail below in conjunction with embodiments and drawings, but the implementation mode of the present invention is not limited thereto.

[0035] Example 1

[0036] 375 mg of 1,3,5-benzenetricarboxylic acid and 75 mg of Bi(NO3)3·5H2O were dissolved in 15 mL of methanol, respectively, and magnetically stirred, named solution A and solution B. Under magnetic stirring, solution A was added to solution B, and magnetic stirring was continued. The above mixture was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene and reacted at 120°C for 24 hours. The product after the reaction was centrifuged, washed and dried to obtain a white powder bismuth-based metal organic framework Bi-BTC (BTC is 1,3,5-benzenetricarboxylic acid).

[0037] Then disperse the prepared 100 mg Bi-BTC in 30 mL methanol and heat to 60 ° C to obtain a suspension of Bi-BTC. Dissolve 22 mg SnCl2 in 30 mL methanol solution to obtain a methanol solution of SnCl2. Pour the methanol solution of SnCl2 into the above Bi-BTC suspension and stir at 60 ° C for 1 hour to obtain a suspension of bismuth-tin-based bimetallic organic framework BiSn-BTC. After the above suspension is cooled to room temperature, centrifuge, wash and dry to obtain white powder BiSn-BTC.

[0038] Finally, BiSn-BTC was heated to 500 °C (heating rate 3 °C / min) in a tube furnace under an atmosphere of 8 vol.% H2 and 92 vol.% Ar and maintained for 2 h to obtain carbon-coated core-shell Bi@Sn particles.

[0039] Figure 1 The SEM (scanning electron microscope) images of Bi-BTC prepared in this example at different magnifications are shown in FIG. Figure 1 The a in the figure is a SEM image magnified 1000 times. Figure 1 Figure b is a SEM image magnified 5000 times. It can be seen that the obtained Bi-BTC has a uniform micron-scale lamellae morphology with an average length of 5-10 μm and an average thickness of 10-100 nm. Figure 2 The SEM images of BiSn-BTC prepared in this example at different magnifications are shown in FIG. Figure 2 The a in the figure is a SEM image magnified 2000 times. Figure 2 Figure b is a SEM image magnified 10,000 times. It can be seen that the morphology and size of the obtained BiSn-BTC have not changed significantly compared to Bi-BTC. The overall structure is still a micron-scale lamellar structure with an average length of 5-10μm and an average thickness of 10-100nm. The only change is that the surface becomes rougher. Figure 3 This is a SEM photograph of the carbon-coated core-shell Bi@Sn particles prepared in this example. It can be seen that the structure of the obtained carbon-coated core-shell Bi@Sn particles does not collapse significantly after calcination, and the metal particles are uniformly coated with the carbon layer. Figure 4 This is a TEM (transmission electron microscope) photograph of the carbon-coated core-shell Bi@Sn particles prepared in this example. It can be seen that the obtained composite metal particles are relatively uniform in size and evenly distributed. Figure 5 This is a STEM (scanning transmission electron microscope) photograph of the carbon-coated core-shell Bi@Sn particles prepared in this example. It can be seen that the obtained composite metal particles are a core-shell structure, in which the Bi core size is about 35nm and the Sn shell thickness is about 3nm.

[0040] Example 2

[0041] 750 mg of 1,3,5-benzenetricarboxylic acid and 200 mg of Bi(NO3)3·5H2O were dissolved in 15 mL of methanol, respectively, and magnetically stirred, named solution A and solution B. Under magnetic stirring, solution A was added to solution B, and magnetic stirring was continued. The above mixture was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene and reacted at 120°C for 24 hours. The product after the reaction was centrifuged, washed and dried to obtain a white powder bismuth-based metal organic framework Bi-BTC (BTC is 1,3,5-benzenetricarboxylic acid).

[0042] Then disperse the prepared 100 mg Bi-BTC in 30 mL methanol and heat to 60 ° C to obtain a suspension of Bi-BTC. Dissolve 22 mg SnCl2 in 30 mL methanol solution to obtain a methanol solution of SnCl2. Pour the methanol solution of SnCl2 into the above Bi-BTC suspension and stir at 60 ° C for 1 hour to obtain a suspension of bismuth-tin-based bimetallic organic framework BiSn-BTC. After the above suspension is cooled to room temperature, centrifuge, wash and dry to obtain white powder BiSn-BTC.

