A bismuth-based photocatalytic material and its preparation method and application
By introducing Cu2O into the BiOBr photocatalyst to improve its specific surface area and adsorption performance, the problems of low BiOBr photocatalytic activity and low Cu2O photocatalytic efficiency are solved, and an efficient photocatalytic degradation effect is achieved, especially in the presence of hydrogen peroxide. Significantly improves degradation efficiency and reduces the risk of photocorrosion.
Patent Information
- Application Number
- CN202111594104.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-22
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-12-22
AI Technical Summary
In the existing technology, the photocatalytic activity of BiOBr photocatalyst is low, and the photocatalytic efficiency of Cu2O is not high, which leads to limitations in its practical application. In particular, the photocorrosion problem affects the application prospects of cuprous oxide.
By uniformly mixing cuprous salt and bismuth salt in an organic solvent, adding a bromine source and reacting at high temperature, a bismuth-based photocatalytic material is formed. Cu2O is introduced to enhance its specific surface area and adsorption performance, and through the replacement structure of Cu2+/Cu+ and Bi3+ Improve electron transfer efficiency and reduce the recombination rate of holes and electrons.
The photocatalytic effect is significantly improved and the adsorption performance of the catalytic material is enhanced. Especially in the presence of hydrogen peroxide, the photocatalytic degradation effect is excellent, the degradation efficiency reaches more than 80%, the cost is low, the operation is simple, and it has industrial application prospects.
Smart Images

Figure CN114405523B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalytic materials, and in particular to a bismuth-based photocatalytic material and a preparation method and application thereof. Background Art
[0002] Dye wastewater is a common industrial wastewater with complex chemical composition, high hardness and difficulty in achieving complete degradation. The general treatment methods can no longer achieve the expected results. In recent years, the rapid development of photocatalytic technology in the treatment of such pollution has provided an effective way to degrade dye wastewater. Among them, the degradation effect of bismuth oxides is particularly significant. More importantly, bismuth oxides have a narrow band gap and can fully absorb photons under visible light, resulting in a wider absorption range of visible light, so the photocatalytic activity under visible light is more prominent. Due to these characteristics, bismuth semiconductor materials have become a hot topic of research.
[0003] Compared with TiO2 semiconductor materials, BiOBr semiconductor materials have better photocatalytic performance under visible light, and thus have become a hot topic in the field of photocatalysis. BiOBr is a new type of semiconductor photocatalytic material with a tetragonal fluorochloropyrite structure, a small bandgap and good visible light response. Literature reports many methods for preparing BiOBr catalysts, such as the BiOBr nanosheet structure prepared by Song Xiaolong et al. by loading Pt. Ding Aiqin et al. also prepared BiOBr nanosheet structure using microwave method. However, its photocatalytic activity is slightly lower than that of the modified BiOBr catalyst, and its practical application is limited. Therefore, researchers have conducted modification research on BiOBr semiconductor materials and achieved great results. In addition, the study found that its photocatalytic performance is closely related to factors such as microstructure, grain size, morphology, etc. Therefore, it is more important to focus on the photocatalytic degradation mechanism, morphology, preparation method, modification and photocatalytic performance of BiOBr.
[0004] Cu2O is a typical P-type narrow bandgap semiconductor and also a direct bandgap semiconductor. As a photocatalyst, Cu2O has the advantages of low price, non-toxicity, simple preparation method and variable bandgap, so it has great application prospects in photocatalytic technology. Studies have shown that Cu2O has considerable photocatalytic performance, and composite catalysis is superior to single catalysis, but the current photocatalytic efficiency is still not high. At the same time, photocorrosion is also the reason why cuprous oxide cannot be fully applied. In order to develop the potential of Cu2O, it is necessary to further find better preparation methods, process conditions and composite materials to improve photocatalytic efficiency and reduce photocorrosion, so as to finally achieve industrialization. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a bismuth-based photocatalytic material and a preparation method and application thereof.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] In a first aspect, the present invention provides a method for preparing a bismuth-based photocatalytic material, specifically comprising: dissolving a cuprous salt and a bismuth salt in an organic solvent, mixing them evenly, and obtaining a solution A; adding a bromine source to the solution A, reacting the solution at a high temperature for a period of time, and then freeze-drying the solution to obtain the bismuth-based photocatalytic material.
