Composite ceramic coated fiber diaphragm and preparation method thereof, lithium battery

By using composite ceramic coated fiber separator in lithium-ion batteries, the heat shrinkage problem of traditional separator under high magnification and high temperature conditions is solved, the safety and cycle life of the battery are improved, and the heat resistance of the separator is enhanced. Mechanical properties.

CN114388979BActive Publication Date: 2024-11-22FULLYMAX BATTERY CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202210041340.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-14
Publication Date
2024-11-22
Estimated Expiration
2042-01-14

AI Technical Summary

Technical Problem

Traditional lithium-ion battery separators have thermal shrinkage problems under high magnification and high temperature conditions, resulting in battery failure, fire and explosion, affecting safety performance.

Method used

Using the preparation method of composite ceramic coated fiber membrane, porous membrane electrospinning operation is performed on the cellulose membrane through electrospinning liquid, and nanoceramic coated slurry is coated on the surface to form heat-resistant and high mechanical strength. Diaphragm.

Benefits of technology

It improves the thermal stability and safety of lithium batteries, extends the cycle life, enhances the high temperature resistance of the diaphragm, prevents large-area shrinkage and perforation of the diaphragm, and improves the rate performance and liquid retention ability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114388979B_ABST
    Figure CN114388979B_ABST
Patent Text Reader

Abstract

The present application provides a composite ceramic coated fiber diaphragm and a preparation method thereof, and a lithium battery. The preparation method of the composite ceramic coated fiber diaphragm comprises the following steps: preparing an electrospinning solution; performing a porous membrane electrospinning operation on a cellulose membrane using the electrospinning solution to obtain a precursor membrane; preparing a nano-ceramic coating slurry; and coating the nano-ceramic coating slurry on both sides of the precursor membrane to obtain a composite ceramic coated cellulose diaphragm. The composite diaphragm prepared by the preparation method of the composite ceramic coated fiber diaphragm has the advantages of strong thermal stability and high safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a composite ceramic coated fiber diaphragm and a preparation method thereof, and a lithium battery. Background Art

[0002] Lithium-ion battery is a secondary battery, which is widely used due to its long life, high energy density, fast charging speed and other characteristics. The separator is one of the key internal components of lithium-ion battery. At present, polyolefin microporous film materials are widely used as separators for lithium-ion batteries. The separator has a vital influence on the actual performance of the battery. It must have good chemical and electrochemical stability, provide channels for lithium ions to penetrate and flow between the positive and negative electrodes, have good electrolyte absorption and liquid retention capabilities, and have certain tensile strength and puncture resistance to prevent lithium-ion batteries from short-circuiting. The interface compatibility between the separator material and the electrode has a great influence on the charge and discharge performance and cycle performance of lithium-ion batteries.

[0003] With the extensive use of new energy vehicles, high-rate and large-capacity batteries have been developed one after another. The traditional diaphragm has a low melting point and its thermal shrinkage problem can cause battery failure, fire and explosion, which undoubtedly poses a great challenge to the safety performance of lithium-ion batteries. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a composite ceramic coated fiber diaphragm with strong thermal stability and high safety, a preparation method thereof, and a lithium battery.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A method for preparing a composite ceramic coated fiber diaphragm comprises the following steps:

[0007] preparing electrospinning solution;

[0008] Performing a porous membrane electrospinning operation on the cellulose membrane by applying the electrospinning solution to obtain a precursor membrane;

[0009] Preparing nano-ceramic coating slurry;

[0010] The nano-ceramic coating slurry is coated on both sides of the precursor film respectively to obtain the composite ceramic coated cellulose separator.

[0011] In one embodiment, the porous membrane electrospinning operation specifically comprises the following steps:

[0012] Performing a first porous membrane electrospinning operation on the surface of the fiber membrane with the electrospinning solution to obtain a first porous membrane;

[0013] Performing a second porous membrane electrospinning operation on the surface of the first porous membrane with the electrospinning solution to obtain a second porous membrane;

[0014] The porosity of the second porous membrane is greater than the porosity of the first porous membrane.

[0015] In one embodiment, the cellulose membrane has a thickness of 5 μm to 20 μm and a porosity of 40% to 90%.

[0016] In one embodiment, the nano-ceramic coating slurry includes the following components in mass:

[0017]

[0018] In one embodiment, the diameter of the aluminum oxide is 0.1 μm to 5 μm.

[0019] In one embodiment, the adhesive is at least one of polytetrafluoroethylene emulsion and polyvinylidene fluoride emulsion.

[0020] In one embodiment, the stabilizer is a silicate.

[0021] The present application also provides a composite ceramic coated fiber diaphragm, which is prepared by the preparation method of the composite ceramic coated fiber diaphragm described in any of the above embodiments.

[0022] The present application also provides a lithium battery, which includes the composite ceramic coated fiber diaphragm as described in the above embodiment.

