A method for eliminating residual stress in flexible integrated devices through interface compensation
Patent Information
- Application Number
- CN202111580209.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-22
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-12-22
AI Technical Summary
TFT由不同的功能层薄膜堆栈组成,薄膜内部和界面处往往存在一定的残余应力,在收到力、热、光、电等外界干扰后,器件残余应力分布更加不均匀,导致器件性能恶化,对于柔性器件来说是致命损伤
[0027] The present invention utilizes the different types of residual stresses of different thin film materials. Through process design, the mutual compensation of stresses in two different directions is realized at the interface, and the residual stress of the flexible integrated device is successfully eliminated. At the same time, the invention uses a copper alloy electrode wiring process that is compatible with the existing CMOS process, has low resistivity, is not easy to diffuse, has good electrical resistance, and has good mechanical flexibility, and can achieve large-scale industrial promotion.
Smart Images

Figure CN114388364B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of microelectronic manufacturing, and in particular relates to a method for eliminating residual stress of a flexible integrated device through interface compensation. Background Art
[0002] The booming development of flexible electronics is one of the milestones in the world of microelectronics. Flexible circuits refer to circuits manufactured on flexible substrates, while flexible integrated circuits are highly integrated large-scale circuits implemented on flexible substrates (such as polyimide). The advantages of flexible integrated circuits are that they are bendable and foldable. At present, silicon-based integrated circuits have entered the post-Moore's Law era, and silicon-based flexible performance is poor and costly, so their further development potential is limited. There is a lot of room for improvement in the integration, performance, and power consumption of flexible integrated circuits, and they are still in the early stages of the Moore's Law development curve. At present, the most advanced flexible device feature size is about 1um, so when the feature size of future flexible integrated circuits is about 200nm, its circuit performance can reach more than 20 times the current level, and its power consumption can reach one percent of the current level. Flexible integrated circuits often use thin-film transistors (TFTs) to complete rectification, modulation, clock generation, and related digital circuits for sensing, detection, logical operations, etc. Generally, indium zinc gallium oxide thin-film transistors (IGZO-TFTs) are used as the smallest device unit, polyimide PI is used as the substrate material, and micron-level photolithography technology is used to integrate dozens or even thousands of TFTs on the PI substrate. TFT is composed of different functional layer thin film stacks. There is often a certain amount of residual stress inside the film and at the interface. After receiving external interference such as force, heat, light, and electricity, the residual stress distribution of the device becomes more uneven, resulting in deterioration of device performance, which is fatal damage to flexible devices. Eliminating residual stress during the device preparation process is the most effective way to solve the problem from the source. Summary of the invention
[0003] In order to address the shortcomings and deficiencies of the prior art, the purpose of the present invention is to provide a method for eliminating residual stress of flexible integrated devices through interface compensation, so as to significantly reduce the residual stress inside the flexible electronic device and improve the reliability of the device.
[0004] The purpose of the present invention is achieved through the following technical solutions:
[0005] A method for eliminating residual stress of a flexible integrated device by interface compensation comprises the following steps:
[0006] (1) treating the flexible substrate with oxygen plasma, wherein the treatment conditions are: power of 50 to 100 W, gas pressure of 0.3 to 1 Torr, and treatment time of 5 to 10 minutes;
[0007] (2) SiO was prepared on a flexible substrate treated with oxygen plasma using plasma enhanced chemical vapor deposition (PECVD) x / SiN x The laminated film is used as a flexible substrate buffer layer under the following conditions: power 80-120 W, air pressure 0.5-2 Pa, temperature 200-400°C;
[0008] (3) preparing a copper alloy gate electrode by pulsed DC sputtering process, and then preparing a patterned gate interconnection line by photolithography process;
[0009] (4) performing nitrogen gradient temperature annealing on the gate at at least two temperatures, 100 to 400° C., for 0.5 to 3 h;
[0010] (5) SiO was prepared by plasma enhanced chemical vapor deposition (PECVD) under the same conditions as step (2) x / SiN x The laminated film serves as a gate insulating layer;
[0011] (6) preparing an IGZO semiconductor layer by a pulsed DC sputtering process, and patterning it by photolithography to cover the back channel with an etch stop layer;
[0012] (7) using a pulsed DC sputtering process to prepare copper alloy source and drain electrodes, and then using photolithography to pattern them to obtain a flexible device integrated array;
[0013] (8) Annealing the flexible device integrated array under the following conditions: annealing at 100-400° C. for 0.5-3 h at a pressure of 5-20 mTorr;
[0014] (9) Depositing SiO on the annealed flexible device integrated array using a plasma enhanced chemical vapor deposition (PECVD) method under the same conditions as step (2) x / SiN x The laminated film acts as a passivation layer.