[0008] The bismuth-based photocatalytic material prepared by the present invention introduces Cu2O into the BiOBr catalytic material, which can greatly improve the photocatalytic effect, increase the specific surface area of the catalytic material, and enhance its adsorption performance. 3+ Hydrolysis to form Bi2O2 + Layered structure, while Br - Inserted into the middle of the layer, forming a stable electrical neutralization structure. 2+ Easily reduced to Cu by glacial acetic acid + , and Cu 2+ / Cu + and Bi 3+ The ionic radius is similar and can replace part of Bi in the structure 3+ If the added amount is large, it can be deposited on the surface of bismuth oxybromide to form Cu2O, which plays a heterojunction role, enhances the electron transfer efficiency, and reduces the recombination rate of holes and electrons.
[0009] Furthermore, the feeding amounts of the cuprous salt and the bismuth salt are calculated based on a molar ratio of Cu:Bi of 0.1 to 0.4.
[0010] Furthermore, the organic solvent is an ethylene glycol solution containing acetic acid. In this method, ethylene glycol is a solvent, and acetic acid plays a role in promoting the dissolution of salts.
[0011] Furthermore, the volume fraction of the acetic acid in the ethylene glycol solution is 5-20%. Furthermore, the optimum volume fraction of the acetic acid in the ethylene glycol solution is 10%.
[0012] Furthermore, the bromine source is an ethylene glycol solution containing hexadecyltrimethylammonium bromide. In the reaction of the present invention, the main function of hexadecyltrimethylammonium bromide is to provide a bromine source and also to provide a certain template effect. Specifically, there are amino groups and bromide ions at the ends of the hexadecyltrimethylammonium bromide structure, which react with Bi2O2 + There is a non-bonding interaction (van der Waals force) between them, which finally makes the whole molecule exist in Bi2O2 + After the reaction is completed, the self-structure is ionized when washed with ultrapure water, and the hexadecyltrimethylamino is eluted.
[0013] Furthermore, the molar concentration of the hexadecyltrimethylammonium bromide in ethylene glycol is 0.1 mol / L.
[0014] Furthermore, the cuprous salt or copper salt is cuprous nitrate, cupric chloride, or copper sulfate; the bismuth salt is bismuth nitrate, bismuth chloride, bismuth acetate, or bismuth sulfate.
[0015] In a second aspect, the present invention provides a bismuth-based photocatalytic material prepared according to the above preparation method.
[0016] In a third aspect, the present invention also provides an application of the above-mentioned bismuth-based photocatalytic material in degrading water pollutants.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The introduction of Cu2O into bismuth-based photocatalytic materials can greatly improve the photocatalytic effect, increase the specific surface area of the catalytic material, and enhance its adsorption performance.
[0019] (2) The operation method is simple and easy, the raw materials are easily available, the cost is low, and the possibility of practical application is high.
[0020] (3) In the presence of hydrogen peroxide, the photocatalytic degradation effect is very excellent. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is the XRD spectrum of the bismuth-based photocatalytic material of Example 1-3;
[0022] Figure 2 The degradation of sulfamethoxazole (SMX) by the bismuth-based photocatalytic material of Examples 1-3 changes with the illumination time;
[0023] Figure 3 The degradation of sulfamethoxazole (SMX) by the bismuth-based photocatalytic material of Example 2 changes with the illumination time under different conditions;
[0024] Figure 4 The graph is a graph showing the degradation of sulfamethoxazole (SMX) by the bismuth-based photocatalytic material of Example 2 as a function of illumination time under different hydrogen peroxide concentrations. DETAILED DESCRIPTION
[0025] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0026] Example 1
[0027] The present invention provides a method for preparing a bismuth-based photocatalytic material, which specifically comprises the following steps: under nitrogen protection, adding cuprous nitrate and bismuth nitrate at a molar ratio of Cu / Bi of 0.1, dissolving them in 100 mL of ethylene glycol containing 10% acetic acid by volume to prepare a solution; and adding 100 mL of ethylene glycol solution containing 0.1 mol / L hexadecyltrimethylammonium bromide to the solution; reacting at 180°C for 10 hours and then freeze-drying. The obtained sample is represented by 10-CB.