[0023] Compared with the prior art, the present invention has at least the following advantages:

[0024] 1. In the preparation method of the composite ceramic coated fiber diaphragm of the present invention, an electrospinning solution is prepared, and then the electrospinning solution is subjected to a porous membrane electrospinning operation on a cellulose membrane. The cellulose membrane is used as a base membrane of the composite diaphragm, which can make the composite diaphragm have good stability. The cellulose membrane has microporous tortuosity, low self-discharge, and good wettability and liquid retention, which is beneficial to improving the liquid retention capacity of the lithium battery diaphragm and preventing the problem of easy drying up in the middle and late stages of the battery cycle, thereby effectively improving the cycle life of the lithium battery and improving the rate performance of the lithium battery.

[0025] 2. In the preparation method of the composite ceramic coated fiber diaphragm of the present invention, a nano-ceramic coating slurry is prepared, and then the nano-ceramic coating slurry is respectively coated on both sides of the precursor film, that is, a layer of ceramic material is coated on the surface of the precursor film, thereby effectively improving the heat shrinkage resistance and mechanical strength of the composite diaphragm. Due to the improvement of heat shrinkage resistance, when the diaphragm passes a large current or discharges at a multiple rate, the high temperature resistance inside the lithium battery is better, and at the same time, it can prevent the diaphragm from shrinking over a large area, avoiding the phenomenon of diaphragm perforation, thereby improving the safety and stability of the lithium battery; and because the electrospinning liquid is subjected to a porous membrane electrospinning operation on the cellulose membrane to form a porous membrane, the bonding force of the nano-ceramics on the cellulose membrane is further enhanced, thereby effectively improving the problem of easy powder shedding of traditional coated ceramics, thereby further improving the thermal stability and heat shrinkage resistance of the composite diaphragm. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0027] Figure 1 The flowchart is a method for preparing a composite ceramic coated fiber diaphragm in one embodiment. DETAILED DESCRIPTION

[0028] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0029] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0031] The present application provides a method for preparing a composite ceramic coated fiber membrane. The method for preparing the composite ceramic coated fiber membrane comprises the following steps: preparing an electrospinning solution; performing a porous membrane electrospinning operation on a cellulose membrane with the electrospinning solution to obtain a precursor membrane; preparing a nano-ceramic coating slurry; and coating the nano-ceramic coating slurry on both sides of the precursor membrane to obtain the composite ceramic coated cellulose membrane.

[0032] In the preparation method of the above-mentioned composite ceramic coated fiber diaphragm, an electrospinning solution is prepared, and then the electrospinning solution is subjected to porous membrane electrospinning operation on a cellulose membrane. The cellulose membrane is used as the base membrane of the composite diaphragm, which can make the composite diaphragm have good stability. The cellulose membrane has microporous tortuosity, low self-discharge, and good wettability and liquid retention, which is beneficial to improving the liquid retention capacity of the lithium battery diaphragm and preventing the problem of easy drying up in the middle and late stages of the battery cycle, thereby effectively improving the cycle life of the lithium battery and improving the rate performance of the lithium battery. Furthermore, by preparing a nano-ceramic coating slurry and then coating the nano-ceramic coating slurry on both sides of the precursor film, that is, coating a layer of ceramic material on the surface of the precursor film, the heat shrinkage resistance and mechanical strength of the composite diaphragm are effectively improved. Due to the improvement of heat shrinkage resistance, when the diaphragm passes a large current or discharges at a multiple rate, the high temperature resistance inside the lithium battery is better, and at the same time, it can prevent the diaphragm from shrinking over a large area, avoiding the phenomenon of diaphragm perforation, thereby improving the safety and stability of the lithium battery; and because the electrospinning liquid is used to perform a porous membrane electrospinning operation on the cellulose membrane to form a porous membrane, the bonding force of the nano-ceramics on the cellulose membrane is further enhanced, thereby effectively improving the problem of easy powder shedding of traditional coated ceramics, thereby further improving the thermal stability and heat shrinkage resistance of the composite diaphragm.

[0033] In order to better understand the preparation method of the composite ceramic coated fiber diaphragm of the present invention, the preparation method of the composite ceramic coated fiber diaphragm of the present invention is further explained below. Figure 1 As shown, a preparation method of a composite ceramic coated fiber diaphragm according to an embodiment of the present invention comprises part or all of the following steps:

[0034] S100, prepare electrospinning solution.

[0035] In this embodiment, the membrane component materials of a preset proportion are sequentially added to the organic solvent, and a stirring and mixing operation is performed to obtain an electrospinning solution. It is understandable that in order to obtain a uniform porous membrane by electrospinning, the electrospinning solution should have a certain fluidity, and the polymer substances in the membrane components need to be evenly dispersed before electrospinning. The membrane component materials of a preset proportion are sequentially added to the organic solvent, ensuring the uniformity of the dispersion of the polymer substances in the organic solvent, thereby ensuring the uniformity of the porous membrane layer.

[0036] S200, performing a porous membrane electrospinning operation on the cellulose membrane using the electrospinning solution to obtain a precursor membrane.