[0043] Finally, BiSn-BTC was heated to 500 °C (heating rate 3 °C / min) in a tube furnace under an atmosphere of 8 vol.% H2 and 92 vol.% Ar and maintained for 2 h to obtain carbon-coated core-shell Bi@Sn particles.

[0044] Example 3

[0045] 386 mg of 1,3,5-benzenetricarboxylic acid and 472 mg of Bi(NO3)3·5H2O were dissolved in 15 mL of a mixed solution of N,N-dimethylformamide / methanol (the volume ratio of N,N-dimethylformamide and methanol was 1:1), named solution A and solution B. Under magnetic stirring, solution A was added to solution B and magnetic stirring was continued. The above mixture was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene and reacted at 100°C for 48 hours. The product after the reaction was centrifuged, washed and dried to obtain a white powder bismuth-based metal organic framework Bi-BTC (BTC is 1,3,5-benzenetricarboxylic acid).

[0046] Then disperse the prepared 100 mg Bi-BTC in 30 mL methanol and heat to 50 ° C to obtain a suspension of Bi-BTC. Dissolve 22 mg SnCl2 in 30 mL methanol solution to obtain a methanol solution of SnCl2. Pour the methanol solution of SnCl2 into the above Bi-BTC suspension and stir at 50 ° C for 12 hours to obtain a suspension of bismuth-tin-based bimetallic organic framework BiSn-BTC. After the above suspension is cooled to room temperature, centrifuge, wash and dry to obtain white powder BiSn-BTC.

[0047] Finally, BiSn-BTC was heated to 300 °C (heating rate 1 °C / min) in a tube furnace under an atmosphere of 8 vol.% H2 and 92 vol.% Ar and maintained for 10 h to obtain carbon-coated core-shell Bi@Sn particles.

[0048] Example 4

[0049] 750 mg of 1,3,5-benzenetricarboxylic acid and 150 mg of Bi(NO3)3·5H2O were dissolved in 15 mL of methanol, respectively, and magnetically stirred, named solution A and solution B. Under magnetic stirring, solution A was added to solution B, and magnetic stirring was continued. The above mixture was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene and reacted at 160°C for 12 hours. The product after the reaction was centrifuged, washed and dried to obtain a white powder bismuth-based metal organic framework Bi-BTC (BTC is 1,3,5-benzenetricarboxylic acid).

[0050] Then disperse the prepared 100 mg Bi-BTC in 30 mL methanol and heat to 60 ° C to obtain a suspension of Bi-BTC. Dissolve 22 mg SnCl2 in 30 mL methanol solution to obtain a methanol solution of SnCl2. Pour the methanol solution of SnCl2 into the above Bi-BTC suspension and stir at 60 ° C for 1 hour to obtain a suspension of bismuth-tin-based bimetallic organic framework BiSn-BTC. After the above suspension is cooled to room temperature, centrifuge, wash and dry to obtain white powder BiSn-BTC.

[0051] Finally, BiSn-BTC was heated to 500 °C (heating rate 3 °C / min) in a tube furnace under an atmosphere of 8 vol.% H2 and 92 vol.% Ar and maintained for 2 h to obtain carbon-coated core-shell Bi@Sn particles.

[0052] Example 5

[0053] 750 mg of 1,3,5-benzenetricarboxylic acid and 150 mg of Bi(NO3)3·5H2O were dissolved in 15 mL of methanol, respectively, and magnetically stirred, named solution A and solution B. Under magnetic stirring, solution A was added to solution B, and magnetic stirring was continued. The above mixture was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene and reacted at 120°C for 24 hours. The product after the reaction was centrifuged, washed and dried to obtain a white powder bismuth-based metal organic framework Bi-BTC (BTC is 1,3,5-benzenetricarboxylic acid).

[0054] Then disperse the prepared 100 mg Bi-BTC in 30 mL methanol and heat to 70 ° C to obtain a suspension of Bi-BTC. Dissolve 33 mg SnCl2 in 30 mL methanol solution to obtain a methanol solution of SnCl2. Pour the methanol solution of SnCl2 into the above Bi-BTC suspension and stir at 70 ° C for 1 hour to obtain a suspension of bismuth-tin-based bimetallic organic framework BiSn-BTC. After the above suspension is cooled to room temperature, centrifuge, wash and dry to obtain white powder BiSn-BTC.