[0015] Preferably, the flexible substrate in step (1) is a polyimide (PI) substrate.
[0016] Preferably, the plasma enhanced chemical vapor deposition (PECVD) method in steps (2), (5) and (9) is used to prepare SiO x / SiN x Laminated film, reaction formula is SiH 4 +O 2 →SiO x +H 2 O,SiH 4 +N 2 →SiN x +NH3 , SiO x The thickness of SiN is 100~300nm. x The thickness is 20 to 100 nm.
[0017] Preferably, the pulsed DC sputtering process in step (3) is: sputtering power of 60-120 W, gas pressure of 1-5 mTorr, pure argon atmosphere, frequency of 10-20 kHz, duty cycle of 80-98%; the thickness of the copper alloy gate electrode is 100-200 nm.
[0018] Preferably, the copper alloy in steps (3) and (7) is a CuCrZr ternary alloy, and the composition ratio is Cu: 98-99.9wt%, Cr: 0-2wt%, Zr: 0-2wt%; more preferably Cu: 98-99wt%, Cr: 0.1-2wt%, Zr: 0.1-2wt%.
[0019] Preferably, the gradient temperature annealing conditions in step (4) are: first heating to 200°C and keeping warm for 20 minutes, then heating to 400°C and keeping warm for 30 minutes, then cooling to 200°C and keeping warm for 30 minutes, then heating to 400°C and keeping warm for 30 minutes, then cooling to 200°C and keeping warm for 30 minutes, and finally cooling to room temperature.
[0020] Preferably, the pulsed DC sputtering process in step (6) is: sputtering power is 60-120 W, gas pressure is 1-5 mTorr, argon / oxygen ratio is 99:1-90:10, frequency is 10-20 kHz, duty cycle is 80-98%, and the thickness of the IGZO semiconductor layer is 10-30 nm.
[0021] Preferably, the pulsed DC sputtering process in step (7) is: sputtering power of 60 to 120 W, gas pressure of 1 to 5 mTorr, pure argon atmosphere, frequency of 10 to 20 kHz, duty cycle of 80 to 98%, and the thickness of the copper alloy source and drain electrode is 100 to 200 nm.
[0022] Preferably, the pulsed DC sputtering in steps (3), (6) and (7) all adopts a sputtering operation mode in which the device power supply provides a DC + reverse pulse voltage.
[0023] Preferably, the photolithography process in step (3) and the photolithography patterning in steps (6) and (7) all use micron-scale photolithography process to pattern the functional layer.
[0024] The principle of the present invention is:
[0025] First, the PI substrate is treated with oxygen plasma to activate the π-bond groups on the surface of the polyimide so that it can better bond with SiO xBonding to achieve high adhesion. Fully cover SiO on the PI substrate x / SiN x The laminated film acts as a buffer layer to protect the flexible substrate and prevent gate sputtering damage, which can effectively avoid excessive residual stress at the PI / gate interface. Pulsed DC sputtering can control the sputtering particle rate by adjusting the frequency and duty cycle, while ensuring that the particles are fully bonded and avoiding destructive bombardment damage. The purpose of gradient nitrogen annealing of the copper alloy gate is to promote grain growth and phase texture reorganization, while expelling trace doped Cr and Zr from the copper lattice to form a precipitation strengthening mechanism, and consuming part of the energy by reacting at the interface, which can convert the mechanical energy of the residual stress into chemical energy, further eliminating the gate / SiO x / SiN x Residual stress of laminated films. The purpose of annealing after depositing the active layer and the source and drain electrodes is as follows: vacuum atmosphere annealing can improve semiconductor mobility, high temperature can promote the reorganization of copper alloy texture, Cr and Zr are discharged to the semiconductor interface at high temperature to react with In and Zn to form an ultra-thin and dense copper diffusion barrier layer. Compared with the traditional microelectronic Damascus laminated copper wiring process, the required electrode thickness is smaller, the cost is lower and it is more effective. At the same time, the interface reaction absorbs energy at the electrode / semiconductor interface, thereby reducing residual stress. In the present invention, not only mechanical energy is absorbed by interface reaction, but also different types of residual stresses at different interfaces are offset each other. For example, in steps (2), (4), (6), the SiO prepared by chemical vapor deposition x / SiN x The laminated film exhibits compressive stress, while the copper alloy film exhibits tensile stress. After the two form an interface, a mutual pulling torque will be generated. After high-temperature annealing, the interface residual stresses can compensate and eliminate each other.