[0037] In the present embodiment, by preparing an electrostatic spinning solution, the electrostatic spinning solution is then subjected to a porous membrane electrostatic spinning operation on a cellulose membrane. The cellulose membrane is used as the base membrane of the composite diaphragm, which can make the composite diaphragm have good stability, and the cellulose membrane has microporous tortuosity, low self-discharge, and good infiltration and liquid retention, which is conducive to improving the liquid retention capacity of the lithium battery diaphragm, and preventing the problem of easy drying in the middle and late stages of the battery cycle, thereby effectively improving the cycle life of the lithium battery and improving the rate performance of the lithium battery. In addition, the fiber filaments of the porous membrane obtained by the electrostatic spinning operation are stacked and arranged in a set direction, have a porous structure, and have a large specific surface area, which can be conducive to the electrolyte passing through the diaphragm, further improving the infiltration and liquid retention effect of the diaphragm. Moreover, the porous membrane obtained by the electrostatic spinning operation has good mechanical properties, thereby improving the safety of the diaphragm during use.

[0038] S300, preparing nano-ceramic coating slurry.

[0039] In this embodiment, a preset amount of nano-ceramic component material is weighed, dissolved in deionized water, and subjected to a high-speed dispersion operation to obtain a uniform nano-ceramic coating slurry, thereby improving the adhesion of the nano-ceramic coating slurry on the precursor film, and also improving the uniformity of the nano-ceramic in the diaphragm, thereby improving the overall heat shrinkage resistance and safety of the composite diaphragm. Further, the high-speed dispersion operation time is 2.5 hours to 3.5 hours, thereby effectively improving the dispersion and uniformity of the nano-ceramic coating slurry.

[0040] S400, coating the nano-ceramic coating slurry on both sides of the precursor film respectively to obtain a composite ceramic coated cellulose separator.

[0041] In this embodiment, by preparing a nano-ceramic coating slurry, the nano-ceramic coating slurry is then applied to both sides of the precursor film, that is, a layer of ceramic material is applied to the surface of the precursor film, thereby effectively improving the heat shrinkage resistance and mechanical strength of the composite diaphragm. Due to the improvement of heat shrinkage resistance, when the diaphragm passes a large current or discharges at a rate, the high temperature resistance inside the lithium battery is better, and at the same time, it can prevent the diaphragm from shrinking over a large area, avoiding the phenomenon of diaphragm perforation, thereby improving the safety and stability of the lithium battery; and because the electrospinning liquid is electrospinned on the cellulose film to form a porous film, the bonding force of the nano-ceramic on the cellulose film is further enhanced, thereby effectively improving the problem of easy powder loss of traditional ceramic coating, thereby further improving the thermal stability and heat shrinkage resistance of the composite diaphragm. Further, after the nano-ceramic coating slurry is applied to both sides of the precursor film, the nano-ceramic coating slurry is dried, so that the nano-ceramic coating slurry is solidified in the precursor film to form a stable composite ceramic coated cellulose diaphragm.

[0042] In one embodiment, before the step of electrospinning the electrospinning solution on the cellulose membrane to perform a porous membrane electrospinning operation, the method for preparing the composite ceramic coated fiber membrane further includes the following steps: performing a solvent spraying operation on the surface of the fiber membrane. It is understandable that in the process of electrospinning the porous membrane, due to the weak bonding force between the spinning and the surface of the cellulose membrane, the spinning is prone to displacement or spinning breakage on the surface of the cellulose membrane, thereby reducing the bonding force between the porous membrane layer and the cellulose membrane layer, and destroying the structural stability and flatness of the composite ceramic coated fiber membrane. In order to improve the structural stability and flatness of the composite ceramic coated fiber diaphragm, in this embodiment, before the porous membrane electrospinning operation, the solvent spraying operation is performed on the upper and lower surfaces of the base membrane, that is, the cellulose membrane. The solvent adopts the solvent of the electrospinning solution. On the one hand, the solvent can corrode the surface of the cellulose membrane, thereby enhancing the adhesion between the surface of the cellulose membrane and the spinning, and preventing the spinning from easily shifting or breaking on the surface of the cellulose membrane; on the other hand, the solvent on the cellulose surface and the solvent in the electrospinning solution are similar and compatible, so that during the electrospinning process, the spinning and the cellulose membrane have a strong bonding force, which effectively solves the problem that the spinning is easily displaced or broken on the surface of the cellulose membrane, thereby improving the bonding force between the porous membrane layer and the cellulose membrane layer, improving the structural stability and flatness of the composite ceramic coated fiber diaphragm, and then improving the heat shrinkage resistance and thermal stability of the composite ceramic coated cellulose diaphragm. Further, the amount of solvent sprayed is just enough to cover the surface of the cellulose membrane.