[0055] Finally, BiSn-BTC was heated to 500 °C (heating rate 3 °C / min) in a tube furnace under an atmosphere of 8 vol.% H2 and 92 vol.% Ar and maintained for 2 h to obtain carbon-coated core-shell Bi@Sn particles.

[0056] Example 6

[0057] 750 mg of 1,3,5-benzenetricarboxylic acid and 150 mg of Bi(NO3)3·5H2O were dissolved in 15 mL of methanol, respectively, and magnetically stirred, named solution A and solution B. Under magnetic stirring, solution A was added to solution B, and magnetic stirring was continued. The above mixture was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene and reacted at 120°C for 24 hours. The product after the reaction was centrifuged, washed and dried to obtain a white powder bismuth-based metal organic framework Bi-BTC (BTC is 1,3,5-benzenetricarboxylic acid).

[0058] Then disperse the prepared 100 mg Bi-BTC in 30 mL methanol and heat to 80 ° C to obtain a suspension of Bi-BTC. Dissolve 44 mg SnCl2 in 30 mL methanol solution to obtain a methanol solution of SnCl2. Pour the methanol solution of SnCl2 into the above Bi-BTC suspension and stir at 80 ° C for 1.5 hours to obtain a suspension of bismuth-tin-based bimetallic organic framework BiSn-BTC. After the above suspension is cooled to room temperature, centrifuge, wash and dry to obtain white powder BiSn-BTC.

[0059] Finally, BiSn-BTC was heated to 500 °C (heating rate 3 °C / min) in a tube furnace under an atmosphere of 8 vol.% H2 and 92 vol.% Ar and maintained for 2 h to obtain carbon-coated core-shell Bi@Sn particles.

[0060] Example 7

[0061] 750 mg of 1,3,5-benzenetricarboxylic acid and 150 mg of Bi(NO3)3·5H2O were dissolved in 15 mL of methanol, respectively, and magnetically stirred, named solution A and solution B. Under magnetic stirring, solution A was added to solution B, and magnetic stirring was continued. The above mixture was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene and reacted at 120°C for 24 hours. The product after the reaction was centrifuged, washed and dried to obtain a white powder bismuth-based metal organic framework Bi-BTC (BTC is 1,3,5-benzenetricarboxylic acid).

[0062] Then disperse the prepared 100 mg Bi-BTC in 30 mL methanol and heat to 60 ° C to obtain a suspension of Bi-BTC. Dissolve 55 mg SnCl2 in 30 mL methanol solution to obtain a methanol solution of SnCl2. Pour the methanol solution of SnCl2 into the above Bi-BTC suspension and stir at 60 ° C for 1 hour to obtain a suspension of bismuth-tin-based bimetallic organic framework BiSn-BTC. After the above suspension is cooled to room temperature, centrifuge, wash and dry to obtain white powder BiSn-BTC.

[0063] Finally, BiSn-BTC was heated to 450 °C (heating rate 2 °C / min) in a tube furnace under an atmosphere of 8 vol.% H2 and 92 vol.% Ar and maintained for 3 h to obtain carbon-coated core-shell Bi@Sn particles.

[0064] Example 8

[0065] 750 mg of 1,3,5-benzenetricarboxylic acid and 150 mg of Bi(NO3)3·5H2O were dissolved in 15 mL of methanol, respectively, and magnetically stirred, named solution A and solution B. Under magnetic stirring, solution A was added to solution B, and magnetic stirring was continued. The above mixture was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene and reacted at 120°C for 24 hours. The product after the reaction was centrifuged, washed and dried to obtain a white powder bismuth-based metal organic framework Bi-BTC (BTC is 1,3,5-benzenetricarboxylic acid).