[0028] Example 2
[0029] The present invention provides a method for preparing a bismuth-based photocatalytic material, which specifically comprises the following steps: under nitrogen protection, adding cuprous nitrate and bismuth nitrate at a molar ratio of Cu / Bi of 0.2, dissolving them in 100 mL of ethylene glycol containing 10% acetic acid by volume to prepare a solution; and adding 100 mL of ethylene glycol solution containing 0.1 mol / L hexadecyltrimethylammonium bromide to the solution; reacting at 180°C for 10 hours and then freeze-drying. The obtained sample is represented by 20-CB.
[0030] Example 3
[0031] The present invention provides a method for preparing a bismuth-based photocatalytic material, which specifically comprises the following steps: under nitrogen protection, adding cuprous nitrate and bismuth nitrate at a molar ratio of Cu / Bi of 0.4, dissolving them in 100 mL of ethylene glycol containing 10% acetic acid by volume to prepare a solution; and adding 100 mL of ethylene glycol solution containing 0.1 mol / L hexadecyltrimethylammonium bromide to the solution; reacting at 180°C for 10 hours and then freeze-drying. The obtained sample is represented by 40-CB.
[0032] Comparative Example 1
[0033] This comparative example is basically the same as Example 2, the only difference being that in this comparative example, copper nitrate and bismuth nitrate are added at a molar ratio of Cu / Bi of 0.2. Compared with Comparative Example 1, the cuprous doped in Example 2 into the bismuth-based material will be oxidized to divalent copper because its unstable part will enrich the copper existence form and increase the surface active sites. Therefore, Example 2 has a better photocatalytic effect than Comparative Example 1, and can increase the specific surface area of the catalytic material and enhance its adsorption performance.
[0034] Comparative Example 2
[0035] This comparative example is basically the same as Example 2, the only difference being that the bromine source in this comparative example is potassium bromide solution. Compared with the potassium bromide in Comparative Example 2, the bromine source in Example 2 is hexadecyl trimethyl ammonium bromide because hexadecyl trimethyl ammonium bromide has a dual role: (1) providing a bromine source, which is the same as potassium bromide; (2) acting as a template, which potassium bromide does not have; specifically, the amino group and bromide ion exist at the end of the structure of hexadecyl trimethyl ammonium bromide, which reacts with Bi2O2 + There is a non-bonding interaction (van der Waals force) between them, which finally makes the whole molecule exist in Bi2O2 + After the reaction is completed, the structure is ionized when washed with ultrapure water, and the hexadecyl trimethylamine is eluted; (3) Hexadecyl trimethyl ammonium bromide is more soluble in ethylene glycol. Comprehensive considerations show that hexadecyl trimethyl ammonium bromide has greater advantages.
[0036] Performance testing
[0037] Figure 1 The XRD spectrum of the bismuth-based photocatalyst prepared in Example 1-3. By comparing the XRD crystal library pdf card, it can be seen that BiOBr (characteristic peak: 31.7°, No.09-0393) and Cu2O (characteristic peak: 36.4°, No.01-078-2086) are present in the sample. This indicates that Cu2O is doped into BiOBr during the preparation process.