[0043] In one embodiment, the coating amount of the nano-ceramic coating slurry is 3g / m 2 ~5g / m 2In this embodiment, the prepared nano-ceramic coating slurry is coated on both sides of the precursor film, and the coating amount on both sides is 3g / m 2 ~5g / m 2 On the one hand, it can effectively ensure the heat shrinkage resistance and high temperature resistance of nano-ceramics, so that the composite diaphragm can maintain the complete shape of the diaphragm at 180℃~250℃. At 250℃~350℃, the diaphragm will not melt immediately, the lithium battery will not short-circuit immediately, and the lithium battery will fail slowly instead of easily experiencing a violent failure mode.

[0044] In one embodiment, the porous membrane electrospinning operation specifically includes the following steps:

[0045] S210, performing a first porous membrane electrospinning operation on the surface of the fiber membrane using the electrospinning liquid to obtain a first porous membrane.

[0046] In this embodiment, the porous membrane obtained by directional electrospinning is regularly stacked and arranged, which is conducive to forming a denser fiber membrane layer, namely the first porous membrane, so that the first porous membrane has a mechanical structure with high strength, thereby effectively improving the heat shrinkage resistance, stability and safety of the composite membrane. In this embodiment, the electrospinning solution is firstly subjected to a porous membrane electrospinning operation on one side of the fiber membrane, and then the electrospinning solution is subjected to a porous membrane electrospinning operation on the other side of the fiber membrane, thereby forming a first porous membrane layer on both sides of the fiber membrane.

[0047] S220, subjecting the electrospinning solution to a second porous membrane electrospinning operation on the surface of the first porous membrane to obtain a second porous membrane; wherein the porosity of the second porous membrane is greater than the porosity of the first porous membrane.

[0048] In this embodiment, the disordered interweaving or random stacking arrangement of the disordered fiber membrane layer obtained by the disordered electrospinning operation is conducive to forming a loose fiber diaphragm layer with a higher porosity, that is, the second porous membrane, so that the second porous membrane has a better liquid locking ability, thereby effectively improving the liquid retention capacity of the lithium battery diaphragm, preventing the problem of easy drying in the middle and late stages of the battery cycle, thereby effectively improving the cycle life of the lithium battery and improving the rate performance of the lithium battery. In this embodiment, the electrospinning solution is first subjected to a porous membrane electrospinning operation on one side of the first porous membrane, and then the electrospinning solution is subjected to a porous membrane electrospinning operation on the other side of the first porous membrane, thereby forming a second porous membrane on both sides of the fiber membrane. Furthermore, the porosity of the second porous membrane is greater than that of the first porous membrane, and the first porous membrane with lower porosity is electrospun on the fiber base membrane, that is, a porous membrane with higher density is formed in the inner layer of the diaphragm, so that the composite diaphragm has a mechanical structure with higher strength, which can improve the heat shrinkage resistance, stability and safety of the composite diaphragm; and the second porous membrane with higher porosity is electrospun on the first porous membrane, that is, a porous membrane with better looseness is formed in the outer layer of the diaphragm, so that the composite diaphragm has better liquid retention ability, preventing the problem of easy drying in the middle and late stages of the battery cycle, thereby effectively improving the cycle life of the lithium battery and improving the rate performance of the lithium battery. By combining the fiber base membrane with the first porous membrane and the second porous membrane, not only can the heat shrinkage resistance of the diaphragm be improved, but also the liquid retention effect of the diaphragm can be improved at the same time.

[0049] Further, the electrospinning solution includes a first electrospinning solution and a second electrospinning solution, the first electrospinning solution is used to perform a first porous membrane electrospinning operation on the surface of the fiber membrane, and the second electrospinning solution is used to perform a second porous membrane electrospinning operation on the surface of the first porous membrane. In the present embodiment, in the first electrospinning solution, the mass percentage of the polymer is 10wt% to 35wt%. It can be understood that in the first electrospinning solution, the content of the polymer is too low, and the first electrospinning solution cannot effectively form a charged jet to form a dense fiber membrane layer with a certain porosity and a large specific surface area. The content of the polymer is too high, and the fluidity of the first electrospinning solution is poor and cannot be electrospun to form a dense fiber membrane layer. Therefore, in the first electrospinning solution, the mass percentage of the polymer substance is made to be 10wt% to 35wt%, ensuring that the first electrospinning solution can be electrospun, and that the obtained dense fiber membrane layer has a certain porosity and a large specific surface area, as well as ensuring the mechanical properties and deformation resistance of the fiber filaments forming the dense fiber membrane layer, thereby ensuring the mechanical properties and deformation resistance of the dense fiber membrane layer.

[0050] Furthermore, in the second electrospinning solution, the mass percentage of the polymer is 10wt% to 35wt%. It can be understood that in the second electrospinning solution, the content of the polymer is too low, and the second electrospinning solution cannot effectively form a charged jet to form a loose fiber membrane layer with a certain porosity and a large specific surface area. The content of the polymer is too high, and the fluidity of the second electrospinning solution is poor and it is impossible to perform electrospinning to form a loose fiber membrane layer. Therefore, in the second electrospinning solution, the mass percentage of the polymer is 10wt% to 35wt%, which ensures that the second electrospinning solution can be electrospun, and ensures that the obtained loose fiber membrane layer has a high porosity and a large specific surface area, as well as the mechanical properties and deformation resistance of the fiber filaments that form the selected loose fiber membrane layer, thereby ensuring the mechanical properties and deformation resistance of the loose fiber membrane layer.