[0066] Then disperse the prepared 100 mg Bi-BTC in 30 mL methanol and heat to 70 ° C to obtain a suspension of Bi-BTC. Dissolve 22 mg SnCl2 in 30 mL methanol solution to obtain a methanol solution of SnCl2. Pour the methanol solution of SnCl2 into the above Bi-BTC suspension and stir at 70 ° C for 1 hour to obtain a suspension of bismuth-tin-based bimetallic organic framework BiSn-BTC. After the above suspension is cooled to room temperature, centrifuge, wash and dry to obtain white powder BiSn-BTC.

[0067] Finally, BiSn-BTC was heated to 600 °C (heating rate 3 °C / min) in a tube furnace under an atmosphere of 8 vol.% H2 and 92 vol.% Ar and maintained for 1.5 h to obtain carbon-coated core-shell Bi@Sn particles.

[0068] Example 9

[0069] 400 mg of 1,3,5-benzenetricarboxylic acid and 200 mg of BiI3 were dissolved in 15 mL of a mixed solution of N,N-dimethylformamide and ethanol (the volume ratio of N,N-dimethylformamide and ethanol was 1:1), and magnetically stirred, named solution A and solution B. Under magnetic stirring, solution A was added to solution B, and magnetic stirring was continued. The above mixture was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene and reacted at 100 ° C for 12 hours. The product after the reaction was centrifuged, washed and dried to obtain a white powder bismuth-based metal organic framework Bi-BTC (BTC is 1,3,5-benzenetricarboxylic acid).

[0070] Then disperse the prepared 100 mg Bi-BTC in 30 mL ethanol and heat to 80 ° C to obtain a suspension of Bi-BTC. Dissolve 10 mg SnCl2 in 30 mL ethanol solution to obtain an ethanol solution of SnCl2. Pour the ethanol solution of SnCl2 into the above Bi-BTC suspension and stir at 80 ° C for 1 hour to obtain a suspension of bismuth-tin-based bimetallic organic framework BiSn-BTC. After the above suspension is cooled to room temperature, centrifuge, wash and dry to obtain white powder BiSn-BTC.

[0071] Finally, BiSn-BTC was heated to 500 °C (heating rate 3 °C / min) in a tube furnace under an atmosphere of 8 vol.% H2 and 92 vol.% Ar and maintained for 2 h to obtain carbon-coated core-shell Bi@Sn particles.

[0072] Example 10

[0073] 375 mg of 1,3,5-benzenetricarboxylic acid and 75 mg of Bi(NO3)3·5H2O were dissolved in 15 mL of methanol, respectively, and magnetically stirred, named solution A and solution B. Under magnetic stirring, solution A was added to solution B, and magnetic stirring was continued. The above mixture was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene and reacted at 120°C for 24 hours. The product after the reaction was centrifuged, washed and dried to obtain a white powder bismuth-based metal organic framework Bi-BTC (BTC is 1,3,5-benzenetricarboxylic acid).

[0074] Then disperse the prepared 100 mg Bi-BTC in 30 mL methanol and heat to 90 ° C to obtain a suspension of Bi-BTC. Dissolve 100 mg SnSO4 in 30 mL methanol solution to obtain a methanol solution of SnSO4. Pour the methanol solution of SnSO4 into the above Bi-BTC suspension and stir at 90 ° C for 0.5 h to obtain a suspension of bismuth-tin-based bimetallic organic framework BiSn-BTC. After the above suspension is cooled to room temperature, centrifuge, wash and dry to obtain white powder BiSn-BTC.

[0075] Finally, BiSn-BTC was heated to 800 °C (heating rate 5 °C / min) in a tube furnace under an atmosphere of 8 vol.% H2 and 92 vol.% Ar and maintained for 0.5 h to obtain carbon-coated core-shell Bi@Sn particles.

[0076] Application Example 1

[0077] The carbon-coated core-shell Bi@Sn particles obtained in Example 1 were applied to magnesium ion batteries in the following steps:

[0078] 18 mg of carbon-coated core-shell Bi@Sn particles, 9 mg of conductive agent Super P, and 3 mg of polyvinylidene fluoride (PVDF) were ground in anhydrous N-methylpyrrolidone according to a mass ratio of 6:3:1 to form a uniform slurry, which was then scraped onto the current collector and vacuum dried at 80°C for 12 h to obtain a carbon-coated core-shell Bi@Sn particle magnesium ion battery negative electrode material.