[0026] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0027] The present invention utilizes the different types of residual stresses in different film materials, and through process design, realizes the mutual compensation of two stresses in different directions at the interface, successfully eliminating the residual stress of the flexible integrated device. At the same time, the present invention uses copper alloy electrode wiring technology that is compatible with the existing CMOS technology, has low resistivity, is not easy to diffuse, has good electrical resistance, and has good mechanical flexibility, and can achieve large-scale industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the gradient annealing temperature curve in Example 1 of the present invention.
[0029] Figure 2The appearance of the flexible bottom grid film in Example 1 and Comparative Example 1 of the present invention, (a) is Example 1, (b) is Comparative Example 1, and the main difference lies in the presence or absence of a buffer layer and interface treatment before and after the preparation of the copper alloy bottom grid.
[0030] Figure 3 The schematic diagram of the minimum unit device structure in Example 1 of the present invention, wherein 1 is a PI substrate, 2 is a SiO x Buffer layer, 3 is SiN x Buffer layer, 4 is copper alloy gate electrode, 5 is SiO x Insulation layer, 6 is SiN x Insulating layer, 7 is IGZO semiconductor layer, 8 is ESL etching barrier layer, 9 is copper alloy source and drain electrode, 10 is SiO x Passivation layer, 11 is SiN x Passivation layer.
[0031] Figure 4 This is a microscopic image of a flexible device array in an embodiment of the present invention.
[0032] Figure 5 These are the measured values of residual stress of the flexible bottom grid film in step (4) of Example 1 of the present invention and step (2) of comparative example 1.
[0033] Figure 6 This is the drift of the transfer curve of the device flexibility bending test in Example 1 of the present invention.
[0034] Figure 7 This is the drift of the transfer curve of the device flexibility bending test in comparative example 1 of the present invention. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0036] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. All raw materials, reagents, etc., whose manufacturers are not specified, are conventional products that can be purchased commercially.
[0037] Example 1
[0038] A method for eliminating residual stress of a flexible integrated device by interface compensation in this embodiment has the following specific steps:
[0039] (1) Cleaning of polyimide PI substrate: First, 100×100 mm PI sheet was irradiated with ultraviolet light for 120 seconds to decompose the organic pollutants that may exist on the surface. After cleaning, it was ultrasonically cleaned twice with deionized water for 15 minutes each time to remove water-soluble pollutants; then ultrasonically cleaned with isopropanol for 15 minutes once to remove the remaining pollutants and moisture. The substrate was placed in a constant temperature drying oven at 80°C for more than 2 hours to obtain a clean and dry substrate.
[0040] (2) The polyimide PI substrate was treated with oxygen plasma for 5 minutes, with a power of 80 W and a gas pressure of 0.5 Torr.
[0041] (3) Preparation of SiO by plasma enhanced chemical vapor deposition (PECVD) x / SiN x The laminated film serves as a PI buffer layer. The reaction formula is SiH 4 +O 2 →SiO x +H 2 O,SiH 4 +N 2 →SiN x +NH 3 ,SiO x :200nm,SiN x :50nm; power 100W, air pressure 1Pa, temperature 300℃.
[0042] (4) A copper alloy gate electrode was prepared by pulsed DC sputtering process, with a composition of Cu: 99at%, Cr: 0.5at%, Zr: 0.5%, a thickness of 200nm, a power of 80W, a gas pressure of 3mTorr, a frequency of 15kHz, and a duty cycle of 90%.
[0043] (5) Use photolithography to prepare patterned gate interconnects: Use positive photoresist to etch away excess copper alloy film.