[0051] In one of the embodiments, the extrusion speed of the electrospinning solution in the electrospinning operation of the porous membrane is 0.03 mL / min to 0.5 mL / min. In this embodiment, the electrospinning is performed using an electrospinning machine with a spinning solution extrusion speed set to 0.03 mL / min to 0.5 mL / min, thereby ensuring the porosity and specific surface area of ​​the nano-silicon dioxide layer, thereby further improving the liquid retention capacity of the silicon-containing diaphragm.

[0052] In one embodiment, the voltage is set to 5kV to 20kV during the electrospinning operation of the porous membrane. In this embodiment, an electrospinning machine with a set voltage of 5kV to 20kV is used for electrospinning, which ensures the porosity and specific surface area of ​​the nano-silicon dioxide layer, thereby further improving the liquid retention capacity of the silicon-containing diaphragm.

[0053] In one of the embodiments, the distance between the spinning solution nozzle and the receiving substrate during the electrospinning operation of the porous membrane is 8 cm to 35 cm. In this embodiment, an electrospinning machine with a distance between the spinning solution nozzle and the receiving substrate set to 8 cm to 35 cm is used for electrospinning, which ensures the porosity and specific surface area of ​​the nano-silicon dioxide layer, thereby further improving the liquid retention capacity of the silicon-containing diaphragm.

[0054] It should be noted that the electrospinning machine includes a reservoir, a syringe, a nozzle, a high-voltage power supply and a receiver. The reservoir is connected to the syringe to provide the syringe with spinning solution, the syringe is connected to the nozzle, the nozzle is used to spray the spinning solution, the nozzle is connected to the high-voltage power supply, and the nozzle and the syringe are arranged correspondingly. The process of electrospinning the spinning solution is that the spinning solution is stored in the reservoir, the spinning solution is extruded from the nozzle, the injection speed of the spinning solution is controlled by the syringe with a capillary, and the spinning solution extruded from the nozzle is subjected to the combined action of the electric field force formed by the high-voltage power supply and the electrostatic repulsion to form a charged jet. Under the action of the electric field force, the charged jet is stretched and thinned, and then received by the receiver. After the spinning solution is fixed and formed, it is deposited on the receiving substrate of the receiver.

[0055] In one embodiment, after the step of preparing the electrospinning solution, and before the step of electrospinning the electrospinning solution on the cellulose membrane to obtain the precursor membrane, the preparation method of the composite ceramic coated fiber membrane also includes the following steps: performing a surface treatment operation on the cellulose membrane. It can be understood that the cellulose membrane provides a carrier for the electrospinning of the composite membrane, and the electrospinning solution containing nano-silicon dioxide is electrospun on the surface of the cellulose membrane by an electrospinning machine. If there are impurities on the surface of the cellulose membrane, it is easy to affect the binding force between the spinning and the cellulose membrane. In order to improve the binding force between the spinning and the cellulose membrane, in this embodiment, the cellulose membrane is washed with water, which can effectively remove impurities on the surface of the cellulose membrane, thereby ensuring the neatness of the surface of the cellulose membrane. Further, the surface of the cellulose membrane is subjected to a corona operation, thereby increasing the roughness and surface area of ​​the cellulose membrane surface, increasing the bonding strength of the cellulose membrane surface, and then increasing the binding force between the spinning and the cellulose membrane, and increasing the structural stability of the composite membrane.

[0056] In one of the embodiments, the thickness of the cellulose membrane is 5μm to 20μm, and the porosity is 40% to 90%. It is understandable that the cellulose membrane is used as the base membrane of the diaphragm. If the structural strength of the cellulose membrane is weak, the safety of the composite diaphragm is likely to be low, and perforation is likely to occur; if the porosity of the cellulose membrane is low, it is likely to cause the composite diaphragm to have poor liquid retention. In order to improve the safety and liquid retention of the composite diaphragm, in this embodiment, the thickness of the cellulose membrane is 5μm to 20μm, and the porosity is 40% to 90%, so that the cellulose membrane not only has a high structural strength, improves the safety and heat shrinkage resistance of the composite diaphragm, but also facilitates the electrolyte to pass through the composite diaphragm, thereby improving the infiltration and liquid retention of the composite diaphragm, preventing the problem of easy drying in the middle and late stages of the battery cycle, thereby effectively improving the cycle life of the lithium battery, while improving the rate performance of the lithium battery. Furthermore, the cellulose membrane used in this embodiment has a dimensional shrinkage of less than 0.1% at 180 degrees Celsius, a thickness of 5um to 20um, a porosity of 40% to 90%, an air permeability of (5s to 700s) / 100cc, an electrolyte absorption rate of 100%-300%, and a mechanical stretching of 3MPa to 30MPa.