[0079] The battery was assembled in an argon-filled glove box using a freshly polished and cleaned magnesium sheet as the counter electrode, 0.4 M (PhMgCl)2-AlCl3 / THF solution as the electrolyte, and Whatman glass fiber membrane (GF / F) as the separator.

[0080] The above-assembled battery was subjected to constant current charge and discharge tests on a Xinwei electrochemical workstation. The test voltage range was 0.01V–0.8V, the current density was 100mA / g, and the specific capacity was calculated based on the active material of the carbon-coated core-shell Bi@Sn particles.

[0081] Figure 6 The cycling performance diagram of the battery assembled with the carbon-coated core-shell Bi@Sn particles prepared in Example 1 as the negative electrode material of the magnesium ion battery. The assembled battery exhibited a cycling performance of 237.5 mA·h·g at a current density of 100 mA / g in the first cycle. –1 The battery has a discharge capacity of 162 mA·h·g after 100 cycles. –1The discharge specific capacity is 2.37 W, and the coulombic efficiency is maintained at 95.5%. It can be seen that the battery has good cycle stability and high coulombic efficiency, indicating that the carbon-coated core-shell Bi@Sn particles have excellent magnesium storage performance as the negative electrode material of magnesium ion batteries.

[0082] The above embodiments are used to illustrate the present invention, and the implementation methods of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a magnesium ion battery negative electrode material with a core-shell structure, It is characterized in that The steps include: (1) dissolving a metal salt and an organic ligand in an organic solvent to perform a solvothermal reaction, and after the reaction, centrifuging, washing, and drying to obtain a porous metal organic framework having metal ions and organic ligands coordinated thereto; (2) dispersing the porous metal organic framework solid powder dried in step (1) in a solvent to obtain a mixture solution, heating it under stirring, dissolving another metal salt in the solvent, adding the obtained solution to the aforementioned mixture solution for reaction, and centrifuging, washing, and drying after the reaction to obtain a porous bimetallic organic framework; (3) placing the porous bimetallic organic framework solid powder dried in step (2) in a tube furnace and calcining it in a hydrogen-argon mixed atmosphere to obtain carbon-coated core-shell X@Y nanoparticles; The metal salt in step (1) is BiCl 3 ,BiI 3 and Bi(NO 3 ) 3 ·5H 2 O; the other metal salt in step (2) is SnCl 2 SnSO 4 and SnC 2 O 4 a kind of; The molar ratio of the metal salt and the organic ligand in step (1) is 1:(1-15); the mass ratio of the porous metal organic framework in step (1) and the other metal salt in step (2) is (10-1):1; The solvent in step (1) and step (2) is a mixture of one or more organic solvents selected from methanol, ethanol and N,N-dimethylformamide; The calcination procedure in step (3) is: heating to 300-800°C at a heating rate of 1-5°C / min and maintaining for 0.5-10h.

2. The method for preparing the magnesium ion battery negative electrode material with a core-shell structure according to claim 1, It is characterized in that The organic ligand in step (1) is one of benzene-1,3,5-tribenzoic acid, 1,3,5-benzenetricarboxylic acid and 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine.

3. The method for preparing the magnesium ion battery negative electrode material with a core-shell structure according to claim 1, It is characterized in that The reaction temperature of the solvent thermal reaction in step (1) is 100-160° C., and the reaction time is 12-48 hours.

4. The method for preparing the magnesium ion battery negative electrode material with a core-shell structure according to claim 1, It is characterized in that The heating temperature in step (2) is 50-90° C.; the reaction time in step (2) is 0.5-12 h.

5. A magnesium ion battery negative electrode material having a core-shell structure prepared by the preparation method according to any one of claims 1 to 4, It is characterized in that The magnesium ion battery negative electrode material has a uniform size and is a micron-layer structure as a whole, wherein the layers are coated with composite metal X@Y nanoparticles with a uniformly distributed core-shell structure; the core of the composite metal X@Y nanoparticles is X and the shell is Y, wherein the size of the core is 10-150nm and the thickness of the shell is 0.5-40nm.

6. The carbon-coated core-shell X@Y nanoparticles with a core-shell structure prepared by the preparation method according to any one of claims 1 to 4 are used as negative electrode active materials in magnesium ion batteries.