[0038] Figure 2 The degradation of sulfamethoxazole (SMX) by the bismuth-based photocatalytic materials of Examples 1-3 changes with the illumination time. The visible light Fenton-like catalytic activity of samples 10-CB, 20-CB and 40-CB was evaluated by the degradation of sulfamethoxazole (SMX) with an initial concentration of 2 mg / L. The experiment used 0.5 g / L of the example sample, and the reaction was carried out under the condition of neutral pH. The reaction was first carried out in the dark for 30 minutes to saturate the adsorption of pollutants by the bismuth-based photocatalytic material, and then hydrogen peroxide was added to make the initial concentration of hydrogen peroxide in the solution 5 mmol / L, and the reaction was carried out under the condition of >400 nm wavelength. Figure 2 The results show that the concentration of SMX changes with the illumination time during the visible light Fenton-like catalytic degradation process. The experiment shows that after 30 minutes of adsorption-desorption equilibrium, the photocatalytic material with the strongest adsorption capacity is 40-CB, with an adsorption efficiency of 40%. After 30 minutes of illumination, the photodegradation of SMX in the presence of 20-CB catalytic material is the largest, with a degradation efficiency of about 80%. In the H2O2-enhanced photocatalytic reaction, 20-CB has the strongest catalytic performance.
[0039] Figure 3The degradation process of sulfamethoxazole (SMX) by 20-CB under different conditions (visible light, hydrogen peroxide, visible light / hydrogen peroxide) is demonstrated. The experiment shows that under visible light / Fenton-like conditions, the performance of 20-CB catalytic material is the strongest, and the SMX degradation efficiency reaches more than 70% within 10 minutes. Therefore, it is determined that visible light combined with Fenton-like reaction conditions can enhance the catalytic performance of 20-CB material.
[0040] Figure 4 The degradation process of sulfamethoxazole (SMX) by 20-CB was demonstrated under different hydrogen peroxide concentrations, where the hydrogen peroxide concentration was 0-20mM. The experiment showed that the performance of 20-CB catalytic material was the strongest under the condition of hydrogen peroxide concentration of 5-20mM. Therefore, it was determined that the optimal concentration of hydrogen peroxide in the visible light Fenton reaction was 5mM.
[0041] The above results show that the cuprous oxide-doped BiOBr material prepared by this method has the best visible light Fenton-like catalytic degradation effect when the hydrogen peroxide concentration is 5mM, and can efficiently catalyze the degradation of pollutants in water bodies, and has good prospects for promotion and application.
[0042] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a bismuth-based photocatalytic material, characterized in that: The cuprous salt and the bismuth salt are dissolved in an organic solvent and mixed evenly to obtain a solution A; a bromine source is added to the solution A, and then the solution is heated for a period of time and freeze-dried to obtain the bismuth-based photocatalytic material; The feeding amount of the cuprous salt and the bismuth salt is calculated based on a molar ratio of Cu:Bi of 0.1 to 0.4; The bromine source is an ethylene glycol solution containing hexadecyltrimethylammonium bromide; The cuprous salt is cuprous nitrate; Add a bromine source to solution A, and heat the reaction at a temperature of 160°C-200°C for a reaction time of 8h-12h.
2. The method for preparing a bismuth-based photocatalytic material according to claim 1, characterized in that: The organic solvent is an ethylene glycol solution containing acetic acid.
3. The method for preparing a bismuth-based photocatalytic material according to claim 2, characterized in that: The volume fraction of the acetic acid in the ethylene glycol solution is 5-20%.
4. The method for preparing a bismuth-based photocatalytic material according to claim 1, characterized in that: The molar concentration of the hexadecyltrimethylammonium bromide in ethylene glycol is 0.1 mol / L.
5. The method for preparing a bismuth-based photocatalytic material according to claim 1, characterized in that: The bismuth salt is bismuth nitrate, bismuth chloride, bismuth acetate or bismuth sulfate.
6. A bismuth-based photocatalytic material obtained by the method according to any one of claims 1 to 5.
7. Use of the bismuth-based photocatalytic material as claimed in claim 6 in degrading water pollutants.
Citation Information
Patent Citations
Cu(I) modified photocatalytic material as well as preparation method and application thereof
CN106732630A
Iron modified photocatalytic material, preparation method and application thereof
CN108311164A
Preparation method and application of Fe(II) and / or Cu(II) modified photocatalytic material
CN109675591A