[0057] In one of the embodiments, the nano-ceramic coating slurry includes the following components by mass: 10 to 30 parts of aluminum oxide, 0.5 to 10 parts of adhesive, 0.1 to 2 parts of stabilizer and 0.2 to 1 part of surfactant. In this embodiment, the nano-ceramic coating slurry is formed by preparing aluminum oxide, adhesive, stabilizer and surfactant, and the nano-ceramic coating slurry is applied to the surface of the cellulose membrane, and the PVDF glue technology is applied to the composite coating, which can effectively improve the powdering problem of traditional ceramic coating and improve the stability of the composite diaphragm. Furthermore, aluminum oxide has good electrical insulation, corrosion resistance and wear resistance. Using 10 to 30 parts of aluminum oxide for nano-ceramic coating slurry can effectively improve the electrical insulation, mechanical strength and high temperature resistance of nano-ceramics. 0.5 to 10 parts of adhesive can effectively improve the bonding force of the nano-ceramic coating slurry, so that the nano-ceramic coating slurry has good adhesion after being applied to the cellulose membrane, and prevent the occurrence of nano-ceramic powdering. Using 0.1 to 2 parts of stabilizer in nano-ceramic coating slurry can slow down the reaction, maintain chemical balance, reduce surface tension, and prevent light, heat or oxidative decomposition. 0.2 to 1 part of surfactant can make the two phases in the slurry have affinity through different parts of the molecule, so that both phases regard it as a component of the original phase, and the molecules are arranged between the two phases, so that the surface of the two phases is equivalent to being transferred into the interior of the molecule. Thus, the surface tension is reduced. Since both phases regard it as a component of the original phase, it is equivalent to that the two phases have no interface with the surfactant molecules, which is equivalent to partially eliminating the interface between the two phases in this way, that is, reducing the surface tension and surface free energy.

[0058] In one embodiment, the diameter of alumina is 0.1 μm to 5 μm. It is understandable that alumina powder has the properties of acid and alkali resistance, high temperature resistance, high hardness, high melting point, high thermal conductivity and high resistivity. The nano-ceramic coating slurry prepared from alumina can have good heat shrinkage resistance and can improve the safety of lithium batteries. However, if the diameter of alumina is too large, it is easy to make the dispersibility of the nano-ceramic coating slurry poor, and the adhesion of the alumina powder is poor, and it is easy to fall off; if the diameter of alumina is too small, there are more nodes forming a network, which makes the thermal conductivity poor. In order to improve the dispersibility and thermal conductivity of the nano-ceramic coating slurry, in this embodiment, the diameter of the alumina powder is 0.1 μm to 5 μm, so that the alumina powder has better dispersibility in the nano-ceramic coating slurry, and at the same time, there are fewer nodes of alumina forming a network in the nano-ceramic coating slurry system, thereby improving the thermal conductivity of the nano-ceramic and effectively improving the heat shrinkage resistance of the composite diaphragm.

[0059] Further, the alumina is a nano alumina powder with a particle size ratio D1 / D2 of 0.10 to 0.20, the large particle size D2 in the nano alumina powder is greater than 0.1um and less than 1.0um, and the content of large particle size alumina is 50% to 90% of the total mass of the alumina powder; the small particle size D1 is less than 0.1um, and the content of small particle size alumina is 10% to 50% of the total mass of the alumina powder. In this embodiment, the nano alumina powder includes large particle size powder and small particle size powder, and the content of large particle size alumina is 50% to 90% of the total mass of the alumina powder, and the content of small particle size alumina is 10% to 50% of the total mass of the alumina powder, which can effectively improve the stacking uniformity of nanoparticles, and make the bonding force of nano ceramic particles larger, effectively prevent powder loss, and at the same time, combined with PVDF glue technology, it is beneficial to exert the ability of the diaphragm to retain liquid and quickly migrate lithium ions, thereby improving the performance of lithium batteries.

[0060] In one embodiment, the adhesive is at least one of polytetrafluoroethylene emulsion and polyvinylidene fluoride emulsion. In the present embodiment, polytetrafluoroethylene has relatively excellent chemical stability, electrical insulation, self-lubrication, non-flammability, atmospheric aging resistance and high and low temperature adaptability, and has high mechanical strength. Using polytetrafluoroethylene emulsion as an adhesive for nano-ceramic coating slurry can effectively improve the mechanical strength and electrical properties of the composite diaphragm, thereby improving the electrical properties of the lithium battery. However, the wetting properties of polytetrafluoroethylene materials are poor and difficult to be bonded. In the present embodiment, by proportioning surfactants, stabilizers and alumina with polytetrafluoroethylene emulsion, the wettability and dispersibility of polytetrafluoroethylene emulsion can be effectively improved, thereby improving the adhesion between polytetrafluoroethylene emulsion and other components of nano-ceramic coating slurry and cellulose film layer, and then improving the stability of the composite diaphragm. In addition, since the base membrane of the composite diaphragm adopts cellulose membrane and the surface is coated with nano-ceramic slurry, the problem of traditional ceramic powder falling can be effectively improved by combining the polyvinylidene fluoride emulsion technology.