[0044] (6) The gate is subjected to nitrogen gradient annealing. The annealing temperature is divided into two temperature platforms of 400°C and 200°C. The annealing temperature curve is as follows: Figure 1 shown.
[0045] (7) Preparation of SiO by plasma enhanced chemical vapor deposition (PECVD) x / SiN x The laminated film is used as the gate insulating layer, and the process is the same as (3).
[0046] (8) The IGZO semiconductor layer was prepared by pulsed DC sputtering process with a thickness of 20 nm, a power of 80 W, a gas pressure of 3 mTorr, an oxygen ratio of 5%, a frequency of 15 kHz, and a duty cycle of 90%; and the back channel was covered with an etch stop layer by photolithography patterning.
[0047] (9) A copper alloy source and drain electrode was prepared by pulsed DC sputtering process, with the composition of Cu: 99at%, Cr: 0.5at%, Zr: 0.5%, and the parameters were the same as (4), and then patterned by photolithography.
[0048] (10) The flexible device integrated array is subjected to vacuum annealing at a pressure of 5 mTorr, a temperature of 300°C, and a time of 1 h.
[0049] (11) Deposition of SiO on the device array x / SiN x The laminated film is used as a passivation layer to isolate the corrosion from external water and oxygen, and the process is the same as (3).
[0050] (12) Figure 2 and 5 As shown in the figure, the flexible film after interface stress compensation is flat, indicating that the internal residual stress is small. Figure 6 As shown, after the device is flexibly bent, the transfer curve drift is small.
[0051] Comparative Example 1
[0052] This comparative example is a conventional process, and a TFT device without interface compensation design is used. The specific steps are as follows:
[0053] (1) Cleaning of polyimide PI substrate: First, 100×100 mm PI sheet was irradiated with ultraviolet light for 120 seconds to decompose the organic pollutants that may exist on the surface. After cleaning, it was ultrasonically cleaned twice with deionized water for 15 minutes each time to remove water-soluble pollutants; then ultrasonically cleaned with isopropanol for 15 minutes once to remove the remaining pollutants and moisture. The substrate was placed in a constant temperature drying oven at 80°C for more than 2 hours to obtain a clean and dry substrate.
[0054] (2) A copper alloy gate electrode was prepared by pulsed DC sputtering process, with a composition of Cu: 99at%, Cr: 0.5at%, Zr: 0.5%, a thickness of 200nm, a power of 80W, a gas pressure of 3mTorr, a frequency of 15kHz, and a duty cycle of 90%.
[0055] (3) Using photolithography to prepare patterned gate interconnects: Using positive photoresist, etch away excess copper alloy film.
[0056] (4) Preparation of SiO by plasma enhanced chemical vapor deposition (PECVD) x / SiNx The stacked film is used as the gate insulating layer, and the reaction formula is SiH 4 +O 2 →SiO x +H 2 O,SiH 4 +N 2 →SiN x +NH 3 ,SiO x :200nm,SiN x :50nm; power 100W, air pressure 1Pa, temperature 300℃.
[0057] (5) The IGZO semiconductor layer was prepared by pulsed DC sputtering process with a thickness of 20 nm, a power of 80 W, a gas pressure of 3 mTorr, an oxygen ratio of 5%, a frequency of 15 kHz, and a duty cycle of 90%, and was patterned by photolithography to cover the back channel with an etch stop layer.
[0058] (6) A copper alloy source and drain electrode was prepared by pulsed DC sputtering process, with the composition of Cu: 99at%, Cr: 0.5at%, Zr: 0.5%, and the parameters were the same as (2), and then patterned by photolithography.
[0059] (7) The flexible device integrated array is subjected to vacuum annealing at a pressure of 5 mTorr, a temperature of 300°C, and a time of 1 h.
[0060] (8) Deposition of SiO on the device array x / SiN x The laminated film is used as a passivation layer to isolate the corrosion from external water and oxygen, and the process is the same as (4).
[0061] (9) Figure 2 and 5 As shown in Figure 1, the flexible film without interface stress compensation using conventional processes is in a curled state, indicating that the internal residual stress is very large, which undoubtedly leads to the deterioration of device performance. Figure 7 As shown, after the device is flexibly bent, the transfer curve drifts significantly.