[0061] In one embodiment, the stabilizer is a silicate. It is understood that silicates exist in the form of complex colloidal particles with negative charges in the solution, which can attract positively charged aluminum ions accumulated near the aluminum metal corrosion point to themselves, interact with silicon dioxide, and generate aluminum silicate; thereby blocking anode corrosion. In this embodiment, 0.1 to 2 parts of stabilizer are used in nano-ceramic slurry, and the ratio of alumina, stabilizer and surfactant is enhanced, so that heat transfer corrosion on the surface of nano-ceramics can be better prevented.

[0062] Example 1

[0063] The membrane component materials of a preset proportion are sequentially added to an organic solvent, and stirred and mixed to obtain an electrospinning solution. The electrospinning solution is then subjected to a porous membrane electrospinning operation on a cellulose membrane to form a porous membrane layer, wherein the thickness of the cellulose membrane is 5 μm and the porosity is 40%. A preset amount of nano-ceramic component materials is weighed, dissolved in deionized water, and subjected to a high-speed dispersion operation to obtain a uniform nano-ceramic coating slurry, wherein the nano-ceramic coating slurry includes 10 wt% of alumina with a diameter of 0.1 μm, 0.5 wt% of an adhesive, 0.1 wt% of a stabilizer, and 0.2 wt% of a surfactant. The nano-ceramic coating slurry is applied to both sides of the precursor membrane to obtain a composite ceramic-coated cellulose membrane.

[0064] Example 2

[0065] The preset proportion of the membrane component materials is sequentially added to the organic solvent, and the stirring and mixing operation is performed to obtain an electrospinning solution. The electrospinning solution is then subjected to a porous membrane electrospinning operation on a cellulose membrane to form a porous membrane layer, wherein the thickness of the cellulose membrane is 20 μm and the porosity is 90%. A preset amount of nano-ceramic component materials is weighed, dissolved in deionized water, and subjected to a high-speed dispersion operation to obtain a uniform nano-ceramic coating slurry, wherein the nano-ceramic coating slurry includes 30 wt% of alumina with a diameter of 5 μm, 10 wt% of an adhesive, 2 wt% of a stabilizer, and 1 wt% of a surfactant. The nano-ceramic coating slurry is applied to both sides of the precursor membrane to obtain a composite ceramic-coated cellulose membrane.

[0066] Example 3

[0067] The membrane component materials of a preset proportion are sequentially added to an organic solvent, and stirred and mixed to obtain an electrospinning solution. The electrospinning solution is then subjected to a porous membrane electrospinning operation on a cellulose membrane to form a porous membrane layer, wherein the thickness of the cellulose membrane is 10 μm and the porosity is 60%. A preset amount of nano-ceramic component materials is weighed, dissolved in deionized water, and subjected to a high-speed dispersion operation to obtain a uniform nano-ceramic coating slurry, wherein the nano-ceramic coating slurry includes 20 wt% of alumina with a diameter of 2 μm, 5 wt% of an adhesive, 1 wt% of a stabilizer, and 0.8 wt% of a surfactant. The nano-ceramic coating slurry is applied to both sides of the precursor membrane to obtain a composite ceramic-coated cellulose membrane.

[0068] Example 4

[0069] The membrane component materials of a preset proportion are sequentially added to an organic solvent, and stirred and mixed to obtain an electrospinning solution. The electrospinning solution is then subjected to a porous membrane electrospinning operation on a cellulose membrane to form a porous membrane layer, wherein the thickness of the cellulose membrane is 12 μm and the porosity is 70%. A preset amount of nano-ceramic component materials is weighed, dissolved in deionized water, and subjected to a high-speed dispersion operation to obtain a uniform nano-ceramic coating slurry, wherein the nano-ceramic coating slurry includes 25 wt% of alumina with a diameter of 3 μm, 8 wt% of an adhesive, 1.5 wt% of a stabilizer, and 0.7 wt% of a surfactant. The nano-ceramic coating slurry is applied to both sides of the precursor membrane to obtain a composite ceramic-coated cellulose membrane.

[0070] Compared with the prior art, the present invention has at least the following advantages:

[0071] 1. In the preparation method of the composite ceramic coated fiber diaphragm of the present invention, an electrospinning solution is prepared, and then the electrospinning solution is subjected to a porous membrane electrospinning operation on a cellulose membrane. The cellulose membrane is used as a base membrane of the composite diaphragm, which can make the composite diaphragm have good stability. The cellulose membrane has microporous tortuosity, low self-discharge, and good wettability and liquid retention, which is beneficial to improving the liquid retention capacity of the lithium battery diaphragm and preventing the problem of easy drying up in the middle and late stages of the battery cycle, thereby effectively improving the cycle life of the lithium battery and improving the rate performance of the lithium battery.

[0072] 2. In the preparation method of the composite ceramic coated fiber diaphragm of the present invention, a nano-ceramic coating slurry is prepared, and then the nano-ceramic coating slurry is respectively coated on both sides of the precursor film, that is, a layer of ceramic material is coated on the surface of the precursor film, thereby effectively improving the heat shrinkage resistance and mechanical strength of the composite diaphragm. Due to the improvement of heat shrinkage resistance, when the diaphragm passes a large current or discharges at a multiple rate, the high temperature resistance inside the lithium battery is better, and at the same time, it can prevent the diaphragm from shrinking over a large area, avoiding the phenomenon of diaphragm perforation, thereby improving the safety and stability of the lithium battery; and because the electrospinning liquid is subjected to a porous membrane electrospinning operation on the cellulose membrane to form a porous membrane, the bonding force of the nano-ceramics on the cellulose membrane is further enhanced, thereby effectively improving the problem of easy powder shedding of traditional coated ceramics, thereby further improving the thermal stability and heat shrinkage resistance of the composite diaphragm.

[0073] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a composite ceramic coated fiber diaphragm, characterized in that: The following steps are involved: preparing electrospinning solution; The cellulose film is subjected to a surface treatment operation, wherein the surface treatment operation comprises the following specific steps: washing the cellulose film with water, and further, performing a corona treatment operation on the surface of the cellulose film; The electrospinning solution is subjected to a porous membrane electrospinning operation on a cellulose membrane to obtain a precursor membrane; wherein the cellulose membrane has microporous tortuosity; The porous membrane electrospinning operation specifically comprises the following steps: First, the electrospinning liquid is subjected to a porous membrane electrospinning operation on one side of the fiber membrane, and then the electrospinning liquid is subjected to a porous membrane electrospinning operation on the other side of the fiber membrane, so as to form a first porous membrane on both sides of the fiber membrane; wherein the porous membrane obtained by directional electrospinning of the first porous membrane is regularly stacked and arranged, which is conducive to forming a denser fiber diaphragm layer; First, an electrospinning liquid is subjected to a porous membrane electrospinning operation on one side of a first porous membrane, and then an electrospinning liquid is subjected to a porous membrane electrospinning operation on the other side of the first porous membrane, thereby forming a second porous membrane on both sides of the fiber membrane; wherein the second porous membrane is subjected to a disordered electrospinning operation to obtain a disordered interweaving or random stacking arrangement of a selectively permeable disordered fiber membrane layer, which is conducive to forming a loose fiber diaphragm layer with a higher porosity; and the porosity of the second porous membrane is greater than the porosity of the first porous membrane; The electrospinning solution comprises a first electrospinning solution and a second electrospinning solution, wherein the first electrospinning solution is used for performing the electrospinning operation of the first porous membrane on the surface of the fiber membrane; In the first electrospinning solution, the mass percentage of the polymer substance is 10wt%~35wt%; In the second electrospinning solution, the mass percentage of the polymer substance is 10wt%~35wt%; Prepare a nano-ceramic coating slurry; wherein the nano-ceramic coating slurry includes the following components in mass: Alumina 10 to 30 parts; Adhesive 0.5~10 parts; Stabilizer 0.1~2 parts; Surfactant 0.2~1 part; The diameter of the aluminum oxide is 0.1 μm to 5 μm; The nano-ceramic coating slurry is coated on both sides of the precursor film respectively to obtain the composite ceramic coated cellulose separator.

2. The method for preparing the composite ceramic coated fiber diaphragm according to claim 1, characterized in that: The cellulose membrane has a thickness of 5 μm to 20 μm and a porosity of 40% to 90%.

3. The method for preparing the composite ceramic coated fiber diaphragm according to claim 1, characterized in that: The adhesive is at least one of polytetrafluoroethylene emulsion and polyvinylidene fluoride emulsion.

4. The method for preparing the composite ceramic coated fiber diaphragm according to claim 1, characterized in that: The surfactant is at least one of tertiary alkyl polyol polyethylene ether and polyether modified silicone.

5. The method for preparing the composite ceramic coated fiber diaphragm according to claim 1, characterized in that: The stabilizer is a silicate.

6. A composite ceramic coated fiber diaphragm, characterized in that: The composite ceramic coated fiber diaphragm is prepared by the preparation method of the composite ceramic coated fiber diaphragm according to any one of claims 1 to 5.

7. A lithium battery, characterized in that: The lithium battery comprises the composite ceramic coated fiber separator as claimed in claim 6.

Citation Information

Patent Citations

  • Ceramic coating diaphragm for lithium battery and preparation method of ceramic coating diaphragm

    CN104269509A

  • Environment friendly battery diaphragm and preparation method thereof

    CN104766937A

  • Composite lithium ion battery diaphragm and preparation method thereof

    CN104766938A

  • Nonwoven fabric lithium ion battery composite diaphragm and preparation method thereof

    CN104835931A

  • Diaphragm, preparation method thereof and battery

    CN109950461A