[0062] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for eliminating residual stress in a flexible integrated device by interface compensation, characterized in that: The following steps are involved: (1) The flexible substrate is subjected to oxygen plasma treatment under the following conditions: power of 50 to 100 W, gas pressure of 0.3 to 1 Torr, and treatment time of 5 to 10 minutes; (2) SiO was prepared on a flexible substrate treated with oxygen plasma using plasma-enhanced chemical vapor deposition. x / SiN x The laminated film is used as a flexible substrate buffer layer under the following conditions: power 80-120 W, air pressure 0.5-2 Pa, temperature 200-400°C; (3) using pulsed DC sputtering to prepare copper alloy gate electrodes, and then using photolithography to prepare patterned gate interconnects; (4) Performing nitrogen gradient temperature annealing on the gate at at least two temperatures, 100 to 400°C, for 0.5 to 3 hours; (5) SiO was prepared by plasma enhanced chemical vapor deposition under the same conditions as step (2). x / SiN x The laminated film serves as a gate insulating layer; (6) preparing an IGZO semiconductor layer by pulsed DC sputtering process and covering the back channel with an etch stop layer by photolithography patterning; (7) Prepare copper alloy source and drain electrodes by pulsed DC sputtering, and then pattern them by photolithography to obtain a flexible device integrated array; (8) Annealing the flexible device integrated array under the following conditions: annealing at 100-400°C for 0.5-3h at a pressure of 5-20mTorr; (9) Plasma enhanced chemical vapor deposition (PECVD) is used to deposit SiO on the annealed flexible device integrated array under the same conditions as step (2). x / SiN x The laminated film acts as a passivation layer; The pulsed DC sputtering process in step (3) is as follows: sputtering power is 60-120 W, gas pressure is 1-5 mTorr, pure argon atmosphere, frequency is 10-20 kHz, duty cycle is 80-98%; the thickness of the copper alloy gate electrode is 100-200 nm; The pulsed DC sputtering process in step (6) is as follows: the sputtering power is 60 to 120 W, the gas pressure is 1 to 5 mTorr, the argon / oxygen ratio is 99:1 to 90:10, the frequency is 10 to 20 kHz, the duty cycle is 80 to 98%, and the thickness of the IGZO semiconductor layer is 10 to 30 nm; The pulsed DC sputtering process in step (7) is as follows: sputtering power is 60-120 W, gas pressure is 1-5 mTorr, pure argon atmosphere, frequency is 10-20 kHz, duty cycle is 80-98%, and the thickness of the copper alloy source and drain electrodes is 100-200 nm.
2. A method for eliminating residual stress of a flexible integrated device by interface compensation according to claim 1, characterized in that: The copper alloy in steps (3) and (7) is a CuCrZr ternary alloy, and the composition ratio is Cu: 98-99.9wt%, Cr: 0-2wt%, Zr: 0-2wt%.
3. The method for eliminating residual stress of a flexible integrated device by interface compensation according to claim 1, characterized in that: Preparation of SiO by plasma enhanced chemical vapor deposition in steps (2), (5) and (9) x / SiN x Layered film, SiO x The thickness of SiN is 100~300nm. x The thickness is 20 to 100 nm.
4. The method for eliminating residual stress of a flexible integrated device by interface compensation according to claim 1, characterized in that: The gradient temperature annealing conditions of step (4) are: first raise the temperature to 200°C and keep it for 20 minutes, then raise the temperature to 400°C and keep it for 30 minutes, then cool down to 200°C and keep it for 30 minutes, then raise the temperature to 400°C and keep it for 30 minutes, then cool down to 200°C and keep it for 30 minutes, finally cool down to room temperature.
5. The method for eliminating residual stress of a flexible integrated device by interface compensation according to claim 1, characterized in that: The photolithography process in step (3) and the photolithography patterning in steps (6) and (7) all use micron-level photolithography technology to pattern the functional layer.
6. The method for eliminating residual stress of a flexible integrated device by interface compensation according to claim 1, characterized in that: The pulsed DC sputtering in steps (3), (6) and (7) all adopts a sputtering working mode in which the equipment power supply provides a DC + reverse pulse voltage.
7. The method for eliminating residual stress of a flexible integrated device by interface compensation according to claim 1, characterized in that: The flexible substrate in step (1) is a polyimide substrate.